A high frequency silicon germanium heterojunction bipolar transistor and a method for manufacturing the same
By introducing SOI structure and high-stress Si3N4 cover layer into SiGeHBT devices and applying uniaxial compressive stress, the problem of device frequency performance limit is solved, and higher frequency characteristics and good integration with CMOS processes are achieved.
Patent Information
- Application Number
- CN202010642151.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-07-06
AI Technical Summary
Existing SiGeHBT devices have limitations in improving frequency performance, which is difficult to meet the needs of high-frequency applications, and traditional processes are difficult to integrate well with CMOS processes.
The SOI structure is formed on a single crystal Si substrate, an insulating layer and SiO2 material are introduced, and a high-stressed Si3N4 cover layer is deposited using a dual-frequency radio frequency power supply PECVD, and a uniaxial compressive stress is applied, which changes the energy band structure of the device and is in the base area. The step-type distribution of Ge components is introduced to form a new SOI SiGe HBT structure.
It improves the carrier mobility, increases the frequency characteristics and amplification coefficient of the device, reduces the base area resistance, increases the cutoff frequency and highest oscillation frequency of the device, and is easier to integrate with the CMOS process.
Smart Images

Figure CN111739939B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electronic technology and relates to a high-frequency silicon-germanium heterojunction bipolar transistor and a manufacturing method thereof. Background Art
[0002] As integrated circuits continue to move toward smaller process nodes, the cutoff frequency f of silicon-based active devices T and the maximum oscillation frequency f max Gradually entering the terahertz frequency band. Compared with traditional III-V semiconductor devices, silicon-based solid-state terahertz devices have the technical advantages of low cost, easy mass production, and compatibility with ultra-large-scale integrated circuit processes, and have gradually attracted the attention of countries around the world. In the 0.1-1 THz frequency band, due to the huge potential and technical advantages shown in SiGeBiCMOS benchmark circuits and system applications, SiGeHBT has become the core device of silicon-based high-frequency integrated circuits. Therefore, research institutions and scholars at home and abroad are committed to using various technical means to optimize its frequency performance and fully tap its potential in high-frequency applications.
[0003] SiGe heterojunction bipolar transistor (HBT) is a silicon-based bipolar junction transistor (BJT) with a small amount of Ge added to its base. The use of SiGe material in the base significantly improves device performance, making SiGeHBT a standard bipolar transistor in high-speed applications. Developed on the basis of mature silicon technology, the heterojunction bipolar transistor (HBT) based on silicon germanium (SiGe) technology takes advantage of the "band engineering" and solves the contradiction between increasing the amplification factor and improving the frequency characteristics. However, there is a limit to relying solely on this technology to improve device performance.
[0004] Research has found that strained Si technology can improve carrier mobility, shorten carrier transit time, and effectively improve device performance. SOI technology can not only reduce the parasitic capacitance effect generated by the PN junction, the power consumption of the device, and reduce production costs, but also speed up the device's operating speed, improve the device's radiation resistance, and wafer utilization. Therefore, using advanced silicon-based SOI technology and continuously reducing the device's feature size, combined with strained Si technology, can greatly improve the device's key performance parameters such as frequency, Early voltage, and breakdown voltage. Summary of the invention
[0005] In view of this, an object of the present invention is to provide a high-frequency silicon-germanium heterojunction bipolar transistor and a method for manufacturing the same.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a high-frequency silicon-germanium heterojunction bipolar transistor comprises the following steps: depositing a buried oxide layer on a single crystal Si substrate, so that the buried oxide layer, the single crystal Si substrate and the Si material in the collector region form an SOI structure, that is, Si on an insulating substrate, wherein the structure has three layers, namely, introducing an insulating layer (mostly SiO2 material) between the top Si material and the substrate Si material; performing boron ion implantation at the collector region corresponding to the base window, and performing a rapid annealing operation to eliminate lattice damage; etching a groove at one end of the collector region to form an STI isolation region, etching another groove, and depositing and filling heavily doped Si material; adopting a step-type distribution of Ge components in the base region; depositing a single crystal Si thin layer as a "cap layer" above the base region; depositing N+ polysilicon on the single crystal Si thin layer as an emitter; using a dual-frequency radio frequency power supply PECVD to deposit a high-stress cover layer Si3N4 material, and etching an emitter window and a base region window; and performing a mirror operation after the stress is introduced.
[0008] The high-stress cap layer Si3N4 material is deposited using dual-frequency RF power PECVD. By using this method, it is easy to transfer its own intrinsic stress to the silicon channel. The applied stress changes the energy band structure of the device, enhances the carrier mobility, and improves the performance of the device. At the same time, due to the different lattice constants of Si and Ge, the high-frequency silicon-germanium heterojunction bipolar transistor designed in this paper is also subject to biaxial stress.
[0009] The external base region outside the SiGe base region is located in the substrate, rather than in the area above the substrate like the conventional SiGe HBT. The advantage of this is that while maintaining a low base series resistance, it effectively increases the junction area of the collector junction, improves the device's amplification factor and frequency, and is easier to integrate with complementary metal oxide semiconductor CMOS.
[0010] According to the physical theory of semiconductor devices, the cutoff frequency f of SOI SiGe HBT is T It can be written as:
[0011]
[0012] τ ec,SOISiGe It includes base region transit time, delay time caused by discontinuity of emitter junction energy band, emitter transit time, collector junction space charge region transit time and collector junction capacitance charging time. ec,SOISiGe It can be written as:
[0013]
[0014] The uniaxial compressive stress introduced in the base region splits the valence band energy band, with the heavy hole band leaving the top of the valence band and the light hole band remaining at the top of the valence band, thereby reducing the effective conductivity mass of the holes in this direction, enhancing the carrier mobility, and reducing the total carrier transit time, thereby increasing the device cutoff frequency.
[0015] f T The relationship with fmax is:
[0016]
[0017] r b is the base resistance. The introduction of stress has no effect on the concentration of the device, but it will enhance the mobility of carriers, so the base resistance will decrease as the mobility of carriers increases. From the above expression, it can be seen that the maximum oscillation frequency is proportional to the cutoff frequency and inversely proportional to the base resistance. Since the cutoff frequency f T increases, the base resistance decreases, so the maximum oscillation frequency f max Increase.
[0018] The beneficial effects of the present invention are: organically combining mature silicon-based integrated circuit technology with rapidly developing SiGe technology, SOI technology and "strain technology", and forming a new SOI SiGe HBT new structure in the terahertz frequency band by introducing uniaxial stress in the base region. The uniaxial stress applied in the base region causes the valence band energy band to split, the heavy hole band leaves the top of the valence band, and the light hole band remains at the top of the valence band, thereby reducing the effective conductivity mass of the holes in this direction, enhancing the mobility of the carriers, and reducing the total transit time of the carriers, thereby improving the cutoff frequency of the device.
[0019] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0021] Figure 1 A schematic diagram of the device structure of a high-frequency silicon-germanium heterojunction bipolar transistor provided by the present invention;
[0022] Figure 2 This is a schematic diagram of a method for manufacturing a high-frequency silicon-germanium heterojunction bipolar transistor in case 1;
[0023] Figure 3A schematic diagram of a method for manufacturing a high-frequency silicon-germanium heterojunction bipolar transistor for case 2;
[0024] Figure 4 The schematic diagram of the method for manufacturing a high frequency silicon germanium heterojunction bipolar transistor is shown in case 3;
[0025] Figure 5 A schematic diagram of a method for manufacturing a high frequency silicon germanium heterojunction bipolar transistor for case 4;
[0026] Figure 6 A schematic diagram of a method for manufacturing a high-frequency silicon-germanium heterojunction bipolar transistor for case 5;
[0027] Figure 7 This is a schematic diagram of the method for manufacturing a high-frequency silicon-germanium heterojunction bipolar transistor for case six. DETAILED DESCRIPTION
[0028] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and the features in the embodiments can be combined with each other without conflict.
[0029] Among them, the drawings are only used for illustrative explanations, and they only represent schematic diagrams rather than actual pictures, and should not be understood as limitations on the present invention. In order to better illustrate the embodiments of the present invention, some parts of the drawings may be omitted, enlarged or reduced, and do not represent the size of actual products. For those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted.
[0030] The same or similar numbers in the drawings of the embodiments of the present invention correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right", "front", "rear", etc. indicate the orientation or position relationship, they are based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the terms describing the position relationship in the drawings are only used for illustrative purposes and cannot be understood as limiting the present invention. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0031] Figure 1 This is a schematic diagram of the device structure of the high-frequency silicon-germanium heterojunction bipolar transistor provided by the present invention. Figure 2 to Figure 7, is a schematic diagram of a method for manufacturing a high-frequency silicon-germanium heterojunction bipolar transistor provided by the present invention, the method comprising:
[0032] 100 A Si substrate with a crystal orientation of (100) and a thickness of 100 nm is prepared;
[0033] A buried oxide layer BOX composed of SiO2 material with a thickness of 190nm is grown on the 101Si substrate material;
[0034] A collector region of Si material is grown on the buried oxide layer BOX. The collector region is divided into two parts. The sub-collector region 102 near the buried oxide layer BOX has a thickness of 120 nm and is doped with P impurities with an impurity concentration of 1.1×10 19 cm -3 The collector region 103 above the sub-collector region has a thickness of 190 nm and is doped with P impurities with an impurity concentration of 1.5×10 17 cm -3 At this time, the SOI structure is as follows Figure 2 As shown;
[0035] Si3N4 material is grown above the collector region, and the Si3N4 material is etched at the position corresponding to the base window. Boron (B) ions are implanted into the etched area to form a P+ intrinsic base region 104. The dose of implanted boron ions is 4×10 13 cm -3 ,After ion implantation, rapid thermal annealing is required to restore the structure and eliminate lattice damage;
[0036] SiO2 material is deposited to form shallow trench isolation 105, the position corresponding to the collector window is etched, and heavily doped Si material 106 is deposited, with P as the doping impurity and the impurity concentration of 1.1×10 19 cm -3 , the device structure at this time is as follows Figure 3 As shown;
[0037] A base region 107 with a thickness of 38 nm is formed above the collector region 103 and part of the P+ inner base region 104. The Ge component of the base region is distributed in a stepped manner. The portion close to the collector region 103 is a SiGe material with a thickness of 16 nm and a Ge component of 30%. The portion close to the emitter region 108 is a SiGe material with a thickness of 16 nm and a Ge component of 17%. The portion between the two portions is a SiGe material with a thickness of 6 nm and a Ge component ranging from 30% to 17%. The impurity doped in the entire base region is B with a concentration of 4×10 18 cm -3 ;
[0038] Deposit strained Si material to form a single crystal Si thin layer 108, deposit N+ polysilicon 109, etch away the polysilicon outside the emitter area, deposit SiO2 material with a thickness of 20nm, form a sidewall 110 outside the N+ polysilicon, deposit N+ polysilicon, and finally retain the N+ polysilicon in the area corresponding to the emitter window. The device structure at this time is as follows: Figure 4 As shown;
[0039] The high stress capping layer Si3N4 material 111 is deposited by dual-frequency RF power PECVD, and the capping layer Si3N4 material provides uniaxial compressive stress. At this time, the device structure is as follows Figure 5 As shown;
[0040] Deposit isolation SiO2 material and deposit base P+ polysilicon 112 with an impurity concentration of 4×10 18 cm -3 , and then etch it to deposit the isolation SiO2 material. The device structure at this time is as follows Figure 6 As shown;
[0041] Deposit collector region N+ polysilicon 113 with an impurity concentration of 1×10 18 cm -3 , metal aluminum 114 is sputtered on the entire device structure to form a metal electrode material, and the area outside the electrode is photolithographically processed. At this time, the device structure is as follows Figure 7 .
[0042] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A high frequency silicon germanium heterojunction bipolar transistor, characterized in that: include, The crystal plane is (100) single crystal Si substrate; A buried oxide layer is deposited on the single crystal Si substrate, and the single crystal Si substrate and the Si material of the collector region form an SOI structure; Boron ions are implanted into the collector region corresponding to the base window; A groove 1 is etched at one end of the collector region to form an STI isolation region, and a groove 2 is deposited to fill the heavily doped Si material; The Ge component of the base region is distributed in a stepped manner; A shallow trench isolation (105) is located between the collector region (103) and the deposited heavily doped Si material (106), and Ge is located on the collector region (103); A thin layer of single-crystal Si is deposited above the base region as a "cap layer"; N+ polysilicon is deposited on the single crystal Si thin layer as the emitter; Use dual-frequency RF power PECVD to deposit high-stress cap layer Si3N4 material, and etch emitter window and base window; The external base region outside the SiGe base region is partially located in the substrate to increase the amplification factor and frequency of the device; In the SOI SiGe HBT heterojunction bipolar transistor structure with uniaxial compressive stress in the base region, a high-stress cap layer Si3N4 material is deposited using a dual-frequency radio frequency power supply PECVD to transfer the intrinsic stress to the emitter region and the base region, as well as the collector region surface. The applied stress changes the energy band structure of the device and enhances the carrier mobility; At the same time, the lattice constants of Si and Ge are different, so that the base region of the high-frequency silicon-germanium heterojunction bipolar transistor is subjected to the uniaxial stress caused by the Si3N4 material and the biaxial stress caused by the substrate, forming a uniaxial strained emission region and a composite strained base region.
2. A method for manufacturing a high-frequency silicon-germanium heterojunction bipolar transistor, characterized in that: The method is: The crystal plane is selected as (100) single crystal Si substrate; Depositing a buried oxide layer on a single crystal Si substrate to form an SOI structure with the single crystal Si substrate and the Si material of the collector region; Performing boron ion implantation at the collector region corresponding to the base window, and performing a rapid annealing operation to eliminate lattice damage; A groove is etched at one end of the collector region to form an STI isolation region, and another groove is etched to deposit and fill heavily doped Si material; The Ge component in the base region adopts a step-type distribution; Deposit a thin layer of single-crystal Si on the base region as a "cap layer"; Deposit N+ polysilicon as the emitter on the single crystal Si thin layer; Use dual-frequency RF power PECVD to deposit high-stress cap layer Si3N4 material, and etch out emitter window and base window; The external base region outside the SiGe base region is partially located in the substrate to increase the amplification factor and frequency of the device; After the high-stress covering layer Si3N4 material is deposited using a dual-frequency RF power supply PECVD, its own intrinsic stress is transferred to the silicon channel. The applied stress changes the energy band structure of the device and enhances the carrier mobility. At the same time, the lattice constants of Si and Ge are different, so that the base region of the high-frequency silicon-germanium heterojunction bipolar transistor is subjected to the uniaxial stress caused by the Si3N4 material and the biaxial stress caused by the substrate, forming a uniaxial strain emission region and a composite strain base region.