Method for producing modified coal

By carrying out carbonization of coal in the range of 300 to 650°C and oxidation treatment in the range of 200 to 240°C, combined with the optional drying process below 150°C, the problem of difficulty in suppressing the spontaneous ignition of low-quality coal in the existing technology is solved. , achieving high yield and high-quality modified coal manufacturing, reducing manufacturing costs and improving safety.

CN111433330BActive Publication Date: 2024-10-18NIPPON STEEL & SUMIKIN ENGINEERING CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201880077972.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-10-16
Publication Date
2024-10-18
Estimated Expiration
2038-10-16

AI Technical Summary

Technical Problem

When the existing technology modifies low-quality coal, despite deactivation treatment, the self-ignitability cannot be fully suppressed. Excessive treatment will lead to a reduction in volatile components and cannot be effectively used as fuel.

Method used

Carbonization is carried out in the range of 300 to 650°C, and the carbonized coal is oxidized in the range of 200 to 240°C for 10 to 60 minutes to reduce the self-heating property of the raw coal, thus inhibiting self-ignition. At the same time, it can be used before the drying process. Drying below 150°C is performed to reduce the moisture content of the coal and improve the yield.

Benefits of technology

It is possible to produce modified coal with fully suppressed self-ignition at a high yield, improve the quality and safety of the modified coal, reduce the manufacturing cost, and improve the efficiency and safety of the oxidation treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111433330B_ABST
    Figure CN111433330B_ABST
Patent Text Reader

Abstract

Provided is a method for producing upgraded coal, comprising: a pyrolysis step of pyrolyzing coal at 300-650°C to obtain pyrolyzed coal; and an oxidation step of oxidizing the pyrolyzed coal at a temperature range of greater than 200°C and less than 240°C for 10-60 minutes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing modified coal. Background Art

[0002] In order to modify low-quality coal such as lignite or sub-bituminous coal, there is a known technology for drying and carbonizing the low-quality coal. However, it is known that when the coal is modified by this technology, its surface is activated and it will spontaneously ignite due to the heat of reaction with oxygen in the air. As a technology to prevent this spontaneous combustion, a technology for deactivating the coal using a treatment gas containing oxygen at a temperature range of 40 to 95°C has been proposed (see Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-139537 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] It is believed that the conventional deactivation treatment as described in Patent Document 1 can deactivate the carbonized coal to some extent. However, according to the research of the present inventors, even if the conventional deactivation treatment is performed, the spontaneous combustion property cannot be sufficiently reduced. On the other hand, if the deactivation treatment is excessively performed in order to reduce the spontaneous combustion property, the volatile components are reduced and the carbonized coal cannot be effectively used as a fuel. Therefore, the object of the present invention is to provide a method for producing modified coal, which can produce modified coal with sufficiently suppressed spontaneous combustion property at a high yield.

[0008] Solutions for solving problems

[0009] The present invention provides a method for producing modified coal, comprising: a carbonization step of carbonizing coal at 300-650°C to obtain carbonized coal; and an oxidation step of oxidizing the carbonized coal at a temperature range of greater than 200°C and less than 240°C for 10-60 minutes.

[0010] The manufacturing method performs oxidation treatment of raw coal at a temperature range of greater than 200° C. and less than 240° C. for 10 to 60 minutes. It is believed that when the oxidation treatment is performed under such conditions, the surface components of the raw coal are oxidized and the surface state is stabilized, so that the self-heating property is reduced and the spontaneous combustion property is suppressed. In addition, the disappearance caused by spontaneous combustion can be suppressed, and the yield rate can be improved.

[0011] The manufacturing method includes a carbonization step of carbonizing coal to obtain carbonized coal before the oxidation treatment step. Carbonization of coal is effective as a means of improving the quality of coal. Here, when the carbonization of coal is performed at a temperature below 650°C, the yield rate during carbonization is improved, but on the other hand, there is a tendency for the spontaneous combustion to increase. In the manufacturing method, the self-heating property can be reduced by the oxidation treatment step. Therefore, the spontaneous combustion can be suppressed even if the carbonization temperature in the carbonization step is set to 650°C or below. Therefore, it is possible to manufacture high-quality modified coal with fully suppressed spontaneous combustion at a high yield rate.

[0012] The production method may include a drying step of drying the coal at 150° C. or less before the oxidation step. This can reduce the moisture content of the coal, and thus higher quality upgraded coal can be obtained through the oxidation step, or the dry distillation step and the oxidation step.

[0013] The above-mentioned manufacturing method may also include a combustion step of burning a gas containing volatile components generated by dry distillation of coal in a combustion furnace. In this case, in the oxidation treatment step, it is preferred to use oxygen-containing exhaust gas from the combustion furnace to oxidize the dry distillation coal. This can reduce the manufacturing cost of the modified coal and improve the efficiency and safety of the oxidation treatment.

[0014] Effects of the Invention

[0015] The present invention can provide a method for producing upgraded coal, which can produce upgraded coal whose spontaneous combustion is sufficiently suppressed at a high yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a flow chart showing an example of a method for producing upgraded coal.

[0017] Figure 2 It is a graph showing the results of the self-ignition evaluation test of Examples 1 and 2, Reference Examples 1 and 2, and Comparative Examples 1 to 4.

[0018] Figure 3 This is a graph showing the temporal change in the calorific value of the pyrolysis coals of Comparative Examples 5 to 8 having different pyrolysis degrees.

[0019] Figure 4 It is a graph showing the temporal change in the calorific value of the upgraded coals of Example 3, Reference Example 4, Comparative Examples 9 and 10, and the pyrolysis coal of Comparative Example 6 at different oxidation treatment temperatures.

[0020] Figure 5 It is a graph showing the concentrations of carbon monoxide and carbon dioxide in the exhaust gas during the oxidation treatment in Examples 5 and 6, Reference Example 7, and Comparative Examples 11 to 13.

[0021] Figure 6It is a graph showing the results of infrared spectrum analysis of Comparative Example 6, Comparative Example 14, and Comparative Example 15.

[0022] Figure 7 This is a graph showing the results of thermogravimetric analysis of Comparative Examples 16 to 19, Examples 8 and 9, and Reference Example 10, which have different oxidation treatment temperatures.

[0023] Figure 8 It is a graph showing the results of differential thermal analysis of Comparative Examples 16 to 19, Examples 8 and 9, and Reference Example 10 having different oxidation treatment temperatures.

[0024] Fig. 9 This is a graph showing the relationship between the height of the maximum peak in the differential thermal analysis results of Comparative Examples 16 to 19, Examples 8 and 9, and Reference Example 10, which have different oxidation treatment temperatures, and the oxidation treatment temperature.

[0025] Fig.10 It is a graph showing the results of the spontaneous combustion evaluation test. DETAILED DESCRIPTION

[0026] The embodiments of the present invention will be described below with reference to the accompanying drawings as appropriate. However, the following embodiments are examples for describing the present invention and are not intended to limit the present invention to the following contents.

[0027] The method for producing modified coal of the present embodiment comprises: a dry distillation step of dry distilling coal at 300 to 650°C to obtain dry distillation coal; and an oxidation treatment step of oxidizing the dry distillation coal at a temperature range of greater than 200°C and less than 240°C. Generally, dry distillation coal tends to be more self-igniting than dried coal. In the present embodiment, modified coal with sufficiently suppressed self-ignition can be obtained from the dry distillation coal by subjecting the dry distillation coal having a surface state different from that of the coal and its dried coal to an oxidation treatment step under predetermined conditions.

[0028] The dry distillation process is a process of dry distilling coal at 300 to 650°C to obtain dry distilled coal. It should be noted that the dry distillation process may be started without the drying process described later. In this case, the moisture content of the coal will decrease at the beginning of the dry distillation process. The dry distillation process is preferably carried out at a temperature range of 300 to 600°C. In this way, the dry distillation of coal can be fully carried out and a high yield can be maintained. The dry distillation process can be carried out using a common dry distillation furnace such as a vertical blast furnace, a coke oven or a tunnel kiln furnace.

[0029] The volatile matter (VM) of the pyrolysis coal obtained in the pyrolysis step is preferably 10 to 30% by mass. The pyrolysis coal generally has high self-ignition property, but in this embodiment, the self-ignition property can be suppressed by performing an oxidation treatment step after the pyrolysis step. Therefore, a high yield can be achieved.

[0030] The coal may include low-quality coal or high-quality coal. When low-quality coal is included, it is preferred to perform a drying process described later before the oxidation treatment process. However, the drying process is not necessarily required. The particle size of the raw coal may be, for example, less than 50 mm, less than 30 mm, or less than 10 mm.

[0031] In the oxidation treatment step, by setting the temperature for the oxidation treatment of the pyrolysis coal (oxidation treatment temperature) to a range of more than 200°C, the surface of the pyrolysis coal can be sufficiently modified, and modified coal with sufficiently suppressed spontaneous combustion can be obtained. By setting the oxidation treatment temperature to 240°C or less, the reduction of volatile components in the oxidation treatment step can be suppressed, and modified coal can be produced with a high yield.

[0032] From the viewpoint of achieving both the suppression of spontaneous combustion and the improvement of the yield at a higher level, the oxidation treatment temperature is preferably 210 to 240°C, more preferably 220 to 240°C. The oxidation treatment process may not be carried out at a fixed oxidation treatment temperature, and the oxidation treatment temperature may vary within the above range. From the viewpoint of producing modified coal with a high yield, the oxidation treatment process time is 10 to 60 minutes. From the viewpoint of fully suppressing spontaneous combustion, the oxidation treatment process time can be 15 to 60 minutes.

[0033] The atmosphere of the oxidation treatment process is not particularly limited as long as it is an atmosphere containing oxygen, and may be air or a mixed atmosphere of an inert gas such as nitrogen and oxygen. In addition, it may be exhaust gas from a combustion furnace. From the perspective of safety and high efficiency of the oxidation treatment, the oxygen concentration may be, for example, 2 to 13% by volume, or 3 to 10% by volume. The "volume %" is the volume fraction under standard conditions (25°C, 100 kPa).

[0034] In the oxidation treatment process, the functional groups on the surface of the raw coal are oxidized. As a result, it is possible to produce a modified coal in which the self-heating property caused by oxidation is reduced and the spontaneous combustion property is fully suppressed. From the viewpoint of improving the usefulness as a fuel, the volatile component (VM) of the modified coal can be 5% by mass or more, or 10% by mass or more. On the other hand, from the viewpoint of further reducing the spontaneous combustion property, the volatile component (VM) of the modified coal can be 30% by mass or less, or 25% by mass or less. It should be noted that the volatile component in this specification is a value on a dry basis measured based on the "square electric furnace method" of JIS M 8812:2006.

[0035] According to the manufacturing method of this embodiment, it is possible to manufacture modified coal with sufficiently suppressed spontaneous combustion at a high yield. The modified coal may also contain a certain degree of volatile components, and thus can be effectively used as a fuel. It can be seen that not only is the usefulness as a fuel high, but also it is possible to safely store coal in the open air and to safely transport it by land or sea from the coal production area.

[0036] Another embodiment of the method for producing upgraded coal includes a drying step of drying the coal at 150° C. or less before the carbonization step. When low-quality coal with a high moisture content (e.g., lignite and subbituminous coal with a moisture content of 50% by mass or more) is used, it is preferable to include a drying step as in the present embodiment.

[0037] In the drying process, the coal is heated to a temperature range of, for example, 40 to 150° C. to dry it. The drying process can be carried out in air or in an inert gas atmosphere. Alternatively, it can be carried out in the exhaust gas of a combustion furnace. In the drying process, the moisture content of the coal is reduced to, for example, 20% by mass or less. By carrying out this drying process, the modification effect brought about by carbonization or oxidation treatment can be fully obtained.

[0038] The drying process may be carried out using a common electric furnace or the like, or may be carried out using an indirect heater or an air fluidized bed dryer. The drying time is not particularly limited and may be adjusted according to the moisture content of the coal, the particle size of the coal, and the like.

[0039] According to the production method of this embodiment, even when low-quality coal is used, upgraded coal with sufficiently suppressed self-ignition can be produced at a high yield. The particle size of the upgraded coal may be, for example, 50 mm or less, or 10 mm or less.

[0040] The modified coal obtained by the above-mentioned manufacturing method can be classified into granular modified coal (e.g., particles with a particle size of 3 mm or more) and powdered modified coal (e.g., powder with a particle size of less than 3 mm). The powdered modified coal (powder) obtained by classification can be formed with or without a binder and mixed with granular modified coal (granules) obtained by classification. Increasing the average particle size of the modified coal in this way can further reduce the generation of dust during transportation and storage of coal, and further improve the operability of the modified coal.

[0041] Figure 1 This is a diagram showing an example of the configuration of an apparatus for carrying out a method for producing upgraded coal according to an embodiment. Figure 1 In the example of the present invention, the drying process is performed in the drying device 10, the carbonization process is performed in the carbonization device 20, and the oxidation process is performed in the oxidation treatment device 30. The gas containing volatile components generated by the carbonization device 20 is consumed as fuel gas in the combustion furnace 40 (combustion process). As the drying device 10, for example, a common dryer can be cited. As the oxidation treatment device 30, for example, a common electric furnace can be cited.

[0042] The exhaust gas generated by the combustion of the fuel gas containing volatile components in the combustion furnace 40 usually contains about 5 to 10% by volume of oxygen. By utilizing the exhaust gas in the oxidation treatment device 30, the efficiency and safety of the oxidation treatment in the oxidation treatment process can be fully improved. In addition, since the temperature of the exhaust gas can be effectively utilized, energy reduction can also be achieved. The exhaust gas generated in the combustion furnace 40 can also be used as a heating gas in the drying device 10. By effectively utilizing the heat generated in the dry distillation process in this way, the manufacturing cost of the modified coal can be reduced.

[0043] Several embodiments of the present invention have been described above, but the present invention is not limited to the above embodiments at all.

[0044] Example

[0045] The present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0046] (Example 1)

[0047] [Manufacturing of modified coal]

[0048] Subbituminous coal (Adaro coal produced in Indonesia), which is commercially available boiler coal, is dried in air using a dryer to obtain dried coal (drying process). The heating temperature in the drying process is 150°C and the heating time is 30 minutes. The volatile component (VM) of the obtained dried coal is 50% by mass and the moisture content is less than 10% by mass. The obtained dried coal is dry-distilled using a dry distillation furnace to obtain dry distilled coal (drying process). The heating temperature in the dry distillation process is 430°C and the heating time is 40 minutes. The volatile component (VM) of the dry distillation coal is 25% by mass.

[0049] Next, the obtained carbonized coal was oxidized using an electric furnace to produce granular reformed coal (particle size: about 1 to 3 mm) (oxidation treatment step). The oxidation treatment conditions were a mixed gas atmosphere of nitrogen and oxygen (oxygen concentration: 8 volume %), a heating temperature of 240° C., and a heating time of 40 minutes.

[0050] [Evaluation of spontaneous combustion ( Figure 2 )]

[0051] The modified coal was subjected to a self-ignition evaluation test in accordance with the United Nations Recommendations on the Transport of Dangerous Goods [Class 4, Division 4.2 (Self-ignitable substances and self-heating substances)]. Specifically, the modified coal was placed in a cube-shaped container with a side length of 10 cm formed by a metal mesh, stored in air at 140°C, and the time-dependent change in the heating temperature was investigated. The results are as follows: Figure 2 As shown in curve A1 (modified coal).

[0052] (Example 2)

[0053] The upgraded coal was produced in the same manner as in Example 1 except that the heating temperature in the oxidation treatment step was 210°C. Then, the spontaneous combustion evaluation test was carried out in the same manner as in Example 1. Figure 2 As shown in curve A2.

[0054] (Reference Example 1)

[0055] The spontaneous combustion evaluation test of the subbituminous coal (Adaro coal produced in Indonesia) used in Example 1 was carried out in the same manner as in Example 1. Figure 2 As shown in curve C1.

[0056] (Reference Example 2)

[0057] The self-ignition evaluation test of bituminous coal (Tayasir coal produced in Australia) which is commercially available for boiler use was carried out in the same manner as in Example 1. Figure 2 As shown in curve C2.

[0058] (Comparative Example 1)

[0059] The same procedure as in Example 1 was followed except that the oxidation treatment step was not performed. That is, a spontaneous combustion evaluation test was performed on the pyrolysis coal obtained in the pyrolysis step. Figure 2 As shown in curve E1.

[0060] (Comparative Example 2)

[0061] The upgraded coal was produced in the same manner as in Example 1 except that the heating temperature in the oxidation treatment step was 200°C. Then, the spontaneous combustion evaluation test was carried out in the same manner as in Example 1. Figure 2 As shown in curve B1.

[0062] (Comparative Example 3)

[0063] The upgraded coal was produced in the same manner as in Example 1 except that the heating temperature in the oxidation treatment step was 290°C. Then, the spontaneous combustion evaluation test was carried out in the same manner as in Example 1. Figure 2 As shown in curve B2.

[0064] (Comparative Example 4)

[0065] Dried coal was obtained in the same manner as in Example 1. The volatile matter (VM) of the dried coal was 50% by mass and the moisture content was 10% by mass or less. The self-ignition property evaluation test of the obtained dried coal was conducted. The results are as follows: Figure 2 As shown in curve D1.

[0066] like Figure 2As shown, the pyrolysis coal (curve E1) of Comparative Example 1, which was not subjected to the oxidation treatment step, generates heat to 250°C or more in about 1 hour. That is, the modified coal has the highest spontaneous combustion. On the other hand, the spontaneous combustion of the dried coal (curve D1) of Comparative Example 4 is lower than that of the pyrolysis coal (curve E1) of Comparative Example 1.

[0067] The modified coal of Comparative Example 2 (curve B1) and the modified coal of Comparative Example 3 (curve B2) which were oxidized at 200°C and 290°C, respectively, have lower spontaneous combustion than Comparative Example 1. Moreover, the modified coal of Example 2 (curve A2) and the modified coal of Example 1 (curve A1) which were oxidized at 210°C and 240°C, respectively, have further lower spontaneous combustion than Comparative Examples 2 and 3.

[0068] The self-ignition property of the modified coal of Example 2 is lower than that of commercially available subbituminous coal, and the self-ignition property of the modified coal of Example 1 is lower than that of commercially available bituminous coal. It can be seen that the self-ignition property of the modified coals of Examples 1 and 2 is sufficiently suppressed despite the carbonization.

[0069] [The effect of retort degree on calorific value ( Figure 3 )]

[0070] (Comparative Example 5)

[0071] Subbituminous coal (Adaro coal produced in Indonesia) which is commercially available as boiler coal is dried in air using a dryer to obtain granular dry coal (particle size: 0.5 mm or less) (drying process). The heating temperature in the drying process is 150° C. and the heating time is 30 minutes. The volatile matter (VM) of the dried coal is 50% by mass and the moisture content is 10% by mass or less.

[0072] The prepared dry coal was subjected to differential scanning calorimetry (DSC) using a commercially available measuring device. Specifically, the dry coal and the reference material were heated to 107°C using a heater in a nitrogen atmosphere. Then, the nitrogen atmosphere was switched to air, and the calorific value when air oxidized at a fixed temperature (107°C) was measured. The results are as follows: Figure 3 As shown in curve D2.

[0073] (Comparative Example 6)

[0074] The dry coal of Comparative Example 5 was used to perform a dry distillation process to prepare dry distillation coal. The heating temperature in the dry distillation process was 430°C and the heating time was 40 minutes. The volatile matter (VM) of the dry distillation coal was 25% by mass. The DSC measurement of the dry distillation coal was performed in the same manner as in Comparative Example 5. The results are as follows: Figure 3 As shown in curve E2.

[0075] (Comparative Example 7)

[0076] Pyrolysis coal was prepared in the same manner as in Comparative Example 6 except that the heating temperature in the pyrolysis step was 550°C. The volatile matter (VM) of the pyrolysis coal was 12% by mass. The DSC measurement of the pyrolysis coal was performed in the same manner as in Comparative Example 5. Figure 3 As shown in curve E3.

[0077] (Comparative Example 8)

[0078] Pyrolysis coal was prepared in the same manner as in Comparative Example 6 except that the heating temperature in the pyrolysis step was 1000° C. The volatile matter (VM) of the pyrolysis coal was 0% by mass. The DSC measurement of the pyrolysis coal was performed in the same manner as in Comparative Example 5. Figure 3 As shown in curve E4.

[0079] According to the results of Comparative Examples 6 to 8, when the carbonization temperature (carbonization degree) is low, the volatile components remaining in the carbonized coal increase, so the yield is high. Figure 3 As shown, it can be confirmed that if the carbonization temperature is lowered, the calorific value generated by oxidation increases. It is believed that this is caused by the increase in the amount of residual volatile components when the carbonization temperature becomes lower, and as a result, the amount of highly active free radicals generated on the surface of the carbonized coal increases. The calorific value (curve E2) of the carbonized coal of Comparative Example 6 with a carbonization temperature of 430°C is greatly increased compared with the calorific value (curve D2) of the dried coal of Comparative Example 5. From this result, it can be confirmed that the yield and self-heating properties of carbonized coal are in a trade-off relationship, and it is difficult to achieve both high yield and suppression of spontaneous combustion in the carbonized coal state.

[0080] like Figure 3 As shown, the calorific value of the dried coal of Comparative Example 5 (curve D2) is lower than that of the pyrolysis coal of Comparative Example 6 (E2). Figure 2 It is also shown that the spontaneous combustion of dried coal (curve D1) is lower than that of pyrolysis coal (E1). Based on these trends, it can be considered that when dried coal is oxidized, the spontaneous combustion can be suppressed in the same way as pyrolysis coal. In other words, oxidation treatment is also effective for dried coal, just like pyrolysis coal.

[0081] [Effect of oxidation treatment temperature ( Figure 4 )]

[0082] (Example 3)

[0083] The carbonized coal of Comparative Example 6 was subjected to an oxidation treatment step to produce modified coal. The oxidation treatment conditions were a mixed gas atmosphere of nitrogen and oxygen (oxygen concentration: 10% by volume), a heating temperature of 240°C, and a heating time of 40 minutes. The DSC measurement of the modified coal produced was carried out in the same manner as in Comparative Example 5. The results are as follows: Figure 4 As shown in curve A3.

[0084] (Reference Example 4)

[0085] The carbonized coal of Comparative Example 6 was subjected to an oxidation treatment step to produce modified coal. The oxidation treatment conditions were a mixed gas atmosphere of nitrogen and oxygen (oxygen concentration: 10% by volume), a heating temperature of 260°C, and a heating time of 40 minutes. The DSC measurement of the modified coal produced was carried out in the same manner as in Comparative Example 5. The results are as follows: Figure 4 As shown in curve A4.

[0086] (Comparative Example 9)

[0087] The carbonized coal of Comparative Example 6 was subjected to an oxidation treatment step to produce modified coal. The oxidation treatment conditions were a mixed gas atmosphere of nitrogen and oxygen (oxygen concentration: 10% by volume), a heating temperature of 200°C, and a heating time of 40 minutes. The DSC measurement of the modified coal produced was carried out in the same manner as in Comparative Example 5. The results are as follows: Figure 4 As shown in curve B3.

[0088] (Comparative Example 10)

[0089] The carbonized coal of Comparative Example 6 was subjected to an oxidation treatment step to produce modified coal. The oxidation treatment conditions were a mixed gas atmosphere of nitrogen and oxygen (oxygen concentration: 10% by volume), a heating temperature of 300°C, and a heating time of 40 minutes. The DSC measurement of the modified coal produced was carried out in the same manner as in Comparative Example 5. The results were Figure 4 As shown in curve B4.

[0090] For ease of comparison, Figure 4 The results of Comparative Example 6 are also shown. The modified coals of Example 3 and Reference Example 4 (curves A3 and A4) can significantly reduce the calorific value compared to the carbonized coal of Comparative Example 6 (curve E2). The calorific value of the modified coals of Example 3 and Reference Example 4 is lower than that of the modified coals of Comparative Examples 9 and 10. It can be confirmed that the modified coals of Example 3 and Reference Example 4 can reduce the self-heating property compared to Comparative Examples 6, 9, and 10.

[0091] [Changes in gas generation due to oxidation treatment temperature ( Figure 5 )]

[0092] (Comparative Example 11)

[0093] The carbonized coal of Comparative Example 6 was heated to 140°C in a nitrogen atmosphere using an electric furnace. After heating, an oxidation treatment process was performed to produce modified coal. The oxidation treatment conditions were a mixed gas atmosphere of nitrogen and oxygen (oxygen concentration: 10% by volume), an oxidation treatment temperature of 140°C, and an oxidation treatment time of 20 minutes. All the exhaust gas during the oxidation treatment process was sampled and averaged, and the concentrations of CO2 and CO in the averaged gas were measured using gas chromatography.

[0094] (Comparative Example 12)

[0095] The upgraded coal was produced in the same manner as in Comparative Example 11 except that the oxidation treatment temperature in the oxidation treatment step was 200° C. In the same manner as in Comparative Example 11, the concentrations of CO 2 and CO in the exhaust gas during the oxidation treatment step were analyzed.

[0096] (Example 5)

[0097] The upgraded coal was produced in the same manner as in Comparative Example 11 except that the oxidation treatment temperature in the oxidation treatment step was 220° C. The concentrations of CO 2 and CO in the exhaust gas during the oxidation treatment step were analyzed in the same manner as in Comparative Example 11.

[0098] (Example 6)

[0099] The upgraded coal was produced in the same manner as in Comparative Example 11 except that the oxidation treatment temperature in the oxidation treatment step was 240° C. The concentrations of CO 2 and CO in the exhaust gas during the oxidation treatment step were analyzed in the same manner as in Comparative Example 11.

[0100] (Reference Example 7)

[0101] The upgraded coal was produced in the same manner as in Comparative Example 11 except that the oxidation treatment temperature in the oxidation treatment step was 260° C. The concentrations of CO 2 and CO in the exhaust gas during the oxidation treatment step were analyzed in the same manner as in Comparative Example 11.

[0102] (Comparative Example 13)

[0103] The upgraded coal was produced in the same manner as in Comparative Example 11 except that the oxidation treatment temperature in the oxidation treatment step was 300° C. In the same manner as in Comparative Example 11, the concentrations of CO 2 and CO in the exhaust gas during the oxidation treatment step were analyzed.

[0104] Figure 5 FIG. 2 is a graph showing the concentrations of CO2 and CO in the exhaust gas obtained in Examples 5 and 6, Reference Example 7, and Comparative Examples 11 to 13. Figure 5 As shown, it can be confirmed that the generation amount of CO2 and CO increases when the oxidation treatment temperature is higher than 200°C. Therefore, it is considered that the surface of the reformed coal can be sufficiently reformed by setting the oxidation treatment temperature to a range higher than 200°C.

[0105] [Analysis of the surface state of dry distilled coal and modified coal ( Figure 6 )]

[0106] (Comparative Example 14)

[0107] The modified coal was produced in the same manner as in Comparative Example 12 except that the oxygen concentration of the mixed gas atmosphere in the oxidation treatment step was 8% by volume (oxidation treatment temperature: 200° C.). Infrared spectroscopy analysis (IR analysis) of the produced modified coal was performed using a commercially available infrared spectrometer. The analysis results are as follows: Figure 6 As shown in curve B5.

[0108] (Comparative Example 15)

[0109] The modified coal was produced in the same manner as in Comparative Example 13 (oxidation treatment temperature: 300° C.), except that the oxygen concentration of the mixed gas atmosphere in the oxidation treatment step was 8% by volume. Then, infrared spectroscopy analysis of the produced modified coal was performed in the same manner as in Comparative Example 14. The analysis results are as follows: Figure 6 As shown in curve B6.

[0110] exist Figure 6 In the infrared spectrum analysis of Comparative Examples 14 and 15, peaks at 2800 to 3000 cm-1 derived from aliphatic hydrocarbon groups were observed. -1 In addition, for comparison, Figure 6 The results of infrared spectrum analysis of the carbonized coal prepared in Comparative Example 6 are also shown (curve E2). Figure 6 As shown, it was confirmed that the surface composition of the pyrolysis coal changed by oxidizing the pyrolysis coal. In addition, it was confirmed that the surface composition of the upgraded coal changed greatly when the oxidation treatment temperature was changed within the temperature range of 200 to 300°C.

[0111] [Thermogravimetric and differential thermal analysis in oxidation treatment process ( Figure 7 and Figure 8 )]

[0112] (Comparative Example 16)

[0113] The pyrolysis coal of Comparative Example 6 was used to perform the oxidation treatment process. A commercially available thermogravimetric and differential thermal simultaneous analysis device was used to measure the weight and differential thermal during the oxidation treatment process. Specifically, the pyrolysis coal was placed in the analysis device and heated to 140°C at a rate of 10°C / minute in a nitrogen atmosphere. Then, the atmosphere was switched to a mixed atmosphere of nitrogen and oxygen (oxygen concentration: 10% by volume), and the oxidation treatment was started. Based on this switching time, a thermogravimetric and differential thermal simultaneous analysis was performed. The results of the thermogravimetric analysis are shown in FIG. Figure 7 The results of differential thermal analysis are shown in curve B7. Figure 8 As shown in curve B7.

[0114] (Comparative Example 17)

[0115] Thermogravimetric and differential thermal analysis was performed in the same manner as in Comparative Example 16 except that the oxidation treatment temperature (temperature for switching to the mixed atmosphere) in the oxidation treatment step was 180°C. The results of the thermogravimetric analysis are as follows: Figure 7 The results of differential thermal analysis are shown in curve B8. Figure 8 As shown in curve B8.

[0116] (Comparative Example 18)

[0117] Thermogravimetric and differential thermal analysis was performed in the same manner as in Comparative Example 16 except that the oxidation treatment temperature (temperature for switching to the mixed atmosphere) in the oxidation treatment step was 200°C. The results of the thermogravimetric analysis are as follows: Figure 7 The results of differential thermal analysis are shown in curve B9. Figure 8 As shown in curve B9.

[0118] (Example 8)

[0119] Thermogravimetric and differential thermal analysis was performed in the same manner as in Comparative Example 16 except that the oxidation treatment temperature (temperature for switching to the mixed atmosphere) in the oxidation treatment step was 220°C. The results of the thermogravimetric analysis are as follows: Figure 7 The results of differential thermal analysis are shown in curve A5. Figure 8 As shown in curve A5.

[0120] (Example 9)

[0121] Thermogravimetric and differential thermal analysis was performed in the same manner as in Comparative Example 16 except that the oxidation treatment temperature (temperature for switching to the mixed atmosphere) in the oxidation treatment step was 240°C. The results of the thermogravimetric analysis are as follows: Figure 7 The results of differential thermal analysis are shown in curve A6. Figure 8 As shown in curve A6.

[0122] (Reference Example 10)

[0123] Thermogravimetric and differential thermal analysis was performed in the same manner as in Comparative Example 16 except that the oxidation treatment temperature (temperature for switching to the mixed atmosphere) in the oxidation treatment step was 260°C. The results of the thermogravimetric analysis are as follows: Figure 7 The results of differential thermal analysis are shown in curve A7. Figure 8 As shown in curve A7.

[0124] (Comparative Example 19)

[0125] Thermogravimetric and differential thermal analysis was performed in the same manner as in Comparative Example 16 except that the oxidation treatment temperature (temperature for switching to the mixed atmosphere) in the oxidation treatment step was 300°C. The results of the thermogravimetric analysis are as follows: Figure 7 The results of differential thermal analysis are shown in curve B10. Figure 8 As shown in curve B10.

[0126] Fig. 9 Yes Display Figure 8 The graph of the relationship between the height of the maximum peak (peak top) in the DTA analysis results (differential thermal analysis results) of each embodiment and each comparative example and the oxidation treatment temperature is shown. Fig. 9 As shown in the figure, when the oxidation treatment temperature is 200°C or less (Comparative Examples 16, 17, and 18), the oxidation reaction (exothermic reaction) does not proceed actively. On the other hand, when the oxidation treatment temperature is higher than 200°C, the oxidation reaction proceeds rapidly. Therefore, it is considered that in order to oxidize the surface of the modified coal to a certain extent, the oxidation treatment temperature needs to be in the range of higher than 200°C.

[0127] However, if Figure 7 to Figure 9 As shown in the figure, if the oxidation treatment temperature is higher than 240°C, there is a tendency for the exothermic reaction to become active and the weight loss to become larger. In addition, when the oxidation treatment temperature is 300°C, the modified coal disappears due to spontaneous combustion about 3 to 4 hours after the start of the oxidation treatment. It can be considered that in order to improve the yield of modified coal in the oxidation treatment process, the oxidation treatment temperature needs to be below 240°C.

[0128] <Mechanism of suppressing spontaneous combustion>

[0129] Elemental analysis was performed on the carbonized coal of Comparative Example 6 and the upgraded coals of Comparative Example 9, Example 3, and Comparative Example 10. The results are shown in Table 1.

[0130] [Table 1]

[0131]

[0132] As shown in Table 1, it was confirmed that the oxygen concentration increased by oxidizing the carbonized coal at 200 to 300° C. That is, the oxidation treatment step has the effect of oxidizing the functional groups to increase the oxygen content. It is believed that the spontaneous combustion is suppressed by this effect.

[0133] <Comparison of spontaneous combustion>

[0134] The dried coal obtained by the drying step of Example 1 was heated at 660°C for 40 minutes to prepare pyrolysis coal. The same self-ignition evaluation test as in Example 1 was carried out to evaluate the self-ignition of the prepared pyrolysis coal. The results are shown in Fig.10 In addition, Fig.10 For comparison, the Figure 2 The curve E1 shown (pyrolysis coal, pyrolysis temperature: 430°C).

[0135] like Fig.10As shown in Figure 1, when the carbonization temperature is higher than 650°C, the spontaneous combustion property is greatly reduced. However, if the carbonization temperature is set to a range higher than 650°C, the yield of the modified coal obtained through the oxidation treatment step is reduced. Therefore, by performing oxidation treatment on the carbonized coal obtained by carbonizing coal at 300 to 650°C in a temperature range higher than 200°C and lower than 240°C, it is possible to produce high-quality modified coal with sufficiently reduced spontaneous combustion property at a high yield.

[0136] Industrial Applicability

[0137] According to the present invention, it is possible to provide a method for producing upgraded coal, which is capable of producing upgraded coal whose self-ignition property is sufficiently suppressed at a high yield.

[0138] Description of Reference Numerals

[0139] 10 ... drying device, 20 ... carbonization device, 30 ... oxidation treatment device, 40 ... combustion furnace.

Claims

1. A method for producing modified coal, comprising: A dry distillation step of dry distilling coal at 300-650°C to obtain dry distilled coal; and The step of performing an oxidation treatment on the pyrolysis coal at a temperature in a range of greater than 200° C. and less than 240° C. for 10 to 60 minutes.

2. The method for producing upgraded coal according to claim 1, further comprising a drying step of drying the coal at 150° C. or less before the carbonization step. In the dry distillation step, the coal dried in the drying step is dry distilled.

3. The method for producing upgraded coal according to claim 1 or 2, wherein: The water content of the coal is 50% by mass or more.

4. The method for producing upgraded coal according to any one of claims 1 to 3, wherein: The volatile matter of the carbonized coal obtained in the carbonization step is 10 to 30% by mass.

5. The method for producing upgraded coal according to any one of claims 1 to 4, wherein: The volatile matter of the modified coal obtained in the oxidation treatment step is 5 to 30% by mass.

6. The method for producing upgraded coal according to any one of claims 1 to 5, comprising a combustion step of combusting a gas containing volatile components generated by dry distillation of the coal in a combustion furnace, In the oxidation treatment step, the pyrolysis coal is oxidized using the oxygen-containing exhaust gas from the combustion furnace.

Citation Information

Patent Citations

  • Method for deactivating coal

    JP2013139537A

  • Coal deactivation processing device

    CN104411808A

  • Method for producing coke, and coke

    US20160257887A1