Hot melt extruded solid-state battery pack components
Through hot melt extrusion and surface treatment technology, a coextruded multi-layer thin film battery module is formed, which solves the problems of dendrites growth and production efficiency in lithium metal anode battery packs, and achieves the production of high energy density and stability battery packs.
Patent Information
- Application Number
- CN201980017309.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-03-05
- Filing Date
- 2019-02-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2039-02-26
AI Technical Summary
Existing lithium metal anode battery packs have limited life and short circuit risk due to dendrite growth, and conventional solid-state separator materials limit high energy density and large-scale production, affecting charging rate and stability.
The thin film battery module is formed by hot melt extrusion method, which reduces the distance between particles, reduces polymer binder and increases ionic conductive materials through surface treatment, forms a coextruded multi-layer film structure, inhibits dendrites' growth, and introduces hybrid solids- Liquid cathode to improve solid-solid interface and production efficiency.
It has achieved the suppression of dendrites under high charging current, improved the life and charging rate of the battery pack, adapted to the needs of large-scale production, and improved the performance and stability of the lithium anode battery pack.
Smart Images

Figure CN111801838B_ABST
Abstract
Description
[0001] Related Applications
[0002] This disclosure claims priority to U.S. Provisional Application No. 62 / 638,657, filed on March 5, 2018, entitled “HOT MELTEXTRUDED ALL SOLID STATE BATTERIES,” the disclosure of which is incorporated herein in its entirety. Technical Field
[0003] The present disclosure relates generally to batteries and, more particularly, to solid-state batteries.
[0004] background
[0005] Unless otherwise indicated herein, the materials described in this section are not prior art to the claims in this application and are not admitted to be prior art by inclusion in this section.
[0006] Several qualities of lithium (Li) metal have prompted efforts to incorporate Li metal-based components into batteries. Li metal has a theoretical capacity of 3860 mAh / g and thus provides the highest capacity of any known anode material for Li-ion batteries. Therefore, batteries containing lithium metal or lithium alloy anodes can have higher specific energies than batteries containing anodes formed from other materials. For example, lithium / sulfur and lithium / air batteries have the potential to reach specific energies of 500 to 1000 Wh / kg or more. However, these desirable qualities are accompanied by drawbacks that prevent Li metal from being used as anodes in batteries.
[0007] In particular, batteries with Li metal anodes typically have a limited lifespan due to the formation of electronically conductive dendrite structures. During charging, Li ions move from the cathode to the anode, and vice versa during discharge. Over successive charge / discharge cycles, the Li ions have a tendency to accumulate in needle- or moss-like structures, or "dendrites," rather than being uniformly deposited. Dendrites can form for a variety of reasons, including discontinuities in the anode surface, impurities within the anode, and properties within the anode such as current density (mA / cm 2 ) during the charging process. Li ions accumulate into dendrites through continuous cycling, thereby extracting Li metal material from the anode and can cause parasitic capacity loss in the battery. Furthermore, in the worst case, the dendrites continue to grow and form a short circuit between the anode and cathode of the battery. Short circuits between battery electrodes can severely reduce the life of the battery and are potentially dangerous.
[0008] In an effort to inhibit dendrite growth, batteries with Li metal anodes typically include mechanically rigid separators, such as solid polymer materials, composite oxides, glass, and other compounds. Such materials can act as mechanical boundaries that physically constrain dendrite growth to prevent short circuits from forming within the battery. However, conventional solid separator materials have drawbacks that impose limitations on methods for forming batteries, materials and structures of batteries, and operating conditions and features of batteries.
[0009] For example, solid oxide separator materials typically require very high temperature formation processes, such as sintering, which may result in temperatures during the battery formation process that are higher than the stability temperatures of other battery components. For example, cathode active materials, typically composed of transition metal oxides (Ni, Co, Al, Fe, Mn, etc.) and phosphates, have a stability temperature lower than the extremely high sintering temperature that occurs during the sintering process. Therefore, the use of solid oxides as separator materials limits the materials that can be used for cathode active materials, or requires the formation of the battery to separate the formation of the separator and the cathode. Conventional cathode active materials, such as those listed above, may also have high solid-solid interface impedances, which can adversely affect the charge rate performance of the battery. Therefore, the use of solid separator materials may also result in batteries having reduced charge rates.
[0010] In another example, solid sulfide separator materials generally have material properties that render such materials unstable or unable to form acceptable separators embodied as thin films (e.g., having a thickness of about 20 microns or less). Thus, such materials can limit the types of batteries that can be formed.
[0011] In addition, for several conventional solid-state separator materials, the ability to inhibit dendrite formation and growth results in drawbacks that reduce the material's usefulness as a separator compared to other materials. In a typical battery, the separator is desirably not electronically conductive and chemically stable to the materials used for the anode and cathode. Many separator materials that inhibit dendrite growth have increased reactivity with battery components or exhibit reduced conductivity compared to other materials.
[0012] Additionally, as a practical consideration, separator materials are desirably amenable to mass production. However, many materials that can inhibit dendrite formation and growth are not well suited to production methods that can be mass produced. Many traditional solid-state materials require processes such as tape-casting, cold / hot pressing, sintering, and annealing, which are batch processes that are generally not output at high throughput.
[0013] Therefore, technology that allows the use of solid-state lithium anodes in high energy density batteries would be beneficial. Separator materials that can withstand high charging currents without dendrite growth would also be beneficial. Improvements in solid-solid interfaces in battery components and manufacturing improvements that allow high-volume production would also be beneficial.
[0014] Overview
[0015] According to an exemplary embodiment of the present disclosure, a method for co-extruding a battery assembly includes forming a first thin film battery assembly by hot melt extrusion, and forming a second thin film battery assembly by hot melt extrusion. The method further includes applying a surface treatment to a surface area of at least one of the first thin film battery assembly and the second thin film battery assembly, so that the surface area has at least one of the following relative to the remainder of the at least one of the first and second thin film assemblies: a reduced interparticle distance, a reduced amount of polymer binder material, and an increased amount of exposed ion conductive material. The method also includes feeding the first thin film battery assembly and the second thin film battery assembly through a co-extrusion die to form a co-extruded multilayer film. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is a schematic diagram of an exemplary embodiment of a battery formed from a thin film assembly according to the present disclosure.
[0018] Figure 2 is a schematic diagram of another exemplary embodiment of a battery pack formed from a thin film assembly according to the present disclosure.
[0019] Figure 3 is a schematic diagram of one exemplary embodiment of a twin-screw extruder apparatus that may be used to form a film assembly for a battery pack by hot melt extrusion according to the present disclosure.
[0020] Figure 4 is a flow chart depicting one exemplary embodiment of a method for forming a battery having a thin film assembly according to the present disclosure.
[0021] Figure 5 is a flow chart depicting one exemplary embodiment of a method for forming a thin film cathode according to the present disclosure.
[0022] Figure 6 is a flow chart depicting another exemplary embodiment of a method for forming a thin film cathode according to the present disclosure.
[0023] Figure 7 is a flow chart depicting one exemplary embodiment of a method for forming a thin film anode according to the present disclosure.
[0024] Figure 8is a flow chart depicting one exemplary embodiment of a method for forming a thin film diaphragm according to the present disclosure.
[0025] Fig. 9 is a flow chart depicting one exemplary embodiment of a system for coextruding multiple thin film battery components to form a coextruded multilayer film according to the present disclosure.
[0026] Fig.10 is a flow chart depicting another exemplary embodiment of a method for forming a thin film diaphragm according to the present disclosure.
[0027] Fig.11 is a flow chart depicting one exemplary embodiment of a method for forming a thin film cathode-separator bilayer according to the present disclosure.
[0028] Fig.12 is a flow chart depicting one exemplary embodiment of a method for forming a thin film separator-anode bilayer according to the present disclosure.
[0029] Fig.13 is a flow chart depicting one exemplary embodiment of a method for forming a thin film cathode-separator-anode trilayer according to the present disclosure.
[0030] Fig.14 is a flow chart depicting one exemplary embodiment of a method for forming a thin film current collector-cathode trilayer according to the present disclosure.
[0031] Fig.15 is a flow chart depicting another exemplary embodiment of a method for coextruding a plurality of thin film battery components to form a coextruded multilayer film according to the present disclosure.
[0032] Details
[0033] In order to facilitate an understanding of the principles of the present disclosure, reference is now made to the drawings and the description in the following written specification. This reference is not intended to limit the scope of the subject matter. The present disclosure also includes any changes and modifications to the illustrated embodiments and includes further applications of the principles of the embodiments as would normally occur to a person skilled in the art.
[0034] A separator for a high energy density battery pack with a lithium-based anode is introduced herein, wherein the separator is configured to inhibit dendrite growth during charging of the battery pack at a high charge rate. A method of forming one or more battery pack components by hot melt extrusion is also introduced herein. Such a method enables fine tuning of various materials and battery pack parameters. A method of forming a battery pack component by coextrusion is further introduced herein. Such a method results in improved solid-solid interfaces between battery pack components. Additionally introduced is a method of forming a hybrid solid-liquid cathode, which allows a liquid electrolyte material to be incorporated into a cathode formed using a roll-to-roll manufacturing method.
[0035] Figure 1 An exemplary battery 100 according to the present disclosure is depicted. The battery 100 includes an anode layer 102, a separator layer 104, and a cathode layer 106. In some embodiments, the battery 100 is a thin film battery having a total thickness of about 100 microns or less. In some embodiments, the battery 100 is rolled or folded to form a battery pack.
[0036] In some embodiments, the anode layer 102 includes a Li-based active material, such as Li metal or a Li alloy, for example, Li-In, Li-Sn, etc. In some embodiments, the anode layer 102 further includes a polymer binder material. Other metal-based anodes are used in other embodiments.
[0037] In some embodiments, cathode layer 106 comprises a mixture of cathode active ("CA") material, electronically conductive material, solid ion conductive ("SIC") material, primary polymer binder material, and secondary polymer binder material. Any acceptable CA material may be used, such as layered oxides, phosphates, and other variants of transition metals such as Ni, Co, Mn, Fe, Al, etc., such as lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA), lithium iron phosphate (LFP), or combinations thereof. In some embodiments, particles of CA material are coated with a surface coating comprising one or more of oxides, such as niobium oxide, titanium oxide, aluminum oxide, AlPO4, ZrP2O7, LiNbO3, MgO, ZrO2, etc., sulfides, such as lithium phosphide sulfide (LPS), fluorides, such as lithium fluoride (LiF) and aluminum fluoride (AlF), etc.
[0038] Any acceptable electronically conductive material may be used for cathode layer 106, such as carbon black ("CB"), graphite, metal particles, graphene nanosheets / flakes, carbon nanotubes, etc., or combinations thereof. The SIC material in cathode layer 106 is ionically conductive to ions transported between anode layer 102 and cathode layer 106. Any acceptable SIC material may be used for cathode layer 106, including oxides (e.g., garnets, perovskites, etc.), sulfides (e.g., argyrodite, phosphosulfides such as LGPS, etc.), glassy materials of oxides / sulfides, other chemical forms such as nitrides / phosphates, and sodium-superionic conductor (NASICON) type compounds such as Na 1+ x Zr 2 Si x P 3-x O 12 (0 ≤ x ≤ 3), and combinations thereof. Any acceptable form of SIC material may be used for cathode layer 106, such as crystalline, amorphous, or a mixture thereof.
[0039] In some embodiments, the SIC material in cathode layer 106 comprises particles of substantially uniform size. In some embodiments, the SIC material in cathode layer 106 comprises a distribution of particles of different sizes. The distribution of particles of different sizes can improve inter-particle contact and increase the amount of material per volume within cathode layer 106. In some embodiments, the particles of the SIC material in cathode layer 106 have surfaces that have been treated or modified as discussed in more detail below to reduce inter-particle contact resistance.
[0040] Any acceptable polymer material can be used for the primary polymer binder, such as polylactone, polyethylene terephthalate (PET), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyolefin, polyimide, polyester, polyamide, thermosensitive polymer, viscose or acrylic photopolymer, rubber, polymer blend, cyanoethyl polyvinyl alcohol (PVA-CN) in succinonitrile (SN), and combinations thereof. In some embodiments, the material of the primary polymer binder matches the polymer binder included in the diaphragm layer 104 as discussed below. In some embodiments, the material of the primary polymer binder is different from the material of the polymer binder of the diaphragm layer 104.
[0041] Any acceptable polymer material can be used for the secondary polymer binder. In some embodiments, the secondary polymer binder comprises an ion-conducting polymer material, such as a high molecular weight polyethylene oxide (PEO) containing a Li conductive salt. In such embodiments, the ion-conducting polymer material acts as a buffer between the SIC material and the CA material.
[0042] In some embodiments, instead of including a secondary polymer binder, cathode layer 106 includes a porous structure filled with a liquid electrolyte material. As discussed in more detail below, in some embodiments, a pore former material such as hydrophilic polyvinyl pyrrolidone (PVP) or camphor is used to form cathode layer 106 instead of a secondary polymer binder, and then the pore former material is removed by heat treatment or by solvent treatment to generate a porous structure within cathode layer 106, which is filled with a liquid electrolyte material. In such embodiments, any acceptable liquid electrolyte material can be used, such as a porous electrolyte material having a stable anion such as PF 6 , TFSI, BF 4 , ClO 4 , FSI, bis(oxalato)borate (BOB), and the like.
[0043] In some embodiments, the surface 113 of the cathode layer 106 facing the separator layer 104 has different properties than the rest of the cathode layer 106, such as by surface treatment as discussed in more detail below. For example, in some embodiments, the different properties include one or more of the following: reduced interparticle distances between SIC particles, exposure of SIC particles on the surface 113 of the cathode layer 106 relative to the rest of the cathode layer 106, or another property that results in an improved interface between the surface 113 of the cathode layer 106 and the separator layer 104. In some embodiments, the opposite surface 114 of the cathode layer has another property that is different from the rest of the cathode layer 106, such as to improve the interface between the cathode layer 106 and the current collector, reduce the interparticle distances between the SIC particles, or expose the SIC particles on the surface 114 of the cathode layer 106.
[0044] The separator layer 104 includes a main portion 108, a first surface region 110 forming an interface with the anode layer 102, and a second surface region 112 forming a second interface with the cathode layer 106. The main portion 108 includes a mixture of a main component and a minor component.
[0045] The main component includes at least one SIC material. Any acceptable SIC material can be used for the diaphragm layer 104, and any acceptable form of the SIC material can be used for the diaphragm layer 104. In some embodiments, the SIC material in the diaphragm layer 104 includes particles of substantially uniform size. In some embodiments, the SIC material in the diaphragm layer 104 includes a distribution of particles of different sizes. In some embodiments, the particles of the SIC material in the diaphragm layer 104 have a surface that has been treated or modified as discussed in more detail below to reduce inter-particle contact resistance.
[0046] The secondary component includes particles of at least one polymer binder such as polycarbonate, polylactone, PET, PVDF, PTFE, polyolefin, polyimide, polyester, polyamide, thermosensitive polymer, viscose or acrylic photopolymer, rubber, polymer blend or a combination thereof. In some embodiments, the polymer binder is ionically conductive. In some embodiments, the polymer binder is not ionically conductive. It should be understood that in embodiments where the polymer binder is not ionically conductive, the diaphragm layer 104 is still ionically conductive due to the SIC in the primary component. In some embodiments, the material stiffness of the polymer binder material causes the polymer binder material to act as a mechanical boundary that inhibits dendrite growth through the diaphragm layer 104.
[0047] The major component constitutes about 60% to about 98% of the total material of the main portion 108 of the separator layer 104 to exceed the amount of SIC material required to reach the conductivity percolation threshold in the three-dimensional composite material. In some embodiments, the major component is uniformly and evenly distributed with the minor component within the main portion 108 of the separator layer 104. In some embodiments, the major component is unevenly distributed according to a graded arrangement corresponding to the materials of the anode layer 102 and the cathode layer 106. For example, in some embodiments, the major component includes various SIC materials arranged in a gradient so that the SIC materials within the surface regions 110 and 112 are less reactive with the materials of the anode layer 102 and the cathode layer 106, respectively, than the various SIC materials in other portions of the separator layer 104.
[0048] In some embodiments, the SIC material includes a relatively high proportion of oxide-rich material in a first surface region 110 of the separator layer 104. In some embodiments, the SIC material includes a relatively high proportion of sulfide-rich material in a second surface region 112 of the separator layer 104 that interfaces with the cathode layer 106. In some embodiments, the SIC material is arranged according to a gradient that changes from a higher proportion of oxide-rich material and a lower proportion of sulfide-rich material in the first surface region 110 to a lower proportion of oxide-rich material and a higher proportion of sulfide-rich material in the second surface region 112.
[0049] In some embodiments, the first surface region 110 and the second surface region 112 comprise a mixture of materials similar to the mixture in the main portion 108. In some embodiments, the first surface region 110 and the second surface region 112 have at least one different property compared to the main portion 108 that can improve the interface with the anode layer 102 and the cathode layer 106, respectively. In some embodiments, the surface regions 110 and 112 have a lower amount of polymer binder than the main portion 108. In some embodiments, the polymer binder is completely removed from the surface regions 110 and 112. In some embodiments, the average inter-particle distance between the particles of the SIC material in the surface regions 110 and 112 is lower than the average inter-particle distance between the particles of the SIC material in the main portion 108. In some embodiments, the surface regions 110 and 112 are structured so that the particles of the SIC material are directly exposed to the anode layer 102 and the cathode layer 106, respectively. In some embodiments, the surface regions 110 and 112 are formed by applying one or more surface treatments to the material mixture of the main portion 108 as discussed in more detail below.
[0050] Figure 2Another exemplary embodiment of a battery pack 200 according to the present disclosure is depicted. The battery pack 200 includes an anode layer 202, a separator layer 204, and a cathode layer 206. The separator layer 204 includes a plurality of sublayers. In some embodiments, the separator layer includes three sublayers 204a-c. In some embodiments, the sublayer 204a forms an interface 210 with the anode layer 202, the sublayer 204c forms an interface 212 with the cathode layer 206, and the sublayer 204b is located between the sublayer 204a and the sublayer 204c. In other embodiments, the separator layer includes other numbers of sublayers.
[0051] Each of the sublayers 204a-c includes the same Figure 1 The SIC material in the sublayer 204a-c is similar to the material mixture in the main part 108 of the separator layer 104 in the battery stack 100 discussed above. However, the material mixture in the sublayer 204a-c varies in at least one property, such as structure, composition, etc. The sublayers 204a-c are arranged in the separator layer 204 to form a gradient of the at least one varying property. In some embodiments, the SIC material in the sublayer 204a includes a relatively high proportion of oxide-rich material and a relatively low proportion of sulfide-rich material, the SIC material in the sublayer 204c includes a relatively high proportion of sulfide-rich material and a relatively low proportion of oxide-rich material, and the SIC material in the sublayer 204b includes a mixture of oxide-rich material and sulfide-rich material. In such an embodiment, the sublayers 204a-c form a gradient from the relatively oxide-rich and sulfide-poor SIC material in the sublayer 204a to the relatively sulfide-rich and oxide-poor SIC material in the sublayer 204c.
[0052] In some embodiments, such as those derived from the various methods discussed below, the layers of the battery are formed by hot melt extrusion. Any acceptable hot melt extrusion method can be used, such as methods using screw extruders, ram extruders, roll extruders, gear extruders, planetary shaft extruders, etc. Figure 3 An exemplary embodiment of a twin-screw extruder 300 that can be used to form a layer of a battery pack by hot melt extrusion according to the present disclosure is depicted. The twin-screw extruder 300 includes a feed port 302, a barrel 304, a screw assembly 306, a die 308, and a heat source 310. The feed port 302 includes a first bay 312 for particles of solid materials (e.g., anode materials, cathode materials, or separator materials, depending on the layer to be extruded) and a second bay 314 for polymeric materials. The feed port 302 is configured to feed a mixture of solid materials and polymeric materials into the barrel 304 at relative rates corresponding to the proportions of those materials present in the resulting layer.
[0053] The screw assembly 306 includes a pair of screws 316 including a first threaded portion 318, a second threaded portion 320, and a mixing portion 322 located between the threaded portions 318 and 320. The screw assembly 306 is disposed within the barrel 304 such that the first threaded portion 318 receives the material mixture from the feed port 302. The screw assembly 306 is operable to rotate the screws 316 about their respective axes, whereby the pitch of the screws 316 moves the material mixture along the barrel 304.
[0054] The heat source 310 is configured to apply heat to the material along the first threaded portion 318 of the screw assembly 306 to melt the material mixture. The heat is equal to or higher than the melting temperature of the polymer material. The mixing portion 322 receives the molten material mixture from the first threaded portion 318 and includes mixing teeth, which further mix the molten material mixture due to the rotation of the screw 316. The second threaded portion 320 homogenizes the molten material mixture and feeds the molten material mixture to the die 308. The die 308 is configured to extrude the molten material mixture onto a cooling substrate 326 in the form of a film. As discussed in more detail below, in various embodiments, the substrate 326 is a temporary surface, a current collector, or another layer of a battery pack.
[0055] Figure 4 A flow chart of an exemplary method 400 of forming a battery pack according to the present disclosure is depicted. In the description of the method herein, it should be understood that, in various embodiments, the steps of the method are performed in any feasible time sequence, regardless of the order shown in the figures or the order in which the steps are described. In some embodiments, multiple steps are performed simultaneously. In addition, in various embodiments, individual steps are repeated or omitted, and additional steps are added.
[0056] At block 402, a cathode layer is formed by hot melt extrusion. At block 404, an anode layer is formed by hot melt extrusion. At block 406, a separator layer is formed by hot melt extrusion. At block 408, at least one surface region of at least one of the anode layer, the separator layer, and the cathode layer is modified by surface treatment. At block 410, the separator layer is positioned between the anode layer and the cathode layer, and at block 412, the anode layer, the separator layer, and the cathode layer are bonded together. Each of the above blocks is discussed in more detail below.
[0057] Figure 5 Depicted is the formation of the cathode layer by hot melt extrusion ( Figure 4An exemplary method 500 of block 402 of the present invention is shown in Figure 402. At 502, a CA material, an electronically conductive material, a SIC material, a primary polymer binder material, and a secondary polymer binder material are combined to form a material mixture. At 504, heat is applied to the material mixture at a melting temperature equal to or higher than the melting temperature of the primary polymer binder material to form a melt. At 506, the melt is extruded through a die as a thin film cathode layer. In some embodiments, the cathode layer is extruded as an independent layer, i.e., not fixed to any other surface or object. In some embodiments, the cathode layer is extruded onto a temporary substrate, which is configured to release the cathode layer for assembly. In some embodiments, the cathode layer is extruded directly onto a current collector, such as a net made of, for example, Ni, Al, Ti, W, stainless steel, etc., or a combination thereof. In some embodiments, the cathode layer is extruded directly onto a separator layer. In some embodiments, the cathode layer is extruded directly onto a separator-anode bilayer. In some embodiments, as discussed in more detail below, the cathode layer is co-extruded with the separator layer or the separator layer and the anode layer.
[0058] Figure 6 Depicted is the formation of the cathode layer by hot melt extrusion ( Figure 4 Another exemplary method 600 of block 402 of the present invention is provided. At 602, a CA material, an electronically conductive material, a SIC material, a primary polymer binder material, and a secondary material are combined to form a material mixture. In some embodiments, the secondary material includes a polymer binder material. In some embodiments, the secondary material includes a pore former material. At 604, heat is applied to the material mixture at a temperature equal to or greater than the melting temperature of the primary polymer binder material to form a melt. At 606, the melt is extruded through a die as a thin film cathode layer.
[0059] At 608, the secondary material is removed to form a porous structure within the cathode layer. In some embodiments, removing the secondary material includes applying heat to the cathode layer above the melting temperature of the secondary material. In some embodiments, removing the secondary material includes applying a solvent configured to dissolve the secondary material to the cathode layer. At 610, a liquid electrolyte is applied to the cathode layer to fill the porous structure.
[0060] Figure 7 Depicted is the formation of the anode layer by hot melt extrusion ( Figure 4 An exemplary method 700 of block 404 of the present invention is shown in FIG. 702. At 702, particles of an active anode material and a polymer binder material are combined to form a material mixture. At 704, heat is applied to the material mixture at a temperature equal to or greater than the melting temperature of the polymer binder material to form a melt. At 706, the melt is extruded through a die as a thin film anode layer.
[0061] Figure 8 Depicted is the formation of a diaphragm layer by hot melt extrusion ( Figure 4An exemplary method 800 of block 406 of the method of claim 1 is provided. At 802, a SIC material as a major component and a polymer binder material as a minor component are combined to form a material mixture. At 804, heat is applied to the material mixture at a melting temperature equal to or higher than the melting temperature of the polymer binder material to form a melt. At 806, the melt is extruded through a die as a thin film diaphragm layer. In some embodiments, the diaphragm layer is extruded as an independent layer, i.e., not fixed to any other surface or object. In some embodiments, the diaphragm layer is extruded onto a temporary substrate that is configured to release the cathode layer for layer assembly. In some embodiments, the diaphragm layer is extruded directly onto the cathode layer. In some embodiments, the diaphragm layer is extruded directly onto the anode layer. In some embodiments, as discussed in more detail below, the diaphragm layer is co-extruded with the cathode layer or the anode layer as a bilayer. In some embodiments, as discussed in more detail below, the diaphragm layer is co-extruded with the cathode layer and the anode layer as a trilayer.
[0062] Fig. 9 An exemplary embodiment of a system 900 for coextruding multiple layers of a battery pack is depicted. The system 900 includes a hot melt extruder for each layer to be coextruded. Fig. 9 In the embodiment depicted in FIG. 9 , the system 900 includes three extruders 902a - c to coextrude three layers of three films 904a - c , but other embodiments use other numbers of extruders to coextrude other numbers of layers. The system 900 further includes a coextrusion die 906 .
[0063] Film 904a-c is fed to coextrusion die 906 from respective extruder 902a-c. In some embodiments, one or more of film 904a-c is fed to coextrusion die 906 directly from its respective extruder 902a-c. In some embodiments, one or more of film 904a-c is formed or arranged on temporary substrate as independent layer, for example, by the method discussed above. In some such embodiments, the previously formed film is reheated to a temperature higher than the melting point of the polymer material in the film before being fed to coextrusion die 906. In some embodiments, one or more of film 904a-c is applied with surface treatment before being fed to coextrusion die 906.
[0064] The coextrusion die 906 joins the films 904a-c and extrude the films 904a-c as a single multilayer film 908. In some embodiments, a surface treatment is applied to one or more of the films 904a-c after being fed to the coextrusion die 906. In some embodiments, the coextruded films are deposited onto a current collector, a temporary substrate, etc., or as a standalone film.
[0065] Fig.10 Depicted is the formation of a diaphragm layer by hot melt extrusion ( Figure 4Another exemplary method 1000 of the invention is described in block 406 of the present invention. In this embodiment, the diaphragm layer comprises a gradient of different SIC materials varying from oxide-rich to sulfide-rich. In block 1002, a first SIC material rich in oxide as a major component and a polymer binder material as a minor component are extruded as a first film by hot melt extrusion. In block 1004, a second SIC material having a balance of sulfide and oxide as a major component and a polymer binder material as a minor component are extruded as a second film by hot melt extrusion. In block 1006, a third SIC material rich in sulfide as a major component and a polymer binder material as a minor component are extruded as a third film by hot melt extrusion. In block 1008, the first, second, and third films are fed to a coextrusion die. In block 1010, the first, second, and third films are coextruded through a coextrusion die to form a multilayer thin film diaphragm.
[0066] Fig.11 An exemplary method 1100 for forming a cathode-separator bilayer according to the present disclosure is depicted. In box 1102, CA material, electronic conductive material, SIC material, primary polymer binder material and secondary polymer binder material are extruded as cathode film by hot melt extrusion. In box 1104, SIC material as a main component and polymer binder material as a secondary component are extruded as separator film by hot melt extrusion. In box 1106, the cathode film and the separator film are fed to a coextrusion die. In some embodiments, feeding the separator film to the coextrusion die includes applying a surface treatment to at least one surface area of the separator film. In some embodiments, feeding the cathode film to the coextrusion die includes applying a surface treatment to at least one surface area of the cathode film. In box 1108, the coextrusion die coextrudes the cathode film and the separator film into a cathode-separator bilayer. In various embodiments, the cathode-separator bilayer is extruded onto a current collector or a temporary substrate, or extruded as an independent layer.
[0067] Fig.12 An exemplary method 1200 for forming a separator-anode bilayer according to the present disclosure is depicted. At box 1202, a SIC material as a major component and a polymer binder material as a minor component are extruded as a separator film by hot melt extrusion. At box 1204, particles of an active anode material and a polymer binder material are extruded as an anode film by hot melt extrusion. At box 1206, the separator film and the anode film are fed to a coextrusion die. In some embodiments, feeding the separator film to the coextrusion die includes applying a surface treatment to at least one surface area of the separator film. At box 1208, the coextrusion die coextrudes the anode film and the separator film into a separator-anode bilayer. In various embodiments, the separator-anode bilayer is extruded onto a current collector or a temporary substrate, or extruded as an independent layer.
[0068] Fig.13 An exemplary method 1300 for forming a cathode-diaphragm-anode trilayer according to the present disclosure is depicted. In box 1302, CA material, electronic conductive material, SIC material, primary polymer binder material and secondary polymer binder material are extruded as cathode film by hot melt extrusion. In box 1304, SIC material as a main component and polymer binder material as a secondary component are extruded as a diaphragm film by hot melt extrusion. In box 1306, particles of active anode material and polymer binder material are extruded as anode film by hot melt extrusion. In box 1308, the cathode film, the diaphragm film and the anode film are fed to a coextrusion die. In some embodiments, feeding the diaphragm film to the coextrusion die includes applying a surface treatment to at least one surface area of the diaphragm film. In some embodiments, feeding the cathode film to the coextrusion die includes applying a surface treatment to at least one surface area of the cathode film.
[0069] At block 1310, a coextrusion die coextrudes the cathode film, the anode film, and the separator film as a cathode-separator-anode trilayer, wherein the separator layer is located between the cathode layer and the anode layer. In various embodiments, the cathode-separator-anode trilayer is extruded onto a current collector or a temporary substrate, or extruded as an independent layer.
[0070] In some embodiments, as in various embodiments discussed above, surface treatment is applied to one or more layers during coextrusion. In some embodiments, surface treatment includes surface melting method to remove polymer binder material from the surface area of the treated layer. Any acceptable surface melting method can be used, such as gas-rich plasma application process, laser-assisted local melting method, etc. In some embodiments, the polymer binder material in the layer to be treated is sensitive to solvent. In some embodiments, surface treatment includes a solvent scrubbing method configured to remove polymer binder material from the surface area of the layer. In some embodiments, surface treatment includes heat treating the layer at a certain temperature to reduce the interparticle distance between SIC particles due to the volatility of the polymer binder material. In some embodiments, surface treatment includes hot rolling the layer to further extrude the polymer binder material and reduce the interparticle distance between the SIC particles in the layer.
[0071] In some embodiments, the current collector of the battery pack according to the present disclosure is a mesh, a plate, etc., which is joined to the cathode layer or the anode layer. In some embodiments, joining the layer to the current collector includes depositing the hot melt extruded layer on the current collector. In some embodiments, joining the layer to the current collector includes hot rolling or calendaring. In some embodiments, the current collector is a layer formed at least in part by hot melt extrusion. In some embodiments, joining the layer to the current collector includes feeding the layer and the current collector through a co-extrusion die.
[0072] Fig.14 An exemplary embodiment of a method 1400 for forming a co-extruded current collector-cathode trilayer according to the present disclosure is depicted. In box 1402, a CA material, an electronically conductive material, a SIC material, a primary polymer binder material, and a secondary polymer binder material are extruded as a first cathode film by hot melt extrusion. In box 1404, a CA material, an electronically conductive material, a SIC material, a primary polymer binder material, and a secondary polymer binder material are extruded as a second cathode film by hot melt extrusion. In box 1406, the first cathode film, the second cathode film, and the current collector layer are fed to a coextrusion die. In box 1408, the coextrusion die coextrudes the first cathode film, the second cathode film, and the current collector layer as a trilayer, wherein the current collector layer is located between the first cathode layer and the second cathode layer.
[0073] Fig.15 Another exemplary embodiment 1500 for co-extruding a battery assembly according to the present disclosure is depicted. At block 1502, a first thin film battery assembly is formed by hot melt extrusion. In some embodiments, the first thin film battery assembly is one of an anode and a cathode. In some embodiments, forming the first thin film battery assembly by hot melt extrusion includes depositing the first thin film battery assembly onto a substrate. In some embodiments, the substrate is a current collector. In some embodiments, the first thin film battery assembly is a sublayer of a multilayer separator. In some embodiments, the first thin film battery assembly is formed to have a porous structure.
[0074] At block 1504, a second thin film battery component is formed by hot melt extrusion. In some embodiments, the second thin film battery component is a separator. In some embodiments, the second thin film battery component is a cathode. In some embodiments, the second thin film battery component is another sublayer of the multilayer separator. At block 1506, a third thin film battery component is formed by hot melt extrusion. In some embodiments, the third thin film battery component is the other of the anode and the cathode.
[0075] At block 1508, a surface treatment is applied to a surface region of at least one of the first thin film battery assembly and the second thin film battery assembly. As a result of the surface treatment, the surface region has at least one of: (i) reduced interparticle distance, (ii) reduced amount of polymer binder material, and (iii) increased amount of exposed ion conductive material relative to the remainder of the at least one of the first and second thin film assemblies. In some embodiments, the surface treatment comprises removing polymer binder material from the surface region by a surface melting process. In some embodiments, the surface treatment comprises removing polymer binder material from the surface region by a solvent brushing process. In some embodiments, the surface treatment comprises reducing interparticle distance by surface heat treatment. In some embodiments, the surface treatment comprises reducing interparticle distance by hot rolling.
[0076] At block 1510, the first thin film battery assembly, the second thin film battery assembly, and the third thin film battery assembly are fed through a coextrusion die to form a coextruded multilayer film. In some embodiments, the second thin film battery assembly is positioned between the first thin film battery assembly and the third thin film battery assembly.
[0077] In some embodiments, instead of feeding the first and second thin film battery assemblies through a coextrusion die, the third thin film battery assembly is joined to the bilayer formed by the coextrusion of the first and second thin film battery assemblies. In some embodiments, the first thin film battery assembly is removed from the substrate on which the first thin film battery assembly is formed before feeding the first thin film battery assembly through a coextrusion die. In some embodiments, the current collector is fed through the coextrusion die with the thin film battery assembly. In some embodiments, a liquid electrolyte is added to the porous structure of the first thin film battery assembly.
[0078] It will be appreciated that variations of the above and other features and functions or their alternatives may be desirably combined into many other different systems, applications or methods. Those skilled in the art may subsequently make various currently unforeseeable or unanticipated substitutions, modifications, changes or improvements, which are also intended to be covered by the above disclosure.
Claims
1. A method for co-extruding a battery pack assembly, comprising: forming a first thin film battery assembly by hot melt extrusion; forming a second thin film battery assembly by hot melt extrusion; and feeding the first thin film battery assembly and the second thin film battery assembly through a coextrusion die to form a coextruded multilayer film, wherein a surface treatment is applied to a surface region of at least one of the first thin film battery assembly and the second thin film battery assembly during the coextrusion process such that, relative to the remainder of the at least one of the first and second thin film assemblies, the surface region has at least one of the following: Reduced inter-particle distance; reduced amount of polymeric binder material; and The increased amount of ion-conducting material exposed, wherein the first thin film battery component is one of an anode and a cathode, and the second thin film battery component is a separator; wherein forming the first thin film battery assembly by hot melt extrusion comprises depositing the first thin film battery assembly onto a substrate; and The surface treatment includes removing the polymer binder material from the surface region by surface melting, removing the polymer binder material from the surface region by solvent brushing, reducing the distance between particles by surface heat treatment, or reducing the distance between particles by hot rolling.
2. The method according to claim 1, further comprising: A third thin film battery component is formed by hot melt extrusion, wherein the third thin film battery component is the other of the anode and the cathode.
3. The method of claim 2, wherein the third thin film battery assembly is fed through a coextrusion die along with the first thin film battery assembly and the second thin film battery assembly to form a coextruded multilayer film, such that in the coextruded multilayer film, the separator is located between the anode and the cathode.
4. The method of claim 2, further comprising bonding a third thin film battery component to the separator of the coextruded multilayer film such that the separator is located between the anode and the cathode. The method of claim 1 , wherein the substrate is a current collector.
6. The method according to claim 1, further comprising: Prior to feeding the first thin film battery assembly and the second thin film battery assembly through a coextrusion die, the first thin film battery assembly is removed from the substrate.
7. The method according to claim 1, wherein: The first thin film battery assembly and the second thin film battery assembly are each a cathode; and The current collector is fed with the first thin film battery assembly and the second thin film battery assembly through a coextrusion die to form a coextruded multilayer film, such that the current collector is located between the first and second thin film battery assemblies in the coextruded multilayer film.
8. The method according to claim 1, further comprising: forming a porous structure within the first thin film battery assembly by removing material from the first thin film battery assembly; and The porous structure is filled with a liquid material.