A rapid analysis method for FeO content in magnetite pellets
The cross-section and sandwich diameter of the pellet ore were measured by the round-head hammer ball smashing method, and the FeO content was calculated using the EXCEL table, which solved the problem of long time and large error in the current technology of the FeO content determination time and large error, and achieved rapid and accurate The analysis results provide rapid adjustment guidance for the blast furnace production line, significantly reducing gas consumption and pollutant emissions, and improving economic benefits.
Patent Information
- Application Number
- CN202010361075.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-04-29
AI Technical Summary
In the prior art, the FeO content determination method for pellet ore has a long test time and a large error rate, which affects the production efficiency and environmental protection of the blast furnace.
采用圆头锤砸球法测量球团矿的截面直径和夹心直径,通过EXCEL表格计算球团矿FeO含量,利用夹心结构修正系数和初始FeO含量进行修正,快速计算成品球FeO含量。
The rapid and accurate analysis of FeO content of pellet ore has been achieved, which reduces analysis time, improves the accuracy of results, optimizes the production line operating parameters, reduces gas consumption and pollutant emissions, and significantly improves economic benefits.
Smart Images

Figure CN111474319B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ferrous metallurgy industry, and in particular relates to a rapid analysis method for FeO content in magnetite pellets. Background Art
[0002] In the process of implementing the present invention, the inventors found that the prior art has at least the following problems:
[0003] Blast furnace ironmaking emphasizes "70% raw materials and 30% operation". With the large-scale and automated blast furnaces and the requirement to minimize the fuel ratio, the quality requirements for blast furnace charges are getting higher and higher. It is generally believed that for every 10% increase in the reduction degree of the blast furnace raw materials, the coke ratio can be reduced by 8%-9%, and for every 1% decrease in the ferrous oxide content, the coke ratio will be reduced by 1%. The FeO content of the pellet is one of the main physical and chemical indicators of magnetite pellets. Reducing the FeO content of the pellet is conducive to improving the metallurgical properties of the pellet, increasing the reduction degree and mechanical strength of the pellet, and is conducive to improving the blast furnace indicators. In actual production, the FeO content of magnetite pellets often fluctuates due to the influence of raw materials, thermal parameters and equipment conditions. The current basis for the determination of FeO content in pellets is GB / T6730.8-1986 "Chemical analysis method for iron ore - Determination of ferrous content by potassium dichromate volumetric method". This method is affected by reagents, instruments, sampling, sample preparation and analysis, and has the disadvantages of long testing time and large error rate. Therefore, it has an adverse effect on pellet and blast furnace production, and is not conducive to energy conservation and emission reduction in the ironmaking process. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a rapid analysis method for the FeO content of magnetite pellets by measuring the internal sandwich data of the pellets, quickly calculating the FeO content of the finished magnetite balls, avoiding the disadvantages of long testing time and large error rate, and providing rapid guidance for the operation adjustment of the magnetite pellet production line.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a rapid analysis method for the FeO content of magnetite pellets, characterized in that it comprises the following steps:
[0006] 1) Prepare a ball-peen hammer;
[0007] 2) Sampling: Take pellets with a particle size of 10 to 16 mm, hit the pellets with a round hammer, and measure the data of the cracked pellets; the data includes the cross-sectional diameter of the pellets and the corresponding diameter of the incompletely reacted core; if there is no incompletely reacted core structure, the incompletely reacted core diameter of the pellet, i.e., the core diameter, is 0 mm;
[0008] 3) Break open 10 pellets and measure the cross-sectional diameter of each ball and the corresponding sandwich diameter;
[0009] 4) By designing a calculation table for the FeO content of the pellets in the EXCEL table, inputting the measured sandwich diameter and cross-sectional diameter data, the FeO content of the pellets can be automatically calculated.
[0010] The above step 4) includes the following steps:
[0011] 4.1) The input column items include the cross-sectional diameter D of the pellet, the core diameter d, the initial FeO content W1 of the pellet, the correction coefficient A of the FeO content of the core structure, and the FeO correction value B of the pellet;
[0012] 4.2) The output column items include single ball FeO content W2 and finished ball FeO content W.
[0013] In the above step 4.1), cross-sectional diameter D: measured after ball smashing; core diameter d: measured after ball smashing, the core diameter and cross-sectional diameter of the same ball should be measured on the same cross-section; initial FeO content of pellets W1: calculated based on the FeO content of the raw materials and the raw material ratio, the calculation formula: initial FeO content of pellets W1 = ∑ the amount of FeO brought into the pellet ore by various raw materials.
[0014] In the above step 4.1), the correction coefficient A for the FeO content in the sandwich structure: since the oxidation reaction does not occur in the sandwich structure of the pellet, but the oxidation reaction is not complete, the FeO content in the sandwich structure needs to be corrected. The correction coefficient value range should be greater than 0 and less than 1. The specific value of the correction coefficient A is determined by the corresponding experiment of the pellet sandwich data and the FeO content of the finished ball.
[0015] In the above step 4.1), the pellet FeO correction value B: In actual production, when the pellets are smashed, 10 pellets have no sandwich structure, but the FeO content of the pellets is measured to be between 0.15% and 0.30%, so the FeO content needs to be corrected again.
[0016] In the above step 4.2), the FeO content of a single ball is calculated by the cross-sectional diameter, the core diameter, the initial FeO content of the pellet, and the correction coefficient of the FeO content of the core structure. The calculation formula is:
[0017]
[0018] In the above step 4.2), the FeO content W of the finished ball is: the FeO content W of the finished ball = the average value of the FeO content of 10 single balls.
[0019] One of the above technical solutions has the following advantages or beneficial effects: by measuring the internal sandwich data of the pellet, the FeO content of the finished magnetite ball can be quickly calculated, avoiding the disadvantages of long testing time and large error rate, and providing rapid guidance for the operation adjustment of the magnetite pellet production line. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 A schematic diagram of the structure of a pellet provided in the method for rapid analysis of FeO content in a magnetite pellet in an embodiment of the present invention; DETAILED DESCRIPTION
[0021] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.
[0022] See also Figure 1 , the incomplete reaction core model theory of magnetite pellets. Fine-grained magnetite concentrate (-200 mesh ratio of more than 80%) is made into 10-18mm green balls with a FeO content of 10-30% through the ball-making process. After the green balls enter the roasting process, under the action of high-temperature air, the oxidation of magnetite concentrate particles first occurs on the surface of the pellets (FeO is oxidized to Fe2O3). As the reaction proceeds, the reaction interface gradually advances inward until the reaction is complete, that is, the incomplete reaction core model, such as Figure 1 shown.
[0023] 1) Prepare a ball-peen hammer. Parameters: hammer face diameter 30mm, hammer head width 80mm, handle length 335mm;
[0024] 2) Make a ball smashing device. The ball smashing device consists of 3 components, all made of ordinary steel. Key parameter design: the distance between steel plate A and steel part B is 8mm; the height of steel part B is 30-50mm; the height of steel plate A is about 7mm higher than the height of steel part B.
[0025] 3) Take samples (10-16mm pellets) and smash them to measure the "sandwich" data. The pellets are placed on the steel part B of the smashing device (close to the steel plate A); the tester uses a round hammer to smash the finished ball. Under the shear force between the hammer head and the steel part B of the smashing device, the pellets are split into two pieces (to avoid crushing the pellets and to facilitate observation of the internal roasting of the pellets). If there is a sandwich structure, measure the cross-sectional diameter of one piece and the corresponding sandwich diameter.
[0026] If there is no sandwich structure, the core diameter of the pellet is 0 mm.
[0027] 4) Using the same method, break open 10 pellets and measure the cross-sectional diameter of each ball and the corresponding core diameter.
[0028] 5) By designing a calculation table for the FeO content of pellets in an EXCEL table, inputting the measured data such as the sandwich diameter and cross-sectional diameter, the FeO content of pellets can be automatically calculated. The formula for calculating the FeO content of pellets is as follows:
[0029] As shown in the table below, the calculation table consists of two parts: input column and output column.
[0030] (1) The input column items include the cross-sectional diameter D of the pellet, the core diameter d, the initial FeO content W1 of the pellet, the correction coefficient A of the FeO content in the core structure, and the FeO correction value B of the pellet.
[0031] ①Cross-sectional diameter D. Measured after the ball is smashed.
[0032] ②Sandwich diameter d. It is measured after the ball is smashed. The sandwich diameter and cross-sectional diameter of the same ball should be measured on the same cross-section.
[0033] ③ The initial FeO content of the pellets W1. Calculated based on the FeO content of each raw material and the raw material ratio, the calculation formula is:
[0034] The initial FeO content of the pellet W1 = ∑ the amount of FeO brought into the pellet by various raw materials.
[0035] ④ Correction coefficient A for the FeO content in the sandwich structure. Since the oxidation reaction does not occur in the sandwich structure of the pellet, but the oxidation reaction is not complete, the FeO content in the sandwich structure needs to be corrected. The correction coefficient value range should be greater than 0 and less than 1. The specific value is determined by the corresponding experiment of the pellet sandwich data and the FeO content of the finished ball.
[0036] ⑤ Pellet FeO correction value B. In actual production, when the balls are smashed, 10 pellets have no sandwich structure, but the FeO content of the pellets is measured to be between 0.15% and 0.30%, so the FeO content needs to be corrected again.
[0037] (2) The output column items include single ball FeO content W2 and finished ball FeO content W.
[0038] ① The FeO content of a single ball is calculated by the cross-sectional diameter, the core diameter, the initial FeO content of the pellet, and the correction coefficient of the FeO content of the core structure. The calculation formula is:
[0039]
[0040] ② FeO content of finished ball W. FeO content of finished ball W = average value of FeO content of 10 single balls.
[0041] Example of calculation table for FeO content in pellets
[0042]
[0043] Implementation effect:
[0044] (1) Effect of the invention: By quickly and accurately analyzing the FeO content of magnetite pellets, the operating parameters are adjusted quickly, and the stability of the FeO content of the pellets is greatly improved. Ma Steel's 2.2 million tons / year chain grate-rotary kiln runs this method. By sampling the finished product belt every shift to determine the FeO content of the finished ball, the operating parameters are adjusted in time. The FeO content of the pellets has dropped from 0.72% to about 0.35%, a decrease of 51.38%, and the proportion of FeO in the pellets exceeding 1.0% has dropped from about 30% to less than 1%.
[0045] (2) Benefit calculation
[0046] 1) For every 1% decrease in FeO content in the raw materials, the coke ratio of the blast furnace decreases by 1%. The original average FeO content of the pellets was 0.72%, and the current average FeO content of the pellets is 0.35%. 3 The cost data of blast furnace is calculated as follows: Class A metallurgical coke is RMB 1,813 / ton, blast furnace coke ratio is 371Kg / t-TFe, blast furnace monthly output is 511,100 tons, pellet ore ratio entering the furnace is 20%, and annual benefit = (0.72-0.35) × 371÷1000 × 51.11 × 1% × 1813 × 12 × 20% = RMB 3,052,700.
[0047] 2) The operating parameters have been optimized, and the gas consumption of the pellet production line has been greatly reduced, with significant cost reduction benefits. By quickly determining the FeO of pellets and adjusting the operating parameters in time, the gas consumption has been reduced to 0.587GJ / t, and the annual benefit has reached more than 6.5858 million yuan.
[0048] Through calculation, the direct economic benefits reached more than 9.6385 million yuan per year. In addition, the indirect benefits brought by extending the service life of key equipment on the production line and reducing pollutant emissions are also very obvious.
[0049] After adopting the above scheme, the time required for analyzing the FeO content of pellets is greatly reduced. This method can calculate the FeO content of pellets by simply measuring the core diameter of the pellets. The whole process takes about 5 minutes, which is about 175 minutes less than the original analysis method (potassium dichromate volumetric method), basically realizing online analysis of the FeO content of pellets.
[0050] The analysis results are highly accurate. The potassium dichromate volumetric method for detecting FeO in pellets is affected by reagents, instruments, sampling, sample preparation and analysis, and often results in large errors. Experiments have shown that this method only measures the core diameter of the pellets to calculate the FeO content in the pellets, avoiding the influence of reagents, instruments, sampling, sample preparation and analysis, and is conducive to improving the accuracy of the analysis results.
[0051] The analysis process and analysis tools are simple and highly operable.
[0052] It can realize the integrated analysis of pellet compressive strength and FeO content. The ball smashing device can be upgraded and modified to add mechanical transmission system, force measurement control system and image distance measurement system, etc., so as to realize that the machine ball pressing replaces manual ball smashing, automatically measure the core diameter of the pellet, automatically calculate the FeO content of the pellet, and display the crushing strength of the pellet at the same time.
[0053] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the specific implementation of the present invention is not limited to the above-mentioned method. As long as various non-substantial improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A rapid analysis method for FeO content in magnetite pellets, characterized in that: The steps include: 1) Prepare a ball-peen hammer; 2) Sampling: Take pellets with a particle size of 10 to 16 mm, hit the pellets with a round hammer, and measure the data of the cracked pellets; the data includes the cross-sectional diameter of the pellets and the corresponding diameter of the incompletely reacted core; if there is no incompletely reacted core structure, the incompletely reacted core diameter of the pellet, i.e., the core diameter, is 0 mm; 3) Break open 10 pellets and measure the cross-sectional diameter of each ball and the corresponding sandwich diameter; 4) By designing a calculation table for the FeO content of the pellets in an EXCEL table, inputting the measured sandwich diameter and cross-sectional diameter data, the FeO content of the pellets can be automatically calculated; The above step 4) includes the following steps: 4.1) The input column items include the cross-sectional diameter D of the pellet, the core diameter d, the initial FeO content W1 of the pellet, the correction coefficient A of the FeO content of the core structure, and the FeO correction value B of the pellet; 4.2) Output column items include single ball FeO content W2, finished ball FeO content W; In the above step 4.1), the correction coefficient A of the FeO content in the sandwich structure: since the pellet sandwich structure does not mean that the oxidation reaction does not occur, but that the oxidation reaction is not complete, the FeO content in the sandwich structure needs to be corrected. The correction coefficient value range should be greater than 0 and less than 1. The specific value of the correction coefficient A is determined by the corresponding experiment of the pellet sandwich data and the FeO content of the finished ball; In the above step 4.1), the pellet FeO correction value B: in actual production, when the pellets are smashed, 10 pellets have no sandwich structure, but the FeO content of the pellets is measured to be between 0.15% and 0.30%, so the FeO content needs to be corrected again; In the above step 4.2), the FeO content of a single ball is calculated by the cross-sectional diameter, the core diameter, the initial FeO content of the pellet, and the correction coefficient of the FeO content of the core structure. The calculation formula is:
2. The rapid analysis method for FeO content in magnetite pellets according to claim 1, characterized in that: In the above step 4.1), cross-sectional diameter D: measured after ball smashing; core diameter d: measured after ball smashing, the core diameter and cross-sectional diameter of the same ball should be measured on the same cross-section; initial FeO content of pellets W1: calculated based on the FeO content of the raw materials and the raw material ratio, the calculation formula: initial FeO content of pellets W1 = ∑ the amount of FeO brought into the pellet ore by various raw materials.
3. The rapid analysis method of FeO content in magnetite pellets according to claim 2, characterized in that: In the above step 4.2), the FeO content W of the finished ball is: the FeO content W of the finished ball = the average value of the FeO content of 10 single balls.
Citation Information
Patent Citations
Online soft measurement method of magnetite oxygenation efficiency distribution in grate pellet material layer
CN102866240A
Manufacturing method of diamond sandwich-type enhanced tungsten carbide composite spherical crown button
CN106670472A