A hollow fiber composite membrane, preparation method and application thereof

By embedding permeable layer in the MABR composite membrane and using hydrophobic materials and polydimethylsiloxane and other materials, the problem of poor strength of the composite membrane is solved, the stability and service life of the membrane are improved, and it is suitable for use in the MABR process .

CN111744370BActive Publication Date: 2024-11-12EVERBRIGHT WATER (SHENZHEN) LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010687029.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-16
Publication Date
2024-11-12
Estimated Expiration
2040-07-16

AI Technical Summary

Technical Problem

The strength of the composite membrane used in the existing MABR process is poor, which leads to prone to rupture and fall off during use, affecting the stability and service life of the membrane.

Method used

A hollow fiber composite membrane was designed. By embedding the permeability layer in the epidermis layer, the thickness of the permeability layer is controlled to be between 0.01-0.5, which improves the bonding strength between the epidermis layer and the support layer, ensuring that the epidermis layer is not prone to breaking and falling off, and The combination of hydrophobic materials and polydimethylsiloxanes is used to enhance the mechanical strength and oxygen transport performance of the film.

Benefits of technology

It improves the performance and stability of the composite membrane, extends the service life of the device, avoids peeling and falling off of the skin layer, enhances mechanical strength and oxygen transmission efficiency, and is suitable for use in MABR processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111744370B_ABST
    Figure CN111744370B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of sewage treatment, and specifically relates to a hollow fiber composite membrane, a preparation method thereof and an application thereof. The present invention relates to a hollow fiber composite membrane. A hollow fiber composite membrane of the present invention comprises a support layer, an intermediate layer and a skin layer arranged in sequence from the inside to the outside; the support layer plays a mechanical support role, the intermediate layer plays an intermediate transition role, and the skin layer is a dense functional skin layer, which plays the role of oxygen transmission and biofilm carrier; the penetration thickness of the skin layer embedded in the intermediate layer accounts for 0.01-0.5 of the thickness of the skin layer. The present invention has good mechanical strength, oxygen transmission performance and biological affinity, and is very suitable for MABR process with bubble-free aeration and oxygen supply.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sewage treatment, and in particular relates to a hollow fiber composite membrane, a preparation method thereof and an application thereof. Background Art

[0002] Membrane Aeration Bio-film Reactor (MABR) is a new type of efficient sewage treatment process that organically couples the traditional biofilm reactor process with gas membrane separation technology. MABR technology has the advantages of high oxygen transmission efficiency, low process energy consumption, good operational flexibility, modular and easy integration, etc., and has received increasing attention in the fields of sewage treatment and water body remediation.

[0003] The MABR process is different from the traditional bubbling aeration method. It uses gas membrane for bubble-free aeration. After oxygen passes through the membrane, it is directly used by microorganisms covering the membrane surface. When the gas pressure is kept lower than the membrane bubble point pressure, air or pure oxygen can enter the water body in the form of molecules, so the efficiency of microorganisms in oxygen utilization is much higher than that of traditional aeration processes.

[0004] The gas membrane plays two main roles in the MABR process, namely, providing a carrier for microbial growth and providing an oxygen source for the microorganisms attached to the membrane surface. Therefore, the MABR membrane must have the following basic properties: low mass transfer resistance and high oxygen permeability, moderate bubble point pressure, good mechanical properties and bioaffinity (CN 203139913U, a composite membrane for MABR).

[0005] At present, there are two main types of membranes actually used in the MABR process:

[0006] (1) Hydrophobic microporous membranes, represented by PTFE hollow fiber membranes and polypropylene (PP) hollow fiber membranes. Due to hydrophobicity, the membrane pores are not wetted by water, that is, water cannot spontaneously enter the membrane pores of the hydrophobic microporous membrane, but oxygen in the gas phase can directly diffuse into the biofilm and be used by microorganisms. Hydrophobic microporous membranes have the advantages of low mass transfer resistance and high oxygen transfer efficiency, but the disadvantage is that the aeration pressure is low, and as the use time increases, the micropores may be clogged by the secretions of microorganisms, causing the membrane pores to be wetted and contaminated, and the gas mass transfer resistance increases dramatically, thereby affecting the efficient conduct of the MABR process;

[0007] (2) Homogeneous dense membrane. Dense membranes are generally made of selectively permeable materials, such as polydimethylsiloxane (PDMS). Since the dense membrane structure has no micropores, there is no need to worry about pollution and clogging. However, its fatal weakness is that the transfer of oxygen is completely controlled by the solubility diffusion coefficient of the membrane material, and the oxygen mass transfer efficiency is low. In addition, PDMS materials also have the disadvantages of high cost, poor mechanical strength, and easy wire breakage during use, which limits their large-scale practical application.

[0008] In view of the above problems, people have tried to couple the structures of the above two membranes to develop a composite membrane, that is, a selectively permeable membrane with high permeability composed of a selectively permeable skin layer and a porous support layer (CN 203139913 U, a composite membrane for MABR; CN 103182254 B, a composite membrane for MABR and a preparation method). Theoretically, the composite membrane is the most suitable membrane for the MABR process. The selectively permeable skin layer material can be PDMS, which has good air permeability and certain oxygen and nitrogen separation performance; the optimal choice of the porous support layer is PTFE, which has good hydrophobicity, high mechanical strength, and low air permeability pressure, which helps to reduce operating energy consumption. However, since the surface pore size of the PTFE microporous membrane is generally large (>0.1μm), when the PDMS layer is prepared by solution coating, heating, and cross-linking, the coated PDMS solution is very easy to leak into the membrane pores due to the large pores of the base membrane, resulting in the inability of the cross-linked product to complete the bridging and collapse, so that the prepared PDMS layer has a large number of defects and cannot form a dense structure. In addition, the PDMS layer is very easy to break and fall off during use, making it difficult to produce a hollow fiber composite membrane with good practicality and stability. Summary of the invention

[0009] 1. Problem to be solved

[0010] In view of the problem of poor strength of the epidermis layer of the composite membrane in the prior art, the present invention provides a hollow fiber composite membrane, in which the epidermis layer is embedded in the permeation layer of the middle layer, which accounts for 0.01-0.5 of the thickness of the epidermis layer. The permeation layer improves the bonding strength between the two layers, making the epidermis layer less likely to break and fall off, thereby solving the problem of poor strength of the epidermis layer.

[0011] Furthermore, the present invention also provides an application of a hollow fiber composite membrane in the MABR process, using a composite membrane with better mechanical strength and stability, thereby extending the service life of the device.

[0012] Furthermore, the present invention also provides a method for preparing a hollow fiber composite membrane, in which a support layer, an intermediate layer and a skin layer are prepared in sequence, and the thickness of the permeation layer in which the skin layer is embedded in the intermediate layer is controlled to be 0.01-0.5 of the skin layer. The process is simple, and a hollow fiber composite membrane with good practicality and stability can be easily prepared with a high yield.

[0013] 2. Technical solution

[0014] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0015] The present invention provides a hollow fiber composite membrane, comprising a support layer, an intermediate layer and a skin layer which are arranged in sequence from the inside to the outside; the average pore size of the side of the intermediate layer away from the support layer is P1, the average pore size of the side of the intermediate layer in contact with the support layer is P2, P1<P2; the permeation thickness of the skin layer embedded in the intermediate layer is H1, the thickness of the skin layer is H2, H1:H2=0.05-0.5.

[0016] Preferably, the support layer has a pore size of 1-5 μm and a porosity of 60%-85%, and / or the average pore size of the intermediate layer on a side away from the support layer is P1, and P1=10-50 nm.

[0017] Preferably, the penetration thickness of the intermediate layer embedded in the support layer is H3, the thickness of the intermediate layer is H4, and H3:H4=0.1-0.5.

[0018] Preferably, the thickness of the middle layer is H4, H4=20-100 μm, and the thickness of the skin layer is H2, H2=0.5-10 μm.

[0019] Preferably, the supporting layer and the intermediate layer are both made of fluorine-containing compounds.

[0020] Preferably, the material of the epidermis layer is polydimethylsiloxane.

[0021] Preferably, the supporting layer is made of polytetrafluoroethylene; the intermediate layer is made of a hydrophobic material, and the hydrophobic material is polyvinylidene fluoride.

[0022] The present invention also provides an application of the hollow fiber composite membrane for MABR in a MABR process.

[0023] The present invention also provides a method for preparing a hollow fiber composite membrane, the specific steps of which are as follows:

[0024] S100, preparation of a support layer: mixing a raw material and a solvent and then ripening them, and then subjecting the ripened mixture to a paste extrusion, stretching and sintering process in sequence to obtain a support layer; the support layer has an average pore size of 1-5 μm and a porosity of 60%-85%;

[0025] S200, preparing a support layer / intermediate layer composite membrane, coating the support layer with a solution, solidifying by phase transformation and forming, to obtain a support layer / intermediate layer composite membrane; the average pore size of the side of the intermediate layer away from the support layer of the support layer / intermediate layer composite membrane is P1, and the average pore size of the side of the intermediate layer in contact with the support layer is P2, P1<P2, and P1=10-50nm;

[0026] S300, preparation of a support layer / middle layer / skin layer composite membrane, applying a coating liquid to the support layer / middle layer composite membrane, and obtaining a support layer / middle layer / skin layer composite membrane after heating; the skin layer of the support layer / middle layer / skin layer composite membrane is embedded in the middle layer with a penetration thickness of H1, and the thickness of the skin layer is H2, H1:H2=0.05-0.5.

[0027] Preferably, the solution coating in S200 further comprises applying pressure, and the applied pressure value is 0.05-0.5 atm.

[0028] 3. Beneficial effects

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) In the hollow fiber composite membrane of the present invention, the support layer plays a mechanical supporting role, the middle layer plays an intermediate transition role, and the epidermis is a dense functional cortex layer, which plays the role of oxygen transmission and biofilm carrier; the middle layer is firmly combined with the support layer and the epidermis, and the epidermis has a certain permeability thickness, which improves the bonding strength between the two layers, avoids peeling and falling off during actual use, enhances the performance of the composite membrane, prolongs its service life, and solves the problem of poor strength of the epidermis of the composite membrane in the prior art.

[0031] (2) In a hollow fiber composite membrane of the present invention, the pore size of the support layer defines its macroporous structure, and its porous characteristics are conducive to reducing gas transfer resistance; when the pore size is 1-5 μm, the middle layer has a certain permeability thickness relative to the support layer, which enhances the mechanical strength of the composite membrane and prevents the middle layer from falling off; and the thickness of the epidermis determines the oxygen permeation flux of the composite membrane.

[0032] (3) In the hollow fiber composite membrane of the present invention, the support layer and the middle layer are both made of hydrophobic materials, which can prevent the wetting of the membrane pores caused by condensation of water vapor during use and will not increase the oxygen mass transfer resistance; the middle layer and the support layer are both fluorine-containing compounds with good affinity, and no peeling problem will occur between the two layers; moreover, when the surface layer is polydimethylsiloxane and the middle layer is polyvinylidene fluoride, the middle layer and the surface layer also have a good bonding ability to avoid peeling.

[0033] (4) The application of a hollow fiber composite membrane in the MABR process of the present invention uses a composite membrane with better mechanical strength and stability, thereby extending the service life of the device.

[0034] (5) The method for preparing a hollow fiber composite membrane of the present invention has a simple preparation process, and the composite membrane is prepared by applying different degrees of pressure, with a high yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a structural schematic diagram of the present invention;

[0036] Figure 2 It is a cross-sectional schematic diagram of the present invention.

[0037] Among them: 100, support layer; 200, middle layer; 210, permeation layer II; 300, epidermis layer; 400, cavity. DETAILED DESCRIPTION

[0038] The present invention is further described below in conjunction with the accompanying drawings. The present invention is described in detail below in conjunction with specific exemplary embodiments. However, it should be understood that various modifications and variations can be made without departing from the scope of the present invention as defined by the appended claims. The detailed description and the accompanying drawings should be considered only as illustrative, not restrictive, and if there are any such modifications and variations, they will fall within the scope of the present invention described herein. In addition, the background technology is intended to illustrate the current status and significance of the research and development of the present technology, and is not intended to limit the present invention or the application field of the present application and the present invention.

[0039] Example 1

[0040] The present invention provides a hollow fiber composite membrane that can be used in MABR technology. Figure 1 As shown, the hollow fiber composite membrane includes a support layer 300, an intermediate layer 200 and a skin layer 100, wherein the intermediate layer 200 is disposed between the support layer 300 and the skin layer 100 to solve the problem that the skin layer 100 is easily peeled off when directly covering the support layer 300. Figure 2 As shown, a cavity 400 for gas to pass through is provided in the hollow fiber composite membrane, and a support layer 300, an intermediate layer 200 and a skin layer 100 are arranged in sequence from the cavity 400 to the outside.

[0041] The support layer 300 is a macroporous support base membrane layer, which plays a mechanical support role to avoid wire breakage during use, and its tensile strength is >20MPa. When the pore size is 1-5μm and the porosity is 60%-85%, the hydrophobic and porous properties are conducive to reducing the gas transmission resistance. The support layer 300 and the intermediate layer 200 are both made of fluorine-containing compounds. Further explanation, the support layer 300 is generally polytetrafluoroethylene (PTFE).

[0042] The intermediate layer 200 is a mesoporous membrane transition layer, which plays an intermediate transition role, firmly combines the support layer 300 and the epidermis layer 100, and realizes the uniform and defect-free preparation of the epidermis layer 100. The intermediate layer 200 is made of a hydrophobic material, generally made of polyvinylidene fluoride (PVDF). The hydrophobic property of the intermediate layer 200 also avoids wetting caused by water vapor condensation, thereby increasing the resistance to oxygen mass transfer and other problems. The thickness of the intermediate layer 200 is H4, H4 = 20-100μm, and a permeation layer II 210 is provided between the intermediate layer 200 and the support layer 300. The permeation layer II 210 is the part where the intermediate layer 200 is embedded in the support layer 300. The thickness of the permeation layer defines the connection form between the two layers of the membrane and determines the bonding strength between the two layers. If there is no permeation layer, the two layers of the membrane will peel off and fall off during actual use, affecting the performance and life of the composite membrane. The thickness of the permeation layer II 210 is H3, and the thickness of the intermediate layer 200 is H4, H3:H4=0.1-0.5. In addition, the intermediate layer 200 is an asymmetric structure. The side of the intermediate layer 200 away from the support layer 300 is a mesoporous structure with an average pore size of P1. The side of the intermediate layer 200 in contact with the support layer 300 is a finger-like macroporous structure with an average pore size of P2, P1<P2, and P1=10-50nm. If the average pore size P1 is too large, it is impossible to achieve uniform preparation of the epidermal layer material on the intermediate layer 200. If the average pore size P1 is too small, the gas permeability of the intermediate layer 200 itself is poor and cannot meet the oxygen transfer requirements of the MABR membrane.

[0043] The epidermis 100 is a dense functional layer, generally polydimethylsiloxane (PDMS), which plays the role of oxygen transmission and biofilm carrier. Its dense structure prevents the wetting and contamination of the MABR membrane. It is worth noting that when the epidermis 100 is a PDMS layer and the middle layer 200 is a PVDF layer, the two have excellent bonding ability to prevent peeling. The thickness of the epidermis 100 is H2, H2 = 0.5-10μm. The thickness of the epidermis 100 determines the oxygen permeation flux of the composite membrane, that is, the treatment efficiency of the MABR process. A permeation layer I is provided between the epidermis 100 and the middle layer 200. The permeation layer I is the part of the epidermis 100 embedded in the middle layer 200. The thickness of the permeation layer I is H1, and the thickness of the epidermis 100 is H2, H1:H2 = 0.05-0.5. This design can improve the bonding strength between the two layers, avoid peeling and falling off during actual use, enhance the performance of the composite membrane, and extend the service life.

[0044] The present invention provides a method for preparing a hollow fiber composite membrane, and the specific steps are as follows:

[0045] S100, preparation of the support layer 100: mixing the raw materials and the solvent and then ripening them, and then subjecting the ripened mixture to paste extrusion, stretching and sintering processes in sequence to obtain the support layer 100; the average pore size of the support layer 100 is 1-5 μm, and the porosity is 60%-85%;

[0046] S200, preparation of a support layer / intermediate layer composite membrane, solution coating, phase conversion solidification and forming of the support layer 100 to obtain a support layer / intermediate layer composite membrane; the average pore size of the side of the intermediate layer 200 away from the support layer 100 of the support layer / intermediate layer composite membrane is P1, and the average pore size of the side of the intermediate layer 200 in contact with the support layer 300 is P2, P1<P2, and P1=10-50nm; the solution coating process also includes applying pressure, and the applied pressure value is 0.05-0.5atm;

[0047] S300, preparation of a support layer / middle layer / skin layer composite membrane, applying a coating liquid to the support layer / middle layer composite membrane, and obtaining a support layer / middle layer / skin layer composite membrane after heating; the thickness of the permeation layer in which the skin layer 100 of the support layer / middle layer / skin layer composite membrane is embedded in the middle layer 200 is H1, and the thickness of the skin layer 100 is H2, H1:H2=0.05-0.5.

[0048] In this embodiment, the specific preparation method is as follows:

[0049] 1) Evenly mix PTFE dispersion resin and solvent oil, with the mass fractions being 76% and 24% respectively;

[0050] 2) The uniformly mixed materials were aged at 40° C. for 12 h;

[0051] 3) loading the matured mixture into a pre-pressing device, and pre-pressing and degassing for 5 minutes at 2.0 MPa to obtain a PTFE blank;

[0052] 4) loading the prepared PTFE blank into a paste extrusion device and extruding at 60° C. to obtain a primary PTFE hollow fiber membrane;

[0053] 5) The nascent PTFE hollow fiber membrane was heat treated at 200°C for 10 min to remove the solvent oil;

[0054] 6) stretching the degreased PTFE hollow fiber membrane in the longitudinal direction by 5.0 times at 250° C. at a stretching speed of 10 m / min;

[0055] 7) The stretched PTFE hollow fiber membrane was sintered at 360° C. for 5 min to obtain a PTFE support layer having an inner diameter of 0.8 mm, an outer diameter of 1.6 mm, an average pore size of 5.0 μm, a porosity of 85%, and a tensile strength of 32 MPa;

[0056] 8) dissolving PVDF in N,N-dimethylacetamide, wherein the mass fraction of PVDF is 10%, and mechanically stirring at 80° C. for 12 h to obtain a uniform and transparent casting solution;

[0057] 9) The casting liquid is coated on the outer surface of the PTFE support layer using a homemade spinning device. During the coating process, a pressure of 0.2 atm is applied to allow the casting liquid to partially penetrate into the pores of the PTFE hollow fiber membrane, and then immersed in a hydrogel system for phase inversion, thereby obtaining a PTFE / PVDF composite membrane. The total thickness H4 of PVDF is 50 μm, the thickness H3 of the permeation layer II210 in the PTFE base membrane is 20 μm, and the PVDF middle layer is an asymmetric structure. The side close to the PTFE support layer is a finger-like macroporous structure, while the side away from the PTFE support layer has smaller surface pores, with an average pore size P1 of 10 nm;

[0058] 10) dissolving vinyl PDMS, hydrogen-containing silicone oil crosslinking agent and platinum catalyst in n-hexane with mass concentrations of 2.0%, 0.5% and 500 ppm respectively, and mechanically stirring to obtain a coating liquid;

[0059] 11) The water droplets on the surface of the PTFE / PVDF composite membrane were removed with an air knife, and the membrane was immersed in the PDMS coating solution for 1 min, which was repeated 3 times; after air drying for 5 min, the membrane was heat treated at 75°C for 120 min to obtain a PTFE / PVDF / PDMS hollow fiber composite membrane; the thickness H1 of the permeation layer I where PDMS penetrated into the PVDF membrane pores was 0.5 μm; the total thickness H2 of the PDMS epidermis was 5.0 μm.

[0060] Example 2

[0061] The basic content of this embodiment is the same as that of embodiment 1, except that a pressure of 0.05 atm is applied during the coating process, and the average pore size of the PTFE support layer in the prepared composite membrane is 3.0 μm, and the porosity is 70%. The total thickness H4 of PVDF is 20 μm, and the thickness of the permeation layer II 210 in the PTFE base membrane is H3:H4=0.5. The PVDF middle layer is an asymmetric structure, and the side close to the PTFE support layer is a finger-like macroporous structure, while the side away from the PTFE support layer has smaller surface pores with an average pore size of 30 nm. The total thickness H2 of the PDMS epidermis is 10 μm; the thickness of the permeation layer I is H1:H2=0.05.

[0062] Example 3

[0063] The basic content of this embodiment is the same as that of embodiment 1, except that a pressure of 0.5 atm is applied during the coating process, and the average pore size of the PTFE support layer in the prepared composite membrane is 1.0 μm, and the porosity is 60%. The total thickness H4 of PVDF is 100 μm, and the thickness of the permeation layer II 210 in the PTFE base membrane is H3:H4=0.1. The PVDF intermediate layer is an asymmetric structure, and the side close to the PTFE support layer is a finger-like macroporous structure, while the side away from the PTFE support layer has smaller surface pores with an average pore size of 50 nm. The total thickness H2 of the PDMS epidermis is 2 μm; the thickness of the permeation layer I is H1:H2=0.5.

[0064] Comparative Example 1

[0065] The basic content of this comparative example is the same as that of Example 1, except that the specific preparation steps are as follows:

[0066] 1) Evenly mix PTFE dispersion resin and solvent oil, with the mass fractions being 76% and 24% respectively;

[0067] 2) The uniformly mixed materials were aged at 40° C. for 12 h;

[0068] 3) loading the matured mixture into a pre-pressing device, and pre-pressing and degassing for 5 minutes at 2.0 MPa to obtain a PTFE blank;

[0069] 4) loading the prepared PTFE blank into a paste extrusion device and extruding at 60° C. to obtain a primary PTFE hollow fiber membrane;

[0070] 5) The nascent PTFE hollow fiber membrane was heat treated at 200°C for 10 min to remove the solvent oil;

[0071] 6) stretching the degreased PTFE hollow fiber membrane in the longitudinal direction by 5.0 times at 250° C. at a stretching speed of 10 m / min;

[0072] 7) Sintering the stretched PTFE hollow fiber membrane at 360° C. for 5 min to obtain a PTFE hollow fiber support base membrane with an inner diameter of 0.8 mm, an outer diameter of 1.6 mm, an average pore size of 5.0 μm, a porosity of 85%, and a tensile strength of 32 MPa;

[0073] 8) dissolving vinyl PDMS, hydrogen-containing silicone oil crosslinking agent and platinum catalyst in n-hexane with mass concentrations of 2.0%, 0.5% and 500 ppm respectively, and mechanically stirring to obtain a coating liquid;

[0074] 9) Remove water droplets on the surface of the PTFE membrane with an air knife, immerse in the PDMS coating liquid, stay for 1 minute, and repeat 3 times; after air drying for 5 minutes, heat treat at 75°C for 120 minutes to obtain a PTFE / PDMS hollow fiber composite membrane.

[0075] Comparative Example 2

[0076] The basic content of this comparative example is the same as that of Example 1, except that the specific preparation steps are as follows:

[0077] 1) dissolving PVDF in N,N-dimethylacetamide, wherein the mass fraction of PVDF is 10%, and mechanically stirring at 80°C for 12 hours to obtain a uniform and transparent casting solution;

[0078] 2) The casting solution was spun into a hollow fiber membrane using a homemade spinning device, and then immersed in a hydrogel system for phase inversion to obtain a PVDF-based membrane. The PVDF-based membrane has an inner diameter of 0.8 mm, an outer diameter of 1.2 mm, and a wall thickness of 200 μm. It has an asymmetric structure, with a finger-like macroporous structure on one side of the inner surface and smaller pores on the outer surface, with an average pore size of 10 nm;

[0079] 3) dissolving vinyl PDMS, hydrogen-containing silicone oil crosslinking agent and platinum catalyst in n-hexane with mass concentrations of 2.0%, 0.5% and 500 ppm respectively, and mechanically stirring to obtain a coating liquid;

[0080] 4) Remove water droplets on the surface of the PVDF base membrane with an air knife, immerse in PDMS coating liquid, stay for 1 minute, repeat 3 times; air dry for 5 minutes, heat treat at 75°C for 120 minutes, and obtain a PVDF / PDMS hollow fiber composite membrane. The depth of PDMS infiltration into the PVDF membrane pores is 0.5 μm; the total thickness of the PDMS dense membrane skin layer is 5.0 μm.

[0081] In this comparative example, the PTFE / PDMS, PVDF / PDMS and PTFE / PVDF / PDMS hollow fiber composite membranes prepared in Example 1, Comparative Example 1 and this comparative example were characterized, as shown in Table 1 below:

[0082] Table 1 Performance characterization of hollow fiber composite membrane

[0083]

[0084] It can be seen from the table that the hollow fiber composite membrane prepared in the present invention has good mechanical strength, oxygen transmission performance and bioaffinity, and is very suitable for the MABR process of bubble-free aeration and oxygen supply.

[0085] More specifically, although exemplary embodiments of the present invention have been described herein, the present invention is not limited to these embodiments, but includes any and all embodiments that are recognizable by those skilled in the art based on the foregoing detailed description, such as combinations between the various embodiments, adaptive changes and / or replacements. The limitations in the claims may be interpreted broadly based on the language used in the claims and are not limited to the examples described in the foregoing detailed description or during the implementation of the application, which examples should be considered non-exclusive. Any steps listed in any method or process claim may be performed in any order and are not limited to the order presented in the claim. Therefore, the scope of the present invention should be determined solely by the attached claims and their legal equivalents, rather than by the description and examples given above.

Claims

1. A hollow fiber composite membrane for MABR process, characterized in that: The invention comprises a support layer (300), an intermediate layer (200) and a skin layer (100) which are arranged in sequence from the inside to the outside; the average pore size of the side of the intermediate layer (200) away from the support layer (300) is P1, and the average pore size of the side of the intermediate layer (200) in contact with the support layer (300) is P2, where P1<P2; ​​a permeable layer I is arranged between the skin layer (100) and the intermediate layer (200), the thickness of the permeable layer I is H1, the thickness of the skin layer (100) is H2, and H1:H2=0.05-0.5; The support layer (300) has an average pore size of 1-5 μm and a porosity of 60%-85%; The support layer (300) and the intermediate layer (200) are both made of fluorine-containing compounds; The supporting layer (300) is made of polytetrafluoroethylene; the intermediate layer (200) is made of a hydrophobic material, which is polyvinylidene fluoride; A permeable layer II (210) is provided between the intermediate layer (200) and the support layer (300), the thickness of the permeable layer II (210) is H3, the thickness of the intermediate layer (200) is H4, and H3:H4=0.1-0.5; The epidermis layer (100) is made of polydimethylsiloxane.

2. A hollow fiber composite membrane for MABR process according to claim 1, characterized in that: The average pore size of the middle layer (200) on the side away from the support layer (300) is P1, where P1=10-50 nm.

3. A hollow fiber composite membrane for MABR process according to claim 1, characterized in that: The thickness of the intermediate layer (200) is H4, H4=20-100 μm, and the thickness of the epidermis layer (100) is H2, H2=0.5-10 μm.

4. A method for preparing a hollow fiber composite membrane for a MABR process according to any one of claims 1 to 3, characterized in that: The specific steps are as follows: S100, preparation of a support layer (300): mixing a raw material and a solvent and then ripening them, and then subjecting the ripened mixture to a paste extrusion, stretching and sintering process in sequence to obtain a support layer (300); the support layer (300) has an average pore size of 1-5 μm and a porosity of 60%-85%; S200, preparation of a support layer (300) / intermediate layer (200) composite membrane, solution coating, phase conversion solidification and forming of the support layer (300) to obtain a support layer (300) / intermediate layer (200) composite membrane; the average pore size of the side of the intermediate layer (200) away from the support layer (300) of the support layer (300) / intermediate layer (200) composite membrane is P1, and the average pore size of the side of the intermediate layer (200) in contact with the support layer (300) is P2, P1<P2, and P1=10-50nm; S300, preparation of a support layer (300) / intermediate layer (200) / skin layer (100) composite membrane, coating the coating liquid on the support layer (300) / intermediate layer (200) composite membrane, and obtaining a support layer (300) / intermediate layer (200) / skin layer (100) composite membrane after heating; the skin layer (100) of the support layer (300) / intermediate layer (200) / skin layer (100) composite membrane has a penetration thickness H1 where the skin layer (100) is embedded in the middle layer (200), and a thickness H2 where H1:H2=0.05-0.

5.

5. The method for preparing a hollow fiber composite membrane for MABR process according to claim 4, characterized in that: The solution coating of S200 also includes applying pressure, and the applied pressure value is 0.05-0.5atm.