Sliding member
By forming a Bi alloy coating with high Sb concentration on the copper alloy liner and using an Ag intermediate layer, the problem of reducing fatigue resistance caused by the formation of Cu-Sb compounds is solved, and high fatigue resistance and run-in properties of the plating layer are achieved.
Patent Information
- Application Number
- CN201980019991.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-04-11
- Filing Date
- 2019-02-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2039-02-28
AI Technical Summary
In the Bi alloy plating layer formed on the copper alloy liner, the formation of Cu-Sb compound leads to deterioration of fatigue resistance, especially the diffusion of Cu promotes the formation of Cu-Sb compound and reduces the fatigue resistance of the plating layer .
By forming an alloy coating of Bi and Sb on the copper alloy liner, the Sb concentration in the plating layer is set to be more than 3.1%, and an intermediate layer with Ag as the main component is used to separate the liner and the plating layer to reduce Cu The diffusion of the coating increases the hardness and fatigue resistance of the coating.
The fatigue resistance and run-in properties of the plating layer are improved, the formation of Cu-Sb compounds is prevented, the service life of the plating layer is extended, and the embrittlement problems caused by excessive Sb concentration are avoided.
Smart Images

Figure CN111902643B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a sliding member having a plating layer of an alloy plating film of Bi and Sb. Background Art
[0002] It is known that a plated layer is formed by a Bi alloy containing 0.1 to 10% by mass of Cu and 0.1 to 20% by mass of Sb (see Patent Document 1). Patent Document 1 discloses that the fatigue resistance of the plated layer is improved by making the crystal structure of the Bi alloy dense by Cu. In addition, Patent Document 1 discloses that the low melting point of the plated layer can be prevented and the running-in property can be maintained by adding Sb.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 3693256 Summary of the invention
[0006] Problems to be solved by the invention
[0007] However, there is a problem that when Cu and Sb coexist in the plating layer as in Patent Document 1, a Cu-Sb compound is formed in the plating layer, and the Cu-Sb compound deteriorates fatigue resistance. In particular, there is a problem that when the plating layer is formed on a lining layer formed of a copper alloy, Cu in the lining layer diffuses into the plating layer, promoting the formation of the Cu-Sb compound.
[0008] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a sliding member capable of exhibiting good fatigue resistance in a plating layer of a Bi alloy containing Sb formed on a lining layer formed of a copper alloy.
[0009] Solutions for solving problems
[0010] In order to achieve the above-mentioned object, the sliding component of the present invention is a sliding component having a plating layer formed by an alloy plating film of Bi and Sb, wherein the concentration of Sb in the plating layer is 3.1 mass % or more, and the plating layer is joined to a lining layer formed by a copper alloy via an intermediate layer mainly composed of Ag.
[0011] In the above-mentioned formation, the coating layer not only includes soft Bi, but also includes hard Sb, so fatigue resistance can be improved by hard Sb. Here, Cu has the property that it is easier to diffuse to Sb than to diffuse to Bi. When the average concentration of Sb in the coating layer is set to be higher (for example, more than 3 mass %), the more there is the possibility that Cu diffuses from the liner to the coating layer to reduce fatigue resistance. It should be noted that the coating layer can be hardened by increasing the average concentration of Sb in the coating layer, but the excess Sb can make the coating layer embrittled and cause fatigue resistance to decrease, so the average concentration of Sb is ideally less than 10 mass %.
[0012] In this regard, by sandwiching an intermediate layer with Ag as the main component, in which Cu is difficult to diffuse, between the lining layer and the plating layer, the amount of Cu diffused from the lining layer into the plating layer can be reduced, and the possibility of reduced fatigue resistance can be reduced. Here, the average concentration of Sb in the plating layer refers to the average concentration of Sb in the entire depth range from the surface of the plating layer. In addition, the higher the concentration of Sb, the harder the plating layer 12 can be made, so by increasing the concentration of Sb, fatigue resistance can be further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a perspective view of a sliding member according to an embodiment of the present invention.
[0014] Figure 2 This is a graph showing the concentration of Sb in the plating layer.
[0015] In Figure 3 Figure 3A and Figure 3B This is a photograph of a cross section of a coating layer.
[0016] Figure 4 This is a diagram illustrating a fatigue test.
[0017] In Figure 5 Figure 5A to Figure 5C This is a photograph of a cross section of a coating layer.
[0018] Figure 6 This is a graph showing the relationship between the Sb concentration and the fatigue area ratio. DETAILED DESCRIPTION
[0019] Here, embodiments of the present invention will be described in the following order.
[0020] (1) First Embodiment
[0021] (1-1) Configuration of Sliding Component
[0022] (1-2) Method for manufacturing sliding member
[0023] (2) Other Implementation Methods
[0024] (1) First Implementation Method:
[0025] (1-1) Composition of sliding member:
[0026] Figure 1 It is a stereoscopic view of a sliding member 1 according to an embodiment of the present invention. The sliding member 1 includes a backing 10, a lining 11, and a plating layer 12. The sliding member 1 is a metal member in a split shape formed by dividing a hollow cylinder into two equal parts in the diameter direction, and its cross section is in the shape of a semicircular arc. By combining two sliding members 1 in a cylindrical manner, a sliding bearing A is formed. The sliding bearing A supports a cylindrical mating shaft 2 (the crankshaft of the engine) through a hollow portion formed inside. The outer diameter of the mating shaft 2 is formed to be slightly smaller than the inner diameter of the sliding bearing A. Lubricating oil (engine oil) is supplied to the gap formed between the outer peripheral surface of the mating shaft 2 and the inner peripheral surface of the sliding bearing A. At this time, the outer peripheral surface of the mating shaft 2 slides on the inner peripheral surface of the sliding bearing A.
[0027] The sliding member 1 has the following structure: a backing 10, a lining 11, an intermediate layer 13, and a plating layer 12 are sequentially stacked in the order of being away from the center of curvature. Therefore, the backing 10 constitutes the outermost layer of the sliding member 1, and the plating layer 12 constitutes the innermost layer of the sliding member 1. The backing 10, the lining 11, the intermediate layer 13, and the plating layer 12 each have a constant thickness in the circumferential direction. The thickness of the backing 10 is 1.8 mm, the thickness of the lining 11 is 0.2 mm, the thickness of the intermediate layer 13 is, for example, 2.0 μm, and the thickness of the plating layer 12 is 20 μm. The radius of the surface of the plating layer 12 on the curvature center side is 55 mm (the inner diameter of the sliding member 1). The width of the sliding bearing A is 19 mm. Hereinafter, the inner side refers to the curvature center side of the sliding member 1, and the outer side refers to the side opposite to the curvature center of the sliding member 1. The inner surface of the plating layer 12 constitutes the sliding surface of the mating shaft 2.
[0028] The backing 10 is made of steel containing 0.15 mass % C, 0.06 mass % Mn, and the remainder Fe. It should be noted that the backing 10 may be made of a material capable of supporting the load from the mating shaft 2 via the lining layer 11 and the plating layer 12, and is not necessarily made of steel.
[0029] The lining layer 11 is a layer stacked on the inner side of the backing 10, and constitutes the base layer of the present invention. The lining layer 11 contains 10% by mass of Sn, 8% by mass of Bi, and the remainder is composed of Cu and inevitable impurities. The inevitable impurities of the lining layer 11 are Mg, Ti, B, Pb, Cr, etc., which are impurities mixed in refined or scrap materials. The total content of the inevitable impurities in the lining layer 11 is 0.5% by mass or less.
[0030] The intermediate layer 13 is formed of pure Ag. The total content of inevitable impurities in the intermediate layer 13 is 0.5 mass % or less.
[0031] The plating layer 12 is a layer stacked on the inner surface of the liner 11. The plating layer 12 is an alloy plating film of Bi and Sb. In addition, the plating layer 12 is composed of Bi, Sb and inevitable impurities. The total content of the inevitable impurities in the plating layer 12 is 0.5 mass % or less.
[0032] [Table 1]
[0033]
[0034] Table 1 is a table showing the concentration (mass concentration) of Sb in the plating layer 12 . Figure 2 It is a graph showing the concentration (mass concentration) of Sb in the plating layer 12 . Figure 2 The horizontal axis represents the distance from the interface with the intermediate layer 13, and the vertical axis represents the concentration of Sb. Figure 2 In FIG. 1 , the Sb concentration of sample A converges to about 2 mass % (triangle), the Sb concentration of sample B converges to about 1 mass % (circle), and the concentration of sample C without a concentration gradient (quadrilateral). Figure 2 As shown, in Sample A and Sample B, the concentration of Sb is the highest at the interface with the intermediate layer 13. Moreover, in Sample A and Sample B, the concentration of Sb continuously decreases as the distance from the interface with the intermediate layer 13 increases (the depth from the surface of the plating layer 12 decreases). The average concentration of Sb in the entire plating layer 12 is 3.05 mass %.
[0035] In Sample A and Sample B, the greater the distance from the interface with the intermediate layer 13, the smaller the slope (absolute value) of the Sb concentration is, and the Sb concentration converges to a substantially constant value in a region where the distance from the interface with the intermediate layer 13 is 4 μm or more. In Sample A and Sample B, the slope and standard deviation of the Sb concentration in a first region where the depth from the surface of the plating layer 12 is a first depth (a region where the distance from the interface X with the intermediate layer 13 is 4 μm or less) are greater than the slope and standard deviation of the Sb concentration in a second region where the depth from the surface of the plating layer is shallower than the first depth (a region where the distance from the interface X with the intermediate layer 13 is greater than 4 μm).
[0036] The slope of the concentration of Sb in the first region of sample A is 7.6 times the slope of the concentration of Sb in the second region. The standard deviation of Sb in the first region of sample A is 18.1 times the standard deviation of the concentration of Sb in the second region. On the other hand, the slope of the concentration of Sb in the first region of sample B is 3.7 times the slope of the concentration of Sb in the second region. The standard deviation of Sb in the first region of sample B is 3.2 times the standard deviation of the concentration of Sb in the second region.
[0037] The plating layer 12 of the present embodiment is formed by the same manufacturing method as that of the sample A, and the Sb concentration on the surface of the plating layer 12 having a film thickness of 20 μm is 1.8 mass %. Therefore, in the present embodiment, it can be determined that there is Figure 2 The concentration gradient of Sb is the same as that of sample A. It should be noted that the concentration of Sb in the plated layer 12 can be adjusted by increasing or decreasing the concentration of Sb in the plating bath for electroplating the plated layer 12 described later.
[0038] Figure 3A and Figure 3B This is a cross-sectional photograph of the plating layer 12 . Figure 3A and Figure 3B The cross-sectional photograph is mapped in a manner that the higher the Sb concentration, the darker the color. As shown in FIG3 , the shallower the depth from the surface of the plated layer 12, the lower the Sb concentration becomes. That is, the deeper the depth from the surface of the plated layer 12, the higher the Sb concentration becomes. In addition, it can be considered that the remaining part other than Sb is Bi, so the deeper the depth from the surface of the plated layer 12, the lower the Bi concentration becomes. That is, the shallower the depth from the surface of the plated layer 12, the higher the Bi concentration becomes. It should be noted that Figure 3A This is a photograph of a cross section of a plating layer 12 having a thickness of approximately 10 μm.
[0039] It should be noted that the concentration of Sb in the plating layer 12 is measured by energy dispersive X-ray spectroscopy using an electron probe microanalyzer (JMS-66610A manufactured by JEOL). Specifically, a plurality of rectangular regions E are set, each with a distance of 1 μm from the interface X between the plating layer 12 and the intermediate layer 13 to the upper end (end on the surface side), and the average mass concentration of Sb in the rectangular region E is measured as the mass concentration of Sb at each distance. An overall region EA consisting of all rectangular regions E is set, and the average mass concentration of Sb in the overall region EA is measured as the average concentration of Sb in the entire plating layer.
[0040] A fatigue test piece (connecting rod R) in which the intermediate layer 13 is omitted from the sliding member 1 described above was made, and its fatigue area rate was measured, and the fatigue area rate was good 30%. Here, as in the present embodiment, when the average concentration of Sb in the entire coating layer 12 is a low concentration of 3.05 mass %, it is confirmed that even if the intermediate layer 13 is not provided, Cu hardly diffuses from the lining layer 11 to the coating layer. Therefore, as in the present embodiment, when the average concentration of Sb in the entire coating layer is a low concentration of 3.05 mass %, it can be thought that the same fatigue area rate can be obtained with and without the intermediate layer 13. Here, when the intermediate layer 13 itself is destroyed or peeling occurs at the interface of the intermediate layer 13, the presence of the intermediate layer 13 affects the fatigue area rate. In the present embodiment, it can be thought that the destruction or peeling of the intermediate layer 13 does not occur, and therefore, the same fatigue area rate can be obtained with and without the intermediate layer 13. Therefore, a fatigue test piece in which the intermediate layer 13 is omitted is used. The fatigue area rate is measured in the following order. Figure 4 This is a diagram illustrating a fatigue test. Figure 4 As shown, a connecting rod R having cylindrical through holes formed at both ends in the longitudinal direction is prepared, and a test shaft H (shaded) is axially supported by the through hole at one end.
[0041] It should be noted that a plating layer 12 (black) similar to the sliding member 1 is formed on the inner peripheral surface of the through hole of the connecting rod R that supports the test shaft H. The test shaft H is supported on both outer sides of the connecting rod R in the axial direction of the test shaft H, and the test shaft H is rotated so that the sliding speed is 6.6 m / sec. The sliding speed is the relative speed between the surface of the plating layer 12 and the test shaft H. The end of the connecting rod R on the opposite side of the test shaft H is connected to a moving body F that reciprocates along the length direction of the connecting rod R, and the reciprocating load of the moving body F is set to 80 MPa. In addition, engine oil at about 140°C is supplied between the connecting rod R and the test shaft H.
[0042] By allowing the above state to continue for 50 hours, a fatigue test of the coating layer 12 was performed. Then, after the fatigue test, the inner surface of the coating layer 12 was photographed from a position on a straight line orthogonal to the inner surface (sliding surface) of the coating layer 12, with the straight line set as the main optical axis, and an evaluation image as the photographed image was obtained. Then, the damaged portion of the surface of the coating layer 12 displayed in the evaluation image was observed and determined through a binocular (magnifying glass), and the percentage of the value obtained by dividing the damaged portion area as the area of the damaged portion by the overall surface area of the coating layer 12 displayed in the evaluation image was measured as the fatigue area rate.
[0043] In the present embodiment described above, the plating layer 12 contains not only soft Bi but also hard Sb, so fatigue resistance can be improved by hard Sb. In addition, as the depth from the surface increases, the concentration of Sb increases, so good running-in can be achieved at the initial stage of wear, and high wear resistance can be achieved at the stage of aggravated wear. Moreover, as the depth from the surface increases, the concentration of Sb increases, so interlayer peeling can be prevented.
[0044] In addition, the slope of the Sb concentration in the first region (region where the distance from the interface X with the intermediate layer 13 is 4 μm or less) at a first depth from the surface of the plating layer 12 is greater than the slope of the Sb concentration in the second region (region where the distance from the interface X with the intermediate layer 13 is greater than 4 μm) at a depth shallower than the first depth from the surface of the plating layer. Thus, the hardness of the plating layer 12 can be sharply increased as wear increases.
[0045] It is conceivable that the higher the average concentration of Sb in the plated layer 12, the greater the effect of Sb described above. However, when the average concentration of Sb in the plated layer 12 is increased, Cu diffuses from the liner 11 to the plated layer 12, and the diffused Cu reduces fatigue resistance. Therefore, the intermediate layer 13 is formed as a structure for suppressing the diffusion of Cu.
[0046] Next, the results of the test for confirming the effect of the intermediate layer 13 will be described.
[0047] [Table 2]
[0048]
[0049] Table 2 is a table showing the results of the effect confirmation test of the intermediate layer 13. In the effect confirmation test of the intermediate layer 13, the concentration of Cu in the plating layer 12 was measured for 6 samples D1, D2, E1, E2, F1 and F2. Samples D1, D2, E1, E2, F1 and F2 are all sliding members 1 in which the plating layer 12 with a high concentration of Sb having an average concentration of 5.0% is formed in order to promote the diffusion of Cu.
[0050] Samples D1 and D2 are sliding members 1 in which the plating layer 12 is formed directly on the lining layer 11 without the intermediate layer 13. Samples E1 and E2 are sliding members 1 in which the plating layer 12 is formed on the lining layer 11 via the intermediate layer 13 having a thickness of 2 μm formed of pure Ag. The intermediate layer 13 of samples E1 and E2 has the same structure as the intermediate layer 13 of the first embodiment. Samples F1 and F2 are sliding members 1 in which the plating layer 12 is formed on the lining layer 11 via the intermediate layer 13 having a thickness of 2 μm formed of an Ag-Sn alloy. In the Ag-Sn alloy, only 30 mass % of Sn is contained.
[0051] Samples D2, E2 and F2 were heat treated (placed in air at 150°C for 50 hours) after the sliding member 1 was completed in order to allow diffusion of Cu. On the other hand, samples D1, E1 and F1 were not heat treated after the sliding member 1 was completed.
[0052] Figure 5A to Figure 5C It is a cross-sectional photograph of the plated layer 12 in the samples D2, E2 and F2. Figure 5A to Figure 5C The cross-sectional photograph of is mapped in a manner that the higher the Cu concentration, the darker the color. As shown in Table 1, it can be seen that Cu diffuses into the plating layer 12 only in the sample D2 where the intermediate layer 13 is not formed and the heat treatment is performed. Figure 5A It can also be observed that Cu diffuses linearly from the lining layer 11 shown in black in the sample D2. It should be noted that it can be understood that the longer the distance from the interface X in the plating layer 12 of the sample D2, the lower the concentration of Cu, and the more Cu diffuses from the lining layer 11. Therefore, it can be understood that when the sliding member 1 in which the plating layer 12 with a high concentration of Sb is formed without forming the intermediate layer 13 is used in the use environment of the actual product, Cu diffuses from the lining layer 11 to the plating layer 12, and the diffused Cu reduces the fatigue resistance.
[0053] In contrast, in the samples E2 and F2 in which the intermediate layer 13 is provided, although heat treatment is performed, the concentration of Cu is 0 mass %. Therefore, even if the concentration of Sb in the coating layer 12 is made high-concentration, the amount of Cu diffused from the liner 11 to the coating layer 12 can be suppressed, and the diffused Cu can be prevented from reducing fatigue resistance. The higher the concentration of Sb, the harder the coating layer 12 can be made, and therefore, by making the concentration of Sb high-concentration, fatigue resistance can be further improved. Of course, as in the first embodiment, in the coating layer 12 where Sb is a low concentration, by forming the intermediate layer 13, the diffusion of Cu can also be reliably prevented. It should be noted that the measurement method of the concentration of Cu in the coating layer 12 is the same as the measurement method of the concentration of Sb.
[0054] (1-2) Method for manufacturing sliding member:
[0055] First, a flat plate of low-carbon steel having the same thickness as the backing 10 is prepared.
[0056] Next, powders of materials constituting the lining layer 11 are spread on a flat plate formed of low-carbon steel. Specifically, powders of Cu, Bi, and Sn are spread on the flat plate of low-carbon steel in such a manner as to satisfy the mass ratio of the components in the lining layer 11. As long as the mass ratio of the components in the lining layer 11 is satisfied, alloy powders such as Cu-Bi and Cu-Sn may be spread on the flat plate of low-carbon steel. The particle size of the powder is adjusted to 150 μm or less using a test sieve (JIS Z8801).
[0057] Next, the low-carbon steel flat plate and the powder dispersed on the flat plate are sintered. The sintering temperature is controlled at 700 to 1000° C. and the sintering is performed in an inert atmosphere. After sintering, the plated layer 11 is cooled. It should be noted that the coating layer 11 does not necessarily have to be formed by sintering, but can also be formed by casting or the like.
[0058] After cooling, a Cu alloy layer is formed on the low-carbon steel flat plate. The Cu alloy layer contains soft Bi particles precipitated during the cooling process.
[0059] Next, the low carbon steel having the Cu alloy layer formed thereon is pressed so that the hollow cylinder has a shape obtained by dividing the hollow cylinder into two equal parts in the diameter direction. At this time, the low carbon steel is pressed so that the outer diameter of the low carbon steel matches the outer diameter of the sliding member 1 .
[0060] Next, the surface of the Cu alloy layer formed on the backing 10 is cut. At this time, the cutting amount is controlled so that the thickness of the Cu alloy layer formed on the backing 10 is the same as that of the lining 11. Thus, the lining 11 can be formed from the cut Cu alloy layer. The cutting is performed by a lathe equipped with a cutting tool material made of, for example, sintered diamond.
[0061] Next, Ag was electroplated to a thickness of only 2 μm on the surface of the plated layer 11, thereby forming the intermediate layer 13. Next, Bi was electroplated to a thickness of only 10 μm on the surface of the intermediate layer 13, thereby forming the plated layer 12. The order of electroplating was set as follows. First, the surface of the intermediate layer 13 was washed with water. Furthermore, the surface of the intermediate layer 13 was pickled to remove unnecessary oxides from the surface of the intermediate layer 13. Then, the surface of the intermediate layer 13 was washed with water again.
[0062] After the above pretreatment was completed, electroplating was performed by supplying current to the lining 11 immersed in the plating bath. The bath composition of the plating bath was set to contain methanesulfonic acid: 150 g / L, methanesulfonic acid Bi: 20 g / L, and organic surfactant: 25 g / L. In the above plating bath, only 0.18 g / L of pure Sb was dissolved by electrolysis. The bath temperature of the plating bath was set to 30°C. In addition, the current supplied to the lining 11 was set to a direct current, and its current density was set to 2.0 A / dm 2 .
[0063] It should be noted that in the plating bath, methanesulfonic acid can be adjusted between 50 and 250 g / L, methanesulfonic acid Bi can be adjusted between 5 and 40 g / L, Sb can be adjusted between 0.1 and 3 g / L, and the organic surfactant can be adjusted between 0.5 and 50 g / L. In addition, the bath temperature of the plating bath can be adjusted between 20 and 50° C., and the current density supplied to the lining layer 11 can be adjusted between 0.5 and 7.5 A / dm2 By increasing the Sb ion concentration in the plating bath, the Sb concentration in the plating layer 12 can be increased.
[0064] For example, by setting the Sb concentration in the plating bath to 0.2 g / L, Figure 2 The concentration of Sb in the plating bath was set to 0.1 g / L, and the Sb concentration in the plating bath was set to 2 mass %. Figure 2 The concentration of Sb converges to about 1 mass % (circle). It is also known that a concentration gradient of Sb can be achieved by using methanesulfonic acid in the plating bath. When the plating layer 12 is formed in a plating bath using EDTA (ethylenediaminetetraacetic acid) instead of methanesulfonic acid, a concentration gradient of Sb is formed. Figure 2 The plating layer 12 does not have a concentration gradient like the sample C of FIG. However, when methanesulfonic acid is used in the plating bath, a concentration gradient of Sb is not necessarily formed, and a concentration gradient of Sb may be formed as shown in FIG. Figure 3A As shown, the plated layer 12 having no Sb concentration gradient is formed.
[0065] After the plating is performed as described above, the sliding member 1 is washed with water and dried. In this way, the sliding member 1 is completed. Furthermore, two sliding members 1 are combined into a cylindrical shape to form a sliding bearing A, which is mounted on an engine.
[0066] (2) Other implementation methods:
[0067] Table 2 shows the results of fatigue area ratio measurement for a plurality of samples 1 to 8 after varying the film thickness of the plating layer 12 and the Sb concentration on the surface. Figure 6 This is a graph showing the fatigue area ratios of samples 1 to 8. Figure 6 The vertical axis represents the fatigue area ratio, and the horizontal axis represents the Sb concentration on the surface.
[0068] [Table 3]
[0069]
[0070] First, the greater the film thickness of the plating layer 12, the greater the fatigue area ratio. It is conceivable that this is because: regardless of the concentration of Sb, when the film thickness of the plating layer 12 becomes larger, the stress acting on the inside of the plating layer 12 becomes larger. However, it can be confirmed that: by containing Sb in the plating layer 12, the fatigue area ratio can be reduced at any film thickness. Therefore, even if the film thickness of the plating layer 12 is set to 20μm as in the above embodiment, a sliding member 1 with good fatigue resistance can be formed.
[0071] In addition, when comparing fatigue area ratios between films of the same film thickness, the higher the surface Sb concentration, the more the fatigue area ratio can be suppressed. The fatigue area ratio can be suppressed by setting the surface Sb concentration to 1.0 mass % or more and 3.0 mass % or less (ideally 1.7 mass % or more and 2.6 mass % or less).
[0072] In the above embodiment, the sliding member 1 constituting the sliding bearing A for supporting the crankshaft of the engine is exemplified, but the sliding member 1 of the present invention can also be used to form the sliding bearing A for other purposes. For example, the sliding member 1 of the present invention can also be used to form a radial bearing such as a gear bushing or a piston pin bushing / hub bushing for a transmission. Furthermore, the sliding member of the present invention can also be a thrust bearing, various washers, or a swash plate for a car air-conditioning compressor. In addition, the matrix of the lining layer 11 is not limited to a Cu alloy, and the material of the matrix can be selected according to the hardness of the mating shaft 2. In addition, the backing 10 is not necessary and can be omitted. The thickness of the intermediate layer 13 is not limited to 2.0 μm, and can be any thickness between 0.5 and 10.0 μm (ideally 1 to 5.0 μm). By making the thickness of the intermediate layer 13 0.1 μm or more, the possibility of defects such as pinholes in the intermediate layer 13 can be reduced. By making the thickness of the intermediate layer 13 thicker than 1 μm, the diffusion of Cu can be reliably prevented by the intermediate layer 13.
[0073] Description of reference numerals:
[0074] 1. Sliding component; 2. Mating shaft; 10. Backing; 11. Lining; 12. Coating layer; A. Bearing; E. Rectangular area; F. Moving body; H. Test shaft; R. Connecting rod; X. Interface.
Claims
1. A sliding member, characterized in that: The sliding member includes a plating layer formed of an alloy plating film of Bi and Sb, The plated layer is bonded to the lining layer formed of a copper alloy via an intermediate layer containing Ag as a main component. The intermediate layer is formed of Ag-Sn alloy, The thickness of the intermediate layer is 0.1 μm or more and 2.0 μm or less. The thickness of the plating layer is not less than 11 μm and not more than 20 μm, The Sb concentration on the surface of the plating layer is 1.7 mass % or more and 2.6 mass % or less.