Nanosheet, method for manufacturing the same, and semiconductor nanocrystal-polymer composite and electronic device comprising the same

By forming non-cadmium-based III-V nanosheets on a two-dimensional template and combining the reaction technology of organic ligands and solvents, the problem of difficulty in preparing non-cadmium-based nanosheets with excellent luminescent properties by traditional methods is solved, achieving high performance. display device applications.

CN111834499BActive Publication Date: 2024-10-15SAMSUNG ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010306370.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-17
Filing Date
2020-04-17
Publication Date
2024-10-15
Estimated Expiration
2040-04-17

AI Technical Summary

Technical Problem

It is difficult to develop cadmium-free semiconductor nanocrystal materials, especially nanosheets, with excellent luminescence properties and stability using existing technology, and it is difficult to manufacture extremely thin InP nanosheets using traditional methods.

Method used

Using a structure including a two-dimensional template of a first semiconductor nanocrystal and a second semiconductor nanocrystal shell disposed on the surface of the template, by controlling the thickness and composition of the shell, a non-cadmium-based III-V group nanosheet is formed, and combined with an organic compound Nanosheets with improved optical properties can be prepared using reaction technology between solids and solvents.

Benefits of technology

Achieved the preparation of non-cadmium-based nanosheets with excellent luminescence properties and stability, capable of emitting visible light, especially green and red light, and controlling the emission wavelength by adjusting the thickness of the shell, thereby improving the color reproducibility of the display device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111834499B_ABST
    Figure CN111834499B_ABST
Patent Text Reader

Abstract

Disclosed are nanosheets, methods for making the same, and semiconductor nanocrystal-polymer composites and electronic devices comprising the same. The nanosheets include: a two-dimensional template including a first semiconductor nanocrystal; and a first shell disposed on a surface of the two-dimensional template including a second semiconductor nanocrystal, the second semiconductor nanocrystal having a different composition from the first semiconductor nanocrystal, wherein the second semiconductor nanocrystal includes a III-V compound, and wherein the nanosheets do not include cadmium.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2019-0045055 filed in the Korean Intellectual Property Office on April 17, 2019, and all rights arising therefrom, the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] Disclosed are a nanoplatelet, a method for manufacturing the same, and a semiconductor nanocrystal-polymer composite and an electronic device (equipment) comprising the same. Background Art

[0004] Unlike bulk (bulk) materials, nanometer-sized semiconductor nanocrystal particles (also referred to as "quantum dots") can have different energy band gaps by controlling the size and composition of the nanocrystals. Quantum dots can exhibit electroluminescence and photoluminescence properties. The luminescent properties of semiconductor nanocrystals can be applied, for example, to be used in a variety of fields. From an environmental point of view, it is desirable to be able to achieve the development of non-cadmium-based materials that, for example, exhibit improved luminescent properties. Summary of the invention

[0005] One embodiment provides non-cadmium-based nanosheets that can exhibit improved luminescence properties (eg, narrow full width at half maximum (FWHM)).

[0006] One embodiment provides a composition including the non-cadmium-based nanosheets.

[0007] One embodiment provides a semiconductor nanocrystal-polymer composite including the non-cadmium-based nanosheets.

[0008] One embodiment provides a stacked structure and an electronic device including the semiconductor nanocrystal-polymer composite.

[0009] In one embodiment, the nanosheet comprises: a two-dimensional template comprising a first semiconductor nanocrystal; and a first shell comprising a second semiconductor nanocrystal disposed on a surface of the two-dimensional template, the second semiconductor nanocrystal having a different composition than the first semiconductor nanocrystal, wherein the second semiconductor nanocrystal comprises a Group III-V compound, and wherein the nanosheet does not include cadmium.

[0010] The first semiconductor nanocrystals may include Group II-VI compounds.

[0011] The II-VI Group compound may include ZnA, wherein A is selenium, tellurium, sulfur, oxygen, or a combination thereof.

[0012] The first semiconductor nanocrystals may include ZnSe, ZnS, ZnTe, ZnTeSe, ZnTeS, ZnTeSeS, ZnO, or combinations thereof.

[0013] The first shell may be disposed on (eg, two) opposite surfaces of the two-dimensional template.

[0014] The first shell may be disposed directly on the two-dimensional template.

[0015] The first shell may have a thickness greater than or equal to about 0.5 nanometers (nm) and less than or equal to about 2 nm.

[0016] The Group III-V compound may include a Group III metal selected from gallium and indium; and phosphorus.

[0017] The Group III-V compound may further include a Group II metal.

[0018] The III-V group compound may include InP, InGaP, GaP, InZnP, GaZnP, InGaZnP, or a combination thereof.

[0019] The energy band gap of the second semiconductor nanocrystal material may be smaller than the energy band gap of the first semiconductor nanocrystal material.

[0020] Transmission electron microscopy energy dispersive X-ray spectroscopy (TEM-EDX) analysis of a surface extending in a thickness direction of the nanosheet (hereinafter, thickness surface) may reveal an element present in the first semiconductor nanocrystal and an element present in the second semiconductor nanocrystal.

[0021] Transmission electron microscopy energy dispersive x-ray spectroscopy analysis of a lateral surface of the nanosheet may reveal elements present in the second semiconductor nanocrystal. TEM-EDX analysis of a lateral surface of the nanosheet may not reveal elements present in the first semiconductor nanocrystal. The lateral surface of the nanosheet may extend in a direction substantially perpendicular to a thickness surface of the nanosheet.

[0022] The nanosheet may further include a second shell including a third semiconductor nanocrystal and disposed on the first shell, wherein the third semiconductor nanocrystal has a composition different from a composition of the second semiconductor nanocrystal.

[0023] The third semiconductor nanocrystals may include Group II-VI compounds.

[0024] The third semiconductor nanocrystal may include ZnA, wherein A is selenium, tellurium, sulfur, oxygen, or a combination thereof.

[0025] The third semiconductor nanocrystals may include ZnSe, ZnS, ZnTe, ZnTeSe, ZnTeS, ZnTeSeS, ZnO, or a combination thereof.

[0026] The energy band gap of the third semiconductor nanocrystal material may be greater than the energy band gap of the second semiconductor nanocrystal material.

[0027] Transmission electron microscopy energy dispersive x-ray spectroscopy analysis of the lateral surfaces of the nanosheets may reveal only elements present in the third semiconductor nanocrystals.

[0028] TEM-EDX analysis of the lateral surface of the nanosheet may not show elements present in the first semiconductor nanocrystal. TEM-EDX analysis of the lateral surface of the nanosheet may not show zinc, selenium, or a combination thereof.

[0029] The nanosheets may have a size greater than about 400 square nanometers (nm 2 )'s lateral dimension (eg, obtained by multiplying the width and the length).

[0030] The nanosheets may have a diameter greater than or equal to about 750 nm. 2 lateral scale.

[0031] The nanosheets may have a diameter greater than or equal to about 1,000 nm. 2 lateral scale.

[0032] The lateral surface of the nanosheet may have at least two pairs of opposite sides.

[0033] The lateral surface of the nanosheet may have an aspect ratio (eg, a ratio between a minor axis length and a major axis length) of greater than or equal to about 1:1.1 and less than or equal to about 1:8.

[0034] The thickness of the nanosheet may be greater than or equal to about 0.5 nm, such as greater than or equal to about 1 nm, or greater than or equal to about 1.5 nm and less than or equal to about 20 nm, such as less than or equal to about 15 nm, or less than or equal to about 10 nm.

[0035] The nanosheets may exhibit two or more absorption peaks within a range of less than or equal to about 500 nm.

[0036] A difference between a first absorption peak of the two-dimensional template and a first absorption peak of the nanosheet may be less than about 100 nm.

[0037] A difference between a first absorption peak of the two-dimensional template and a first absorption peak of the nanosheet may be less than about 50 nm.

[0038] The first semiconductor nanocrystal may include ZnA (wherein A is selenium, tellurium, sulfur, oxygen, or a combination thereof), the second semiconductor nanocrystal may include a Group III metal and phosphorus, and in the nanosheet, the content of the Group III metal may be greater than or equal to about 0.05 mole and less than or equal to about 2 moles, the content of zinc may be greater than or equal to about 1 mole and less than or equal to about 10 moles, and the content of phosphorus may be greater than or equal to about 0.05 mole and less than or equal to about 5 moles, based on 1 mole of element A.

[0039] In one embodiment, the method for making the aforementioned nanosheets comprises:

[0040] reacting a first metal precursor of the first semiconductor nanocrystal and a first non-metal precursor of the first semiconductor nanocrystal in an organic solvent in the presence of an organic ligand at a temperature below about 175° C. to synthesize a two-dimensional template; and

[0041] A second metal precursor of the second semiconductor nanocrystal and a second non-metal precursor of the second semiconductor nanocrystal are reacted in an organic solvent in the presence of an organic ligand and the two-dimensional template at a temperature less than or equal to about 200° C. to form a first shell including the second semiconductor nanocrystal on the surface of the two-dimensional template and produce the nanosheet.

[0042] The method may further include reacting a third metal precursor and a third non-metal precursor for a third semiconductor nanocrystal in an organic solvent in the presence of an organic ligand and particles on which the first shell is formed (e.g., particles including the first shell formed on the surface of the two-dimensional template) to form a second shell on the first shell.

[0043] In one embodiment, the composition comprises:

[0044] (e.g., a plurality of) semiconductor nanocrystal particles;

[0045] dispersants (e.g., binder monomers or polymers including carboxylic acid groups);

[0046] a polymerizable (e.g., photopolymerizable) monomer comprising a carbon-carbon double bond;

[0047] initiator; and

[0048] Solvents,

[0049] The plurality of semiconductor nanocrystal particles include the aforementioned nanosheets.

[0050] The composition may further include a polythiol compound having at least two thiol groups (eg, at the terminal end), metal oxide particles, or a combination thereof.

[0051] In one embodiment, a semiconductor nanocrystal-polymer composite includes: a polymer matrix; and a plurality of semiconductor nanocrystal particles dispersed in the polymer matrix, wherein the plurality of semiconductor nanocrystal particles include the aforementioned nanosheets.

[0052] The polymer matrix may include a cross-linked polymer, a binder polymer having carboxylic acid groups, or a combination thereof.

[0053] The cross-linked polymer may include a polymerization product of a (photo)polymerizable monomer including a carbon-carbon double bond, a polymerization product of the (photo)polymerizable monomer and a polythiol compound having at least two thiol groups at the terminal, or a combination thereof.

[0054] The semiconductor nanocrystal-polymer composite may further include metal oxide particles in the polymer matrix.

[0055] In one embodiment, the display device includes a light emitting element (eg, a photoluminescent element), wherein the light emitting element includes the aforementioned semiconductor nanocrystal-polymer composite. The display device may further include a light source and the light source is configured to supply incident light to the light emitting element.

[0056] The incident light may have an emission peak wavelength in the range of about 440 nm to about 470 nm (or 460 nm).

[0057] The light emitting element may include a sheet of the semiconductor nanocrystal-polymer composite.

[0058] The display device may further include a liquid crystal panel, and

[0059] The sheet of semiconductor nanocrystal-polymer composite may be disposed between the light source and the liquid crystal panel.

[0060] The light-emitting element may have a stacked structure including a substrate and an emission layer (e.g., a light-emitting layer) disposed on the substrate, wherein the emission layer includes a pattern of the semiconductor nanocrystal-polymer composite and the pattern may include (e.g., at least one) repeated segment (portion) that emits light of a predetermined wavelength.

[0061] The display device may be configured to have color reproducibility of the BT2020 standard of greater than or equal to about 80%.

[0062] The pattern may include a first segment configured to emit a first type of light and a second segment configured to emit a second type of light having a different central wavelength than the first type of light.

[0063] The light source may include a plurality of light emitting units corresponding to the first segment and the second segment, respectively, wherein the light emitting units may include a first electrode and a second electrode facing each other and an electroluminescent layer disposed between the first and second electrodes.

[0064] The display device may further include a lower substrate, a polarizer disposed under the lower substrate, and a liquid crystal layer disposed between the stacked structure and the lower substrate, wherein the stacked structure may be disposed such that the emission layer faces the liquid crystal layer.

[0065] The display device may further include a polarizer between the liquid crystal layer and the emission layer.

[0066] The light source may further include a light emitting diode (LED) and optionally a light guide.

[0067] One embodiment provides an electronic device including the aforementioned nanosheet.

[0068] The electronic device may be an electroluminescent device, an organic light emitting diode (OLED), a sensor, an imaging sensor, a solar cell, or a liquid crystal display (LCD) device.

[0069] The nanosheet according to the embodiment can present various wavelengths of light with improved optical properties (e.g., half width (FWHM) of the peak of the absorption spectrum or the luminescence spectrum) by controlling the thickness of the first shell. The nanosheet can be applied to various display devices capable of achieving high color reproducibility, biomarkers (e.g., biosensors or bioimaging, etc.), photodetectors, solar cells, hybrid composites, etc., for example, used therein. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] The above and other advantages and features of the present disclosure will become more apparent by further describing in detail exemplary embodiments of the present disclosure with reference to the accompanying drawings, in which:

[0071] Figure 1 Schematic cross-sectional views of a two-dimensional template and a nanosheet according to an embodiment.

[0072] Figure 2 is a schematic cross-sectional view of a nanosheet according to one embodiment.

[0073] Figure 3 is a schematic cross-sectional view of a device according to one embodiment.

[0074] Figure 4 is a schematic cross-sectional view of a device according to one embodiment.

[0075] Figure 5is a schematic cross-sectional view of a device according to one embodiment.

[0076] Figure 6 is a graph of absorption wavelength (nm) versus InP thickness (nm), which shows the change in ultraviolet-visible (UV-Vis) absorption wavelength of a nanosheet (e.g., a ZnSe and / or ZnS shell having a predetermined thickness) according to an embodiment relative to the thickness of an emission layer (e.g., an InP emission layer). To achieve visible light, the thickness of the InP layer may be less than or equal to about 2 nm. For green light (about 500 nm to 560 nm), the thickness of the InP layer may be about 0.4 nm (e.g., 0.48 nm) to about 0.8 nm. Figure 7 is a graph of absorption wavelength (nm) versus nanosheet (NPL) thickness (nm) or (quantum) dot diameter (nm), which shows the variation of the UV-visible absorption wavelength of the nanosheets comprising indium and phosphorus with respect to the thickness of the InP layer and the variation of the UV-visible absorption wavelength with respect to the diameter of the InP core comprising indium and phosphorus.

[0077] Figure 8 A transmission electron micrograph of the two-dimensional template fabricated in Example 3 is shown.

[0078] Fig. 9 is a graph of absorption intensity (arbitrary unit (au)) versus absorption wavelength (nm), which shows the UV-visible absorption spectrum of the two-dimensional template fabricated in Example 3.

[0079] Fig.10 is a graph of absorption intensity (arbitrary unit (au)) versus absorption wavelength (nm), which shows the UV-visible absorption spectra of the two-dimensional template and the nanosheets fabricated in Example 4. DETAILED DESCRIPTION

[0080] With reference to the following example embodiments together with the accompanying drawings attached hereto, the advantages and characteristics of the present disclosure, and the methods for realizing the same will become clear. However, the embodiments should not be interpreted as being limited to the embodiments set forth herein. If not otherwise defined, all terms (including technical and scientific terms) in the specification may be defined as commonly understood by those skilled in the art. Unless clearly defined, the terms defined in the general dictionary may not be interpreted ideally or exaggeratedly. In addition, unless explicitly described to the contrary, the word "include" and variations such as "comprise" or "contain" will be understood to imply the inclusion of stated elements, but do not exclude any other elements.

[0081] Furthermore, the singular includes the plural unless otherwise mentioned.

[0082] In the drawings, the thickness of layers, films, panels, regions, etc., are exaggerated for clarity. The same reference numerals denote the same elements throughout the specification.

[0083] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it can be directly on the other element or intervening elements may also be present. Conversely, when an element is referred to as being "directly on" another element, there are no intervening elements.

[0084] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe various elements, components, regions, layers and / or segments, these elements, components, regions, layers and / or segments should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or segment from another element, component, region, layer or segment. Therefore, without departing from the teachings herein, the "first element", "component", "region", "layer" or "segment" discussed below may be referred to as a second element, component, region, layer or segment.

[0085] The terms used herein are only for the purpose of describing specific embodiments and are not intended to be restrictive. As used herein, "a kind (individual)", "said (the)" and "at least one (individual)" do not represent the limitation of quantity, and are intended to include both the singular and the plural, unless the context clearly states otherwise. For example, "(an) element" has the same meaning as "at least one element", unless the context clearly states otherwise. "At least one (individual)" will not be interpreted as limiting "a kind (individual)". "Or" means "and / or". As used herein, the term "and / or" includes any and all combinations of one or more of the relevant listed items. It will be further understood that the term "comprising" or "including" when used in this specification, means that there are stated features, regions, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, regions, wholes, steps, operations, elements, components, and / or their sets.

[0086] In addition, relative terms such as "lower" or "bottom" and "upper" or "top" may be used herein to describe the relationship of one element to another element as shown in the figure. It will be understood that, in addition to the orientation shown in the figure, relative terms are also intended to include different orientations of the device. For example, if the device in one of the figures is turned over, the element described as being on the "lower" side of the other element will be oriented on the "upper" side of the other element. Therefore, depending on the specific orientation of the figure, the exemplary term "lower" may include both "lower" and "upper" orientations. Similarly, if the device in one of the figures is turned over, the element described as "below" or "below" the other element will be oriented "above" the other element. Therefore, the exemplary terms "below..." or "below..." may include both "above..." and "below..." orientations.

[0087] As used herein, "about" includes the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" may mean that the deviation from the stated value is within one or more standard deviations, or within ±10% or 5%.

[0088] Exemplary embodiments are described herein with reference to cross-sectional views as schematic diagrams of idealized embodiments. Thus, deviations from the shapes of the figures as a result of, for example, manufacturing techniques and / or tolerances are to be expected. Therefore, the embodiments described herein should not be construed as being limited to the specific shapes of the regions as illustrated herein, but rather include deviations in shape caused by, for example, manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. Moreover, the illustrated sharp corners may be rounded. Therefore, the regions illustrated in the figures are schematic in nature and their shapes are not intended to illustrate the precise shapes of the regions and are not intended to limit the scope of the claims.

[0089] As used herein, when no definition is otherwise provided, "substituted" means that a hydrogen of a compound or group is replaced by a substituent such as a C1-C30 alkyl, a C2-C30 alkenyl, a C2-C30 alkynyl, a C6-C30 aryl, a C7-C30 alkaryl, a C1-C30 alkoxy, a C1-C30 heteroalkyl, a C3-C30 heteroalkaryl, a C3-C30 cycloalkyl, a C3-C15 cycloalkenyl, a C6-C30 cycloalkynyl, a C2-C30 heterocycloalkyl, a halogen (-F, -Cl, -Br or -I), a hydroxyl (-OH), a nitro (-NO 2 ), cyano (-CN), amino (-NRR', wherein R and R' are independently hydrogen or C1-C6 alkyl), azido (-N 3 ), amidino (-C(=NH)NH 2 ), hydrazino (-NHNH 2 ), hydrazone (=N(NH 2 )), aldehyde group (-C(=O)H), carbamoyl group (-C(O)NH 2 ), thiol group (-SH), ester group (-C(=O)OR, wherein R is C1-C6 alkyl or C6-C12 aryl), carboxyl group (-COOH) or its salt (-C(=O)OM, wherein M is an organic or inorganic cation), sulfonic acid group (-SO 3 H) or its salt (-SO 3 M, where M is an organic or inorganic cation), a phosphate group (-PO 3 H 2 ) or its salt (-PO 3 MH or -PO3 M 2 , wherein M is an organic or inorganic cation), and combinations thereof.

[0090] As used herein, when a definition is not otherwise provided, "alkylene" refers to a straight-chain or branched saturated aliphatic hydrocarbon group having a valence of at least 2 and optionally substituted with (eg, at least one) substituent.

[0091] As used herein, "arylene" refers to a functional group obtained by removing at least two hydrogens from (eg, at least one) aromatic ring having a valence of at least 2 and optionally substituted with (eg, at least one) substituent.

[0092] In addition, the “aliphatic hydrocarbon group” refers to a C1-C30 straight chain or branched alkyl group, the “aromatic hydrocarbon group” refers to a C6-C30 aryl group or a C2-C30 heteroaryl group, and the “alicyclic hydrocarbon group” refers to a C3-C30 cycloalkyl group, a C3-C30 cycloalkenyl group, and a C3-C30 cycloalkynyl group.

[0093] As used herein, "(meth)acrylate" refers to acrylate, methacrylate, or a combination thereof. The (meth)acrylate may include (C1-C10 alkyl)acrylate, (C1-C10 alkyl)methacrylate, or a combination thereof.

[0094] In an embodiment, the "hydrophobic portion" may include a group that provides a tendency for the corresponding compound to agglomerate in an aqueous solution and repel water. For example, the hydrophobic portion may include an aliphatic hydrocarbon group (alkyl, alkenyl, alkynyl, etc.) with a carbon number of 1 or more (e.g., 2 or more, 3 or more, 4 or more, or 5 or more), an aromatic hydrocarbon group (phenyl, naphthyl, aralkyl, etc.) with a carbon number of 6 or more, or an alicyclic hydrocarbon group (cyclohexyl, norbornene, norbornyl, tricyclodecyl, etc.) with a carbon number of 5 or more.

[0095] As used herein, "visible light" refers to light having a wavelength of about 390 nm to about 700 nm. As used herein, "ultraviolet" or "UV" refers to light having a wavelength greater than or equal to about 200 nm and less than about 390 nm.

[0096] As used herein, "dispersion" refers to a dispersion in which the dispersed phase is solid and the continuous phase comprises a liquid. For example, "dispersion" refers to a colloidal dispersion in which the dispersed phase has a size greater than or equal to about 1 nm, such as greater than or equal to about 2 nm, greater than or equal to about 3 nm, or greater than or equal to about 4 nm and several (several) micrometers (μm) or less (e.g., about 2 μm or less or about 1 μm or less).

[0097] As used herein, "Group" refers to a Group of the Periodic Table.

[0098] As used herein, “Group I” refers to Group IA and Group IB, and examples may include Li, Na, K, Rb, and Cs, but are not limited thereto.

[0099] As used herein, “Group II” refers to Group IIA and Group IIB, and examples of Group II metals may be Cd, Zn, Hg, and Mg, but are not limited thereto.

[0100] As used herein, “Group III” refers to Group IIIA and Group IIIB, and examples of Group III metals may be Al, In, Ga, and Tl, but are not limited thereto.

[0101] As used herein, "Group IV" refers to Group IVA and Group IVB, and examples of Group IV metals may be Si, Ge, and Sn, but are not limited thereto. As used herein, the term "metal" may include semimetals such as Si.

[0102] As used herein, "Group V" refers to Group VA, and examples may include nitrogen, phosphorus, arsenic, antimony, and bismuth, but are not limited thereto.

[0103] As used herein, "Group VI" refers to Group VIA, and examples may include oxygen, sulfur, selenium, and tellurium, but are not limited thereto.

[0104] As used herein, "size" may refer to the size of a particle or the average size of a particle. As used herein, "lateral dimension" may refer to the area of ​​a lateral surface of a particle or the average area of ​​a lateral surface of a particle. As used herein, the "lateral surface" of a particle or nanosheet refers to the two-dimensional surface (e.g., top / bottom or major surface) of the nanosheet and "thickness" refers to the distance (e.g., vertical length) between these two (bottom and top) lateral surfaces.

[0105] Semiconductor nanocrystal particles are crystalline materials of several nanometers in size. Such semiconductor nanocrystal particles can have a large surface area per unit volume due to very small size and can present different characteristics from bulk materials with the same composition due to quantum confinement effects. Semiconductor nanocrystal particles can absorb light from an excitation source and become excited, and can emit energy corresponding to the energy band gap of the semiconductor nanocrystal particles.

[0106] Semiconductor nanocrystal particles have potential applicability for various electronic devices, for example, in various electronic devices, due to unique photoluminescent properties. For improved luminescent properties, core-shell quantum dots in which a semiconductor nanocrystal shell is formed on a three-dimensional core comprising a semiconductor nanocrystal have been proposed. On the other hand, cadmium-based (cadmium-based) quantum dots can present improved properties. However, cadmium can cause environmental and health problems and is one of the regulated elements. Examples of semiconductor nanocrystals that do not contain cadmium can be nanocrystals based on III-V groups. Compared with cadmium-based materials, the semiconductor nanocrystals that do not contain cadmium can have less desirable luminescent properties (e.g., half width (FWHM)) and stability.

[0107] In addition to core-shell quantum dots, nanocrystalline particles can have a variety of shapes such as nanosheets, nanorods and multi-legged. In the case of spherical particles, charge carriers are restricted in three dimensions. However, nanosheets (e.g., colloidal nanosheets that can be prepared in a colloidal manner) have a vertical thickness of a few nanometers and a lateral dimension of about 10 to 100nm, which can form quantum wells. The lateral dimension of the nanosheet can be greater than the exciton Bohr radius, and the quantum confinement in the nanosheet can be, for example, only strong in the vertical direction, which can lead to unique properties such as one-dimensional exciton confinement. Although it is not desired to be bound by any theory, it is understood that the nanosheet can present luminescent properties different from core-shell quantum dots. Nanosheets that emit visible light (e.g., light with a wavelength greater than 450nm) can be based on cadmium-containing semiconductor nanocrystals. Exemplary cadmium-free semiconductor nanocrystal materials can include indium phosphide. Nanosheets based on InP can have an extremely thin thickness less than or equal to about 1nm and can emit light in the visible light wavelength region. However, solution synthesis processes cannot manufacture InP nanosheets with such a thin thickness. Non-cadmium semiconductor nanocrystals such as InP that can emit light in a visible light wavelength region and have a nanosheet shape are provided.

[0108] The nanosheet according to the embodiment is based on non-cadmium semiconductor nanocrystals. In an embodiment, the semiconductor nanocrystal nanosheet (hereinafter, also referred to as NPL) adopts (e.g., includes) a template, and in addition, the III-V semiconductor nanocrystal material is optionally coated (covered) with (e.g., at least one) II-VI semiconductor nanocrystal material (e.g., on the surface of the template) to obtain the non-cadmium semiconductor nanocrystal NPL.

[0109] In an embodiment, a nanosheet based on a III-V semiconductor nanocrystal includes: a two-dimensional template including a first semiconductor nanocrystal; and a first shell including a second semiconductor nanocrystal disposed on (e.g., at least one) surface of the two-dimensional template, the second semiconductor nanocrystal having a different composition than the first semiconductor nanocrystal, wherein the second semiconductor nanocrystal includes a III-V compound. The nanosheet does not include cadmium.

[0110] Reference Figure 1 , a nanosheet according to an embodiment has: a template; and an emission layer formed on (eg, at least one) surface (or both surfaces) thereof.

[0111] The template is a two-dimensional nanoparticle. As used herein, a nanosheet (hereinafter, also referred to as NPL) or a two-dimensional template or a nanoparticle refers to a particle in which the spacing (i.e., thickness or vertical thickness) between two lateral surfaces facing each other is nanoscale (e.g., less than 100 nm, such as less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, less than or equal to about 40 nm, less than or equal to about 30 nm, less than or equal to about 20 nm, less than or equal to about 10 nm, or less than or equal to about 5 nm). In the nanosheet or two-dimensional template or nanoparticle, the maximum dimension constituted by, for example, the lateral surface (e.g., length (L) or width (W)) may be about 5 times or more, about 6 times or more, about 7 times or more, about 8 times or more, about 9 times or more, or about 10 times or more and about 100 times or less, about 90 times or less, about 80 times or less, about 70 times or less, about 60 times or less, about 50 times or less, about 40 times or less, about 30 times or less, or about 20 times or less of the thickness (e.g., compared to the thickness).

[0112] In the two-dimensional template, the first semiconductor nanocrystal may include a II-VI compound. The first semiconductor nanocrystal may include ZnA (wherein A is selenium, tellurium, sulfur, oxygen, or a combination thereof). The first semiconductor nanocrystal may include a zinc chalcogenide (e.g., zinc selenide). The first semiconductor nanocrystal may include ZnSe, ZnS, ZnTe, ZnTeSe, ZnTeS, ZnTeSeS, ZnO, or a combination thereof. In one embodiment, the two-dimensional template may include zinc and selenium.

[0113] The inventors have found that when the first semiconductor nanocrystal serving as a template has a predetermined thickness (e.g., when the template has a predetermined range of thickness), it may not have a significant effect on the emission wavelength of the final NPL. In one embodiment, the thickness of the template may be greater than or equal to about 0.3nm, such as greater than or equal to about 0.4nm, or greater than or equal to about 0.5nm. In one embodiment, the thickness of the template may be less than or equal to about 10nm, such as less than or equal to about 9nm, less than or equal to about 8nm, less than or equal to about 7nm, less than or equal to about 6nm, less than or equal to about 5nm, less than or equal to about 4nm, less than or equal to about 3nm, less than or equal to about 2nm, or less than or equal to about 1nm.

[0114] In the NPL according to the embodiment, the emission layer is included in the stacked structure (e.g., as a first shell), and the luminescent center exists in the emission layer (i.e., the first shell) formed on the template. The first shells may be respectively arranged on two opposite surfaces of the two-dimensional template. The first shell may be directly arranged on the two-dimensional template (e.g., opposite main surfaces (i.e., top and bottom surfaces) of the template).

[0115] The III-V compound included in the first shell may include a III-group metal selected from gallium, indium, or a combination thereof; and phosphorus. The III-V compound may further include a II-group metal (e.g., zinc). The III-V compound may include InP, InGaP, GaP, InZnP, GaZnP, InGaZnP, or a combination thereof. The energy band gap of the second semiconductor nanocrystal material may be smaller than the energy band gap of the first semiconductor nanocrystal material. In one embodiment, the template may include ZnSe and the first shell may include InP or InZnP.

[0116] In an embodiment of the NPL, the first shell acts as an emissive layer. Therefore, the emission wavelength can be controlled by adjusting the thickness of the first shell. In an embodiment, the thickness of the first shell can be less than or equal to about 3 nm, such as less than or equal to about 2 nm, less than or equal to about 1 nm, less than or equal to about 0.5 nm, less than or equal to about 0.4 nm, less than or equal to about 0.3 nm, or less than or equal to about 0.2 nm and greater than or equal to about 0.1 nm.

[0117] In one embodiment, the NPL may emit light in the visible wavelength region. The first shell may include indium and phosphorus. The thickness of the first shell may be less than or equal to about 2nm and greater than or equal to about 0.5nm. In one embodiment, the NPL may emit green light and the first shell may include indium and phosphorus. The thickness of the first shell may be less than or equal to about 5nm, less than or equal to about 4nm, less than or equal to about 3nm, less than or equal to about 2nm, less than or equal to about 1nm, less than or equal to about 0.9nm, or less than or equal to about 0.8nm and greater than or equal to about 0.1nm, greater than or equal to about 0.2nm, greater than or equal to about 0.3nm, greater than or equal to about 0.4nm, or greater than or equal to about 0.5nm. In one embodiment, the NPL may emit red light and the first shell may include indium and phosphorus. The thickness of the first shell may be less than or equal to about 5 nm, for example, less than or equal to about 4 nm, less than or equal to about 3 nm, less than or equal to about 2 nm, less than or equal to about 1.9 nm, or less than or equal to about 1.8 nm and greater than or equal to about 0.1 nm, greater than or equal to about 0.3 nm, greater than or equal to about 0.5 nm, greater than or equal to about 1 nm, greater than or equal to about 1.1 nm, or greater than or equal to about 1.2 nm.

[0118] The wavelength of the green light may be greater than or equal to about 500 nm, for example, greater than or equal to about 510 nm, or greater than or equal to about 520 nm and less than or equal to about 560 nm, for example, less than or equal to about 550 nm, or less than or equal to about 540 nm. The wavelength of the red light may be greater than or equal to about 600 nm, for example, greater than or equal to about 610 nm, or greater than or equal to about 620 nm and less than or equal to about 650 nm, or less than or equal to about 640 nm.

[0119] The nanosheet according to an embodiment may further include a second shell including a third semiconductor nanocrystal and disposed on the first shell, wherein the third semiconductor nanocrystal has a composition different from that of the second semiconductor nanocrystal. The second shell may include one or more layers. When the second shell is a multilayer shell of two or more layers, adjacent layers may have different compositions. The second shell may have a composition that varies in the thickness direction.

[0120] The third semiconductor nanocrystal included in the second shell may include a II-VI compound. The third semiconductor nanocrystal may include ZnA (wherein A is selenium, tellurium, sulfur, oxygen, or a combination thereof). The third semiconductor nanocrystal may include ZnSe, ZnS, ZnTe, ZnTeSe, ZnTeS, ZnSeS, ZnTeSeS, ZnO, or a combination thereof.

[0121] The energy band gap of the third semiconductor nanocrystal material may be the same as or greater than the energy band gap of the second semiconductor nanocrystal material. The energy band gap of the third semiconductor nanocrystal material may be the same as or greater than the energy band gap of the first semiconductor nanocrystal material. In one embodiment, the first semiconductor nanocrystal may include zinc and selenium, and the third semiconductor nanocrystal may include zinc and sulfur.

[0122] The thickness of the second shell can be appropriately adjusted. For example, the thickness of the second shell can be greater than or equal to about 0.3 nm, such as greater than or equal to about 0.5 nm, greater than or equal to about 0.6 nm, greater than or equal to about 0.9 nm, or greater than or equal to about 1 nm and less than or equal to about 10 nm, less than or equal to about 9 nm, less than or equal to about 8 nm, less than or equal to about 7 nm, less than or equal to about 6 nm, less than or equal to about 5 nm, less than or equal to about 4 nm, less than or equal to about 3 nm, or less than or equal to about 2 nm.

[0123] The nanosheets may be based on non-cadmium semiconductor nanocrystals. The nanosheets may not include heavy metals such as cadmium, mercury or lead.

[0124] The nanosheet may have a total thickness of less than or equal to about 20 nm, less than or equal to about 19 nm, less than or equal to about 18 nm, less than or equal to about 17 nm, less than or equal to about 16 nm, less than or equal to about 15 nm, less than or equal to about 14 nm, less than or equal to about 13 nm, less than or equal to about 12 nm, less than or equal to about 11 nm, less than or equal to about 10 nm, less than or equal to about 9 nm, less than or equal to about 8 nm, less than or equal to about 7 nm, less than or equal to about 6 nm, less than or equal to about 5 nm, less than or equal to about 4 nm, less than or equal to about 3 nm, less than or equal to about 2.5 nm, or less than or equal to about 2 nm. The total thickness of the nanosheet may be greater than or equal to about 0.5 nm, for example, greater than or equal to about 0.7 nm, or greater than or equal to about 1 nm. The nanosheet may have a laterally increasing size. In one embodiment, the nanosheet may have a thickness greater than about 400 nm. 2 , for example, greater than or equal to about 450 nm 2 , greater than or equal to about 500nm 2 , greater than or equal to about 600nm 2 , greater than or equal to about 650nm 2 , greater than or equal to about 700nm 2 , greater than or equal to about 750nm 2 , greater than or equal to about 800nm 2 , greater than or equal to about 850nm 2, greater than or equal to about 900nm 2 , greater than or equal to about 950nm 2 , greater than or equal to about 1,000nm 2 , greater than or equal to about 1100nm 2 , greater than or equal to about 1200nm 2 , greater than or equal to about 1300nm 2 , greater than or equal to about 1400nm 2 , or greater than or equal to about 1500nm 2 In one embodiment, the lateral dimension of the nanosheet may be less than or equal to about 10,000 nm. 2 , for example, less than or equal to about 9,000 nm 2 , less than or equal to about 8,000nm 2 , less than or equal to about 7,000nm 2 , less than or equal to about 6,000nm 2 , less than or equal to about 5,000nm 2 , less than or equal to about 4,000nm 2 , less than or equal to about 3,000nm 2 , or less than or equal to about 2,000 nm 2 .

[0125] The lateral surface of the nanosheet may have a predetermined two-dimensional shape, but there is no particular limitation. The lateral surface may have at least two dimensions (e.g., length and width). The lateral surface of the nanosheet may be a polygon (triangle, quadrilateral, parallelogram, rhombus, pentagon, hexagon, etc.). The lateral surface of the nanosheet may not be substantially circular. The lateral surface of the nanosheet may have a non-circular shape. The lateral surface of the nanosheet may have a pair of sides opposite to each other (e.g., facing each other), such as at least one pair or at least two pairs of sides opposite to each other (e.g., facing each other). In one embodiment, the lateral surface of the nanosheet may have a substantially rectangular shape.

[0126] The lateral surface of the nanosheet may have a length and a width. The lateral surface of the nanosheet may have an aspect ratio (e.g., width: length) of greater than or equal to about 1:1.1, such as greater than or equal to about 1:2, greater than or equal to about 1:2.5, greater than or equal to about 1:3, greater than or equal to about 1:3.5, or greater than or equal to about 1:4 and less than or equal to about 1:8, such as less than or equal to about 1:7.5, less than or equal to about 1:7, less than or equal to about 1:6.5, less than or equal to about 1:6, or less than or equal to about 1:5.5. Aspect ratio may refer to the ratio between the length of the minor axis and the length of the major axis (e.g., width: length).

[0127] The nanosheet may have a stacked structure and a transmission electron microscope energy dispersive X-ray spectroscopy (TEM-EDX) analysis of its lateral surface may only show elements present in the outermost semiconductor nanocrystal of the stacked structure, such as the semiconductor nanocrystal constituting the outermost semiconductor nanocrystal of the stacked structure. In one embodiment, in the case where the second semiconductor nanocrystal forms the outermost layer of the stacked structure, the TEM-EDX analysis of the lateral surface of the nanosheet may (only) show, for example, show or include elements present in the second semiconductor nanocrystal, such as constituting the second semiconductor nanocrystal (for example, when the second semiconductor nanocrystal includes indium phosphide, the TEM-EDX result may show indium and phosphorus and not show selenium included in the template). In one embodiment, in the case where the third semiconductor nanocrystal forms the outermost layer of the stacked structure, the TEM-EDX analysis of the lateral surface of the nanosheet may (only) show, for example, include elements present in the third semiconductor nanocrystal, such as constituting the third semiconductor nanocrystal (for example, when the third semiconductor nanocrystal includes ZnS or ZnSeS, the result may show zinc and sulfur and optionally selenium). In this case, TEM-EDX analysis of the lateral surface of the nanosheet may not show phosphorus and indium present in the second semiconductor nanocrystals.

[0128] In TEM-EDX analysis, the result for the thickness surface of the nanosheet (i.e., the surface extending in the thickness direction and connecting the two lateral surfaces of the nanosheet, i.e., the bottom surface and the top surface, and optionally substantially perpendicular to the two lateral surfaces of the nanosheet) may be different from the result for the lateral surface of the nanosheet. In TEM-EDX on the thickness surface, the nanosheet may show: the elements present in the template (e.g., the first semiconductor nanocrystal), such as constituting the template, and the elements present in the first shell (e.g., the second semiconductor nanocrystal), such as constituting the first shell, and, if present, the elements present in the second shell (e.g., the third semiconductor nanocrystal), such as constituting the second shell.

[0129] The nanosheet may exhibit two or more main absorption peaks (first absorption peak and second absorption peak) within a range of less than or equal to about 500 nm, such as less than or equal to about 490 nm, less than or equal to about 480 nm, less than or equal to about 470 nm, less than or equal to about 460 nm, less than or equal to about 450 nm, less than or equal to about 440 nm, less than or equal to about 430 nm, less than or equal to about 420 nm, less than or equal to about 410 nm, less than or equal to about 400 nm, less than or equal to about 390 nm, or less than or equal to about 380 nm. The first absorption peak may be a first main peak in a low energy region and the second absorption peak may be a main peak adjacent to the first main peak, which shows higher energy than the first absorption peak (i.e., appears at a wavelength smaller than the first absorption peak). The intensity of the second absorption peak may be greater than or equal to the intensity of the first absorption peak. The difference between the first absorption peak and the second absorption peak may be less than or equal to about 50 nm, for example, less than or equal to about 45 nm, less than or equal to about 40 nm, less than or equal to about 35 nm, less than or equal to about 30 nm, less than or equal to about 25 nm, or less than or equal to about 20 nm. The difference between the first absorption peak and the second absorption peak may be greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 15 nm, or greater than or equal to about 20 nm.

[0130] In the nanosheet of the embodiment, the shift of the absorption peak wavelength caused by the formation of the first shell and the optional second shell relative to the absorption peak wavelength of the template may be limited (e.g., insignificant). Therefore, in the nanosheet according to the embodiment, the difference between the first absorption peak of the template and the first absorption peak of the nanosheet may be less than about 100nm, such as less than or equal to about 90nm, less than or equal to about 80nm, less than or equal to about 70nm, less than or equal to about 60nm, less than or equal to about 50nm, less than or equal to about 40nm, less than or equal to about 30nm, less than or equal to about 20nm, or less than or equal to about 10nm. In one embodiment, the difference between the first absorption peak of the two-dimensional template and the first absorption peak of the nanosheet may be less than about 50nm.

[0131] The NPL may exhibit an improved half width (FWHM) in the absorption spectrum or emission spectrum. The core-shell quantum dots that emit green light without cadmium may have a half width (FWHM) greater than 35nm. In contrast, the NPL of the embodiment may exhibit a half width (FWHM) less than or equal to about 35nm, such as less than or equal to about 34nm, less than or equal to about 33nm, less than or equal to about 32nm, less than or equal to about 31nm, or less than or equal to about 30nm. The core-shell quantum dots that emit red light without cadmium may have a half width (FWHM) greater than (or at least) 40nm. In contrast, the NPL of the embodiment may exhibit a half width (FWHM) less than or equal to about 39nm, less than or equal to about 38nm, less than or equal to about 37nm, less than or equal to about 36nm, less than or equal to about 35nm, less than or equal to about 34nm, less than or equal to about 33nm, less than or equal to about 32nm, or less than or equal to about 31nm.

[0132] In the nanosheet according to an embodiment, the first semiconductor nanocrystals may include ZnA (wherein A is selenium, tellurium, sulfur, oxygen, or a combination thereof), and the second semiconductor nanocrystals may include a Group III metal and phosphorus.

[0133] In the nanosheets, the amount of the Group III metal may be greater than or equal to about 0.05 mol, for example, greater than or equal to about 0.06 mol, greater than or equal to about 0.07 mol, greater than or equal to about 0.08 mol, greater than or equal to about 0.09 mol, greater than or equal to about 0.1 mol, greater than or equal to about 0.15 mol, greater than or equal to about 0.2 mol, greater than or equal to about 0.25 mol, greater than or equal to about 0.3 mol, greater than or equal to about 0.35 mol, greater than or equal to about 0.4 mol, greater than or equal to about 0.45 mol, greater than or equal to about 0.5 mol, greater than or equal to about 0.55 mol, greater than or equal to about 0.6 mol, greater than or equal to about 0.65 mol, greater than or equal to about 0.7 mol, greater than or equal to about 0.75 mol, or greater than or equal to about 0.8 mol, based on 1 mol of element A.

[0134] The amount of the Group III metal may be less than or equal to about 2 moles, for example, less than or equal to about 1.9 moles, less than or equal to about 1.8 moles, less than or equal to about 1.7 moles, less than or equal to about 1.6 moles, less than or equal to about 1.5 moles, less than or equal to about 1.4 moles, less than or equal to about 1.3 moles, less than or equal to about 1.2 moles, less than or equal to about 1.1 moles, less than or equal to about 1 mole, or less than or equal to about 0.9 moles, based on 1 mole of element A.

[0135] In the nanosheet, the amount of zinc may be greater than or equal to about 1 mol, greater than or equal to about 1.5 mol, greater than or equal to about 2 mol, greater than or equal to about 2.5 mol, greater than or equal to about 3 mol, greater than or equal to about 3.5 mol, greater than or equal to about 4 mol, greater than or equal to about 4.5 mol, greater than or equal to about 5 mol, or greater than or equal to about 5.5 mol, based on 1 mol of element A.

[0136] The amount of zinc may be less than or equal to about 20 moles, less than or equal to about 19 moles, less than or equal to about 18 moles, less than or equal to about 17 moles, less than or equal to about 16 moles, less than or equal to about 15 moles, less than or equal to about 14 moles, less than or equal to about 13 moles, less than or equal to about 12 moles, less than or equal to about 10 moles, less than or equal to about 9 moles, less than or equal to about 8 moles, less than or equal to about 7 moles, or less than or equal to about 6 moles, based on 1 mole of element A.

[0137] In the nanosheet, the amount of phosphorus may be greater than or equal to about 0.05 mol, greater than or equal to about 0.06 mol, greater than or equal to about 0.07 mol, greater than or equal to about 0.08 mol, greater than or equal to about 0.09 mol, greater than or equal to about 0.1 mol, greater than or equal to about 0.11 mol, greater than or equal to about 0.12 mol, or greater than or equal to about 0.13 mol, based on 1 mol of element A.

[0138] The amount of phosphorus may be less than or equal to about 10 moles, less than or equal to about 9 moles, less than or equal to about 8 moles, less than or equal to about 7 moles, less than or equal to about 6 moles, less than or equal to about 5 moles, less than or equal to about 4.5 moles, less than or equal to about 4 moles, less than or equal to about 3.5 moles, less than or equal to about 3 moles, less than or equal to about 2.5 moles, less than or equal to about 2 moles, or less than or equal to about 1.8 moles, based on 1 mole of element A.

[0139] The NPL may include an organic ligand described later, an organic solvent, or a combination thereof on the surface of the NPL (eg, bound to the surface of the NPL). The NPL may be dispersed in an organic solvent described later and precipitated in a non-solvent described later.

[0140] In an embodiment, a method of making the aforementioned nanosheets comprises:

[0141] reacting a first metal precursor and a first non-metal precursor for a first semiconductor nanocrystal in an organic solvent in the presence of an organic ligand at a temperature below about 175° C. to synthesize a two-dimensional template; and

[0142] A second metal precursor and a second non-metal precursor for a second semiconductor nanocrystal are reacted in an organic solvent in the presence of an organic ligand and the two-dimensional template at a temperature of less than or equal to about 200°C, e.g., less than or equal to about 170°C, less than or equal to about 165°C to form a first shell including the second semiconductor nanocrystal on (e.g., at least one) surface of the two-dimensional template.

[0143] The method may further include reacting a third metal precursor and a third non-metal precursor for a third semiconductor nanocrystal in an organic solvent in the presence of an organic ligand and particles on which the first shell is formed at a shelling temperature to form a second shell on the first shell.

[0144] The organic ligand may include RCOOH, RNH 2 , R 2 NH, R 3 N, RSH, RH 2 PO, R 2 HPO, R 3 PO, RH 2 P.R 2 HP, R 3 P, ROH, RCOOR, RPO(OH) 2 , RPOOH, RHPOOH, R 2POOH, or a combination thereof, wherein R is the same or different and independently a substituted or unsubstituted C1-C40 aliphatic hydrocarbon group (e.g., C1-C40 alkyl, C2-C40 alkenyl, C2-C40 alkynyl), a substituted or unsubstituted C6-C40 aromatic hydrocarbon group (e.g., C6-C20 aryl). The organic ligand may coordinate with the surface of the obtained nanocrystal and may contribute to the dispersion of the nanosheet in the solution, and / or affect the photoluminescence and electrical properties of the quantum dots. Examples of the organic ligand may include methyl mercaptan, ethyl mercaptan, propyl mercaptan, butyl mercaptan, pentyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecanethiol, hexadecyl mercaptan, octadecyl mercaptan, benzyl mercaptan; methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, octylamine, dodecylamine, hexadecylamine, octadecylamine, dimethylamine, diethylamine, dipropylamine; formic acid, acetic acid, propionic acid, butyric acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, dodecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid or benzoic acid; phosphine such as substituted or unsubstituted methyl phosphine (e.g., trimethyl phosphine, methyl diphenyl phosphine, etc.), substituted or unsubstituted ethyl phosphine (e.g., triethyl phosphine, ethyl diphenyl phosphine, etc.), substituted or unsubstituted propyl phosphine , substituted or unsubstituted butyl phosphine, substituted or unsubstituted pentyl phosphine, or substituted or unsubstituted octyl phosphine (e.g., trioctyl phosphine (TOP)); phosphine oxides such as substituted or unsubstituted methyl phosphine oxide (e.g., trimethyl phosphine oxide, methyl diphenyl phosphine oxide, etc.), substituted or unsubstituted ethyl phosphine oxide (e.g., triethyl phosphine oxide, ethyl diphenyl phosphine oxide, etc.), substituted or unsubstituted propyl phosphine oxide, substituted or unsubstituted butyl phosphine oxide, or substituted or unsubstituted octyl phosphine oxide (e.g., trioctyl phosphine oxide (TOPO)); diphenyl phosphine, diphenyl phosphine oxide, triphenyl phosphine, triphenyl phosphine oxide; C2-C30 phosphonic acid; C2-C30 phosphinic acid; etc., but not limited thereto. Two or more different organic ligands may be used. In the reaction for forming the template and the first shell, the organic ligand may include a primary amine having 6 or more carbon atoms. In the reaction for forming the template and the first shell, two or more different organic ligands may be used.

[0145] The organic solvent may be a C6-C22 primary amine such as hexadecylamine, oleylamine, etc.; a C6-C22 secondary amine such as dioctylamine; a C6-C40 tertiary amine such as trioctylamine; a nitrogen-containing heterocyclic compound such as pyridine; a C6-C40 aliphatic hydrocarbon (e.g., alkane, alkene, alkyne, etc.) such as hexadecane, octadecane, octadecene, or squalane; a C6-C30 aromatic hydrocarbon such as phenyldodecane, phenyltetradecane, or phenylhexadecane; a phosphine substituted with a C6-C22 alkyl group such as trioctylphosphine; a phosphine oxide substituted with a C6-C22 alkyl group such as trioctylphosphine oxide; a C12-C22 aromatic ether such as phenyl ether or benzyl ether; or a combination thereof. The type and amount of the solvent may be appropriately selected in consideration of the type and amount of the precursor and the organic ligand.

[0146] In one embodiment, during the formation of the template and the first shell, the organic solvent may not include a tertiary amine including (e.g., at least one (e.g., two or three)) C6-20 alkyl group, such as trioctylamine. In one embodiment, during the formation of the template and the first shell, the organic solvent may not include an olefin compound such as octadecene. In one embodiment, the organic solvent may include an alkyl phosphine including three C6-C22 alkyl groups.

[0147] The (first, second or third) metal precursor may be a metal powder, an alkylated metal, a metal carboxylate, a metal hydroxide, a metal halide, a metal oxide, a metal inorganic salt (e.g., a nitrate, etc.), a metal sulfate or a metal acetylacetonate, but is not limited thereto. Considering the composition of the first semiconductor nanocrystal, the second semiconductor nanocrystal and the third semiconductor nanocrystal, the (first, second or third) metal precursor may include a desired metal (e.g., zinc, indium, gallium, etc.).

[0148] Considering the composition of the first semiconductor nanocrystal, the second semiconductor nanocrystal and the third semiconductor nanocrystal, the (first, second or third) metal precursor may include a desired non-metallic element. The metal precursor may be in the form of a suitable compound for synthesizing semiconductor nanocrystals, and is not particularly limited.

[0149] Hereinafter, a nanosheet optionally having a second shell is described including, but not limited to, a first semiconductor nanocrystal including zinc selenide, a second semiconductor nanocrystal including indium and phosphorus, and optionally a third semiconductor nanocrystal including zinc and a chalcogen (e.g., sulfur, selenium, or a combination thereof).

[0150] In one embodiment, the type of zinc precursor can be appropriately selected. Examples of the zinc precursor may include Zn metal powder (e.g., dimethyl zinc, diethyl zinc, etc.), alkylated Zn compounds, Zn alkoxides, carboxylic acid Zn, Zn nitrate, Zn perchlorate, Zn sulfate, Zn acetylacetonate, Zn halides, Zn cyanides, Zn hydroxides, Zn oxides, Zn peroxides, or combinations thereof. Two or more different zinc precursors may be used.

[0151] The selenium precursor may include selenium-trioctylphosphine (Se-TOP), selenium-tributylphosphine (Se-TBP), selenium-triphenylphosphine (Se-TPP), selenium-diphenylphosphine (Se-DPP), or a combination thereof, but is not limited thereto.

[0152] The type of indium precursor may be appropriately selected. Examples of the indium precursor may be trimethyl indium, indium carboxylates such as indium acetate, indium palmitate, indium stearate, etc., indium hydroxide, indium chloride, indium oxide, indium nitrate, indium sulfate, or a combination thereof.

[0153] The type of the gallium precursor may be appropriately selected. Examples of the gallium precursor may be trimethylgallium, gallium carboxylates such as gallium acetate, gallium palmitate, gallium stearate, etc., gallium hydroxide, gallium chloride, gallium oxide, gallium nitrate, gallium sulfate, or a combination thereof.

[0154] The type of the phosphorus precursor may be appropriately selected. Examples of the phosphorus precursor may be tris(trimethylsilyl)phosphine, tris(dimethylamino)phosphine, triethylphosphine, tributylphosphine, trioctylphosphine, triphenylphosphine, tricyclohexylphosphine, or a combination thereof.

[0155] In order to form a two-dimensional template, the reaction can be carried out at a temperature of less than about 175°C, such as less than or equal to about 170°C, less than or equal to about 165°C, less than or equal to about 160°C, less than or equal to about 155°C, less than or equal to about 150°C, less than or equal to about 145°C, or less than or equal to about 140°C. The reaction temperature may be greater than or equal to about 100°C, such as greater than or equal to about 120°C, or greater than or equal to about 130°C. The reaction time may be appropriately selected, but is not particularly limited. The reaction time may be less than about 2 hours, such as less than about 1.5 hours, less than about 1 hour, less than or equal to about 50 minutes. The reaction time may be greater than or equal to about 20 minutes, such as greater than or equal to about 30 minutes.

[0156] In order to form indium phosphide or the like as a first shell having a desired thickness on the template instead of forming particles, the reaction may be carried out at a temperature of less than or equal to about 200° C., for example, less than or equal to about 175° C., less than or equal to about 170° C., less than or equal to about 165° C., less than or equal to about 160° C., less than or equal to about 155° C., less than or equal to about 150° C., less than or equal to about 145° C., or less than or equal to about 140° C. The reaction temperature may be greater than or equal to about 100° C., for example, greater than or equal to about 120° C. The reaction time may be appropriately selected, but is not particularly limited. The reaction time may be less than about 1 hour, for example, less than or equal to about 50 minutes. The reaction time may be greater than or equal to about 20 minutes, for example, greater than or equal to about 30 minutes.

[0157] After forming the template and / or the first shell, the obtained product can be separated by adding a non-solvent, but there is no limitation. The method can be carried out in a continuous process without a separation process. When separating the template, the particles formed by the first shell (including the particles of the first shell formed on the surface of the template), or a combination thereof, or separating the final NPL, by adding the non-solvent to be described later to the final reaction solution obtained, the nanocrystal particles coordinated by the organic ligand can be separated (for example, precipitated). The separated product can be washed with the non-solvent. The non-solvent can be a polar solvent that is miscible with the solvent used in the reaction and in which the nanocrystals cannot be dispersed. The non-solvent can be selected in consideration of the solvent used in the reaction and can be, for example, acetone, ethanol, butanol, isopropanol, ethylene glycol, water, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), diethyl ether, formaldehyde, acetaldehyde, a solvent with a solubility parameter similar to the aforementioned solvent, or a combination thereof. Separation can be carried out by centrifugation, precipitation, chromatography or distillation. If desired, the separated nanocrystals can be added to a washing solvent and washed. The washing solvent is not particularly limited and may have a solubility parameter similar to that of the ligand, and may include, for example, hexane, heptane, octane, chloroform, toluene, benzene, and the like.

[0158] In each process, the amounts of the precursor and the organic ligand used can be determined in consideration of the final NPL composition, the thickness of each layer, the reactivity of the precursor, and the like.

[0159] Embodiments provide a composition including the aforementioned NPL, a composite including the aforementioned NPL, or a combination thereof.

[0160] The composition according to the embodiment includes (e.g., multiple) semiconductor nanocrystal particles; an optional dispersant (e.g., a binder including a carboxylic acid group); and an optional (organic) solvent, wherein the semiconductor nanocrystal particles include the aforementioned nanosheets. The dispersant may include a binder monomer or polymer including a carboxylic acid group. The composition may further include a (photo)polymerizable monomer including a carbon-carbon double bond and an optional (thermal or photo)initiator.

[0161] The amount of the aforementioned semiconductor nanocrystal particles (or NPL, hereinafter semiconductor nanocrystal particles may also be referred to as NPL) in the composition may be appropriately adjusted in view of the desired end use (e.g., color filter, etc.). In one embodiment, the amount of the semiconductor nanocrystal particles may be greater than or equal to about 1 weight percent (wt%), such as greater than or equal to about 2 weight %, greater than or equal to about 3 weight %, greater than or equal to about 4 weight %, greater than or equal to about 5 weight %, greater than or equal to about 6 weight %, greater than or equal to about 7 weight %, greater than or equal to about 8 weight %, greater than or equal to about 9 weight %, greater than or equal to about 10 weight %, greater than or equal to about 15 weight %, greater than or equal to about 20 weight %, greater than or equal to about 25 weight %, greater than or equal to about 30 weight %, greater than or equal to about 35 weight %, or greater than or equal to about 40 weight %, based on the solid content of the composition (i.e., based on the total weight of the solids in the composition). The amount of the semiconductor nanocrystal particles can be less than or equal to about 70 wt %, for example, less than or equal to about 65 wt %, less than or equal to about 60 wt %, less than or equal to about 55 wt %, or less than or equal to about 50 wt %, based on the solid content of the composition. As used herein, the solid content of the composition can represent the amount of a given component in the composite to be further described below.

[0162] Composition according to embodiment can be used for manufacturing the pattern of semiconductor nanocrystal-polymer composite.Composition according to embodiment can be the photoresist composition comprising semiconductor nanocrystal particles, photolithography method can be applied to the photoresist composition.Composition according to embodiment can be ink composition, and the ink composition can provide pattern by printing (for example, droplet discharge method such as inkjet printing).Composition according to embodiment can not include conjugated polymer (except cardo adhesive to be described later).Composition according to embodiment can include conjugated polymer.In this article, conjugated polymer can refer to the polymer (for example, polyphenylene vinylene etc.) with conjugated double bonds in the main chain of polymer.

[0163] In the composition according to the embodiment, the dispersant or binder monomer or polymer may include a carboxylic acid group. The binder polymer may include a copolymer comprising a monomer mixture including a first monomer including a carboxylic acid group and a carbon-carbon double bond, a second monomer including a carbon-carbon double bond and a hydrophobic portion and not including a carboxylic acid group, and optionally a third monomer including a carbon-carbon double bond and a hydrophilic portion and not including a carboxylic acid group;

[0164] A polymer containing multiple aromatic rings (hereinafter, cardo binder) having a backbone structure in which two aromatic rings are bonded to a quaternary carbon atom which is a constituent atom of another cyclic part in the main chain and including a carboxylic acid group (—COOH); or

[0165] Its combination.

[0166] The copolymer may include a first repeating unit derived from the first monomer and a second repeating unit derived from the second monomer, and optionally a third repeating unit derived from the third monomer.

[0167] The polymer including a carboxylic acid group may include a polymer including a plurality of aromatic rings. The polymer including a plurality of aromatic rings is known as a cardo binder resin and may be commercially available.

[0168] In the composition, the amount of the binder polymer may be greater than or equal to about 0.5 wt %, such as greater than or equal to about 1 wt %, greater than or equal to about 5 wt %, greater than or equal to about 10 wt %, greater than or equal to about 15 wt %, or greater than or equal to about 20 wt %, based on the total weight or solid content of the composition, but is not limited thereto. The amount of the binder polymer may be less than or equal to about 55 wt %, less than or equal to about 35 wt %, such as less than or equal to about 33 wt %, or less than or equal to about 30 wt %, based on the total weight or solid content of the composition.

[0169] In the composition, the polymerizable (e.g., photopolymerizable) monomer including a carbon-carbon double bond may include a (e.g., photopolymerizable) acryl-based monomer. The monomer may be a precursor for an insulating polymer. The amount of the monomer may be greater than or equal to about 0.5 wt %, such as greater than or equal to about 1 wt %, or greater than or equal to about 2 wt %, based on the total weight or solid content of the composition. The amount of the photopolymerizable monomer may be less than or equal to about 30 wt %, such as less than or equal to about 28 wt %, less than or equal to about 25 wt %, less than or equal to about 23 wt %, less than or equal to about 20 wt %, less than or equal to about 18 wt %, less than or equal to about 17 wt %, less than or equal to about 16 wt %, or less than or equal to about 15 wt %, based on the total weight or solid content of the composition.

[0170] The initiator in the composition can be used for the polymerization of the aforementioned monomers. The initiator is a compound that accelerates free radical reactions (e.g., free radical polymerization of monomers) by generating free radical chemical species under mild conditions (e.g., by heat or light). The initiator can be a thermal initiator or a photoinitiator.

[0171] In the composition, the amount of the initiator may be appropriately adjusted in consideration of the type and amount of the polymerizable monomer. In an embodiment, the initiator may be used in an amount of about 0.01 wt % to about 10 wt % based on the total weight of the composition, but is not limited thereto.

[0172] The composition may further include a (multi- or monofunctional) thiol compound having (eg, at least one) thiol group at a terminal, metal oxide particles, or a combination thereof.

[0173] The metal oxide particles may include TiO 2 、SiO 2 、BaTiO 3 , Ba 2 TiO 4 , ZnO, or a combination thereof. In the composition, the amount of the metal oxide may be greater than or equal to about 1 wt % and less than or equal to about 35 wt %, less than or equal to about 25 wt %, less than or equal to about 10 wt %, or less than or equal to about 5 wt %, based on the solid content of the composition. The diameter of the metal oxide particles is not particularly limited and may be appropriately selected. The diameter of the metal oxide particles may be greater than or equal to about 100 nm, for example, greater than or equal to about 150 nm, or greater than or equal to about 200 nm and less than or equal to about 1000 nm, or less than or equal to about 800 nm.

[0174] The amount of the thiol compound may be less than or equal to about 40 wt %, less than or equal to about 30 wt %, less than or equal to about 20 wt %, less than or equal to about 10 wt %, less than or equal to about 9 wt %, less than or equal to about 8 wt %, less than or equal to about 7 wt %, less than or equal to about 6 wt %, or less than or equal to about 5 wt %, based on the total weight or solid content of the composition. The amount of the thiol compound may be greater than or equal to about 0.1 wt %, such as greater than or equal to about 0.5 wt % or greater than or equal to about 1 wt %, based on the total weight of the composition.

[0175] The composition may further include an organic solvent (or liquid vehicle). The type of available organic solvent is not particularly limited. By taking into account the aforementioned main components (i.e., the semiconductor nanocrystal particles, dispersants, polymerizable monomers, initiators, and the thiol compounds if used) and the type and amount of the additives described later, the type and amount of the organic solvent can be appropriately determined. The composition may include solvent in a residual amount except the desired amount of (non-volatile) solids. If desired, in addition to the aforementioned components, the composition may further include multiple additives such as light diffusing agents, leveling agents or coupling agents. The amount of the additive is not particularly limited, and may be controlled in the following appropriate range: wherein the additive does not adversely affect the preparation of the composition and the manufacture of the semiconductor nanocrystal-polymer composite and optionally the patterning of the composite.

[0176] If used, the additive can be used in an amount greater than or equal to about 0.1 wt %, such as greater than or equal to about 0.5 wt %, greater than or equal to about 1 wt %, greater than or equal to about 2 wt %, or greater than or equal to about 5 wt %, based on the total weight of the composition, but is not limited thereto. If used, the amount of the additive can be less than or equal to about 20 wt %, such as less than or equal to about 19 wt %, less than or equal to about 18 wt %, less than or equal to about 17 wt %, less than or equal to about 16 wt %, or less than or equal to about 15 wt %, based on the total weight of the composition, but is not limited thereto.

[0177] The specific type of the composition (for example, the first monomer, the second monomer, the third monomer, a polymer including a carboxylic acid group, an acryl-based monomer, an initiator, a solvent, a polythiol compound, a variety of additives, etc.), the preparation of the composition, etc. can be referred to US-2017-0059988-A1, the contents of which are all incorporated herein by reference.

[0178] The composition can provide a semiconductor nanocrystal-polymer composite by (e.g., free radical) polymerization. Therefore, in an embodiment, the semiconductor nanocrystal-polymer composite includes a polymer matrix; and a plurality of semiconductor nanocrystal particles dispersed in the polymer matrix, wherein the plurality of semiconductor nanocrystal particles include the aforementioned nanosheets.

[0179] The polymer matrix may include: a dispersant (e.g., a binder polymer including a carboxylic acid group), a polymerization product of a polymerizable monomer having (at least one, e.g., at least two, at least three, at least four, or at least five) carbon-carbon double bonds (e.g., an insulating polymer), a polymerization product of a polymerizable monomer and a polythiol compound having at least two thiol groups at the end, metal oxide particles, or a combination thereof.

[0180] In an embodiment, the polymer matrix may include a cross-linked polymer and a dispersant (e.g., a (carboxyl-containing) binder polymer). The polymer matrix may not include a conjugated polymer (except for cardo resin). The cross-linked polymer may include a thiol-ene resin, a cross-linked poly (meth) acrylate, or a combination thereof. In one embodiment, the cross-linked polymer may be a polymerization product of the aforementioned polymerizable monomer and the optional polythiol compound.

[0181] The nanosheets, dispersant or binder polymer, polymerizable monomer and polythiol compound are the same as described above.

[0182] A film of a semiconductor nanocrystal-polymer composite or a semiconductor nanocrystal-polymer composite pattern to be described later may have a thickness of, for example, less than or equal to about 30 μm, for example, less than or equal to about 25 μm, less than or equal to about 20 μm, less than or equal to about 15 μm, less than or equal to about 10 μm, less than or equal to about 8 μm, less than or equal to about 7 μm and greater than about 2 μm, for example, greater than or equal to about 3 μm, greater than or equal to about 3.5 μm, or greater than or equal to about 4 μm.

[0183] In an embodiment, the patterned film includes a repeating segment, the repeating segment includes a first segment emitting a first light, wherein the first segment includes the aforementioned semiconductor nanocrystal-polymer composite. The repeating segment may include a second segment emitting a second light having a wavelength different from the first light, wherein the second segment may include a semiconductor nanocrystal-polymer composite. The semiconductor nanocrystal-polymer composite of the second segment may include a second semiconductor nanocrystal particle configured to emit the second light. The second semiconductor nanocrystal particle may include the aforementioned nanosheet. The first light or the second light may be a red light having a maximum emission peak wavelength between about 600nm and about 650nm (e.g., about 620nm to about 650nm) or a green light having a maximum emission peak wavelength between about 500nm and about 550nm (e.g., about 510nm to about 540nm). The patterned film may further include a third segment, the third segment emitting a third light (e.g., blue light) different from the first light and the second light or passing it. The third light may have a maximum peak wavelength ranging from about 380nm to about 480nm.

[0184] In an embodiment, a display device includes a light source and a photoluminescent element, and the photoluminescent element includes a substrate and an emission layer disposed on the substrate, and the emission layer includes a film or a patterned film of the semiconductor nanocrystal-polymer composite. The light source is configured to provide incident light to the photoluminescent element. The incident light may have an emission peak wavelength greater than or equal to about 440 nm, for example, greater than or equal to about 450 nm and less than or equal to about 500 nm, for example, less than or equal to about 480 nm, less than or equal to about 470 nm, or less than or equal to about 460 nm.

[0185] In the emission layer of a device according to one embodiment (e.g., the patterned film of the semiconductor nanocrystal-polymer composite), the first segment may be a segment emitting red light, the second segment may be a segment emitting green light, and the light source may be an element emitting blue light.

[0186] An optical element for blocking (eg, reflecting or absorbing) blue light (a blue light blocking layer or a first filter layer to be described later) may be provided on the front surfaces (light emitting surfaces) of the first segment and the second segment.

[0187] In the aforementioned display device, the light source includes a plurality of light-emitting units corresponding to the first segment and the second segment, respectively, and the light-emitting units may include a first electrode and a second electrode facing each other and an electroluminescent layer disposed between the first electrode and the second electrode. The electroluminescent layer may include an organic light-emitting material. For example, each light-emitting unit of the light source may include an electroluminescent device (e.g., an organic light-emitting diode (OLED)) configured to emit light of a predetermined wavelength (e.g., blue light, green light, or a combination thereof). The structure and material of the electroluminescent device and the organic light-emitting diode (OLED) are not particularly limited. The light source includes an organic light-emitting diode (OLED) that emits blue light (and optionally green light).

[0188] Figure 3 and 4 is a schematic cross-sectional view of a display device according to a non-limiting embodiment. Figure 3 and 4 , the light source may include an organic light emitting diode (OLED) emitting blue light. The organic light emitting diode OLED may include: (at least two, for example, three or more) pixel electrodes 90a, 90b, 90c formed on a substrate 100; pixel defining layers 150a, 150b formed between adjacent pixel electrodes 90a, 90b, 90c; organic light emitting layers 140a, 140b, 140c formed on the pixel electrodes 90a, 90b, 90c; and a common electrode layer 130 formed on the organic light emitting layers 140a, 140b, 140c.

[0189] A thin film transistor and a substrate may be disposed under the organic light emitting diode (OLED). Pixel regions of the OLED may be disposed corresponding to first, second, and third sections, respectively, which will be described in detail below.

[0190] A stacked structure including a semiconductor nanocrystal-polymer composite pattern (e.g., including a first repeating segment comprising nanosheets emitting green light, a second repeating segment comprising nanosheets emitting red light, or a combination thereof) and a substrate, or the semiconductor nanocrystal-polymer composite pattern can be disposed on or above a light source, for example, directly on the light source.

[0191] The first and second sections are configured such that blue light emitted from the light source enters therein and red light and green light may be emitted therefrom, respectively. The blue light emitted from the light source may pass through the third section.

[0192] Light (e.g., blue light) emitted from the light source may enter the second segment 21 and the first segment 11 of the pattern 170 to emit (e.g., converted) red light R and green light G, respectively. Blue light B emitted from the light source passes through the third segment 31 or is transmitted from the third segment 31. An optical element 160 may be disposed above the second segment 21 emitting red light, the first segment 11 emitting green light, or a combination thereof. The optical element may be a blue cutoff layer that cuts off (e.g., reflects or absorbs) blue light and optionally green light, or a first filter layer. The blue cutoff layer 160 may be disposed on the upper substrate 240. The blue cutoff layer 160 may be disposed between the upper substrate 240 and the quantum dot-polymer composite pattern and above the first segment 11 and the second segment 21. The details of the blue cutoff layer are the same as those described below for the first filter layer 310.

[0193] The device can be obtained by separately manufacturing the aforementioned stacked structure and an LED or OLED (eg, emitting blue light) and then assembling them. Alternatively, the device can be obtained by directly forming a semiconductor nanocrystal-polymer composite pattern on the LED or OLED.

[0194] The substrate may be a substrate including an insulating material. The substrate may include glass; various polymers such as polyethylene terephthalate (PET) or polyethylene naphthalate (PEN), polyesters of polycarbonate and polyacrylate; polysiloxanes such as polydimethylsiloxane (PDMS); inorganic materials such as Al 2 O 3 or ZnO; or a combination thereof, but not limited thereto. The thickness of the substrate may be appropriately selected in consideration of the substrate material, but is not particularly limited. The substrate may be flexible. The substrate may have a transmittance of greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 80%, or greater than or equal to about 90% for light emitted from the semiconductor nanocrystal particles.

[0195] A wiring layer including a thin film transistor and the like is formed on the substrate. The wiring layer may further include a gate line, a sustaining voltage line, a gate insulating layer, a data line, a source electrode, a drain electrode, a semiconductor, a protective layer, and the like. According to one embodiment, the detailed structure of the wiring layer can be confirmed. The gate line and the sustaining voltage line are electrically isolated from each other, and the data line is insulated and crosses the gate line and the sustaining voltage line. The gate electrode, the source electrode, and the drain electrode form a control terminal, an input terminal, and an output terminal of the thin film transistor, respectively. The drain electrode is electrically connected to a pixel electrode to be described later.

[0196] The pixel electrode can function as an anode of the display device. The pixel electrode can be formed of a transparent conductive material such as indium tin oxide (ITO) or indium zinc oxide (IZO). The pixel electrode can be formed of a material with light blocking properties such as gold (Au), platinum (Pt), nickel (Ni), tungsten (W), chromium (Cr), molybdenum (Mo), iron (Fe), cobalt (Co), copper (Cu), palladium (Pd) or titanium (Ti). The pixel electrode can have a two-layer structure in which the aforementioned transparent conductive material and the material with light blocking properties are sequentially stacked.

[0197] Between two adjacent pixel electrodes, a pixel defining layer (PDL) overlaps the ends of the pixel electrodes to divide the pixel electrodes into pixel units. The pixel defining layer is an insulating layer that can electrically isolate the at least two pixel electrodes.

[0198] The pixel defining layer covers a portion of an upper surface of the pixel electrode, and a remaining area of ​​the pixel electrode not covered by the pixel defining layer may provide an opening. An organic emission layer to be described later may be formed on an area defined by the opening.

[0199] The organic emission layer defines each pixel region through the aforementioned pixel electrode and the pixel defining layer. In other words, one pixel region may be defined as a region where one organic emission unit layer is formed in contact with one pixel electrode divided by the pixel defining layer.

[0200] For example, in a display device according to an embodiment, the organic emission layer may be defined as a first pixel region, a second pixel region, and a third pixel region, and the pixel regions are spaced apart from each other by the pixel defining layer, leaving a predetermined interval.

[0201] In one embodiment, the organic emission layer may emit a third light belonging to the visible light wavelength region (e.g., in the visible light wavelength region) or to the UV wavelength region (e.g., in the UV wavelength region). That is, the first to third pixel regions of the organic emission layer may each emit a third light. In one embodiment, the third light may be light with the highest energy in the visible light wavelength region, for example, blue light. When all pixel regions of the organic emission layer are designed to emit the same light, the pixel regions of the organic emission layer may all be formed of the same or similar materials or may display the same or similar properties. In this way, the process difficulties of forming the organic emission layer may be alleviated, and the display device may be applied to large-scale / large-area processes, for example, formed by large-scale / large-area processes. However, the organic emission layer according to the embodiment is not limited thereto, but the organic emission layer may be designed to emit at least two different lights.

[0202] The organic emission layer includes an organic emission unit layer in each pixel area, and each organic emission unit layer may further include an auxiliary layer (e.g., a hole injection layer (HIL), a hole transport layer (HTL), an electron transport layer (ETL), etc.) in addition to the emission layer.

[0203] The common electrode (layer) may function as a cathode of the display device. The common electrode may be formed of a transparent conductive material such as indium tin oxide (ITO) or indium zinc oxide (IZO). The common electrode may be formed on the organic emission layer and may be integrated therewith.

[0204] A planarization layer or a passivation layer (not shown) may be formed on the common electrode. The planarization layer may include an (eg, transparent) insulating material to ensure electrical insulation from the common electrode.

[0205] In one embodiment, the display device may further include a lower substrate, a polarizer disposed below the lower substrate, and a liquid crystal layer disposed between the stacked structure and the lower substrate, and in the stacked structure, the light emitting layer may be disposed to face the liquid crystal layer. The display device may further include a polarizer between the liquid crystal layer and the emission layer. The light source may further include an LED and, if necessary, a light guide plate.

[0206] Non-limiting examples of display devices (eg, liquid crystal display devices) according to embodiments are described with reference to the accompanying drawings. Figure 5 Schematic cross-sectional view showing a liquid crystal display according to an embodiment. Figure 5 , a display device of an embodiment includes a liquid crystal panel 200 , a polarizer 300 disposed under the liquid crystal panel 200 , and a backlight unit (BLU) disposed under the polarizer 300 .

[0207] The liquid crystal panel 200 includes a lower substrate 210, a stacked structure, and a liquid crystal layer 220 disposed between the stacked structure and the lower substrate. The stacked structure includes an upper substrate 240 and a photoluminescent layer 230 including a pattern of a quantum dot polymer composite. The upper substrate 240 is transparent.

[0208] The lower substrate 210, also referred to as an array substrate, may be a transparent insulating material substrate. The substrate is the same as described above. A wiring board 211 is disposed on the upper surface of the lower substrate 210. The wiring board 211 may include a plurality of gate lines (not shown) and data lines (not shown) defining pixel regions, a thin film transistor disposed adjacent to the intersection region of the gate lines and the data lines, and a pixel electrode of each pixel region, but is not limited thereto. The details of such a wiring board are not particularly limited.

[0209] The liquid crystal layer 220 may be disposed on the wiring board 211. The liquid crystal layer 220 may include an alignment layer 221 on and below the liquid crystal layer 220 to initially align the liquid crystal material included therein. Details of the liquid crystal material and the alignment layer (e.g., liquid crystal material, alignment layer material, method of forming the liquid crystal layer, thickness of the liquid crystal layer, etc.) are not particularly limited.

[0210] The lower polarizer 300 is disposed under the lower substrate. The material and structure of the polarizer 300 are not particularly limited. A backlight unit (eg, emitting blue light) may be disposed under the polarizer 300.

[0211] The upper optical element or upper polarizer 300 may be disposed between the liquid crystal layer 220 and the upper substrate 240, but is not limited thereto. For example, the upper polarizer may be disposed between the liquid crystal layer 220 and the photoluminescent layer 230. The polarizer may be any polarizer used in a liquid crystal display device. The polarizer may be TAC (triacetyl cellulose) having a thickness of less than or equal to about 200 μm, but is not limited thereto. In one embodiment, the upper optical element may be a coating that controls a refractive index without a polarization function.

[0212] The backlight unit includes a light source 110. The light source may emit blue light or white light. The light source may include a blue LED, a white LED, a white OLED, or a combination thereof, but is not limited thereto.

[0213] The backlight unit may further include a light guide plate 120. In one embodiment, the backlight unit may be an edge-type lighting device. For example, the backlight unit may include: a reflector (not shown); a light guide plate (not shown) disposed on the reflector and providing a planar light source to the liquid crystal panel 200; (e.g., at least one) optical sheet (not shown) on the light guide plate, such as a diffuser, a prism sheet, etc.; or a combination thereof, but not limited thereto. The backlight unit may not include a light guide plate. In one embodiment, the backlight unit may be a direct lighting device. For example, the backlight unit may have a reflector (not shown) and may have a plurality of fluorescent lamps disposed on the reflector at regular intervals, or may have an LED operating substrate on which a plurality of light-emitting diodes may be disposed, a diffuser plate thereon, and optionally (e.g., at least one) optical sheet. The details of such a backlight unit (e.g., components of light-emitting diodes, fluorescent lamps, light guide plates, a plurality of optical sheets, and reflectors) are not particularly limited.

[0214] The black matrix 241 is disposed under the upper substrate 240 and has an opening and hides the gate lines, data lines and thin film transistors of the wiring board on the lower substrate. For example, the black matrix 241 may have a lattice shape. The photoluminescent layer 230 is disposed in the opening of the black matrix 241 and has a semiconductor nanocrystal-polymer composite pattern including the following: a first segment (R) configured to emit a first light (e.g., red light), a second segment (G) configured to emit a second light (e.g., green light), and a third segment (B) configured to emit / transmit, for example, blue light. If desired, the photoluminescent layer may further include (e.g., at least one) fourth segment. The fourth segment may include semiconductor nanocrystals (or NPLs) that emit a color different from the light emitted from the first to third segments (e.g., cyan, magenta and yellow light).

[0215] In the photoluminescent layer 230, segments of a pattern may be repeatedly formed corresponding to the pixel region formed on the lower substrate. A transparent common electrode 231 may be disposed on the photoluminescent color filter layer (eg, the photoluminescent layer 230).

[0216] The third segment (B) configured to emit / transmit blue light may be a transparent color filter that does not change the light emission spectrum of the light source. In this case, the blue light emitted from the backlight unit may enter in a polarized state and may be emitted as is through the polarizer and liquid crystal layer. If desired, the third segment may include an NPL that emits blue light.

[0217] If desired, the display device may further include a light blocking layer (blue light blocking layer or blue cut filter) or a first filter layer 310. The blue light blocking layer may be disposed between the bottom surface of the first segment (R) and the second segment (G) and the upper substrate 240 or on the top surface of the upper substrate 240. The blue light blocking layer may include a sheet having an opening corresponding to a pixel area (e.g., the third segment) displaying blue and may be formed on portions corresponding to the first and second segments. Figure 5 As shown in , the first filter layer 310 may be integrally formed as an integral structure at the remaining positions except the position overlapping the third segment, but is not limited thereto. At least two first filter layers may be spaced apart and disposed at each of the positions overlapping the first and second segments.

[0218] For example, the first filter layer may block light in a visible light wavelength region, such as light in a certain visible light wavelength region, and transmit light in other wavelength regions, such as light in other wavelength regions except the certain visible light wavelength region. For example, the first filter layer may block blue light and transmit light except blue light. For example, the first filter layer may transmit green light, red light, yellow light as a mixed light thereof, or a combination of green light, red light, and yellow light.

[0219] For example, the first filter layer may substantially block blue light having a wavelength less than or equal to about 500 nm, and may transmit light in other visible light wavelength regions greater than about 500 nm and less than or equal to about 700 nm.

[0220] For example, for other visible light greater than about 500nm and less than or equal to about 700nm, the first filter layer may have a light transmittance greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 90%, or about 100%.

[0221] The first filter layer may include a polymer film including a dye that absorbs light having a wavelength to be blocked, a pigment that absorbs light having a wavelength to be blocked, or a combination thereof. The first filter layer may block at least 80%, at least 90%, or at least 95% of blue light having a wavelength less than or equal to about 480 nm, and for other visible light greater than about 500 nm and less than or equal to about 700 nm, the first filter layer may have a light transmittance greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 90%, or about 100%.

[0222] The first filter layer may block (e.g., absorb) and substantially block blue light having a wavelength of less than or equal to about 500 nm, and may selectively transmit green light or red light, for example. In this case, at least two first filter layers may be spaced apart and respectively disposed on each of the portions overlapping the first and second segments. For example, respectively, a first filter layer that selectively transmits red light may be disposed on a portion overlapping the segment emitting red light, and a first filter layer that selectively transmits green light may be disposed on a portion overlapping the segment emitting green light. For example, the first filter layer may include a first region, a second region, or a combination thereof, wherein the first region blocks (e.g., absorbs) blue light and red light and transmits a wavelength of a predetermined range (e.g., greater than or equal to about 500 nm, greater than or equal to about 510 nm, or greater than or equal to about 515 nm and less than or equal to about 550 nm, less than or equal to about 545 nm, less than or equal to about 540 nm, less than or equal to about 535 nm, less than or equal to about 530 nm, less than or equal to about 525 nm, or less than The first region may be disposed at a location overlapping with a segment emitting green light, and the second region may be disposed at a location overlapping with a segment emitting red light. The first region and the second region may be optically isolated. The first filter layer may contribute to improving the color purity of the display device.

[0223] The first filter layer may be a reflective filter including a plurality of layers (e.g., inorganic material layers) having different refractive indices. For example, two layers having different refractive indices may be alternately stacked, or, for example, a layer having a high refractive index and a layer having a catadioptric index may be alternately stacked.

[0224] When the refractive index difference between the layer with a high refractive index and the layer with a low refractive index is high, a first filter layer with high wavelength selectivity can be provided. The thickness and stacking number of the layer with a high refractive index and the layer with a low refractive index can be determined according to the refractive index and the reflection wavelength of each layer, for example, each layer with a high refractive index can have a thickness of about 3nm to about 300nm, and each layer with a low refractive index can have a thickness of about 3nm to about 300nm.

[0225] The total thickness of the first filter layer may be, for example, about 3 nm to about 10,000 nm, about 300 nm to about 10,000 nm, or about 1,000 nm to about 10,000 nm. All layers having a high refractive index may have the same thickness and the same material or different thicknesses and / or materials from each other, and all layers having a low refractive index may have the same thickness and the same material or different thicknesses and / or materials from each other.

[0226] The display device may further include a second filter layer (e.g., a red / green or yellow light recycling layer) disposed between the photoluminescent layer and the liquid crystal layer (e.g., between the photoluminescent layer and the upper polarizer) and transmitting at least a portion of the third light and reflecting at least a portion of the first light and the second light. The second filter layer may reflect light in a wavelength region greater than about 500 nm. The first light may be red light, the second light may be green light, and the third light may be blue light.

[0227] In the display device according to an embodiment, the second filter layer may be formed as an integral one layer having a relatively flat surface.

[0228] In one embodiment, the second filter layer may include a single layer having a low refractive index, for example, the second filter layer may be a transparent film having a refractive index of less than or equal to about 1.4, less than or equal to about 1.3, or less than or equal to about 1.2.

[0229] The second filter layer having a low refractive index may be, eg include or consist of, eg porous silicon oxide, a porous organic material, a porous organic / inorganic composite, or a combination thereof.

[0230] In one embodiment, the second filter layer may include a plurality of layers having different refractive indices, for example, the second filter layer may be formed by alternately stacking two layers having different refractive indices, or for example, the second filter layer may be formed by alternately stacking a material having a high refractive index and a material having a low refractive index.

[0231] The layer with a high refractive index in the second filter layer may include, for example, hafnium oxide, tantalum oxide, titanium oxide, zirconium oxide, magnesium oxide, cesium oxide, lanthanum oxide, indium oxide, niobium oxide, aluminum oxide, silicon nitride, or a combination thereof, but according to one embodiment, the layer with a high refractive index in the second filter layer may include multiple materials having a higher refractive index than the layer with a low refractive index.

[0232] The layer with a low refractive index in the second filter layer may include, for example, silicon oxide, but according to one embodiment, the layer with a low refractive index in the second filter layer may include a plurality of materials having a lower refractive index than the layer with a high refractive index.

[0233] When the refractive index difference between the layer having a high refractive index and the layer having a low refractive index is high, the second filter layer may have a high wavelength selectivity.

[0234] In the second filter layer, each thickness of the layer with a high refractive index and the layer with a low refractive index and the number of stacking thereof may be determined in consideration of the refractive index and the reflection wavelength of each layer, for example, each layer with a high refractive index in the second filter layer may have a thickness of about 3 nm to about 300 nm, and each layer with a low refractive index in the second filter layer may have a thickness of about 3 nm to about 300 nm. The total thickness of the second filter layer may be, for example, about 3 nm to about 10,000 nm, about 300 nm to about 10,000 nm, or about 1,000 nm to about 10,000 nm. The layer with a high refractive index and the layer with a low refractive index in the second filter layer may each have the same thickness and material or different thicknesses and materials from each other.

[0235] The second filter layer may reflect (e.g., at least one) part of the first light (R) and the second light (G), and transmit (e.g., at least one) part (e.g., the entire part) of the third light (B). For example, the second filter layer may transmit only the third light (B) in the blue light wavelength region less than or equal to about 500 nm and reflect light in the wavelength region greater than about 500 nm, that is, green light (G), yellow light, red light (R), etc. may not pass through the second filter layer and be reflected. Therefore, the reflected green light and red light may pass through the first and second segments to be emitted to the outside of the display device 10.

[0236] The second filter layer may reflect light in a wavelength region greater than about 500 nm with a reflectivity of greater than or equal to about 70%, greater than or equal to about 80%, or greater than or equal to about 90%, or about 100%.

[0237] At the same time, the second filter layer may have a transmittance of, for example, greater than or equal to about 90%, greater than or equal to about 92%, greater than or equal to about 94%, greater than or equal to about 96%, greater than or equal to about 98%, greater than or equal to about 99%, or about 100% for light in a wavelength region less than or equal to about 500 nm.

[0238] In one embodiment, the aforementioned stacked structure can be manufactured by a method using a photoresist composition. When the semiconductor nanocrystal-polymer composite pattern has a plurality of repeating segments, a plurality of compositions including semiconductor nanocrystal particles (e.g., NPL emitting red light, NPL emitting green light, or optional NPL emitting blue light) with desired photoluminescent properties (emission peak wavelength, etc.) are prepared for forming each repeating segment, and then the pattern forming process of each NPL composition can be repeated (e.g., twice or more or three times or more) to obtain the pattern of the desired semiconductor nanocrystal-polymer composite. For example, the pattern of the semiconductor nanocrystal-polymer composite can have a pattern in which at least two segments of different colors (e.g., RGB color segments) are repeated. Such a semiconductor nanocrystal-polymer composite pattern can be used as a photoluminescent color filter in a display device.

[0239] In one embodiment, the aforementioned stacked structure can be manufactured using an ink composition. The method may include: using an appropriate system (e.g., a droplet discharge device such as inkjet printing or nozzle printing equipment) to deposit it on a desired substrate (e.g., to provide a desired pattern) and heating it to remove the solvent and polymerize it. The method can provide a highly accurate semiconductor nanocrystal-polymer composite film or pattern in a short time in a simple manner.

[0240] Embodiments provide an electronic device including the aforementioned NPL. The electronic device may include a light emitting diode (LED), an organic light emitting diode (OLED), a sensor, a solar cell, an imaging sensor, or a liquid crystal display (LCD), but is not limited thereto.

[0241] Hereinafter, the embodiments are described in more detail with reference to Examples. However, they are exemplary embodiments of the present disclosure, and the present disclosure is not limited thereto.

[0242] Example

[0243] Analytical methods

[0244] 1. Ultraviolet-visible (UV-Vis) spectroscopy analysis

[0245] UV-Vis spectroscopy was performed using an Agilent Cary 5000 spectrometer and UV-Vis absorption spectra were obtained.

[0246] 2. Inductively coupled plasma atomic emission spectrometry (ICP-AES) analysis

[0247] Inductively coupled plasma atomic emission spectrometry (ICP-AES) analysis was performed using Shimadzu ICPS-8100.

[0248] 3. Transmission Electron Microscopy (TEM) Analysis

[0249] Transmission electron microscopy analyses were performed using a Titan ChemiSTEM electron microscope.

[0250] Example 1

[0251] In a nanosheet having an indium phosphide layer, a zinc selenide layer, and a zinc sulfide layer, an absorption wavelength depending on changes in the thicknesses of the zinc selenide layer and the indium phosphide layer was calculated by computer simulation using the effective mass approximation (EMA). Figure 6 is a graph showing the absorption wavelength of the nanosheets depending on the thickness of the indium phosphide layer.

[0252] From the results, it is confirmed that when the thickness of the zinc selenide layer is greater than 0.5 nanometers (nm), the emission wavelength may not be affected.

[0253] Figure 6 The results show that when the thickness of the indium phosphide layer is less than or equal to about 2 nm, the final nanosheet can emit visible light, and when the thickness of the indium phosphide layer is greater than or equal to about 0.4 nm and less than or equal to 0.8 nm, the final nanosheet can emit green light.

[0254] Example 2

[0255] For indium phosphide nanosheets and indium phosphide spherical cores, the absorption wavelength depending on the layer thickness or core diameter was calculated by computer simulation using EMA, and the results are shown in Figure 7 middle.

[0256] Figure 7 The results show that when the thickness of the indium phosphide layer is greater than or equal to 0.5 nm and less than or equal to about 2 nm, the final nanosheet can absorb light from about 300 nm to about 700 nm and emit visible light.

[0257] Example 3: ZnSe template synthesis

[0258] Se / TOP stock solution was obtained by dispersing selenium in trioctylphosphine (TOP).

[0259] Zinc acetate and oleic acid were added to a 50 milliliter (mL) reaction flask including oleylamine and heated at 120° C. under vacuum. After about 1 hour, the atmosphere in the reactor was replaced with an inert gas (nitrogen). While the reactor temperature was raised up to 170° C., oleylamine and Se / TOP stock solutions were injected therein. After the injection was completed, the reaction was carried out for greater than or equal to 70 minutes.

[0260] After the reaction was completed, acetone was added to the reaction solution, the reaction solution was rapidly cooled to room temperature and centrifuged to provide a precipitate, and the precipitate was dispersed in toluene to provide a ZnSe template.

[0261] The content ratio (ie, molar ratio, hereinafter, the word "content ratio" refers to the molar ratio) of the Zn precursor and the Se precursor used was adjusted to about 1:3.

[0262] Transmission electron microscopy analysis was performed on the template and the results are shown in Figure 8 In. From Figure 8 , confirming that the lateral dimensions of the template have a length of 85 nm and a width of 20 nm (about 85 nm×about 20 nm=1700 nm 2 lateral dimension), and the template thickness is about 1.5 nm.

[0263] The template was subjected to UV-visible absorption spectroscopy analysis, and the results are shown in Fig. 9 In. From Fig. 9 , confirming that the template has two UV-visible absorption peaks.

[0264] Embodiment 4:

[0265] Indium acetate was added to a 300 mL reaction flask containing oleylamine together with the organic ligand palmitic acid and heated at 120° C. under vacuum. The atmosphere in the flask was replaced with nitrogen (N 2 The obtained toluene dispersion of the ZnSe template was quickly added to the reaction flask, followed by the TOP dispersion of tris(trimethylsilyl)phosphine (hereinafter, also referred to as "TMSP") injected.

[0266] After the injection was completed, the reaction was carried out at 120° C. for 30 minutes.

[0267] The content ratio of the indium precursor used and the phosphorus precursor used was adjusted to about 1:8. The content ratio of the zinc precursor used to the indium precursor used (Zn:In) in the template was adjusted to about 3:1.

[0268] After the reaction was completed, ethanol was added to the reaction solution, the reaction solution was quickly cooled to room temperature and centrifuged to obtain a precipitate, and the precipitate was dispersed in toluene to obtain a nanosheet. The average lateral size of the obtained nanosheet was similar to that of the template, and the total thickness was about 1.7 nm.

[0269] The template and nanosheets were analyzed by UV-visible absorption spectroscopy, and the results are shown in Fig.10 In. From Fig.10, it was confirmed that the obtained nanosheets had two absorption peaks, and the difference between the first absorption peak of the template and the first absorption peak of the nanosheets was less than 100 nm.

[0270] The nanosheets were subjected to ICP-AES analysis, and the results are shown in Table 1.

[0271] Example 5

[0272] Nanosheets were obtained according to the same procedure as in Example 4, except that zinc oleate was further added to the reaction flask as a zinc precursor together with the organic ligand.

[0273] The content ratio of the used indium precursor, zinc precursor and phosphorus precursor was adjusted to about 1:1:8. The content ratio of the used zinc precursor to the used indium precursor (Zn:In) in the template was adjusted to about 1:1.

[0274] After the reaction is completed, ethanol is added to the reaction solution, the reaction solution is quickly cooled to room temperature and centrifuged to obtain a precipitate, and the precipitate is dispersed in toluene to obtain a nanosheet. The average lateral size of the obtained nanosheet is similar to that of the template, and the thickness is about 2nm. The template and the nanosheet are analyzed by ultraviolet-visible absorption spectroscopy. As a result, it is confirmed that the obtained nanosheet has two absorption peaks, and the difference between the first absorption peak of the template and the first absorption peak of the nanosheet is less than 100nm.

[0275] The nanosheets were subjected to ICP-AES analysis, and the results are shown in Table 1.

[0276] Table 1

[0277]

[0278] The bulk energy band gap of indium phosphide is about 1.3 eV and the bulk energy band gap of zinc selenide is about 2.82 eV.

[0279] TEM-EDX analysis showed that at the lateral surface of the NPL, the components of the first shell (e.g., indium and phosphorus) were present, and at the thickness surface of the NPL, all components of the first shell and template (i.e., indium, phosphorus, zinc, and selenium) were present.

[0280] While the present disclosure has been described in relation to what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments. On the contrary, it is intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

Claims

1. Nanosheets, which include: a two-dimensional template comprising a first semiconductor nanocrystal; as well as a first shell disposed on a surface of the two-dimensional template comprising a second semiconductor nanocrystal, the second semiconductor nanocrystal having a different composition than the first semiconductor nanocrystal, wherein the second semiconductor nanocrystal comprises a III-V compound, wherein the nanosheets do not include cadmium, wherein the two-dimensional template has a thickness greater than or equal to 0.3 nm and less than or equal to 10 nm, wherein the first semiconductor nanocrystal comprises a Group II-VI compound, and The thickness of the first shell is greater than or equal to 0.1 nanometers and less than or equal to 2 nanometers. 2 . The nanosheet of claim 1 , wherein the two-dimensional template has a thickness greater than or equal to 0.5 nm and less than or equal to 10 nm.

3. The nanosheet of claim 1, wherein the first semiconductor nanocrystal comprises ZnA, wherein A is selenium, tellurium, sulfur, oxygen, or a combination thereof.

4. The nanosheet of claim 3, wherein the first semiconductor nanocrystal comprises ZnSe, ZnS, ZnTe, ZnTeSe, ZnSeS, ZnTeS, ZnTeSeS, ZnO, or a combination thereof. The nanosheet of claim 1 , wherein the first shell is disposed on opposite surfaces of the two-dimensional template. The nanosheet of claim 1 , wherein the first shell is disposed directly on the two-dimensional template.

7. The nanosheet of claim 1, wherein the Group III-V compound comprises a Group III metal selected from gallium and indium; and phosphorus.

8. The nanosheet of claim 1, wherein the Group III-V compound further comprises a Group II metal.

9. The nanosheet of claim 1, wherein the III-V compound comprises InP, InGaP, GaP, InZnP, GaZnP, InGaZnP, or a combination thereof.

10. The nanosheet of claim 1, wherein the energy band gap of the second semiconductor nanocrystal material is smaller than the energy band gap of the first semiconductor nanocrystal material.

11. The nanosheet of claim 1, wherein the nanosheet has a lateral dimension greater than 400 square nanometers.

12. The nanosheet of claim 1, wherein the nanosheet has a lateral dimension greater than or equal to 1,000 square nanometers.

13. The nanosheet of claim 1, wherein the nanosheet has a lateral dimension less than or equal to 10,000 square nanometers.

14. The nanosheet of claim 1, wherein a lateral surface of the nanosheet has an aspect ratio greater than or equal to 1:1.1 and less than or equal to 1:

8. 15 . The nanosheet of claim 1 , wherein a thickness of the first shell of the nanosheet is greater than or equal to 0.5 nanometers and less than or equal to 2 nanometers. 16 . The nanosheet of claim 1 , wherein the nanosheet further comprises a second shell comprising a third semiconductor nanocrystal and disposed on the first shell, wherein the third semiconductor nanocrystal has a composition different from a composition of the second semiconductor nanocrystal.

17. The nanosheet of claim 16, wherein the third semiconductor nanocrystal comprises a Group II-VI compound.

18. The nanosheet of claim 16, wherein the third semiconductor nanocrystal comprises ZnA, wherein A is selenium, tellurium, sulfur, oxygen, or a combination thereof.

19. The nanosheet of claim 16, wherein the energy band gap of the third semiconductor nanocrystal material is greater than the energy band gap of the second semiconductor nanocrystal material.

20. The nanosheet of claim 1, wherein transmission electron microscopy energy dispersive x-ray spectroscopy analysis of a lateral surface of the nanosheet exhibits elements present in the outermost layer.

21. The nanosheet of claim 1, wherein the nanosheet exhibits two or more absorption peaks within a range of less than or equal to 500 nanometers.

22. The nanosheet of claim 1, wherein a difference between a first absorption peak of the two-dimensional template and a first absorption peak of the nanosheet is less than 100 nanometers.

23. The nanosheet of claim 1, wherein The first semiconductor nanocrystal comprises zinc chalcogenide, and The second semiconductor nanocrystals include indium and phosphorus, and Wherein in the nanosheet, the amount of indium based on 1 mole of the chalcogen element is 0.05 mole to 2 moles, the amount of zinc based on 1 mole of the chalcogen element is greater than or equal to 1 mole and less than or equal to 10 moles, and the amount of phosphorus based on 1 mole of the chalcogen element is 0.05 to 5 moles.

24. The nanosheet of claim 1, wherein transmission electron microscopy energy dispersive x-ray spectroscopy analysis of a surface of the nanosheet extending in a thickness direction exhibits an element present in the first semiconductor nanocrystal and an element present in the second semiconductor nanocrystal.

25. A method for producing a nanosheet as claimed in any one of claims 1 to 24, wherein include: reacting a first metal precursor of the first semiconductor nanocrystal and a first non-metal precursor of the first semiconductor nanocrystal in an organic solvent in the presence of an organic ligand at a temperature below 175° C. to synthesize a two-dimensional template; as well as A second metal precursor of the second semiconductor nanocrystal and a second non-metal precursor of the second semiconductor nanocrystal are reacted in an organic solvent in the presence of an organic ligand and the two-dimensional template at a temperature less than or equal to 200° C. to form a first shell including the second semiconductor nanocrystal on the surface of the two-dimensional template and produce the nanosheet.

26. A semiconductor nanocrystal-polymer composite, include: polymer matrix; and a plurality of semiconductor nanocrystal particles dispersed in the polymer matrix, The plurality of semiconductor nanocrystal particles include nanosheets as described in any one of claims 1-24.