Semiconductor photoresist composition and method for forming pattern using the composition

By using a semiconductor photoresist composition composed of an organic metal compound copolymer in extreme ultraviolet lithography technology, the deficiencies in resolution and photosensitivity of traditional photoresists are solved, and high aspect ratio patterns are realized. Formation and sensitivity improvements improve line edge roughness and etch resistance.

CN111856879BActive Publication Date: 2024-10-29SAMSUNG SDI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202010357520.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-29
Publication Date
2024-10-29
Estimated Expiration
2040-04-29

AI Technical Summary

Technical Problem

In existing extreme ultraviolet lithography technology, traditional chemically amplified photoresists have deficiencies in resolution, photosensitivity speed and line edge roughness, especially under small feature size and high sensitivity requirements, and their materials It is difficult to improve the shelf life stability and structure.

Method used

A semiconductor photoresist composition composed of an organic metal compound and a solvent is used to copolymerize the organic metal compound represented by Chemical Formula 1 and Chemical Formula 2 to form a photoresist with improved etching resistance, sensitivity and resolution, combined with Additives such as surfactants and cross-linkers to optimize coating and patterning.

Benefits of technology

It achieves the formation of high aspect ratio patterns in extreme ultraviolet lithography, maintaining sensitivity and resolution while reducing line edge roughness, improving the pattern's etch resistance and commercial availability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111856879B_ABST
    Figure CN111856879B_ABST
Patent Text Reader

Abstract

The present invention discloses a semiconductor photoresist composition and a method for forming a pattern using the same, wherein the semiconductor photoresist composition comprises an organic metal compound represented by Chemical Formula 1, an organic metal compound represented by Chemical Formula 2, and a solvent. The details of Chemical Formula 1 and Chemical Formula 2 are as defined in the detailed description. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2019-0050856 filed in the Korean Intellectual Property Office on April 30, 2019, and Korean Patent Application No. 10-2019-0160169 filed in the Korean Intellectual Property Office on December 4, 2019, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to a semiconductor photoresist composition and a method of forming a pattern using the composition. Background Art

[0004] Extreme ultraviolet (EUV) lithography has attracted attention as a key technology for manufacturing next-generation semiconductor devices. EUV lithography is a pattern forming technology that uses EUV rays with a wavelength of about 13.5 nm as an exposure light source. According to EUV lithography, it is well known that very fine patterns (e.g., less than or equal to about 20 nm) can be formed in the exposure process during the manufacture of semiconductor devices.

[0005] Extreme ultraviolet (EUV) lithography is enabled by the development of compatible photoresists that can be performed at a spatial resolution of less than or equal to about 16 nm. Currently, efforts are underway to meet the inadequate specifications of conventional chemically amplified (CA) photoresists for next-generation devices, such as resolution, photospeed, and feature roughness (or line edge roughness (LER)).

[0006] Intrinsic image blurring due to acid-catalyzed reactions in these polymer-based photoresists limits resolution of small feature sizes, as is well known in electron beam (e-beam) lithography. Chemically amplified (CA) photoresists are designed for high sensitivity, but may have more difficulty with EUV exposure in part because their typical elemental makeup reduces the photoresist's light absorption at about 13.5 nm wavelength and thus reduces its sensitivity.

[0007] In addition, CA photoresists may have difficulty with small feature sizes due to roughness issues, and experiments have shown that the line edge roughness (LER) of CA photoresists increases because the photospeed is reduced due in part to the nature of the acid catalyst process. Therefore, due to these deficiencies and problems of CA photoresists, new high performance photoresists are needed in the semiconductor industry.

[0008] Inorganic photoresists based on peroxypolyacids of tungsten mixed with tungsten, niobium, titanium and / or tantalum have been reported as radiation-sensitive materials for patterning ( US5061599, H. Okamoto, T. Iwayanagi, K. Mochiji, H. Umezaki, T. Kudo, Applied Physics Letters, 49(5), 298-300, 1986 ).

[0009] These materials are effective for patterning large pitches of bilayer configurations with ultraviolet (UV) (deep UV), X-ray and electron beam sources. Recently, impressive performance was achieved when cationic hafnium metal oxide sulfate (HfSOx) materials were used with peroxo complexing agents for imaging 15 nm half-pitch (HP) by projection EUV exposure (US 2011-0045406; JK Stowers, A. Telecky, M. Kocsis, BL Clark, DA Keszler, A. Grenville, CN Anderson, PP Naulleau, Proc. SPIE, 7969, 796915, 2011). This system exhibits the highest performance of non-CA photoresists and has a feasible photospeed approaching that required for EUV photoresists. However, hafnium metal oxide sulfate materials with peroxide complexing agents have some practical disadvantages. First, these materials are coated with a corrosive sulfuric acid / hydrogen peroxide mixture and have insufficient shelf life stability. Second, as a complex mixture, it is not easy to change its structure to improve performance. Third, development should be carried out in a very high concentration of tetramethylammonium hydroxide (TMAH) solution of about 25% by weight, etc.

[0010] In order to overcome the above-mentioned disadvantages of chemically amplified (CA) photosensitive compositions, inorganic photosensitive compositions have been studied. The inorganic photosensitive compositions are mainly used for negative patterning, which has resistance to removal by a developer composition due to chemical modification by a non-chemical amplification mechanism. The inorganic composition contains an inorganic element having a higher EUV absorption rate than hydrocarbons, and thus can ensure sensitivity by a non-chemical amplification mechanism, and in addition, is less sensitive to stochastic effects, and is therefore known to have low line edge roughness and a small number of defects.

[0011] In recent years, active research has been conducted because molecules containing tin are known to have excellent extreme ultraviolet absorption. Regarding the organotin polymers therein, the alkyl ligands dissociate through light absorption or secondary electrons generated thereby, and crosslink with adjacent chains through oxo bonds, thereby enabling negative patterning that may not be removed by organic developing solutions. Such organotin polymers show greatly improved sensitivity while maintaining resolution and line edge roughness, but additional improvement in patterning characteristics is required for commercial availability. Summary of the invention

[0012] One embodiment provides a semiconductor photoresist composition having improved etch resistance, sensitivity, resolution, and pattern forming ability.

[0013] Another embodiment provides a method of forming a pattern using a semiconductor photoresist composition.

[0014] The semiconductor photoresist composition according to an embodiment includes an organic metal compound represented by Chemical Formula 1, an organic metal compound represented by Chemical Formula 2, and a solvent.

[0015] [Chemical formula 1]

[0016]

[0017] In Chemical Formula 1,

[0018] R is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethylene oxide group, a propylene oxide group, or a combination thereof,

[0019] X, Y and Z are independently -OR 1 or -OC(=O)R 2 ,

[0020] R 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and

[0021] R 2 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.

[0022] [Chemical formula 2]

[0023]

[0024] In chemical formula 2,

[0025] X' is -OR 3 or -OC(=O)R 4 ,

[0026] R 3 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and

[0027] R 4 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.

[0028] R may be a substituted or unsubstituted C1 to C8 alkyl group, a substituted or unsubstituted C3 to C8 cycloalkyl group, a substituted or unsubstituted C2 to C8 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C20 aryl group, an ethylene oxide group, a propylene oxide group, or a combination thereof, and

[0029] R 1 and R 3 may independently be a substituted or unsubstituted C1 to C8 alkyl group, a substituted or unsubstituted C3 to C8 cycloalkyl group, a substituted or unsubstituted C2 to C8 alkenyl group, a substituted or unsubstituted C2 to C8 alkynyl group, a substituted or unsubstituted C6 to C20 aryl group, or a combination thereof, and

[0030] R 2 and R 4 It may independently be hydrogen, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C3 to C8 cycloalkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted C6 to C20 aryl, or a combination thereof.

[0031] R can be methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, vinyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, ethylene oxide, propylene oxide or a combination thereof,

[0032] R 1 and R 3 may independently be methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, vinyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, or a combination thereof, and

[0033] R 2 and R 4 It may independently be hydrogen, methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl or a combination thereof.

[0034] The compound represented by Chemical Formula 1 may be a compound represented by Chemical Formula 3, a compound represented by Chemical Formula 4, a compound represented by Chemical Formula 5, a compound represented by Chemical Formula 6, or a combination thereof.

[0035] [Chemical formula 3]

[0036]

[0037] [Chemical formula 4]

[0038]

[0039] [Chemical formula 5]

[0040]

[0041] [Chemical formula 6]

[0042]

[0043] In Chemical Formula 3 to Chemical Formula 6,

[0044] R is the same as defined in Chemical Formula 1,

[0045] R a , R b , R c , R i , R k and R l Independently with R in Formula 1 1 The definition of is the same as

[0046] R d , R e , R f , R g , R hand R j Independently with R in Formula 1 2 The definition is the same.

[0047] The semiconductor photoresist composition may include the organic metal compound represented by Chemical Formula 1 and the organic metal compound represented by Chemical Formula 2 in a weight ratio of about 20:1 to about 1:1.

[0048] The semiconductor photoresist composition may include about 0.01 wt % to about 30 wt % of the organic metal compound represented by Chemical Formula 1 and about 0.01 wt % to about 15 wt % of the organic metal compound represented by Chemical Formula 2, based on 100 wt % of the semiconductor photoresist composition.

[0049] The semiconductor photoresist composition may further include additives of a surfactant, a crosslinking agent, a leveling agent, or a combination thereof.

[0050] According to another embodiment, a method for forming a pattern includes forming an etching target layer on a substrate, coating a semiconductor photoresist composition on the etching target layer to form a photoresist layer, patterning the photoresist layer to form a photoresist pattern, and etching the etching target layer using the photoresist pattern as an etching mask.

[0051] The photoresist pattern may be formed using light having a wavelength of about 5 nm to about 150 nm.

[0052] The method of forming a pattern may further include providing a resist underlayer formed between the substrate and the photoresist layer.

[0053] The photoresist pattern may have a width of about 5 nm to about 100 nm.

[0054] The semiconductor photoresist composition according to the embodiment has relatively improved etching resistance, sensitivity, resolution, and pattern forming ability, and thus may provide a photoresist pattern having improved sensitivity and a high aspect ratio without pattern collapse. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figures 1 to 5 2 is a cross-sectional view explaining a method of forming a pattern using a semiconductor resist composition according to an embodiment.

[0056] [Explanation of Symbols]

[0057] 100: Semiconductor substrate

[0058] 102: Thin layer

[0059] 104: Resist base

[0060] 106: Photoresist layer

[0061] 106b: Exposed area

[0062] 106a: Unexposed area

[0063] 108: Photoresist pattern

[0064] 110: Patterned Hard Mask

[0065] 112: Organic layer pattern

[0066] 114: Thin layer pattern DETAILED DESCRIPTION

[0067] Hereinafter, exemplary embodiments of the present invention will be described in detail with reference to the accompanying drawings. However, in the description of the present disclosure, descriptions of known functions or components will be omitted in order to clarify the gist of the present disclosure.

[0068] For clear description of the present disclosure, the parts not related to the description are omitted, and the same reference numerals refer to the same or similar components throughout the specification. In addition, since the size and thickness of each component shown in the figure are optionally represented for ease of description, the present disclosure is not limited to the drawings.

[0069] In the drawings, the thickness of layers, films, panels, regions, etc., are exaggerated for clarity. In the drawings, the thickness of a portion of a layer or region, etc., is exaggerated for clarity. It will be understood that when an element (such as a layer, film, region, or substrate) is referred to as being "on" another element, the element may be directly on the other element or intervening elements may also be present.

[0070] In the present disclosure, "substituted" means that the hydrogen atom is replaced by: deuterium, halogen, hydroxyl, cyano, nitro, -NRR' (wherein, R and R' are independently hydrogen, substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or substituted or unsubstituted C6 to C30 aromatic hydrocarbon group), -SiRR'R" (wherein, R, R' and R" are independently hydrogen, substituted or unsubstituted C1 to C30 saturated or unsaturated aliphatic hydrocarbon group, substituted or unsubstituted C3 to C30 saturated or unsaturated alicyclic hydrocarbon group, or substituted or unsubstituted C6 to C30 aromatic hydrocarbon group), C1 to C30 alkyl group, C1 to C10 haloalkyl group, C1 to C10 alkylsilanyl group, C3 to C30 cycloalkyl group, C6 to C30 aryl group, C1 to C20 alkoxy group, or a combination thereof. "Unsubstituted" means that a hydrogen atom is not replaced with another substituent and the remaining hydrogen atoms.

[0071] As used herein, when no definition is otherwise provided, "hetero" means including 1 to 3 heteroatoms selected from N, O and S. The alkyl group may be a "saturated alkyl group" without any double bond or triple bond.

[0072] The alkyl group may be a C1 to C8 alkyl group. For example, the alkyl group may be a C1 to C7 alkyl group, a C1 to C6 alkyl group, a C1 to C5 alkyl group, or a C1 to C4 alkyl group. For example, the C1 to C4 alkyl group may be a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, or a 2,2-dimethylpropyl group.

[0073] As used herein, when no definition is otherwise provided, "cycloalkyl" refers to a monovalent cyclic aliphatic hydrocarbon group.

[0074] The cycloalkyl group may be a C3 to C8 cycloalkyl group, such as a C3 to C7 cycloalkyl group, a C3 to C6 cycloalkyl group, a C3 to C5 cycloalkyl group, or a C3 to C4 cycloalkyl group. For example, the cycloalkyl group may be a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, or a cyclohexyl group, but is not limited thereto.

[0075] As used herein, the "aliphatic unsaturated organic group" refers to a hydrocarbon group including a double bond, a triple bond or a combination thereof in which the bonds between carbon atoms in the molecule are double bonds, triple bonds or a combination thereof.

[0076] The aliphatic unsaturated organic group may be a C2 to C8 aliphatic unsaturated organic group. For example, the aliphatic unsaturated organic group may be a C2 to C7 aliphatic unsaturated organic group, a C2 to C6 aliphatic unsaturated organic group, a C2 to C5 aliphatic unsaturated organic group, or a C2 to C4 aliphatic unsaturated organic group. For example, the C2 to C4 aliphatic unsaturated organic group may be vinyl, ethynyl, allyl, 1-propenyl, 1-methyl-1-propenyl, 2-propenyl, 2-methyl-2-propenyl, 1-propynyl, 1-methyl-1-propynyl, 2-propynyl, 2-methyl-2-propynyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-butynyl, 2-butynyl, or 3-butynyl.

[0077] As used herein, "aryl" refers to a substituent in which all atoms in the cyclic substituent have p orbitals and the p orbitals are conjugated, and may include monocyclic or fused-ring polycyclic (ie, rings which share adjacent pairs of carbon atoms) functional groups.

[0078] As used herein, unless otherwise defined, "alkenyl" refers to an aliphatically unsaturated alkenyl group including at least one double bond, as a straight or branched aliphatic hydrocarbon group.

[0079] As used herein, unless otherwise defined, "alkynyl" refers to an aliphatically unsaturated alkynyl group including at least one triple bond, as a straight or branched aliphatic hydrocarbon group.

[0080] Hereinafter, semiconductor photoresist compositions according to embodiments are described.

[0081] The semiconductor photoresist composition according to an embodiment of the present invention includes an organic metal compound and a solvent, and the organic metal compound is composed of compounds represented by Chemical Formula 1 and Chemical Formula 2.

[0082] [Chemical formula 1]

[0083]

[0084] In Chemical Formula 1,

[0085] R is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethylene oxide group, a propylene oxide group, or a combination thereof,

[0086] X, Y and Z are independently -OR 1 or -OC(=O)R 2 ,

[0087] R 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and

[0088] R 2 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.

[0089] [Chemical formula 2]

[0090]

[0091] In chemical formula 2,

[0092] X' is -OR 3 or -OC(=O)R 4 ,

[0093] R 3 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and

[0094] R 4 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.

[0095] The organotin copolymer including the organometallic compound represented by Chemical Formula 1 and Chemical Formula 2 can be prepared by copolymerizing the following: the organometallic compound represented by Chemical Formula 1, having an R group and three -OR groups; 1 or -OC(=O)R 2 and an organometallic compound represented by Chemical Formula 2, having four -OR 1 or -OC(=O)R 2 Substituted tin atoms.

[0096] The compounds represented by Chemical Formula 1 and Chemical Formula 2 are organic tin compounds, in which tin can strongly absorb extreme ultraviolet (UV) light of 13.5 nm, and thus has excellent sensitivity to light having high energy, and R of Chemical Formula 1 can impart photosensitivity to the compound represented by Chemical Formula 1, and further, can bind to tin and form a Sn-R bond, thereby imparting solubility in an organic solvent to the organic tin compound. In addition, X, Y, and Z, -OR of Chemical Formula 1 3 or -OC(=O)R 4 And X' of Chemical Formula 2 can determine the solubility of these two compounds in the solvent.

[0097] Regarding R of Chemical Formula 1, when an organotin copolymer having structural units represented by Chemical Formula 1 and Chemical Formula 2 and formed by copolymerization of the compounds is exposed to extreme ultraviolet (UV), the R functional group dissociates from the Sn-R bond and forms a free radical, and this free radical forms an additional -Sn-O-Sn- bond and initiates a condensation reaction between the organotin copolymers, thereby facilitating the formation of a semiconductor photoresist from the composition according to an embodiment.

[0098] In the organometallic compound represented by Chemical Formula 1, the substituent represented by R may be a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group including at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethylene oxide group, a propylene oxide group, or a combination thereof.

[0099] In addition to the substituent R, the compound represented by Chemical Formula 1 may further include three organic ligands X, Y and Z, each of which is hydrolyzed to form a Sn-O bond. In addition, the compound represented by Chemical Formula 2 is hydrolyzed, thereby including four X' substituents that form Sn-O bonds with the tin element. X, Y, Z and X' may independently be -OR 1 or -OC(=O)R 2 , its organic ligand can be hydrolyzed by heat treatment or non-heat treatment under an acidic or alkaline catalyst to form a Sn-O-Sn bond between the organic tin compounds, and therefore, the organic metal compounds represented by Chemical Formula 1 and Chemical Formula 2 can form an organic tin copolymer.

[0100] The semiconductor photoresist composition according to an embodiment of the present invention includes both the organic metal compound represented by Chemical Formula 1 and the organic metal compound represented by Chemical Formula 2, and thus can exhibit improved sensitivity compared to a semiconductor photoresist composition including only the organic metal compound represented by Chemical Formula 1 or Chemical Formula 2.

[0101] The ratio of the organic metal compound represented by Chemical Formula 1 and the organic metal compound represented by Chemical Formula 2 in the copolymer can be appropriately controlled to adjust the dissociation degree of the ligand represented by R and the copolymer, and thus adjust the crosslinking degree of the oxo bond of the free radical generated by the dissociation of the ligand and the adjacent chain, thereby providing a semiconductor photoresist with excellent sensitivity, small line edge roughness and excellent resolution. In other words, by including both the organic metal compound represented by Chemical Formula 1 and the organic metal compound represented by Chemical Formula 2, a semiconductor photoresist with improved sensitivity, line edge roughness and resolution can be provided.

[0102] R can be, for example, a substituted or unsubstituted C1 to C8 alkyl group, a substituted or unsubstituted C3 to C8 cycloalkyl group, a substituted or unsubstituted C2 to C8 aliphatic unsaturated organic group including at least one double bond or triple bond, a substituted or unsubstituted C6 to C20 aryl group, an oxirane group, an oxirane group, or a combination thereof, such as a methyl group, an ethyl group, a propyl group, a butyl group, an isopropyl group, a tert-butyl group, a 2,2-dimethylpropyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a vinyl group, a propenyl group, a butenyl group, an ethynyl group, a propynyl group, a butynyl group, a phenyl group, a tolyl group, a xylyl group, a benzyl group, an oxirane group, a oxirane group, or a combination thereof.

[0103] R 1 and R 3The alkyl radicals may independently be, for example, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C3 to C8 cycloalkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted C6 to C20 aryl, or a combination thereof, such as methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, or a combination thereof.

[0104] R 2 and R 4 The alkyl radicals may independently be, for example, hydrogen, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C3 to C8 cycloalkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted C6 to C20 aryl, or a combination thereof, such as hydrogen, methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, or a combination thereof.

[0105] The compound represented by Chemical Formula 1 may include a compound represented by Chemical Formula 3, a compound represented by Chemical Formula 4, a compound represented by Chemical Formula 5, a compound represented by Chemical Formula 6, or a combination thereof.

[0106] [Chemical formula 3]

[0107]

[0108] [Chemical formula 4]

[0109]

[0110] [Chemical formula 5]

[0111]

[0112] [Chemical formula 6]

[0113]

[0114] In Chemical Formula 3 to Chemical Formula 6,

[0115] R is the same as defined in Chemical Formula 1,

[0116] R a , R b , R c , R i , R k and Rl Independently with R in Formula 1 1 The definition of is the same as

[0117] R d , R e , R f , R g , R h and R j Independently with R in Formula 1 2 The definition is the same.

[0118] The semiconductor photoresist composition according to an embodiment of the present invention includes a compound having substituents respectively connected to three oxygen atoms bonded to a tin atom and as shown in Chemical Formula 1 or Chemical Formulas 3 to 6, and a compound having four substituents connected to an oxygen atom bonded to a tin atom as shown in Chemical Formula 2, and thus provides a photoresist pattern including an organic metal copolymer obtained by copolymerization of the compounds, and this photoresist has relatively improved etching resistance, sensitivity and resolution and excellent pattern forming ability, so that its pattern is not destroyed despite having a high aspect ratio.

[0119] The organometallic compound represented by Chemical Formula 1 and the organometallic compound represented by Chemical Formula 2 may be included in the semiconductor photoresist composition in a weight ratio of about 20:1 to about 1:1, for example, about 18:1 to about 1:1, about 15:1 to about 1:1, about 12:1 to about 1:1, about 10:1 to about 1:1, about 8:1 to about 1:1, about 5:1 to about 1:1, about 3:1 to about 1:1, or about 2:1 to about 2:1, but is not limited thereto. When the weight ratio of the organometallic compound represented by Chemical Formula 1 and the organometallic compound represented by Chemical Formula 2 satisfies the range, a semiconductor photoresist composition having improved sensitivity may be provided.

[0120] The semiconductor photoresist composition may include about 0.01 wt % to about 30 wt % of the organic metal compound represented by Chemical Formula 1 and about 0.01 wt % to about 15 wt % of the organic metal compound represented by Chemical Formula 2, based on 100 wt % of the semiconductor photoresist composition. For example, it may include about 0.1 wt % to about 20 wt % of the organic metal compound represented by Chemical Formula 1 and about 0.1 wt % to about 10 wt % of the organic metal compound represented by Chemical Formula 2, for example, about 0.1 wt % to about 10 wt % of the organic metal compound represented by Chemical Formula 1 and about 0.1 wt % to about 5 wt % of the organic metal compound represented by Chemical Formula 2, but is not limited thereto.

[0121] The semiconductor photoresist composition according to the embodiment includes the organic metal compound represented by Chemical Formula 1 and the organic metal compound represented by Chemical Formula 2 within the above ranges, and when a photoresist is formed from the composition, a coating process may be facilitated and sensitivity of the photoresist may be improved.

[0122] The solvent included in the semiconductor photoresist composition according to the embodiment may be an organic solvent. The solvent may be, for example, an aromatic compound (e.g., xylene, toluene, etc.), an alcohol (e.g., 4-methyl-2-pentenol, 4-methyl-2-propanol, 1-butanol, methanol, isopropanol, 1-propanol, etc.), an ether (e.g., anisole, tetrahydrofuran, etc.), an ester (n-butyl acetate, propylene glycol monomethyl ether acetate, ethyl acetate, ethyl lactate), a ketone (e.g., methyl ethyl ketone, 2-heptanone) or a mixture thereof, but is not limited thereto.

[0123] In an embodiment, the semiconductor photoresist composition may further include a resin in addition to the aforementioned organometallic compound and solvent.

[0124] The resin may be a phenol-based resin including at least one or more aromatic moieties of Group 1.

[0125] [Group 1]

[0126]

[0127] The weight average molecular weight of the resin may be about 500 to about 20,000.

[0128] The resin may be included in an amount of about 0.1 wt % to about 50 wt % based on the total amount of the semiconductor resist composition.

[0129] When the resin is included in the amount range, it may have excellent etching resistance and heat resistance.

[0130] On the other hand, the semiconductor resist composition according to the embodiment is ideally composed of an organometallic compound, a solvent and a resin. However, the semiconductor resist composition according to the above-described embodiment may also include additives as required. The example of the additive may include a surfactant, a cross-linking agent, a leveling agent or a combination thereof.

[0131] The surfactant may include, for example, alkylbenzene sulfonate, alkyl pyridinium salt, polyethylene glycol, quaternary ammonium salt, or a combination thereof, but is not limited thereto.

[0132] The crosslinking agent may be, for example, a melamine-based crosslinking agent, a substituted urea-based crosslinking agent or a polymer-based crosslinking agent, but is not limited thereto. For example, it may be a crosslinking agent having at least two crosslinking-forming substituents, such as methoxymethylated glycoluril, butoxymethylated glycoluril, methoxymethylated melamine, butoxymethylated melamine, methoxymethylated benzoguanamine, butoxymethylated benzoguanamine, methoxymethylated urea, butoxymethylated urea, methoxymethylated thiourea and other compounds.

[0133] The leveling agent may be used to improve the flatness of the coating during printing, and may be a known leveling agent that is commercially available.

[0134] The amount of additives used can be controlled depending on the desired properties.

[0135] In addition, the semiconductor resist composition may further include a silane coupling agent as an adhesion enhancer to improve the close contact force with the substrate (for example, to improve the adhesion of the semiconductor resist composition to the substrate). The silane coupling agent may be, for example, a silane compound including a carbon-carbon unsaturated bond, such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltrichlorosilane, vinyltri(β-methoxyethoxy)silane; or 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, p-phenylyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane; trimethoxy[3-(phenylamino)propyl]silane, etc., but are not limited thereto.

[0136] Semiconductor photoresist compositions can be formed into patterns with high aspect ratios without collapse. Therefore, in order to form fine patterns with a width of, for example, about 5nm to about 100nm, about 5nm to about 80nm, about 5nm to about 70nm, about 5nm to about 50nm, about 5nm to about 40nm, about 5nm to about 30nm, or about 5nm to about 20nm, semiconductor resist compositions can be used for photoresist processes using wavelengths between about 5nm to about 150nm, for example, about 5nm to about 100nm, about 5nm to about 80nm, about 5nm to about 50nm, about 5nm to about 30nm, or about 5nm to about 20nm. Therefore, semiconductor photoresist compositions according to embodiments can be used for realizing extreme ultraviolet (UV) lithography using an EUV light source having a wavelength of about 13.5nm.

[0137] According to another embodiment, a method for forming a pattern using a semiconductor photoresist composition is provided. For example, the pattern produced can be a photoresist pattern.

[0138] The method of forming a pattern according to an embodiment includes forming an etching target layer on a substrate, coating a semiconductor photoresist composition on the etching target layer to form a photoresist layer, patterning the photoresist layer to form a photoresist pattern, and etching the etching target layer using the photoresist pattern as an etching mask.

[0139] Below, reference Figures 1 to 5 A method for forming a pattern using a semiconductor photoresist composition is described. Figures 1 to 5 2 is a cross-sectional view explaining a method of forming a pattern using a semiconductor resist composition according to an embodiment.

[0140] refer to Figure 1 , an object for etching is prepared. The object for etching may be a thin layer 102 formed on a semiconductor substrate 100. Hereinafter, the object for etching is limited to the thin layer 102. The entire surface of the thin layer 102 is washed to remove impurities and the like remaining thereon. The thin layer 102 may be, for example, a silicon nitride layer, a polysilicon layer, or a silicon oxide layer.

[0141] Subsequently, a resist base layer composition for forming a resist base layer 104 is spin-coated on the surface of the washed thin layer 102. However, the embodiment is not limited thereto, and various known coating methods such as spray coating, dip coating, knife edge coating, printing methods such as inkjet printing and screen printing, etc. may be used.

[0142] The coating process of the resist underlayer may be omitted, and hereinafter, a process including coating of the resist underlayer is described.

[0143] Then, the applied composition is dried and baked to form a resist bottom layer 104 on the thin layer 102. The baking may be performed at about 100°C to about 500°C, for example, about 100°C to about 300°C.

[0144] The resist bottom layer 104 is formed between the substrate 100 and the photoresist layer 106, so when the radiation reflected from the interface between the substrate 100 and the photoresist layer 106 or the hard mask between the layers is scattered into the unintended photoresist area, the non-uniformity of the photoresist line width and the pattern forming ability can be prevented.

[0145] refer to Figure 2 , a photoresist layer 106 is formed by coating a semiconductor resist composition on the resist base layer 104. The photoresist layer 106 is obtained by coating the above-mentioned semiconductor resist composition on the thin layer 102 formed on the substrate 100 and then curing it by heat treatment.

[0146] More specifically, forming a pattern by using a semiconductor resist composition may include coating the semiconductor resist composition on the substrate 100 having the thin layer 102 by spin coating, slit coating, inkjet printing, etc., and then drying it to form a photoresist layer 106 .

[0147] The semiconductor resist composition has been described in detail and will not be described again.

[0148] Subsequently, the substrate 100 having the photoresist layer 106 is subjected to a first baking process. The first baking process may be performed at about 80°C to about 120°C.

[0149] refer to Figure 3 , the photoresist layer 106 can be selectively exposed.

[0150] For example, exposure can use activating radiation having the following light: light with a high energy wavelength, such as extreme ultraviolet (EUV; a wavelength of about 13.5 nm), an electron beam (E-Beam), etc.; and light with a short wavelength, such as i-line (a wavelength of about 365 nm), a KrF excimer laser (a wavelength of about 248 nm), an ArF excimer laser (a wavelength of about 193 nm), etc.

[0151] More specifically, according to embodiments, the light used for exposure may have a short wavelength between about 5 nm and about 150 nm and a high energy wavelength, such as extreme ultraviolet light (EUV; wavelength of about 13.5 nm), an electron beam (E-Beam), or the like.

[0152] The exposed region 106 b of the photoresist layer 106 (ie, the region not covered by the patterned hard mask 110 ) has a different solubility from the unexposed region 106 a of the photoresist layer 106 by forming a polymer through a cross-linking reaction (eg, condensation between organic metal compounds).

[0153] Subsequently, the substrate 100 is subjected to a second baking process. The second baking process may be performed at a temperature of about 90° C. to about 200° C. Due to the second baking process, the exposed region 106 b of the photoresist layer 106 becomes easily insoluble in a developing solution.

[0154] exist Figure 4 In the process, a developing solution is used to dissolve and remove the unexposed area 106a of the photoresist layer to form a photoresist pattern 108. Specifically, an organic solvent such as 2-heptanone is used to dissolve and remove the unexposed area 106a of the photoresist layer to complete the photoresist pattern 108 corresponding to the negative image.

[0155] As described above, the developing solution used in the method for forming a pattern according to an embodiment may be an organic solvent. The organic solvent used in the method for forming a pattern according to an embodiment may be, for example, a ketone, such as methyl ethyl ketone, acetone, cyclohexanone, 2-heptanone, etc.; an alcohol, such as 4-methyl-2-propanol, 1-butanol, isopropanol, 1-propanol, methanol, etc.; an ester, such as propylene glycol monomethyl ether acetate, ethyl acetate, ethyl lactate, n-butyl acetate, butyrolactone, etc.; an aromatic compound, such as benzene, xylene, toluene, etc.; or a combination thereof.

[0156] However, the photoresist pattern according to the embodiment is not necessarily limited to a negative image, but may be formed to have a positive image. Herein, the developer for forming the positive image may be a quaternary ammonium hydroxide composition, such as tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, or a combination thereof.

[0157] As described above, exposure to light having high energy such as extreme ultraviolet (EUV; wavelength of about 13.5 nm), electron beam (E-Beam), and light having a wavelength such as i-line (wavelength of about 365 nm), KrF excimer laser (wavelength of about 248 nm), ArF excimer laser (wavelength of about 193 nm), etc. can provide a photoresist pattern 108 having a width of about 5 nm to about 100 nm. For example, the photoresist pattern 108 may have a width of about 5 nm to about 90 nm, about 5 nm to about 80 nm, about 5 nm to about 70 nm, about 5 nm to about 60 nm, about 10 nm to about 50 nm, about 10 nm to about 40 nm, about 10 nm to about 30 nm, or about 10 nm to about 20 nm.

[0158] On the other hand, the photoresist pattern 108 may have a half pitch pitch of less than or equal to about 50 nm, for example, less than or equal to about 40 nm, less than or equal to about 30 nm, or less than or equal to about 25 nm, and a line width roughness of less than or equal to about 10 nm, or less than or equal to about 5 nm.

[0159] Subsequently, the resist bottom layer 104 is etched using the photoresist pattern 108 as an etching mask. Through this etching process, an organic layer pattern 112 is formed. The organic layer pattern 112 may also have a width corresponding to the width of the photoresist pattern 108.

[0160] refer to Figure 5 , the exposed thin layer 102 is etched using the photoresist pattern 108 as an etching mask. As a result, the thin layer is formed with a thin layer pattern 114.

[0161] The etching of the thin layer 102 may be, for example, dry etching using an etching gas, and the etching gas may be, for example, CHF 3 , CF 4 , Cl 2 , BCl 3 and a mixed gas thereof.

[0162] In the exposure process, the thin layer pattern 114 formed by using the photoresist pattern 108 may have a width corresponding to the width of the photoresist pattern 108, which is formed by the exposure process performed using the EUV light source. For example, the thin layer pattern 114 may have a width of about 5 nm to about 100 nm, which is equal to the width of the photoresist pattern 108. For example, like the width of the photoresist pattern 108, the thin layer pattern 114 formed by using the photoresist pattern 108 may have a width of about 5 nm to about 90 nm, about 5 nm to about 80 nm, about 5 nm to about 70 nm, about 5 nm to about 60 nm, about 10 nm to about 50 nm, about 10 nm to about 40 nm, about 10 nm to about 30 nm, and about 10 nm to about 20 nm, or specifically less than or equal to about 20 nm, which is formed by the exposure process performed using the EUV light source.

[0163] Hereinafter, the present invention is described in more detail by way of examples regarding the preparation of the above-mentioned semiconductor photoresist composition. However, the present invention is not technically limited to the following examples.

[0164] Examples

[0165] Synthesis example 1

[0166] 20g (51.9mmol) of Ph3SnCl was dissolved in 70ml of tetrahydrofuran (THF) in a 250mL 2-neck round-bottom flask and then cooled to 0°C in an ice bath. Subsequently, 1M butylmagnesium chloride (BuMgCl) THF solution (62.3mmol) was slowly added dropwise thereto. When the addition was completed, the resulting mixture was stirred at room temperature for 12 hours, thereby obtaining the compound represented by Chemical Formula 7 with a yield of 85%.

[0167] [Chemical formula 7]

[0168]

[0169] Synthesis example 2

[0170] The compound represented by Chemical Formula 8 was obtained in a yield of 88% according to the same method as Synthesis Example 1, except that 2M isopropylmagnesium chloride (iPrMgCl) THF solution (62.3 mmol) was used instead of 1M butylmagnesium chloride (BuMgCl) THF solution.

[0171] [Chemical formula 8]

[0172]

[0173] Synthesis example 3

[0174] The compound represented by Chemical Formula 9 was obtained in a yield of 76% according to the same method as Synthesis Example 1, except that 1 M neopentylmagnesium chloride THF solution (62.3 mmol) was used instead of 1 M butylmagnesium chloride (BuMgCl) THF solution.

[0175] [Chemical formula 9]

[0176]

[0177] Synthesis example 4

[0178] The compound represented by Chemical Formula 7 according to Synthesis Example 1 (10 g, 24.6 mmol) was dissolved in 50 mL of CH2Cl2, and 3 equivalents (73.7 mmol) of 2M HCl diethyl ether solution were slowly added dropwise thereto at -78°C for 30 minutes. Subsequently, the resulting mixture was stirred at room temperature for 12 hours, and then, by concentrating the solvent and performing vacuum distillation, a compound represented by Chemical Formula 10 was obtained with a yield of 80%.

[0179] [Chemical formula 10]

[0180]

[0181] Synthesis example 5

[0182] The compound represented by Chemical Formula 11 was obtained in a yield of 75% according to the same method as Synthesis Example 4, except that the compound represented by Chemical Formula 8 according to Synthesis Example 2 was used instead of the compound represented by Chemical Formula 7 according to Synthesis Example 1.

[0183] [Chemical formula 11]

[0184]

[0185] Synthesis example 6

[0186] The compound represented by Chemical Formula 12 was obtained in a yield of 70% according to the same method as Synthesis Example 4, except that the compound represented by Chemical Formula 9 according to Synthesis Example 3 was used instead of the compound represented by Chemical Formula 7 according to Synthesis Example 1.

[0187] [Chemical formula 12]

[0188]

[0189] Synthesis Example 7

[0190] At room temperature, 25 mL of acetic acid was slowly added dropwise to 10 g (25.6 mmol) of the compound represented by Chemical Formula 10 according to Synthesis Example 4, and then heated and refluxed for 12 hours. The temperature was lowered to room temperature, and then the acetic acid was vacuum distilled to obtain the compound represented by Chemical Formula 13 with a yield of 90%.

[0191] [Chemical formula 13]

[0192]

[0193] Synthesis example 8

[0194] At room temperature, 25 mL of acrylic acid was slowly added dropwise to 10 g (25.4 mmol) of the compound represented by Chemical Formula 11 according to Synthesis Example 5, and then heated and refluxed at 80° C. for 6 hours. The temperature was lowered to room temperature, and then the acrylic acid was vacuum distilled to obtain the compound represented by Chemical Formula 14 at a yield of 50%.

[0195] [Chemical formula 14]

[0196]

[0197] Synthesis example 9

[0198] At room temperature, 25 mL of propionic acid was slowly added dropwise to 10 g (23.7 mmol) of the compound represented by Chemical Formula 12 according to Synthesis Example 6, and then heated and refluxed at 110° C. for 12 hours. The temperature was lowered to room temperature, and then propionic acid was vacuum distilled to obtain the compound represented by Chemical Formula 15 with a yield of 40%.

[0199] [Chemical formula 15]

[0200]

[0201] Synthesis example 10

[0202] 30 mL of anhydrous pentane was added to 10 g (35.4 mmol) of the compound represented by Chemical Formula 10 according to Synthesis Example 4, and then cooled to 0° C. 7.8 g (106.3 mmol) of diethylamine was slowly added dropwise thereto, and then 7.9 g (106.3 mmol) of tert-butyl alcohol was added thereto, and then stirred at room temperature for 1 hour. When the reaction was completed, the resultant was filtered, concentrated and vacuum dried to obtain a compound represented by Chemical Formula 16 with a yield of 60%.

[0203] [Chemical formula 16]

[0204]

[0205] Synthesis example 11

[0206] 30 mL of anhydrous pentane was added to 10 g (37.3 mmol) of the compound represented by Chemical Formula 11 according to Synthesis Example 5, and then cooled to 0° C. 8.2 g (111.9 mmol) of diethylamine was slowly added dropwise thereto, and then 6.7 g (111.9 mmol) of isopropanol was added thereto, and then stirred at room temperature for 1 hour. When the reaction was completed, the resultant was filtered, concentrated and vacuum dried to obtain a compound represented by Chemical Formula 17 with a yield of 60%.

[0207] [Chemical formula 17]

[0208]

[0209] Synthesis example 12

[0210] 30 mL of anhydrous pentane was added to 10 g (18.7 mmol) of the compound represented by Chemical Formula 12 according to Synthesis Example 6, and then cooled to 0° C. 7.4 g (101.3 mmol) of diethylamine was slowly added dropwise thereto, and then 6.1 g (101.3 mmol) of ethanol was added thereto, and then stirred at room temperature for 1 hour. When the reaction was completed, the resultant was filtered, concentrated and vacuum dried to obtain a compound represented by Chemical Formula 18 with a yield of 60%.

[0211] [Chemical formula 18]

[0212]

[0213] Synthesis example 13

[0214] 10 g (25.4 mmol) of the compound represented by Chemical Formula 8 was put into a 100 mL round-bottom flask, and 25 mL of formic acid was slowly dropped thereinto at room temperature, followed by heating and reflux at 100° C. for 24 hours.

[0215] Subsequently, the temperature was lowered to room temperature, and then formic acid was vacuum distilled, thereby obtaining the compound represented by Chemical Formula 19 at a yield of 90%.

[0216] [Chemical formula 19]

[0217]

[0218] Synthesis example 14

[0219] Ph4Sn (20 g, 46.8 mmol) was put into a 100 mL round-bottom flask, and 50 ml of propionic acid was slowly added thereto, followed by heating and reflux at 110° C. for 26 hours. Subsequently, the temperature was lowered to room temperature, and propionic acid was vacuum distilled to obtain the compound represented by Chemical Formula 20 with a yield of 95%.

[0220] [Chemical formula 20]

[0221]

[0222] Synthesis Example 15

[0223] 154 mL of 1 M sodium ethoxide ethanol solution was put into a 100 mL round bottom flask, and 10 g (38.4 mmol) of SnCl4 was slowly dropped thereinto at 0° C. The temperature was raised to room temperature, and then the resulting mixture was stirred for 12 hours and vacuum distilled to obtain the compound represented by Chemical Formula 21 with a yield of 70%.

[0224] [Chemical formula 21]

[0225]

[0226] Instance 1 to Instance 14

[0227] Compounds 13 to 19 according to Synthesis Examples 7 to 13 were dissolved in xylene at a concentration of 2 wt %, and compounds 20 and 21 according to Synthesis Examples 14 and 15 were dissolved in xylene in which compounds 13 to 19 according to Synthesis Examples 7 to 13 were dissolved at a concentration of 0.2 wt %, and then filtered with a 0.1 μm polytetrafluoroethylene (PTFE) injection filter to prepare semiconductor photoresist compositions according to Examples 1 to 14. The specific compound combinations of the semiconductor photoresist compositions are shown in Table 1.

[0228] A disk-shaped silicon wafer having a natural oxide surface and a diameter of 4 inches was used as a substrate for thin film coating and treated in a UV ozone cleaning system for 10 minutes before coating the composition. On the treated substrate, the semiconductor photoresist composition according to Example 1 to Example 14 was spin-coated at 1500 rpm for 30 seconds, respectively, and then baked (post-apply bake, PAB) at 100° C. for 120 seconds to form a photoresist film.

[0229] After coating and baking, the thickness of the film was measured by ellipsometer and was about 25 nm.

[0230] Comparative Example 1

[0231] A semiconductor photoresist composition according to Comparative Example 1 and a photoresist film including the composition were prepared according to the same method as in Example 1, except that the compound represented by Chemical Formula 13 according to Synthesis Example 7 was dissolved in xylene at a concentration of 2 wt %. After coating and baking, the thickness of the film was about 25 nm.

[0232] Comparative Example 2

[0233] A semiconductor photoresist composition according to Comparative Example 2 and a photoresist thin film including the same were manufactured according to the same method as Example 1, except that nBuSnOOH (TCI Inc.) was used instead of the compound represented by Chemical Formula 13. After coating and baking, the thickness of the film was about 25 nm.

[0234] (Table 1)

[0235] Organometallic compound (A) Organometallic compounds (B) Example 1 Chemical formula 13 Chemical formula 20 Example 2 Chemical formula 14 Chemical formula 20 Example 3 Chemical formula 15 Chemical formula 20 Example 4 Chemical formula 16 Chemical formula 20 Example 5 Chemical formula 17 Chemical formula 20 Example 6 Chemical formula 18 Chemical formula 20 Example 7 Chemical formula 19 Chemical formula 20 Example 8 Chemical formula 13 Chemical formula 21 Example 9 Chemical formula 14 Chemical formula 21 Example 10 Chemical formula 15 Chemical formula 21 Example 11 Chemical formula 16 Chemical formula 21 Example 12 Chemical formula 17 Chemical formula 21 Example 13 Chemical formula 18 Chemical formula 21 Example 14 Chemical formula 19 Chemical formula 21 Comparative Example 1 Chemical formula 13 - Comparative Example 2 nBuSnOOH (Antimony Xi Ai Company) Chemical formula 20

[0236] evaluate

[0237] By changing the energy and focus, the film according to Example 1 to Example 14 and Comparative Example 1 to Comparative Example 2 formed on a disk-shaped silicon wafer in the coating method was exposed to extreme ultraviolet light (UV) to form a line / space pattern of 12nm to 100nm. After exposure, the film was baked at 180°C for 120 seconds, then immersed in a petri dish containing 2-heptanone for 60 seconds and taken out, and washed with the same solvent for 10 seconds. Finally, the film was baked at 150°C for 5 minutes, and then its pattern image was obtained by scanning electron microscopy (SEM). Through the SEM image, the highest resolution, best energy and line edge roughness (LER) are provided in Table 2.

[0238] (Table 2)

[0239] Resolution(nm) <![CDATA[Energy (mJ / cm 2 )]]> LER(nm) Example 1 15.0 53 2.5 Example 2 16.0 35 2.9 Example 3 15.1 48 2.5 Example 4 14.5 50 3.0 Example 5 15.6 48 3.0 Example 6 15.0 42 3.3 Example 7 15.6 35 3.0 Example 8 15.3 55 2.5 Example 9 15.8 35 3.0 Example 10 14.8 44 3.2 Example 11 15.5 52 2.5 Example 12 15.0 44 2.9 Example 13 14.3 37 3.6 Example 14 15.2 35 3.2 Comparative Example 1 18.5 75 4.6 Comparative Example 2 19.1 96 4.5

[0240] Referring to Table 2, a photoresist film formed by using the semiconductor photoresist composition according to Examples 1 to 14 simultaneously containing one of the compounds represented by Chemical Formulas 13 to 19 and the compound represented by Chemical Formula 20 or 21 exhibited excellent resolution, sensitivity, and line edge roughness (LER).

[0241] On the contrary, compared with the resolution, energy and line edge roughness of the examples, the photoresist films formed by the semiconductor photoresist composition of Comparative Example 1 containing only the compound represented by Chemical Formula 13 and the semiconductor photoresist composition of Comparative Example 2 containing nBuSnOOH (Antimony Si Ai Company) and the compound represented by Chemical Formula 20 both exhibited the highest resolution, optimal energy and excellent line edge roughness (LER).

[0242] In the above, certain exemplary embodiments of the present invention have been described and illustrated, however, it is obvious to those skilled in the art that the present invention is not limited to the exemplary embodiments described, and various modifications and changes can be made without departing from the spirit and scope of the present invention. Therefore, the modified or changed exemplary embodiments themselves may not be understood separately from the technical ideas and aspects of the present invention, and the modified exemplary embodiments are within the scope of the claims of the present invention.

Claims

1. A semiconductor photoresist composition comprising: An organic metal compound represented by Chemical Formula 1, an organic metal compound represented by Chemical Formula 2, and a solvent: [Chemical formula 1] in, In Chemical Formula 1, R is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethylene oxide group, a propylene oxide group, or a combination thereof, X, Y and Z are independently -OR 1 or -OC(=O)R 2 , R 1 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and R 2 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof; [Chemical formula 2] Wherein, in Chemical Formula 2, X' is -OR 3 or -OC(=O)R 4 , R 3 is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, and R 4 is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof, The organic metal compound represented by Chemical Formula 1 and the organic metal compound represented by Chemical Formula 2 are included in a weight ratio of 20:1 to 1:

1.

2. The semiconductor photoresist composition according to claim 1, wherein R is a substituted or unsubstituted C1 to C8 alkyl group, a substituted or unsubstituted C3 to C8 cycloalkyl group, a substituted or unsubstituted C2 to C8 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C20 aryl group, an ethylene oxide group, a propylene oxide group, or a combination thereof, R 1 and R 3 are independently substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C3 to C8 cycloalkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted C6 to C20 aryl, or a combination thereof, and R 2 and R 4 are independently hydrogen, substituted or unsubstituted C1 to C8 alkyl, substituted or unsubstituted C3 to C8 cycloalkyl, substituted or unsubstituted C2 to C8 alkenyl, substituted or unsubstituted C2 to C8 alkynyl, substituted or unsubstituted C6 to C20 aryl, or a combination thereof.

3. The semiconductor photoresist composition according to claim 1, wherein R is methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, vinyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, ethylene oxide, propylene oxide or a combination thereof, R 1 and R 3 are independently methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, vinyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, or a combination thereof, and R 2 and R 4 are independently hydrogen, methyl, ethyl, propyl, butyl, isopropyl, tert-butyl, 2,2-dimethylpropyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, ethenyl, propenyl, butenyl, ethynyl, propynyl, butynyl, phenyl, tolyl, xylyl, benzyl, or a combination thereof.

4. The semiconductor photoresist composition according to claim 1, wherein the compound represented by Chemical Formula 1 comprises a compound represented by Chemical Formula 3, a compound represented by Chemical Formula 4, a compound represented by Chemical Formula 5, a compound represented by Chemical Formula 6, or a combination thereof: [Chemical formula 3] [Chemical formula 4] [Chemical formula 5] [Chemical formula 6] in, In Chemical Formula 3, Chemical Formula 4, Chemical Formula 5 and Chemical Formula 6, R is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 aliphatic unsaturated organic group containing at least one double bond or triple bond, a substituted or unsubstituted C6 to C30 aryl group, an ethylene oxide group, a propylene oxide group, or a combination thereof, R a , R b , R c , R i , R k and R l are independently substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof, and R d , R e , R f , R g , R h and R j and R is independently hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof.

5. The semiconductor photoresist composition according to claim 1, wherein the composition comprises 0.01 wt % to 30 wt % of the organic metal compound represented by Chemical Formula 1 and 0.01 wt % to 15 wt % of the organic metal compound represented by Chemical Formula 2, based on 100 wt % of the semiconductor photoresist composition. 6 . The semiconductor photoresist composition according to claim 1 , wherein the semiconductor photoresist composition comprises an additive of a surfactant, a crosslinking agent, a leveling agent, or a combination thereof.

7. A method for forming a pattern, comprising: forming an etching target layer on a substrate; coating the semiconductor photoresist composition according to claim 1 on the etching target layer to form a photoresist layer; patterning the photoresist layer to form a photoresist pattern; and The etch target layer is etched using the photoresist pattern as an etch mask. 8 . The method of forming a pattern according to claim 7 , wherein the photoresist pattern is formed using light having a wavelength of 5 nm to 150 nm.

9. The method for forming a pattern according to claim 7, further comprising providing a resist bottom layer formed between the substrate and the photoresist layer. 10 . The method of claim 7 , wherein the photoresist pattern has a width of 5 nm to 100 nm.

Citation Information

Patent Citations

  • Optical near-field measurement

    KR1020190050856A

  • Solution processed thin films and laminates, devices comprising such thin films and laminates, and method for their use and manufacture

    US20110045406A1

  • Radiation sensitive materials

    US5061599A

  • Organotin oxide hydroxide patterning compositions, precursors, and patterning

    CN108351594A