Lead acid battery

By providing cross-configured inner and outer convex strips on the isolation parts of the lead-acid battery, the problem of insufficient joint strength in the prior art is solved, the joint strength and penetration resistance of the lead-acid battery are improved, and the occurrence of short circuit and penetration short circuit is significantly reduced. Rate.

CN111316472BActive Publication Date: 2024-11-05GS YUASA INT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201880070741.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-10-31
Filing Date
2018-10-05
Publication Date
2024-11-05
Estimated Expiration
2038-10-05

AI Technical Summary

Technical Problem

In the conventional lead-acid batteries, sufficient bond strength cannot be obtained by forming convex strips on the joint surface of the spacer, resulting in a decrease in bond strength and a performance deviation.

Method used

The first and second convex strips in cross-configured configurations are provided on the first and second surfaces of the spacer so that they intersect at the joint to improve the joint strength, and by optimizing the pattern and spacing configuration of the convex strips, ensuring that The intersection of the inner and outer convex strips for higher bonding strength.

Benefits of technology

Through the cross-configured inner and outer convex strips, the bonding strength and permeability resistance of the lead-acid battery are significantly improved, and the incidence of the lower short circuit in the middle and lower vibration tests and the number of cycles of the permeability short circuit are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111316472B_ABST
    Figure CN111316472B_ABST
Patent Text Reader

Abstract

The present invention is a lead-acid battery having a bag-shaped separator, the separator having: a first surface and a second surface facing each other constituting the inner surface of the bag; a plurality of first ridges provided on the first surface and a plurality of second ridges provided on the second surface; a plurality of third ridges provided on the back side of the first surface constituting the outer surface of the bag, i.e., a third surface; a fourth surface constituting the outer surface of the bag, i.e., the back side of the first surface, i.e., the third surface, and the back side of the second surface; a plurality of third ridges provided on the third surface and a fourth ridge provided on the fourth surface; and a junction between the first surface and the second surface. At least one of the first ridges provided on the first surface and at least one of the second ridges provided on the second surface intersect at the junction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to lead storage batteries. Background Art

[0002] Lead-acid batteries are used for various purposes in addition to automotive and industrial applications. Lead-acid batteries include a negative electrode plate, a positive electrode plate, a separator interposed between the negative electrode plate and the positive electrode plate, and an electrolyte. The electrolyte generally uses a sulfuric acid aqueous solution.

[0003] Patent Document 1 discloses an example in which a negative electrode plate is housed in a bag-shaped polyethylene separator and convex strips are provided on the negative electrode plate side. In this example, the convex strips are formed inside the bag-shaped separator.

[0004] When the separator is formed into a bag shape, the separator is generally bent into a U-shape and the two side edges are joined. As a method for joining the two side edges, there can be cited a method using meshing sealing, heat sealing and ultrasonic sealing, or a method using an adhesive material or an adhesive tape (for example, refer to Patent Document 2).

[0005] Patent Document 1: Japanese Patent Application Publication No. 2015-22796

[0006] Patent Document 2: Japanese Patent Application Publication No. 2009-245901 Summary of the invention

[0007] In the production of the bag-shaped separator having convex lines formed inside as exemplified in Patent Document 1, when the separators are joined, separators having convex lines formed on the joining surfaces can be used.

[0008] However, when spacers having ridges formed on the joining surfaces are overlapped and joined, sufficient joining strength may not be obtained depending on the arrangement of the ridges.

[0009] One aspect of the present invention relates to a lead-acid battery, wherein a plurality of positive plates and a plurality of negative plates are stacked with a separator interposed therebetween and an electrolyte is contained in a battery cell chamber, wherein the separator is in the shape of a bag having an opening.

[0010] The separator comprises: a first surface and a second surface which are opposite to each other and constitute the inner surface of the bag; a plurality of first ridges arranged on the first surface and a plurality of second ridges arranged on the second surface;

[0011] a third surface which is the back side of the first surface and a fourth surface which is the back side of the second surface, constituting the outer surface of the bag; a plurality of third ridges provided on the third surface and a fourth ridge provided on the fourth surface; and

[0012] a junction between the first surface and the second surface,

[0013] At least one of the first ridges provided on the first surface and at least one of the second ridges provided on the second surface intersect at the joining portion.

[0014] According to the present disclosure, it is possible to improve the strength of the joint portion of the bag-shaped separator used in the lead-acid battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a diagram schematically showing the appearance of a separator used in a lead-acid battery according to one aspect of the present invention.

[0016] Figure 2 This is a schematic diagram showing a separator sheet before the lead-acid battery separator is processed into a bag shape.

[0017] Figure 3 It is a schematic diagram showing the state of the inner convex strip when the separator sheets are overlapped.

[0018] Figure 4 It means Figure 2 A schematic diagram showing a separator sheet before the lead acid battery separator is processed into a bag shape according to another embodiment.

[0019] Figure 5 It means Figure 2 A schematic diagram showing a separator sheet before the lead acid battery separator is processed into a bag shape according to another embodiment.

[0020] Figure 6 It means Figure 2 A schematic diagram showing a separator sheet before the lead acid battery separator is processed into a bag shape according to another embodiment.

[0021] Figure 7 This is a partially cutaway exploded perspective view showing the appearance and internal structure of a lead-acid battery according to one aspect of the present invention. DETAILED DESCRIPTION

[0022] The lead-acid battery involved in one aspect of the present invention is a lead-acid battery in which a plate group formed by stacking a plurality of positive plates and a plurality of negative plates with an insulator is contained in a battery cell chamber together with an electrolyte, and the insulator is in the shape of a bag with an opening. The insulator comprises: a first surface and a second surface that are opposite to each other and constitute the inner surface of the bag; and a plurality of first ridges arranged on the first surface and a plurality of second ridges arranged on the second surface. In addition, the insulator comprises: a third surface that is the back side of the first surface and a fourth surface that is the back side of the second surface that constitute the outer surface of the bag; and a plurality of third ridges arranged on the third surface and a fourth ridge arranged on the fourth surface. Furthermore, the insulator comprises a junction between the first surface and the second surface, and at least one of the first ridges arranged on the first surface intersects with at least one of the second ridges arranged on the second surface at the junction.

[0023] The separator has a first surface with a first convex strip facing a second surface with a second convex strip, and the first and second surfaces of the separator are joined to form a bag shape. A joint portion for stapling the first and second surfaces into a bag shape is formed on the end side of the separator.

[0024] Specifically, for example, a separator sheet is bent into two halves and superimposed into a U-shape, the bent portion is set as the lower end, and a joint is set on the left end side and the right end side to form a bag-shaped separator with an opening at the upper end. In addition, the right end (or left end) of the separator sheet can also be used as a bent portion, and a joint is formed on the left end side (or right end side) and the lower end side to form a bag-shaped. In addition, two separator sheets can also be overlapped, and a joint is formed on the left end side, the right end side, and the lower end side to form a bag-shaped. In this case, the bag-shaped separator has a roughly quadrilateral shape. The outer shape of the separator is not limited to a quadrilateral, and can also be any shape (for example, a polygon or an arc shape, etc.). The sides constituting the polygon do not need to be strictly straight lines, and can also have curved parts and curved parts. For example, in the case of a bag-shaped separator whose outer shape is roughly triangular by bending, the joint only needs to be set on one end side corresponding to one side of the triangle.

[0025] Here, in the bag-shaped separator, the direction in which the opening for inserting the positive electrode plate or the negative electrode plate is provided is defined as the upper side (vertical direction) of the separator, and the opposite side is defined as the lower side. In addition, when defining the upper and lower sides of the separator in this way, the direction on the left side is defined as the left side of the separator, and the direction on the right side is defined as the right side of the separator.

[0026] The convex stripes are protruding portions protruding from one side of the separator, and are provided to inhibit close contact between the separator and the electrode plate, and to inhibit damage and / or permeation short circuit caused by oxidation degradation of the separator. The convex stripes are provided on the surface of the separator in a predetermined pattern.

[0027] The first surface and the second surface of the separator constitute the inner surface of the bag facing each other. Preferably, the separator has a joint area and a plate area. The joint area is an area including a joint portion that stitches the first surface and the second surface into a bag shape, and is set to be wider than the joint portion in consideration of the positioning margin related to the joint. Preferably, the joint area is arranged on the end side of the separator, and the peripheral area within a prescribed distance from the end can be used as the joint area. In contrast, the plate area is an area separated from the joint area, and is an area opposite to the positive plate or the negative plate when the positive plate or the negative plate is accommodated in the separator.

[0028] In the case where the joining region is provided on the end side of the isolating member, the joining portion is preferably provided in a manner including the end. Alternatively, within the joining region, the joining portion may be formed to extend parallel to the contour of the end of the isolating member, or may be formed to extend in any contour shape different from the contour of the end of the isolating member.

[0029] A plurality of first ridges are provided on the first surface of the separator, and a plurality of second ridges are provided on the second surface of the separator. The first ridges are formed in the electrode plate region on the first surface, thereby preventing the electrode plate of either the positive electrode plate or the negative electrode plate from being in close contact with the first surface. Similarly, the second ridges are formed in the electrode plate region on the second surface, thereby preventing the electrode plate of either the positive electrode plate or the negative electrode plate from being in close contact with the second surface. The first ridges provided in the electrode plate region and the second ridges are formed on the inner surface of the bag-shaped separator, preventing damage and / or penetration short circuit caused by oxidation degradation of the separator when accommodating the positive electrode plate or the negative electrode plate. Hereinafter, the first ridges and the second ridges are collectively referred to as "inner ridges".

[0030] Generally speaking, the first convex stripes and the second convex stripes are arranged in a linear pattern so that the plurality of convex stripes are parallel to adjacent convex stripes in a predetermined area and have a certain interval therebetween.

[0031] The first convex strip and the second convex strip (inner convex strip) are also formed in the joining area on the first surface and the second surface. In the case where the inner convex strip is formed in the joining area, the first convex strip on the first surface and the second convex strip on the second surface can overlap when joining. However, according to this overlapping method, there is a case where sufficient joining strength cannot be obtained.

[0032] For example, at the joint of the first face and the second face, the second convex strip can be embedded in the valley between the adjacent first convex strips (or the first convex strip can be embedded in the valley between the adjacent second convex strips). In this case, compared with the situation where the first convex strip and the second convex strip overlap, the bonding strength is reduced. In particular, in the case of crimping methods such as meshing seals, the reduction trend of bonding strength becomes larger. However, considering the positioning accuracy of the joint based on the joint device, it is difficult to completely prevent the second convex strip from being embedded in the valley between the first convex strip (or the first convex strip from being embedded in the valley between the second convex strip), which becomes one of the reasons for the deviation of bonding strength. As a result, the performance of the lead-acid battery also produces deviations.

[0033] This is a common problem when an inner convex strip is provided, and it has nothing to do with whether it is welded or bonded, but it is particularly significant in a method of joining by compressing the joint portion to a specified thickness, such as a meshing sealing method or a heat welding method, because the convex strip of one of the first and second convex strips is embedded between the grooves of the convex strip of the other convex strip, so that the thickness of the joint portion before crimping is thinner than the assumed thickness. As a result, the compression rate when compressed to the specified thickness is reduced, which easily leads to a reduction in the joint strength.

[0034] Therefore, in one aspect of the present invention, the arrangement pattern of the inner convex stripes is studied, and at least one of the first convex stripes provided on the first surface and at least one of the second convex stripes provided on the second surface intersect at the joint portion. By arranging the inner convex stripes in a manner that the first convex stripes intersect the second convex stripes, it is possible to suppress the embedding of other convex stripes in the valleys between adjacent convex strips.

[0035] Here, the "intersection" of the first ridge and the second ridge refers to a state in which the first surface and the second surface are opposite and the first ridge and the second ridge are in at least point contact. The first ridge and the second ridge may also be in line or surface contact. In addition, the portion that is in at least point contact is not limited to one place. The linear pattern of the ridge may be a straight line or a curve. In addition, it may be a dotted line in which a part of the straight line or curve is missing. From the perspective of ease of manufacturing the ridge, the pattern of the ridge is preferably a stripe-shaped pattern composed of a plurality of ridges composed of respectively parallel straight lines. Regarding the angle at which the first ridge and the second ridge intersect, the pattern of the first ridge and the pattern of the second ridge may intersect at an angle preferably of 0.2° or more, more preferably of 0.3° or more. If the intersection angle is 0.2° or more, sufficient bonding strength is obtained.

[0036] According to the method for forming the joint, it is also considered that it is difficult to judge whether the first ridge and the second ridge intersect in the joint according to the state of the joint. Even in this case, it is possible to infer whether the first ridge and the second ridge intersect in the joint according to the configuration of the first ridge and the second ridge in the peripheral area of ​​the joint. For example, in the joint area, when the first ridge and the second ridge are respectively formed in a plurality of linear shapes extending in a certain direction at a certain interval, it can be inferred that in the joint, the first ridge and the second ridge are also formed in a linear shape extending in the same direction as the extension direction of the ridge in the joint area at the same ridge interval as the ridge interval in the joint area. That is, the intersection of the first ridge and the second ridge can be inferred from the ridge pattern in the peripheral area of ​​the joint by interpolating or extrapolating the ridge pattern in the joint.

[0037] Preferably, when the first ridge is set as a linear pattern extending in the first direction in the peripheral area (joining area) on the first surface of the joint, the second ridge can be set as a linear pattern extending in a second direction different from the first direction in the peripheral area (joining area) on the second surface of the joint. By making the second ridge extend in a direction different from the first ridge and in a direction inclined relative to the first ridge, the intersection of the first ridge and the second ridge is easy to occur in the joint. As a result, the deviation of the joint strength can be reduced, thereby maintaining the joint strength.

[0038] In addition, in this case, from the perspective of the ease of processing the convex stripes, it is preferred that the first convex stripes in the electrode plate region also extend in the same direction as the first convex stripes in the junction region. Similarly, from the perspective of the ease of processing the convex stripes, it is preferred that the second convex stripes in the electrode plate region extend in the same direction as the second convex stripes in the junction region.

[0039] Preferably, the first ridges include a plurality of first joining ridges arranged at a certain interval in the joining region on the first surface, and a plurality of first pole plate ridges arranged at a certain interval in the pole plate region on the first surface. In this case, the intervals at which the first joining ridges are set may be narrower than the intervals at which the first pole plate ridges are set. Thus, more first ridges can intersect with the second ridges in the joining region.

[0040] Similarly, the second convex strips preferably include a plurality of second joining convex strips arranged at a certain interval in the joining area on the second surface, and a plurality of second electrode plate convex strips arranged at a certain interval in the electrode plate area on the second surface. In this case, the interval at which the second joining convex strips are set can also be narrower than the interval at which the second electrode plate convex strips are set. Thus, the first convex strips can intersect with more second convex strips in the joining area.

[0041] By increasing the number of intersections between the first ridges and the second ridges in the joint portion, the joint strength can be maintained high.

[0042] Preferably, the separator has a plurality of third ridges arranged on the back side of the first surface constituting the outer surface of the bag, that is, the third surface. In addition, more preferably, the separator has a plurality of fourth ridges arranged on the back side of the second surface constituting the outer surface of the bag, that is, the fourth surface. The third ridges and the fourth ridges inhibit the other side of the positive plate and the negative plate that is not contained in the bag of the separator from adhering closely to the separator. The third ridges and the fourth ridges arranged in the plate area are formed on the outer surface of the bag-shaped separator to inhibit the damage and / or penetration short circuit caused by the oxidation degradation of the separator caused by contact with any other plate. Hereinafter, the third ridges and the fourth ridges are collectively referred to as "external ridges".

[0043] The performance of the battery can be improved by providing a bag-shaped separator with inner and outer convex strips. However, in this case, in order to maintain high charge and discharge characteristics, the total thickness of the separator needs to be suppressed, and the thickness of the base part of the separator has to be thinned. As a result, the bonding strength of the ends of the separator is easily reduced, and the problem of bonding strength deviation becomes more serious.

[0044] The third ridge may also be provided in an area on the third surface corresponding to the joining area on the first surface (i.e., an area on the back side of the joining area on the first surface). In addition, the fourth ridge may also be provided in an area on the fourth surface corresponding to the joining area on the second surface (i.e., an area on the back side of the joining area on the second surface). In this case, when the joining is formed by crimping or the like, the third ridge or the fourth ridge (outer ridge) is also compressed together. Thus, the compression rate can be increased and the joining strength can be enhanced. On the other hand, the deviation in the joining strength becomes more significant with the deviation in the positioning of the joining end. However, by configuring the inner ridge in such a manner that the first ridge intersects with the second ridge, it is possible to suppress the embedding of another ridge between the valleys between adjacent ridges, and the joining strength can be maintained at a high level.

[0045] In this way, in the joint portion of the bag-shaped separator, the first convex strip and the second convex strip are crossed, so that the joint strength can be maintained. The method of achieving the above effect is not limited to the crimping method using meshing seal, and the effect can also be obtained in heat welding and the like. In these cases, the separator forms a joint using crimping or a joint using welding at the joint portion.

[0046] The bag-shaped separator is effective when the bag-shaped separator accommodates the negative electrode plate, and can improve the resistance to short circuiting due to permeation.

[0047] Hereinafter, the lead-acid battery involved in the embodiment of the present invention, in particular, the form of the separator will be described in detail with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments. In addition, in the following drawings, the inner convex strips in the joint area of ​​the separator are emphasized, and there is a situation where the structural ratio of each part of the actual separator is inconsistent with the structural ratio of each part corresponding to the accompanying drawings.

[0048] Figure 1 A schematic diagram showing a bag-shaped separator used in a lead-acid battery according to an embodiment of the present invention, viewed from the outside of the bag, is shown. Figure 2 Schematically indicating that Figure 1 The separator 100 is a separator sheet before being processed into a bag shape. The separator 100 includes a bag-shaped base 101 made of a microporous film, inner convex strips 102a to 102d protruding from the inner surface (first surface or second surface) of the base 101, and outer convex strips 104a and 104b protruding from the outer surface (third surface) of the base 101. However, the inner convex strips 102a to 102d are located inside the bag-shaped separator and are therefore not Figure 1 When the negative electrode plate is housed in the separator 100, the inner convex strips 102a to 102d are located on the negative electrode plate side, and the outer convex strips 104a and 104b are located on the positive electrode plate side. When the positive electrode plate is housed in the separator 100, the outer convex strips 104a and 104b are located on the negative electrode plate side, and the inner convex strips 102a to 102d are located on the positive electrode plate side. Both the structure in which the negative electrode plate is housed in the separator 100 and the structure in which the positive electrode plate is housed in the separator 100 are possible.

[0049] The separator 100 may be formed of a polymer material. At least the base is a porous sheet, which may also be called a porous film. The separator 100 may contain a filler (e.g., a particulate filler such as silicon dioxide and / or a fibrous filler) dispersed in a matrix formed of a polymer material. The separator 100 is preferably made of an acid-resistant polymer material. As such a polymer material, polyolefins such as polyethylene and polypropylene are preferred.

[0050] The average thickness of the base 101 is, for example, 0.15 mm or more and 0.3 mm or less, preferably 0.18 mm or more and 0.27 mm or less. When the average thickness of the base is within such a range, it is easy to maintain the charge-discharge characteristics at a high level while ensuring the height of the inner convex strips and the height of the outer convex strips as required. The average thickness of the base is obtained by measuring the thickness of the base at five arbitrarily selected locations in the cross-sectional photograph of the separator and averaging the measured values.

[0051] The separator 100 has a plate region 106, a bonding region 108a provided at the left end of the separator, and a bonding region 108b provided at the right end of the separator. The bonding regions 108a and 108b respectively form bonding (bonding portions) 109a and 109b between the first surface and the second surface.

[0052] On the first and second surfaces of the electrode region 106, inner convex strips 102a (first electrode convex strips) and inner convex strips 102b (second electrode convex strips) are provided (refer to Figure 2 to Figure 5 ), an outer convex strip 104a is provided on the third surface of the plate region 106. When a lead-acid battery is constructed, in the plate region 106, the separator 100 is opposite to the positive plate or the negative plate. At this time, the inner convex strips 102a, 102b and the outer convex strip 104a prevent the base 101 from directly contacting the positive plate or the negative plate. On the other hand, an inner convex strip 102c (first joining convex strip) and an inner convex strip 102d (second joining convex strip) are provided on the first and second surfaces of the joining regions 108a, 108b (refer to Figure 2 to Figure 5 ). In addition, an outer convex strip 104b is provided on the third surface of the joint regions 108a and 108b.

[0053] Figure 1 The separator 100 shown is formed by folding a separator sheet having inner convex strips 102a to 102d and outer convex strips 104a and 104b formed in advance into two halves into a U shape, and joining the left end side and the right end side by a method such as meshing sealing. Figure 2 The schematic diagram shows a separator sheet 110 that is folded in half and formed before joining at the left and right end sides. Figure 2 This is a schematic diagram of the separator sheet viewed from the first and second surfaces on which the inner convex lines 102a to 102d are formed. The outer convex lines 104a and 104b are not shown in the figure because they exist on the back surface.

[0054] like Figure 2 As shown, the electrode area 106 on the first surface is provided with an inner convex stripe 102a, and the electrode area 106 on the second surface is provided with an inner convex stripe 102b. The first surface of the bonding area 108a, 108b is provided with an inner convex stripe 102c, and the second surface of the bonding area 108a, 108b is provided with an inner convex stripe 102d. The inner convex stripes 102a to 102d are formed into a linear stripe pattern at a predetermined interval in a direction parallel to the long side of the isolation sheet. Figure 2 In the embodiment, the ridge intervals of the inner ridges 102 c and 102 d provided in the bonding regions 108 a and 108 b are made narrower than the ridge intervals of the inner ridges 102 a and 102 b provided in the electrode region 106 .

[0055] In this embodiment, Figure 2The isolation sheet shown is bent to form Figure 1 In the case of the bag-shaped separator 100 shown in FIG. 1 , the separator sheet is not bent with the direction X parallel to the short side of the separator sheet as the axis, but is bent as shown in FIG. Figure 2 As shown by the dot-dash line, the separator sheet is bent in a direction Y slightly deviated from the direction parallel to the short side as an axis, and the left and right end sides of the bonding areas 108a and 108b are bonded. As a result, when the first surface and the second surface are placed opposite to each other to form a bag-shaped separator, the inner convex strips 102a to 102d extend in a direction slightly inclined from the vertical direction. In addition, the inner convex strips 102a and 102c on the first surface and the inner convex strips 102b and 102d on the second surface extend obliquely from the vertical direction in opposite directions to each other, so when the first surface and the second surface are placed opposite to each other, the inner convex strips 102c and the inner convex strips 102d can be made to intersect in each bonding area 108a and 108b. At this time, the inner convex strips 102a and the inner convex strips 102b also intersect in the electrode area 106. Moreover, the bonding is formed in the area where at least one inner convex strip 102c and the inner convex strip 102d intersect in the bonding areas 108a and 108b.

[0056] When the left and right end sides of the joining regions 108a and 108b are joined, the inner convex strips 102c and the inner convex strips 102d intersect at the joining portion, thereby easily preventing an inner convex strip 102c from being embedded in the valleys between the inner convex strips 102d provided at a predetermined interval on the second surface, or an inner convex strip 102d from being embedded in the valleys between the inner convex strips 102c provided at a predetermined interval on the first surface. As a result, the deviation in the joining strength can be reduced and the joining strength can be maintained.

[0057] Figure 3 The figure shows the state of the inner convex strip of the separator sheet in the joint area 108a when the first surface and the second surface are facing each other. Figure 3 In order to avoid complicating the record, the record of the outer convex strip is omitted.

[0058] In the Figure 2 When the isolation sheet shown in FIG. 1 is bent into two halves, when the bending axis deviates from the direction X parallel to the short side of the isolation sheet and the deviation angle is small, according to the positional relationship between the inner convex strips 102c and 102d, as shown in FIG. Figure 3 As shown in (a), there is a case where the inner convex stripes 102c and the inner convex stripes 102d do not overlap. In this case, the inner convex stripes 102d are embedded in the valleys between the inner convex stripes 102c, and the inner convex stripes 102c are embedded in the valleys between the inner convex stripes 102d.

[0059] On the other hand, in the case of a large deviation angle, such as Figure 3As shown in (b), the inner convex ridges 102c and 102d intersect with each other regardless of the positional relationship between the inner convex ridges 102c and 102d. In this case, the joining strength can be maintained high.

[0060] When the separator sheet is bent in half, even if the deviation angle of the bending axis is the same, the relative position of the inner convex strip 102d with respect to the inner convex strip 102c in the left-right direction will deviate depending on the position of the separator sheet being bent (the position in the long side direction of the separator sheet). Even when the deviation angle is small, a separator sheet in which the inner convex strip 102c intersects with the inner convex strip 102d can be obtained. However, depending on the bending position, the inner convex strip 102c intersects with the inner convex strip 102d and the inner convex strip 102d do not intersect. Figure 3 Both (a) and (b) may occur, so the bonding strength may vary. However, compared with the case where the separator sheet is bent about the X axis, the variation in bonding strength can be reduced.

[0061] The interval at which the inner convex strip 102d is set is set as D, and the length of the inner convex strip 102d is set as L. If the angle of deviation of the axis Y of the bent isolation sheet from the direction X parallel to the short side is set as θ, the inner convex strip 102c and the inner convex strip 102d are inclined only by θ in the opposite directions, so the intersection angle becomes 2θ. In this case, when tan2θ≥D / L is satisfied, the inner convex strip 102c and the inner convex strip 102d can be reliably crossed at one or more positions, the bonding strength can be improved, and the deviation of the bonding strength can be maintained low. In this case, if the width of the joint portion from the end of the isolation sheet is set in a manner including the inner convex strip 102d located at the second position from the end side, the joint portion includes at least one intersection of the inner convex strip 102c and the inner convex strip 102d. If the distance from the inner convex strip 102d located at the end side to the end is set as W, the joint portion including the end portion can be set in an area with a width of more than D+W. In order to prevent the generation of unjoined portions, the width of the joint portion is preferably set to exceed the deviation of the end of the separator (the length of the end of the separator on the joint portion side when folded in half is set to L). 2 , L 2 tan2θ).

[0062] Figure 4 , Figure 5 It means Figure 2 Schematic diagram of the morphology of different isolation sheets. Figure 4 In the isolation sheet 111 shown, the inner convex strips 102a to 102d are not as good as those in FIG. Figure 2In this case, if the separator sheet is bent with the direction parallel to the short side of the separator sheet as the axis, the inner convex strips 102a and 102c on the first surface and the inner convex strips 102b and 102d on the second surface extend obliquely from the vertical direction in opposite directions to each other. Therefore, when the first surface and the second surface are placed opposite to each other and the joint is formed on the left and right end sides, the inner convex strips 102c and the inner convex strips 102d can be made to cross in the joint portion in the joint area 108a and 108b. In addition, at this time, in the electrode area 106, the inner convex strips 102a and the inner convex strips 102b cross.

[0063] exist Figure 4 In the embodiment, the axis for folding the isolation sheet 111 in half may be as follows: Figure 2 The inner convex strips 102c and 102d are inclined from the direction parallel to the short side of the separator sheet as shown in the figure. The angle at which the inner convex strips 102c and 102d intersect can be further increased, and the inner convex strips 102c and 102d intersect easily in the joint.

[0064] Figure 5 The inner convex stripes 102c and 102d in the bonding area of ​​the separator sheet 112 shown are not formed as straight lines, but are formed as a stripe pattern of a curve that undulates and extends substantially in the vertical direction. In this case, if the separator sheet is bent with the direction parallel to the short side of the separator sheet as an axis so that the first surface and the second surface face each other, one inner convex stripe 102c can intersect with one or more inner convex stripes 102d at multiple locations in the bonding areas 108a and 108b. In addition, one inner convex stripe 102d can intersect with one or more inner convex stripes 102c at multiple locations. Since the number of intersections increases, the deviation of the bonding strength can be further reduced, and the high bonding strength can be maintained.

[0065] For the average height of the inner convex strips in the joint area, it is preferably 0.05 mm or more from the perspective of the puncture strength at the end, and preferably 0.5 mm or less from the perspective of suppressing poor joining caused by insufficient joining energy, etc. For the average height of the inner convex strips in the plate area, in the case of being opposite to the positive plate, in order to suppress oxidative degradation, it is preferably 0.3 mm or more, and in the case of being opposite to the negative plate, in order to suppress penetration short circuit, it is preferably 0.05 mm or more. On the other hand, from the perspective of maintaining the charge and discharge characteristics higher, the average height of the inner convex strips in the plate area is preferably 0.5 mm or less. In addition, the height of the inner convex strips refers to the distance from one main surface (first surface or second surface) of the base (separating sheet) at the specified position of the inner convex strips to the top of the inner convex strips. The average height of the inner convex strips is obtained by averaging the height of the inner convex strips measured at ten locations of the inner convex strips arbitrarily selected on one main surface of the base.

[0066] exist Figure 2 to Figure 5 In the example, the pattern of the inner convex stripes 102a to 102d is a stripe pattern. However, the pattern of the inner convex stripes is not particularly limited. The inner convex stripes can be formed randomly, and can be formed in a stripe shape, a curve shape, a grid shape, etc. In addition, as Figure 5 As shown, the pattern of the inner convex stripes may also be different in the electrode area and the joint area. From the viewpoint of easier diffusion of the electrolyte, it is preferred that a plurality of inner convex stripes are formed in a striped manner on at least the electrode plate on the first side or the second side. There is no particular restriction on the orientation of the striped inner convex stripes. For example, a plurality of inner convex stripes may also be formed along the height direction and the width direction. From the viewpoint of suppressing the increase in internal resistance caused by the retention of gas generated during charging, it is preferred that the plurality of inner convex stripes be formed in stripes along the height direction. On the other hand, from the viewpoint of suppressing the precipitation of high-concentration sulfuric acid generated during charging and suppressing stratification, it is preferred that the plurality of inner convex stripes be formed in stripes along the width direction. In addition, the height direction refers to the direction in which the opening of the bag-shaped separator is located, and the width direction refers to the direction perpendicular to the height direction.

[0067] Figure 6 It means Figure 2 , Figure 4 as well as Figure 5 Schematic diagram of the morphology of different separator sheets. Figure 6 This is a diagram of observing the isolation sheet 114 from the third side (fourth side), and by folding the right triangle area on the upper right side back to the paper side, the state of the first side (second side) side is shown together. The isolation sheet 114 is folded in half (mountain fold) in a manner that the paper side of the isolation sheet 114 is the outer surface and the back side of the paper is the inner surface, forming a bag-shaped isolation piece. At this time, one side of the mutually opposing inner surfaces of the folded isolation sheet 114 constitutes the first side, and the other side constitutes the second side. The outer surface of the folded isolation sheet 114 located on the back side of the first side constitutes the third side, and the outer surface located on the back side of the second side constitutes the fourth side.

[0068] exist Figure 6 In the isolation sheet 114 shown, a plurality of outer convex stripes 104a and 104b are formed in a stripe-like arrangement in the height direction. On the other hand, a plurality of inner convex stripes 102e are formed in a stripe-like arrangement in the width direction. The spacing of the inner convex stripes 102e is the same in both the joint area and the plate area. On the other hand, the spacing of the outer convex stripes 104b in the joint area is made narrower than the spacing of the outer convex stripes 104a in the plate area. The isolation sheet 114 is suitable for the case where the negative electrode plate is accommodated in a bag-shaped isolation member. The isolation sheet 114 is also formed by bending the isolation sheet with a direction Y slightly deviated from the direction parallel to the short side of the isolation sheet as an axis to form a joint portion, so that the opposing inner convex strips 102e can cross each other.

[0069] By using Figure 2 and Figures 4 to 6 The separator sheet shown may have a plurality of inner convex strips extending in a direction slightly inclined from the height direction of the bag-shaped separator or in a direction slightly inclined from the width direction. Even in this case, the above-mentioned effect can be obtained.

[0070] From the viewpoint of puncture strength, oxidation resistance, and permeation short circuit resistance, the spacing of the stripe-shaped or grid-shaped inner ridges in the electrode area is preferably 0.5 mm or more and 10 mm or less. For example, the inner ridges are preferably formed at such spacing over 70% or more of the electrode area.

[0071] In contrast, the spacing of the inner convex stripes in the junction area is denser than that in the electrode area, so that the inner convex stripes can be reliably crossed and the number of crossing parts can be increased, which is preferred. Specifically, the spacing of the stripe-shaped or grid-shaped inner convex stripes in the junction area is narrower than that of the inner convex stripes in the electrode area, preferably 0.5 mm or more and 2.0 mm or less.

[0072] In addition, the interval between the inner convex lines refers to the distance between the tops of adjacent first convex lines or second convex lines (more specifically, the distance between the centers of adjacent inner convex lines in a direction crossing the inner convex lines).

[0073] For the average height of the outer convex strips, in the electrode area, when facing the positive electrode, in order to suppress oxidative degradation, it is preferably 0.3 mm or more, and when facing the negative electrode, in order to suppress penetration short circuit, it is preferably 0.05 mm or more. On the other hand, from the viewpoint of maintaining the charge and discharge characteristics higher, the average height of the outer convex strips in the electrode area is preferably 0.5 mm or less. For the average height of the outer convex strips in the junction area, from the perspective of the puncture strength at the end, it is preferably 0.05 mm or more, and from the perspective of suppressing poor bonding caused by insufficient bonding energy, it is preferably 0.5 mm or less.

[0074] The average height of the outer ridges is determined from the inner ridges. The height of the outer ridges is the distance from the outer surface (third surface or fourth surface) of the base at a predetermined position of the outer ridges to the top of the outer ridges.

[0075] The pattern and direction of the outer convex strips are not particularly limited, as are the inner convex strips. For example, the inner convex strips can be selected from the above-mentioned inner convex strips. From the viewpoint of puncture strength, oxidation resistance, and resistance to permeation short circuit, the spacing of the stripe-shaped or grid-shaped outer convex strips in the electrode area is preferably 0.5 mm or more and 10 mm or less. For example, it is preferred that the outer convex strips with such spacing are formed on more than 70% of the area of ​​the electrode area.

[0076] In contrast, from the perspective of increasing the compression rate when joining using a crimping method or the like and improving the joining strength, the spacing between the outer ridges in the joining area is narrower than the spacing between the outer ridges in the electrode area, preferably being greater than 0.5 mm and less than 2.0 mm.

[0077] In addition, the interval between the outer convex lines refers to the distance between the tops of the adjacent third convex lines or fourth convex lines (more specifically, the distance between the centers of the adjacent outer convex lines in the direction crossing the outer convex lines).

[0078] Unless otherwise specified, the above-mentioned ranges of the spacing and height of the inner convex strips and the spacing and height of the outer convex strips are preferred ranges, especially when the separator accommodates the negative electrode plate. When the separator accommodates the positive electrode plate, as the range of the spacing and height of the inner convex strips in the electrode plate region, the above-mentioned range of the spacing and height of the outer convex strips in the electrode plate region can be selected, and as the range of the spacing and height of the outer convex strips in the electrode plate region, the above-mentioned range of the spacing and height of the inner convex strips in the electrode plate region can be selected.

[0079] The separator is obtained, for example, by extruding a resin composition containing a pore-forming agent (solid pore-forming agent such as polymer powder and / or liquid pore-forming agent such as oil) and a polymer material into a sheet, removing the pore-forming agent, and forming pores in the matrix of the polymer material. The convex stripes can be formed, for example, during extrusion molding, or by transferring using a roller having grooves corresponding to the convex stripes after molding into a sheet or removing the pore-forming agent. When a filler is used, it is preferably added to the resin composition.

[0080] Hereinafter, each main component of the lead-acid battery according to the embodiment of the present invention will be described in detail, but the present invention is not limited to the following embodiments. In addition, as the separator of the lead-acid battery, the separator of the present embodiment described above is used, so the components other than the separator will be described.

[0081] (Electrolyte)

[0082] The electrolyte is an aqueous solution containing sulfuric acid. The electrolyte can be gelled as needed. The electrolyte can contain additives used in lead-acid batteries as needed.

[0083] The specific gravity of the electrolyte in a fully charged lead-acid battery after chemical conversion at 20°C is, for example, 1.10 g / cm 3 Above and 1.35g / cm 3 the following.

[0084] (Positive plate)

[0085] The positive plates of lead-acid batteries are of two types: pasted type and clad type.

[0086] The paste-coated positive plate comprises a positive current collector and a positive electrode material. The positive electrode material is held by the positive current collector. In the paste-coated positive plate, the positive electrode material is the portion of the positive plate from which the positive current collector is removed. The positive current collector can be formed in the same manner as the negative current collector, and can be formed by casting lead or a lead alloy, or by processing a lead or a lead alloy sheet.

[0087] The clad positive plate comprises a plurality of porous tubes, a core metal inserted into each tube, a positive electrode material filled in the tubes into which the core metal is inserted, and a connection base connecting the plurality of tubes. In the clad positive plate, the positive electrode material is the portion of the positive plate from which the tubes, the core metal and the connection base are removed.

[0088] As the lead alloy used in the positive electrode collector, Pb-Ca alloy and Pb-Ca-Sn alloy are preferred from the aspects of corrosion resistance and mechanical strength. The positive electrode collector may have lead alloy layers with different compositions, and the alloy layers may also be multiple. Pb-Ca alloy and Pb-Sb alloy are preferably used for the core.

[0089] The positive electrode material includes a positive electrode active material (lead dioxide or lead sulfate) that develops capacity through an oxidation-reduction reaction. The positive electrode material may contain other additives such as antimony (Sb) as needed.

[0090] The unconverted pasted positive electrode plate is obtained by filling a positive electrode paste into a positive electrode collector, aging, and drying the positive electrode paste, depending on the negative electrode plate. The positive electrode paste is prepared by kneading lead powder, additives, water, sulfuric acid, and the like.

[0091] The non-chemically converted clad positive electrode plate is formed by filling a tube into which a core metal is inserted with a mixture of an additive and lead powder or lead powder in a slurry form as required, and connecting a plurality of tubes with a connecting base.

[0092] Thereafter, the positive electrode plate which has not been chemically converted is chemically converted to form a positive electrode plate.

[0093] (Negative plate)

[0094] The negative plate of the lead-acid battery is composed of a negative electrode collector and a negative electrode material. The negative electrode material is the portion of the negative electrode plate from which the negative electrode collector is removed. The negative electrode collector can be formed by casting lead (Pb) or a lead alloy, or by processing a lead or lead alloy sheet. As a processing method, for example, a drawing process and a punching process can be cited.

[0095] The lead alloy used in the negative electrode current collector may be any one of a Pb-Sb alloy, a Pb-Ca alloy, and a Pb-Ca-Sn alloy. These lead or lead alloys may further contain at least one selected from Ba, Ag, Al, Bi, As, Se, Cu, etc. as an additive element.

[0096] The negative electrode material contains a negative electrode active material (lead or lead sulfate) that develops capacity through a redox reaction, and may contain a shrinkage preventer, a carbonaceous material such as carbon black, barium sulfate, and other additives as necessary.

[0097] The active material of the negative electrode in the charged state is spongy lead, but the negative plate that has not been chemically converted is usually made of lead powder.

[0098] The negative electrode plate can be formed by filling a negative electrode paste into a negative electrode collector, aging and drying to produce a non-chemically converted negative electrode plate, and then chemically converting the non-chemically converted negative electrode plate. The negative electrode paste is produced by adding water and sulfuric acid to lead powder, an organic shrink-proofing agent, and various additives used as needed, and kneading them.

[0099] The chemical conversion can be carried out by accommodating the unconverted positive and negative electrode groups in the electrolytic cell of the lead-acid battery. It is also possible to carry out the chemical conversion in the electrolytic cell by injecting electrolyte after the battery cells are connected and the lids are welded as needed. In addition, the lead-acid battery or the electrode group can be assembled after the chemical conversion of the positive and negative plates is respectively carried out.

[0100] Figure 7 The external appearance of an example of a lead acid battery according to an embodiment of the present invention is shown.

[0101] The lead-acid battery 1 includes an electrolytic cell 12 for storing a plate group 11 and an electrolyte (not shown). The electrolytic cell 12 is divided into a plurality of battery cell chambers 14 by a partition wall 13. Each battery cell chamber 14 contains a plate group 11. The opening of the electrolytic cell 12 is sealed by a cover 15 having a negative terminal 16 and a positive terminal 17. A liquid port plug 18 is provided on the cover 15 for each battery cell chamber. When replenishing water, the liquid port plug 18 is removed and replenished with replenishing liquid. The liquid port plug 18 may also have the function of discharging the gas generated in the battery cell chamber 14 to the outside of the battery.

[0102] The electrode group 11 is formed by stacking a plurality of negative plates 2 and positive plates 3 respectively with a separator 4 interposed therebetween. Here, a bag-shaped separator 4 containing a negative plate 2 is shown, but the bag-shaped separator 4 may also contain a positive plate 3. In the battery cell chamber 14 located at one end of the electrolytic cell 12, a negative electrode frame 6 connecting a plurality of negative plates 2 in parallel is connected to a through connector 8, and a positive electrode frame 5 connecting a plurality of positive plates 3 in parallel is connected to a positive electrode column 7. The positive electrode column 7 is connected to a positive electrode terminal 17 on the outside of the cover 15. In the battery cell chamber 14 located at the other end of the electrolytic cell 12, a negative electrode column 9 is connected to the negative electrode frame 6, and a through connector 8 is connected to the positive electrode frame 5. The negative electrode column 9 is connected to a negative electrode terminal 16 on the outside of the cover 15. Each through connector 8 connects the electrode group 11 of the adjacent battery cell chambers 14 in series through a through hole provided in the partition 13.

[0103] [Example]

[0104] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0105] 《Lead-acid battery A1》

[0106] (1) Production of negative electrode plate

[0107] Lead powder, water, dilute sulfuric acid, carbon black, and an organic shrinkage-proofing agent are mixed to obtain a negative electrode paste. The negative electrode paste is filled into the mesh of a Pb-Ca-Sn alloy expanded mesh grid as a negative electrode current collector, aged and dried to obtain a negative electrode plate that is not chemically converted. Sodium lignin sulfonate is used as an organic shrinkage-proofing agent. The amount of carbon black and the organic shrinkage-proofing agent added is adjusted so that each of the contents contained in 100% by mass of the negative electrode material is 0.2% by mass, and the negative electrode paste is prepared.

[0108] (2) Production of positive electrode plates

[0109] Lead powder, water and sulfuric acid are kneaded to prepare a positive electrode paste, which is filled into the mesh of a Pb-Ca-Sn alloy expanded grid as a positive electrode current collector, aged and dried to obtain a non-chemically converted positive electrode plate.

[0110] (3) Fabrication of Isolators

[0111] A separator A is formed by folding a separator sheet made of a polyethylene microporous film and having convex strips on both sides in half, and joining the left and right ends. Figure 2In the separator sheet shown, the spacing of the inner convex strips is set to 2.0 mm in the electrode area, 1.0 mm in the bonding area (the peripheral area of ​​5 mm from the left and right ends), and the height of the inner convex strips is set to 0.1 mm in both the electrode area and the bonding area. In addition, the spacing of the outer convex strips is set to 8.0 mm in the electrode area and 1.0 mm in the bonding area, and the height of the outer convex strips is set to 0.4 mm in the electrode area and 0.2 mm in the bonding area. In addition, the average thickness of the base of the separator is 0.25 mm.

[0112] In addition, the cross-sectional shape of the protruding portion of all the convex strips including the inner convex strips and the outer convex strips is a substantially isosceles trapezoid, and the width of the convex strips is 0.25 mm at the bottom of the base surface of the separator and 0.15 mm at the top. The convex strips are arranged in the separator sheet in such a manner that the inner convex strips are formed on both sides (the first side and the second side) of the inner surface of the bag-shaped separator and the outer convex strips are formed on both sides (the third side and the fourth side) of the outer surface. The separator sheet is a rectangle with a long side length of 250 mm and a short side length of 152 mm, and all the convex strips are parallel to the long sides of the separator sheet, forming a stripe pattern extending in a straight line.

[0113] When the separator sheet is folded in half, the direction of the separator sheet being folded is slightly deviated from the direction parallel to the short side so that the opposing inner convex strips do not overlap each other ( Figure 3 (a)) is bent. Thereafter, the 3mm area of ​​the left and right ends is joined by a meshing sealing method to obtain a bag-shaped separator. The length L of the inner convex strips excluding the bent portion is 124mm in both the joining area and the plate area, and the interval D between the tops of the inner convex strips in the joining area is 1.0mm as described above. The distance W between the top of the inner convex strip located on the endmost side and the end is 0.4mm. The angle θ at which the axis Y for bending the insulating sheet deviates from the direction X parallel to the short side is 0.2° (the intersection angle 2θ between the inner convex strips is 0.4°).

[0114] While the unconverted negative electrode plate is pressed against the electrode plate region of the separator sheet, the separator sheet is folded and the left and right ends are joined, and the separator is formed into a bag shape and the negative electrode plate is accommodated at the same time.

[0115] (4) Production of lead-acid batteries

[0116] The bag-shaped separator A containing the negative electrode plate and the positive electrode plate are stacked, and each battery cell is formed into an electrode plate group by eight chemically unconverted negative electrode plates and eight chemically unconverted positive electrode plates.

[0117] The electrode assembly was inserted into a polypropylene electrolytic cell, and an electrolyte was injected to carry out chemical conversion in the electrolytic cell, thereby assembling a liquid lead-acid battery A1 having a rated voltage of 12 V and a rated capacity of 48 Ah (5 hour rate).

[0118] 《Lead-acid battery A2》

[0119] In the manufacture of the separator S1, when the separator sheet is folded in half, the axis for bending the separator sheet is changed so that the opposing inner convex strips cross each other ( Figure 3 (b)), the angle θ of the axis Y of the separator sheet being bent from the direction X parallel to the short side was set to 0.5° (intersection angle 2θ of the inner convex lines = 1°). Lead acid battery A2 was produced in the same manner as lead acid battery A1 except for this.

[0120] 《Lead-acid battery A3》

[0121] A bag-shaped separator different from separator S1 was produced.

[0122] A separator sheet made of a polyethylene microporous film and having convex strips on both sides is folded in half, and the left and right ends are joined to form a bag-shaped separator S2. Figure 6 In the isolation sheet shown, the spacing of the inner convex strips in the electrode area and the bonding area (the peripheral area of ​​5 mm from the left and right ends) is set to 0.5 mm, and the height of the inner convex strips in the electrode area and the bonding area is set to 0.1 mm. In addition, the spacing of the outer convex strips in the electrode area is set to 8.0 mm, and in the bonding area is set to 0.5 mm, and the height of the outer convex strips in the electrode area is set to 0.4 mm, and in the bonding area is set to 0.2 mm. In addition, the average thickness of the base of the isolation member is 0.25 mm.

[0123] In addition, the cross-sectional shape of the protruding portion of all the convex strips including the inner convex strips and the outer convex strips is a substantially isosceles trapezoid, and the width of the convex strips is set to 0.2 mm at the bottom of the base surface of the separator and 0.1 mm at the top. The convex strips are arranged in the separator sheet in such a manner that the inner convex strips are formed on both sides (the first side and the second side) of the inner surface of the bag-shaped separator and the outer convex strips are formed on both sides (the third side and the fourth side) of the outer surface. The separator sheet is a rectangle with a long side length of 250 mm and a short side length of 152 mm. All the inner convex strips are perpendicular to the long sides of the separator sheet, and all the outer convex strips are parallel to the long sides of the separator sheet, forming a stripe pattern extending in a straight line.

[0124] When the separator sheet is folded in half, the direction of the folded separator sheet is slightly deviated from the direction parallel to the short side, and the opposite inner convex strips are bent in a manner that does not overlap each other. Thereafter, the 3mm area of ​​the left and right ends is joined by the meshing sealing method to obtain a bag-shaped separator. The length L of the inner convex strips other than the bent portion is equal to the length of the short side of the separator sheet in any joining area of ​​the first and second areas and the pole plate area, which is 152mm, and the spacing D between the tops of the inner convex strips in the joining area is 0.5mm as described above. The distance W between the top of the inner convex strip located at the endmost side and the end is 0mm. The angle θ at which the axis Y for the separator sheet to bend deviates from the direction X parallel to the short side is 0.05° (the angle between the inner convex strips is 2θ=0.1°). In addition, the length of the outer convex strips other than the bent portion is 124mm in both the joining area and the pole plate area, and the spacing between the tops of the outer convex strips in the joining area is 0.5mm as described above. The top of the outer convex strip located at the endmost side is 0.4 mm away from the endmost side.

[0125] The negative electrode plate was housed in the separator S2 to form an electrode plate group, thereby manufacturing the lead acid battery A3.

[0126] 《Lead-acid battery A4》

[0127] In the manufacture of the separator S2, when the separator sheet is folded in half, the axis for bending the separator sheet is changed. The angle θ of the axis Y of the separator sheet bent so that the opposing inner convex strips intersect each other is set to 0.5° (the intersection angle 2θ between the inner convex strips = 1°). In addition, the lead-acid battery A4 is manufactured in the same manner as the lead-acid battery A3.

[0128] 《Lead-acid battery B1》

[0129] A lead acid battery B1 was produced in the same manner as the lead acid battery A1 except that the positive electrode plate was housed in the separator S1 to form an electrode plate group.

[0130] 《Lead-acid battery B2》

[0131] A lead acid battery B2 was produced in the same manner as the lead acid battery A2, except that the positive electrode plate was housed in the separator S1 to form an electrode plate group.

[0132] In lead-acid batteries B1 and B2, the spacing of the inner convex strips of the separator sheet was set to 8.0 mm in the plate region and 1.0 mm in the joint region (the peripheral region of 5 mm from the left and right ends), and the height of the inner convex strips was set to 0.4 mm in the plate region and 0.2 mm in the joint region. In addition, the spacing of the outer convex strips was set to 2.0 mm in the plate region and 1.0 mm in the joint region, and the height of the outer convex strips was set to 0.1 mm in both the plate region and the joint region.

[0133] 《Lead-acid battery B3》

[0134] In the manufacture of the separator S2, the separator S3 is manufactured by bending the separator sheet in the opposite direction. That is, the relationship between the inner convex strips and the outer convex strips of the separator S3 is opposite to that of the separator S2, the inner convex strips are parallel to the long side of the separator sheet, and the outer convex strips are perpendicular to the long side of the separator sheet and extend in a straight line. The spacing, height and length of the inner convex strips of the separator S3 are respectively the same as the spacing, height and length of the outer convex strips of the separator S2, and the spacing, height and length of the outer convex strips in the separator S3 are respectively the same as the spacing, height and length of the inner convex strips in the separator S2.

[0135] A lead acid battery B3 was produced in the same manner as the lead acid battery A3, except that the positive electrode plate was housed in the separator S3 to form an electrode plate group.

[0136] 《Lead-acid battery B4》

[0137] A lead acid battery B4 was produced in the same manner as the lead acid battery A4 except that the positive electrode plate was housed in the bag-like separator S3 to form an electrode plate group.

[0138] [Evaluation 1: Occurrence of lower short circuit caused by vibration]

[0139] After the heavy-load life test specified in JIS D 5301: 2006 was cycled 150 times, the following vibration test was performed to compare the incidence of lower short circuits.

[0140] Vibration direction: single vibration up and down

[0141] Acceleration: 6G

[0142] Vibration frequency: 30Hz

[0143] Vibration time: 2 hours

[0144] [Evaluation 2: Resistance to penetration short circuit]

[0145] The charge and discharge were repeated in the following cycle, and the number of cycles at which permeation short circuit occurred was evaluated.

[0146] 1. Discharge: 9.6A (end voltage 10.5V)

[0147] 2. Constant resistance discharge: 10Ω resistor connected × 7 days

[0148] 3. Charging: 14.4V / 50A×60 minutes

[0149] The above steps 1 to 3 were repeated as one cycle, and the number of cycles at which the charging current and voltage became unstable due to penetration short circuiting was determined. The penetration short circuit resistance of each lead acid battery was evaluated relative to the number of cycles of lead acid battery A1 as 100.

[0150] Table 1 shows the results of evaluations 1 and 2 of lead-acid batteries A1 to A4 and B1 to B4.

[0151] [Table 1]

[0152] Battery Isolation containment Cross-ribbed Short circuit occurrence ratio in the lower part of the vibration test (%) Permeation short circuit cycle number (%) A1 Negative plate none 20 100 A2 Negative plate have 0 120 A3 Negative plate none 20 100 A4 Negative plate have 0 120 B1 Positive plate none 20 120 B2 Positive plate have 0 120 B3 Positive plate none 20 120 B4 Positive plate have 0 120

[0153] As shown in Table 1, in the lead-acid batteries A2 and A4, which are arranged in a manner that the inner convex strips cross in the joint area, no lower short circuit occurs during the vibration test. This is believed to be due to the improved joint strength of the bag-shaped separator, so the seal at the end of the separator does not fall off, and the short circuit caused by the contact between the precipitate from the positive active material accumulated in the lower part of the electrolytic cell due to the heavy-load life test and the negative plate is suppressed. In contrast, in lead-acid batteries A1 and A3, a lower short circuit occurs with a high probability of 20%. This is believed to be due to the insufficient joint strength of the bag-shaped separator, so in the middle of the vibration test, a part of the joint of the bag-shaped separator falls off, and the precipitate from the positive active material contacts the negative plate through the part of the joint that falls off, resulting in a short circuit.

[0154] In addition, the lead-acid batteries A2 and A4 also have improved resistance to penetration short circuits compared to the lead-acid battery A1. This is believed to be because the crimping portion after the meshing seal is slightly thickened by the intersection of the inner convex strips, and the distance between the negative plate and the separator is slightly increased in the bonding area at the end of the separator or in the area between the bonding area and the plate area, thereby suppressing the contact between the negative plate and the separator around the end, thereby suppressing penetration short circuits.

[0155] As described above, the lead acid battery of this embodiment has a remarkable effect when the negative electrode plate is housed in the bag-shaped separator, and can partially solve the unique problems that occur in the lead acid battery having a structure in which the negative electrode plate is housed in the bag-shaped separator.

[0156] The positive plate is housed in a bag-shaped separator, and the lead-acid battery is manufactured in the same way. The vibration test is also carried out to evaluate the resistance to penetration short circuit. The results are shown in lead-acid batteries B1 to B4 in Table 1. As in the case where the negative plate is housed in a bag-shaped separator, the lower short circuit is suppressed by arranging the inner convex strips in a cross manner in the joint. On the other hand, when the positive plate is housed in a bag-shaped separator, the distance between the negative plate at the end of the separator and the separator is fully ensured because the negative plate is not housed. Therefore, lead-acid batteries B2 and B4 in which the inner convex strips are arranged in a cross manner in the joint, and lead-acid batteries B1 and B3 in which the inner convex strips do not cross in the joint, all obtain the same resistance to penetration short circuit as lead-acid batteries A2 and A4.

[0157] Industrial Applicability

[0158] The lead acid battery according to one aspect of the present invention can be applied to valve-controlled type and liquid-type lead acid batteries, and can be suitably used as a starting power source for automobiles, motorcycles, and the like.

[0159] Description of Reference Numerals

[0160] 1…lead-acid battery; 2…negative plate; 3…positive plate; 4…spacer; 5…positive frame; 6…negative frame; 7…positive column; 8…through connector; 9…negative column; 11…plate group; 12…electrolytic cell; 13…partition wall; 14…cell chamber; 15…cover; 16…negative terminal; 17…positive terminal; 18…liquid port plug; 100…spacer; 101…base; 102a~102e…inner convex strip; 104a, 104b…outer convex strip; 106…plate region; 108a, 108b…joining region; 109a, 109b…joining portion; 110~112, 114…spacer sheet.

Claims

1. A lead-acid battery, wherein a plurality of positive plates and a plurality of negative plates are stacked with separators interposed therebetween and an electrolyte is housed in a battery cell chamber, wherein: The separator is in the shape of a bag with an opening, The isolating element comprises: A first surface and a second surface that are opposite to each other and constitute the inner surface of the bag; a plurality of first convex strips disposed on the first surface, and a plurality of second convex strips disposed on the second surface; a third surface which is the back side of the first surface and a fourth surface which is the back side of the second surface, constituting the outer surface of the bag; a plurality of third ridges disposed on the third surface, and a fourth ridge disposed on the fourth surface; and a junction between the first surface and the second surface, At least one of the first convex strips disposed on the first surface and at least one of the second convex strips disposed on the second surface intersect at the joint portion, The separator has a bonding region including the bonding portion and a plate region separated from the bonding region on the first surface and the second surface, respectively. The third convex strip is formed in a region on the third surface corresponding to the bonding region on the first surface.

2. The lead acid battery according to claim 1, wherein The separator accommodates the negative electrode plate.

3. The lead acid battery according to claim 1, wherein In the peripheral area on the first surface of the joint portion, the first convex strip extends linearly along a first direction, In a peripheral area on the second surface of the joint portion, the second convex strip extends linearly along a second direction different from the first direction.

4. The lead acid battery according to any one of claims 1 to 3, wherein The first convex strips include a plurality of first joint convex strips arranged at a certain interval in the joint area on the first surface, and a plurality of first electrode plate convex strips arranged at a certain interval in the electrode plate area on the first surface. The first joining ridges are set at intervals narrower than the intervals between the first electrode plate ridges.

5. The lead acid battery according to claim 4, wherein: The second convex strips include a plurality of second joining convex strips arranged at a certain interval in the joining area on the second surface, and a plurality of second electrode plate convex strips arranged at a certain interval in the electrode plate area on the second surface. The intervals between the second joining ridges are narrower than the intervals between the second electrode plate ridges.

6. The lead acid battery according to any one of claims 1 to 3, wherein The joining portion is formed by compression joining or welding joining.