Device and method for measuring intracrystalline diffusion coefficient of porous materials by zero-length column method
By using the zero-long column method in porous materials, using thin layer adsorbent and forced-flow carrier gas, the problems of complexity and error in the experimental device in the prior art are solved, and high-precision in-crystal diffusion coefficient measurement is achieved, which simplifies the The experimental process was carried out and the determination accuracy was improved.
Patent Information
- Application Number
- CN202011014183.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-09-24
AI Technical Summary
The existing methods for measuring the in-crystal diffusion coefficient of adsorbents in porous materials have problems such as complex experimental equipment, difficult loading of adsorbents, difficult temperature control, and large influence of external mass transfer, resulting in large experimental errors.
Using the zero-long column method, the influence of mass transfer and heat transfer on the outer surface is reduced by setting a very thin adsorbent layer and forced flowing carrier gas in the adsorption and desorption chamber, and the gas chamber system, adsorption and desorption system and data are used. The acquisition and processing system determines the intra-crystal diffusion coefficient and solves the diffusion time constant through mathematical models to obtain the accurate diffusion coefficient.
The experimental device is simplified, the amount of adsorbent is used is reduced, the impact of external mass transfer and heat transfer on the experimental results is reduced, the determination accuracy is improved, and the intra-crystal diffusion coefficient value is obtained with high precision.
Smart Images

Figure CN111999218B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a device and method for measuring the intracrystalline diffusion coefficient of porous materials, and in particular to a device and method for measuring the intracrystalline diffusion coefficient of porous materials by a zero-length column method, which can be used to measure the intracrystalline diffusion coefficient of adsorbate in porous materials. Background Art
[0002] As a low-energy separation technology, adsorption separation has received more and more attention in the fields of chemical engineering and environmental protection. The adsorption or desorption process of adsorbates inside the adsorbent material mainly includes three processes: intracrystalline diffusion process, intercrystalline diffusion, and transfer process with the external airflow body. When the resistance of other diffusion processes is much smaller than the resistance of the intracrystalline diffusion process, the entire adsorption (desorption) process can be regarded as controlled by the intracrystalline diffusion process, and the measured diffusion coefficient is called the intracrystalline diffusion coefficient. In the study of adsorption separation, determining the intracrystalline diffusion coefficient of the adsorbate in the adsorbent is a crucial research content. Studying the intrinsic reaction kinetics of multiphase reactions and designing multiphase reactors also requires knowing the intracrystalline diffusion coefficient of the reaction molecules inside the catalyst, which is an important parameter for studying the mass transfer process inside porous materials.
[0003] The study of intracrystalline diffusion coefficient is a relatively difficult task. At present, the main methods for determining intracrystalline diffusion coefficient include adsorption uptake method (including weight method and volume method), frequency response method, time lag method and pulse gradient field nuclear magnetic resonance method. These methods have the following main problems: (1) The experimental device is relatively complex and it is difficult to load the adsorbent; (2) The experimental temperature conditions are difficult to control; (3) It is greatly affected by external mass transfer, heat transfer and axial diffusion, which easily leads to experimental errors. Summary of the invention
[0004] In view of the technical problems existing in the measurement of intracrystalline diffusion coefficient, the object of the present invention is to provide a device for measuring the intracrystalline diffusion coefficient of porous materials using a zero-length column method.
[0005] Another object of the present invention is to use the device to measure the intracrystalline diffusion coefficient.
[0006] The basic principle of the zero-length column method is to reduce the influence of mass transfer and heat transfer on the outer surface by introducing a very thin (thickness close to 0) adsorbent layer (column) and using a forced flow of carrier gas. When the zero-length column method is used to determine the intracrystalline diffusion coefficient, the resistance of other diffusion processes is much smaller than the intracrystalline diffusion resistance, so the entire adsorption (desorption) process can be regarded as the control of the intracrystalline diffusion process.
[0007] The basic theoretical model of the zero-length column method is as follows: Assume that the adsorbent particles are spheres of uniform shape, the entire adsorption-desorption process is carried out under isothermal conditions, the diffusion of adsorbate molecules in the pores conforms to Fick's law and adsorption occurs in the linear region. Based on the above assumptions, the diffusion equation expressed in terms of the relative concentration of the effluent can be expressed as follows:
[0008]
[0009] where β n Determined by the following equation:
[0010] β n cotβ n +L-1=0#(2)
[0011] L is determined by the following formula:
[0012]
[0013] Where F is the carrier gas flow rate, mL / min; K is the Henry coefficient, dimensionless; V s is the volume of adsorbent, m 3 ; R is the adsorbent particle size, m. Therefore, the diffusion time constant can be obtained by combining the above equations (1), (2), and (3): Then the intracrystalline diffusion coefficient D is calculated.
[0014] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0015] A device for determining the intracrystalline diffusion coefficient of porous materials by a zero-length column method comprises a gas chamber system, an adsorption-desorption system and a data acquisition and processing system, wherein the adsorption-desorption system comprises a vaporization chamber, an adsorption-desorption chamber and a detection chamber in sequence in the direction of carrier gas flow, wherein the vaporization chamber is an adsorbate loading chamber, and the adsorption-desorption chamber is composed of a blank chamber and a measuring chamber connected in parallel, wherein the blank chamber is not filled with an adsorbent for a blank experiment, and the measuring chamber is filled with a porous material for measuring the intracrystalline diffusion coefficient; the adsorption-desorption chamber comprises a coaxial variable diameter cylindrical cavity, wherein the carrier gas flows along the axial direction, and the cavity contains two overlapping circular carriers, wherein the carriers are porous materials, and an adsorbent layer is filled between the carriers, wherein the carrier diameter is slightly smaller than the large cylindrical cavity, and the carrier is loaded into the large cylindrical cavity to the variable diameter, and the other end is screwed into an inner nut to be tightened in a threaded manner.
[0016] In the device of the present invention, the carrier is loaded into a large cylindrical cavity, and an internal thread is provided on one side of the cavity at a diameter change point, and an internal nut is provided with an external thread. When the carrier is loaded into the large cylindrical cavity to the diameter change point, the other end is screwed into the internal nut to fix the carrier and the adsorbent at the diameter change point in a threaded manner. After tightening, the thinnest possible adsorbent layer can be obtained, which is close to the state of "zero length column" and ensures the stability of the adsorbent layer during the measurement process.
[0017] Furthermore, both ends of the adsorption-desorption chamber cavity are connected to the gas pipe via external threads and nuts.
[0018] Furthermore, the two circular carriers are composed of a flat circular bottom carrier with a smaller diameter and a flat disc-shaped cover carrier with a larger diameter, the adsorbent is mounted on the surface of the bottom carrier, and the cover carrier is tightly fastened to the bottom carrier. With this structure, the adsorbent is not easily blown away by the carrier gas.
[0019] The carrier sheet is made of porous metal material.
[0020] Furthermore, the detection chamber is equipped with a hydrogen flame ionization detector (FID).
[0021] Furthermore, the gas chamber system includes a nitrogen cylinder. The nitrogen cylinder is used as a carrier gas and a purge gas supply for the device of the present invention; the carrier gas and the purge gas are switched by a three-way valve. It can also include a hydrogen cylinder and an air cylinder (using FID), which are used as a fuel gas supply for the detection chamber FID in the adsorption and desorption system.
[0022] Furthermore, the data acquisition and processing system includes an amplifier and a recorder, and the recorder uses a computer-installed data acquisition on-line / offline workstation to record data.
[0023] The present invention also relates to an experimental method for measuring the intracrystalline diffusion coefficient of porous materials using the above-mentioned zero-length column method device, the steps comprising: (1). Spreading the accurately weighed porous material flat between the carriers and loading it into the measuring chamber, tightening it to form a thin layer, and loading the adsorbent into the vaporization chamber. (2). Opening the gas source of the gas chamber system (nitrogen, hydrogen and air cylinder valves), connecting the adsorption and desorption system and the power supply of the data acquisition and processing system. (3). Adjusting the set temperature of the adsorption and desorption system to the temperature to be measured, opening the detection chamber, adjusting the device to the adsorption state, measuring the blank chamber and the measuring chamber in turn, and starting data acquisition. (4). After the adsorption is stable, measuring the carrier gas flow rate. (5). After achieving complete adsorption, adjusting the device to the desorption state, when the vertical coordinate of the time response curve returns to zero or approaches zero and is a stable straight line, it means that the desorption is complete. (6). Obtaining the time-voltage response data on the data acquisition and processing system, normalizing the time-voltage response data, and using MATLAB to establish a mathematical model to obtain the measured intracrystalline diffusion coefficient value.
[0024] When processing experimental data, first normalize the time-voltage response data obtained by the data acquisition online workstation. Take the desorption separation mutation point time point as the 0 time point, and normalize the voltage data. The processing formula is as follows:
[0025]
[0026] Where X0 is the voltage value at time 0, X1 is the voltage value at the end of desorption, and X m is the voltage value at each time point. The above voltage values are all in mV.
[0027] After normalization, select 30-50 groups of data in a suitable range and import them into the MATLAB program, and use nonlinear least squares fitting to perform parameter fitting on equations (1) to (3). and L as fitting parameters, given and the initial value of L, substitute L into formula (2) to obtain a series of β1, β2, …, βn, and then convert the experimental data (relative concentration of effluent, i.e. X in equation (4)), t and L and β1, β2, ..., βn are substituted into equation (1), and the parameters are fitted using the lsqcurvefit function to obtain the diffusion time constant: and L value. The obtained diffusion time constant Substitute the L value and experimental data into formula (1) to obtain the relative concentration The relative concentrations were calculated based on the fitted values. Plot the experimental value and the fitted value against time t, and observe the degree of fit of the fitted curve to the experimental curve to determine the diffusion time constant obtained. and L value accuracy to meet the pre-set standards.
[0028] The beneficial effects of the present invention are as follows: (1). The experimental device is simple, and the adsorbent can be easily loaded and used in small amounts; (2). The adsorption-desorption chamber adopts a structure in which a blank chamber and a measuring chamber are connected in parallel. The adsorption-desorption chamber used for the blank experiment and the adsorption-desorption chamber used for measuring the diffusion coefficient can be switched through a three-way valve, which is convenient for blank correction and avoids repeated disassembly and assembly of the adsorption-desorption chamber; (3). The adsorption-desorption chamber adopts a variable diameter structure, so that the circular metal carrier and the adsorbent can be fully fixed in the adsorption-desorption chamber; (4). Two circular metal carriers can be tightly buckled to form a closed space to obtain an adsorbent layer that is as thin as possible, close to a "zero length column" state, and ensure the stability of the adsorbent layer during the measurement process, avoiding the loss of the adsorbent due to the carrier gas; (5). It can better eliminate the influence of external mass transfer, heat transfer and axial diffusion on the experimental results.
[0029] The device and method of the present invention are simpler than other measurement methods and devices, and the required amount of adsorbent is only on the order of tens of milligrams, which is less than that of other methods. Due to the introduction of a very thin adsorbent layer (column) and the use of forced flow of carrier gas, the influence of mass transfer, heat transfer and axial diffusion on the experimental results can be greatly reduced, and the measured intracrystalline diffusion coefficient value has a high accuracy. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of the device structure for determining the intracrystalline diffusion coefficient of porous materials using the zero-length column method;
[0031] Among them, 1. Nitrogen cylinder; 2. Hydrogen cylinder; 3. Air cylinder; 4. Nitrogen flow regulating valve; 5. Hydrogen flow regulating valve; 6. Air flow regulating valve; 7. Nitrogen stop valve; 8. Hydrogen stop valve; 9. Air stop valve; 10. Three-way valve; 11. Vaporization chamber; 12. Discharge port; 13, 14. Three-way valve; 15. Blank chamber; 16. Measuring chamber; 17. Detector; 18. Vent port; 19. Amplifier; 20. Recorder.
[0032] Figure 2 Schematic diagram of the adsorption-desorption chamber structure;
[0033] Among them, 31. carrier sheet; 32. inner nut;
[0034] Figure 3 Schematic diagram of the metal carrier, (a) top view, (b) cross-sectional view along line AA in Figure a;
[0035] Among them, 41. cover slide; 42. bottom slide;
[0036] Figure 4 Scanning electron microscope image of the metal slide surface;
[0037] Figure 5 Fitting curve of ethanol-HKUST-1 system at 20℃;
[0038] Figure 6 Fitting curve of ethanol-HKUST-1 system at 30℃;
[0039] Figure 7 Fitting curve of ethanol-HKUST-1 system at 40℃;
[0040] Figure 8 Fitting curve of acetone-NaA system at 20℃;
[0041] Fig. 9 Fitting curve of acetone-NaA system at 30℃;
[0042] Fig.10 Fitting curve of acetone-NaA system at 40℃. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. It should be understood that the specific implementation methods described below are only used to explain the present invention and are not intended to limit the present invention. The protection scope of the present invention is not limited by the specific implementation methods and is determined by the claims.
[0044] Example 1
[0045] like Figure 1 As shown, the device for determining the intracrystalline diffusion coefficient of porous materials by the zero-length column method of the present invention includes a gas chamber system, an adsorption-desorption system, and a data acquisition and processing system. Among them, the gas chamber system is composed of three gas cylinders, namely, a nitrogen cylinder 1, a hydrogen cylinder 2 and an air cylinder 3. The nitrogen cylinder 1 is used as the carrier gas and purge gas supply of the device; the hydrogen cylinder 2 and the air cylinder 3 are used as the fuel gas supply of the detection chamber 17 in the adsorption-desorption system. The flow rates of nitrogen, hydrogen and air can be adjusted by flow regulating valves 4, 5, and 6. The adsorption-desorption system consists of three parts: a vaporization chamber 11, adsorption-desorption chambers 15 and 16, and a detection chamber 17. The vaporization chamber 11 is an adsorbate loading chamber. When replacing the adsorbate, the upper cover of the vaporization chamber 11 and the lower discharge port 12 are opened to replace the adsorbate; the adsorption and desorption chambers 15 and 16 are connected to the vaporization chamber 11 and the detection chamber 17 through nuts and gas pipes, and the carrier gas containing the adsorbate and the purge gas (pure carrier gas) are switched through the three-way valve 10 to achieve the switching of adsorption and desorption; the detection chamber 17 is equipped with a hydrogen flame ionization detector (FID), which uses high-purity hydrogen and air from the hydrogen bottle 2 and the air bottle 3 for combustion detection. The data processor includes an amplifier 19 and a recorder 20, and the recorder 20 uses a computer-installed data acquisition on / offline workstation to record data.
[0046] In the above device, the adsorption and desorption chambers 15 and 16 are composed of a blank chamber 15 and a measuring chamber 16 connected in parallel, wherein the blank chamber 15 is used for a blank experiment without adsorbent, and the measuring chamber 16 is used for measuring the intracrystalline diffusion coefficient with adsorbent, and the two can be switched by three-way valves 13 and 14.
[0047] The structural diagram of the adsorption and desorption chambers 15 and 16 is shown in FIG. Figure 2 As shown, it includes a coaxial variable diameter cylindrical cavity, the carrier gas flows along the axial direction, the cavity contains two overlapping circular carriers 31, an adsorbent layer is filled between the carriers 31, the diameter of the carrier 31 is slightly smaller than the large cylindrical cavity, the carrier 31 is inserted into the large cylindrical cavity to the variable diameter position, the variable diameter position is provided with an internal thread on one side of the cavity, and the other end is screwed into the internal nut 32, the internal nut 32 is provided with an external thread, the carrier and the adsorbent are fixed at the variable diameter position in a threaded manner, after tightening, the thinnest possible adsorbent layer can be obtained, close to the state of "zero length column".
[0048] Two circular metal carriers 31 are composed of a flat circular bottom carrier 42 with a smaller diameter and a flat disc-shaped cover carrier 41 with a larger diameter. The schematic diagram of the structure is shown in FIG. Figure 3 As shown, the adsorbent is mounted on the surface of the bottom carrier 42, and the cover carrier 41 is tightly fastened with the bottom carrier 42. After fastening, the thinnest possible adsorbent layer can be obtained, and the stability of the adsorbent layer during the measurement process can be ensured so that the adsorbent is not easily blown away by the carrier gas.
[0049] The carrier sheet is made of porous metal material, and its surface scanning electron microscope image is as follows Figure 4 From the scanning electron microscope image, it can be seen that there are a large number of three-dimensional interconnected pore structures distributed on the carrier, which has good ventilation performance. At the same time, the size of the pores inside the carrier is small enough relative to the diameter of the adsorbent particles, so that the adsorbent will not enter the pores inside the carrier or be blown away along the pores by the carrier gas.
[0050] The method for measuring the intracrystalline diffusion coefficient of porous materials using the above-mentioned zero-length column method device comprises the following steps: (1) accurately weighing a certain mass of adsorbent using an electronic balance, fixing the weighed adsorbent on two dry and clean experimental slides and loading them into the measuring chamber 16, and loading a certain amount of adsorbate into the vaporization chamber 11. (2) opening the valves of nitrogen, hydrogen and air cylinders, connecting the adsorption and desorption system and the power supply of the terminal computer of the data acquisition and processing system. (3) adjusting the set temperature of the adsorption and desorption system to the temperature to be measured, igniting the FID, adjusting the three-way valve 10 to the adsorption state, measuring the blank chamber and the measuring chamber in turn, and selecting data acquisition on the computer data acquisition online workstation. (4) after the adsorption is stable, measuring the carrier gas (purge gas) flow rate using a gas flow meter. (5) after achieving complete adsorption, adjusting the three-way valve 10 to the desorption state, and when the vertical coordinate of the time response curve returns to zero or approaches zero and is a stable straight line, it means that the desorption is complete. (6) Save the experimental data as a text document on the terminal computer recorder to obtain the time-voltage response data. (7) Disconnect the power supply of the adsorption-desorption system and the data acquisition terminal computer, open the vaporization chamber 11 and the discharge port 12, and end the experiment when no liquid flows out of the discharge port 12 and the residual liquid in the vaporization chamber 11 is naturally dried. (8) Normalize the time-voltage response data obtained in (6), and use MATLAB to establish a mathematical model to obtain the measured intracrystalline diffusion coefficient value.
[0051] Example 2 Measurement of the intracrystalline diffusion coefficient of ethanol in HKUST-1 type MOF material at different temperatures (20°C, 30°C and 40°C) using the zero-length column method
[0052] Experimental setup Figure 1, Experimental methods and steps: (1). Accurately weigh 10 mg of HKUST-1 material with an electronic balance, spread the weighed HKUST-1 material on two dry and clean experimental slides and load it into the adsorption-desorption chamber 16, adjust the three-way valves 13 and 14 to the measurement state, and inject 200 mL of ethanol into the vaporization chamber 11. (2). Open the valves of nitrogen, hydrogen and air cylinders, and connect the power of the adsorption-desorption system and the terminal computer of the data acquisition and processing system. (3). Adjust the set temperature of the adsorption-desorption system to 20°C, ignite the FID, adjust the three-way valve 10 to the adsorption state, measure the blank chamber and the measurement chamber in turn, and select data acquisition on the computer data acquisition online workstation. (4). After the adsorption is stable, use a gas flow meter to measure the carrier gas (purge gas) flow rate, and the measured flow rate is 108 mL / min. (5). After achieving complete adsorption, adjust the three-way valve 10 to the desorption state. When the vertical coordinate of the time response curve returns to zero or approaches zero and becomes a stable straight line, it means that the desorption is complete. (6). Save the experimental data as a text document on the terminal computer recorder to obtain the time-voltage response data. (7). Adjust the set temperature of the adsorption-desorption system to 30°C, wait for the display temperature to stabilize to the set temperature, and then start the next set of experiments. (8). After all three sets of experiments are completed, disconnect the power supply of the adsorption-desorption system and the terminal computer, close the gas circuit control valve, open the vaporization chamber 11 and the discharge port 12, and end the experiment when no liquid flows out of the discharge port 12 and the residual liquid in the vaporization chamber 11 is naturally dried. (9). Import the time-voltage response data obtained in (6) into an Excel table for normalization, and use MATLAB to establish a mathematical model for data processing to obtain the value of the intracrystalline diffusion coefficient.
[0053] When processing experimental data, the time-voltage response text data obtained by the data acquisition online workstation is first normalized. First, the desorption separation mutation point is found, and then the time point is taken as the zero time point, and the voltage data is normalized using formula (4).
[0054] After normalization, select 30-50 appropriate data sets and import them into the dat file of the prepared MATLAB program. The present invention uses nonlinear least squares fitting to perform parameter fitting on equations (1) to (3), setting the initial value of L to 1.5 and the diffusion time constant to The initial value is 0.58. Substituting L into formula (2) can obtain a series of β1, β2, ..., βn. Substitute t and L and β1, β2, …, βn into equation (1) and use lsqcurvefit function to fit the parameters to obtain the diffusion time constant. and L value. The obtained diffusion time constant Substitute the L value and experimental data into formula (1) to obtain the relative concentration The relative concentrations were calculated based on the fitted values. Plot the experimental value and the fitted value against time t, and observe the degree of fit of the fitted curve to the experimental curve to determine the diffusion time constant obtained. The accuracy of the L value. The intracrystalline diffusion coefficient D can be finally obtained through the diffusion time constant.
[0055] According to the above data processing method, the fitting curves of ethanol in HKUST-1 at different temperatures are as follows: Figure 5 — Figure 7 As shown in the figure, it can be seen that in the initial stage of desorption, the concentration of the adsorbate in the desorption curves at all temperatures decreases rapidly, and then gradually slows down, indicating that the diffusion of ethanol in HKUST-1 is a process controlled by intracrystalline diffusion; the experimental value and the fitting curve fit well, indicating that the measured diffusion time constant The value is more accurate. The diffusion time constants measured at three temperatures The values of and L are shown in Table 1. As can be seen from the table, as the temperature increases, the diffusion time constant It also gradually increases, which satisfies the rule that when other conditions are the same, the intracrystalline diffusion coefficient of the same adsorbate and the same adsorbent increases with increasing temperature, which further illustrates the reliability of the experimental data obtained by this experimental method.
[0056] Table 1 Diffusion data of ethanol-HKUST-1 system
[0057]
[0058] Example 3 Measurement of the intracrystalline diffusion coefficient of acetone in NaA molecular sieve at different temperatures (20°C, 30°C and 40°C) using the zero-length column method
[0059] Experimental setup Figure 1, Experimental methods and steps: (1). Accurately weigh 10 mg of NaA molecular sieve using an electronic balance, spread the weighed NaA molecular sieve flat on two dry and clean experimental slides and load it into the adsorption-desorption chamber 16, adjust the three-way valves 13 and 14 to the measurement state, and inject 200 mL of acetone into the vaporization chamber 11. (2). Open the valves of nitrogen, hydrogen and air cylinders, and connect the adsorption-desorption system and the terminal computer recorder power supply. (3). Adjust the set temperature of the adsorption-desorption system to 20°C, ignite the FID, adjust the three-way valve 10 to the adsorption state, measure the blank chamber and the measurement chamber in turn, and select data acquisition on the computer adsorption-desorption system online workstation. (4). After the adsorption is stable, use a gas flow meter to measure the carrier gas (purge gas) flow rate, and the measured flow rate is 108 mL / min. (5). After achieving complete adsorption, adjust the three-way valve 10 to the desorption state, and wait until the vertical coordinate of the time response curve returns to zero or tends to zero and is a stable straight line, indicating that the desorption is complete. (6). Save the experimental data as a text document on the terminal computer recorder to obtain the time-voltage response data. (7). Adjust the set temperature of the adsorption-desorption system to 30°C, wait for the display temperature to stabilize to the set temperature, and then start the next set of experiments. (8). After all three sets of experiments are completed, disconnect the power supply of the adsorption-desorption system and the terminal computer, close the gas circuit control valve, open the vaporization chamber 11 and the discharge port 12, and end the experiment when no liquid flows out of the discharge port 12 and the residual liquid in the vaporization chamber 11 is naturally dried. (9). Import the time-voltage response data obtained in (6) into an Excel spreadsheet for normalization, and use MATLAB to establish a mathematical model for data processing to obtain the value of the intracrystalline diffusion coefficient.
[0060] When processing experimental data, the time-voltage response text data obtained by the data acquisition online workstation is first imported into an Excel spreadsheet for normalization. First, the desorption separation mutation point is found, and then the voltage data is normalized using formula (4) with this time point as the zero time point.
[0061] After normalization, select 30-50 groups of data in a suitable range and import them into the dat file of the prepared MATLAB program. The present invention uses nonlinear least squares fitting to perform parameter fitting on equations (1) to (3), setting the initial value of L to 1.5 and the diffusion time constant to The initial value is 0.58. Substituting L into formula (2) can obtain a series of β1, β2, ..., βn. Substitute t and L and β1, β2, …, βn into equation (1) and use lsqcurvefit function to fit the parameters to obtain the diffusion time constant. and L value. The obtained diffusion time constant Substitute the L value and experimental data into formula (1) to obtain the relative concentration The relative concentrations were calculated based on the fitted values. Plot the experimental value and the fitted value against time t, and observe the degree of fit of the fitted curve to the experimental curve to determine the diffusion time constant obtained. The accuracy of the L value. The intracrystalline diffusion coefficient D can be finally obtained through the diffusion time constant.
[0062] According to the above data processing method, the fitting curves of acetone in NaA molecular sieve at different temperatures are as follows: Figure 8 — Fig.10 As shown in the figure, it can be seen that in the initial stage of desorption, the concentration of the adsorbate in the desorption curve at all temperatures decreases rapidly, and then gradually slows down, indicating that the diffusion of acetone in the NaA molecular sieve is a process controlled by intracrystalline diffusion; the experimental value and the fitting curve fit well, indicating that the measured diffusion time constant The value is more accurate. The diffusion time constants measured at three temperatures The values of and L are shown in Table 2. As can be seen from the table, as the temperature increases, the diffusion time constant It also gradually increases, which satisfies the rule that when other conditions are the same, the intracrystalline diffusion coefficient of the same adsorbate and the same adsorbent increases with increasing temperature, which further illustrates the reliability of the experimental data obtained by this experimental method.
[0063] Table 2 Diffusion data of acetone-NaA system
[0064]
Claims
1. A device for determining the intracrystalline diffusion coefficient of porous materials by zero-length column method, comprising a gas chamber system, an adsorption-desorption system and a data acquisition and processing system, characterized in that: The adsorption-desorption system comprises a vaporization chamber (11), an adsorption-desorption chamber and a detection chamber (17) in sequence in the direction of carrier gas flow, wherein the vaporization chamber (11) is an adsorbate loading chamber, and the adsorption-desorption chamber is composed of a blank chamber (15) and a measuring chamber (16) connected in parallel, wherein the blank chamber (15) is not filled with adsorbent for blank experiments, and the measuring chamber (16) is filled with porous materials for measuring intracrystalline diffusion coefficients; the adsorption-desorption chamber comprises a coaxial variable diameter cylindrical cavity, wherein the carrier gas flows in the axial direction, and the cavity contains two superimposed A circular carrier (31), wherein the carrier (31) is made of a porous metal material, an adsorbent layer is filled between the carriers (31), the diameter of the carrier (31) is slightly smaller than the large cylindrical cavity, and the carrier (31) is inserted into the large cylindrical cavity to the diameter change point, and the other end is screwed into the inner nut (32) to be tightened in a threaded manner; the carrier (31) is composed of a flat circular bottom carrier (42) with a smaller diameter and a flat disc-shaped cover carrier (41) with a larger diameter, the adsorbent is installed on the surface of the bottom carrier (42), and the cover carrier (41) is tightly fastened with the bottom carrier (42); The gas chamber system comprises a nitrogen bottle (1) for supplying carrier gas and purge gas; the carrier gas and purge gas are switched via a three-way valve (10).
2. The device for measuring the intracrystalline diffusion coefficient of porous materials by the zero-length column method according to claim 1, characterized in that: The two ends of the adsorption-desorption chamber cavity are connected to the gas transmission pipe through external threads and nuts.
3. The device for measuring the intracrystalline diffusion coefficient of porous materials by the zero-length column method according to claim 1, characterized in that: The detection chamber (17) is equipped with a hydrogen flame ionization detector.
4. The device for measuring the intracrystalline diffusion coefficient of porous materials by the zero-length column method according to claim 1, characterized in that: The data acquisition and processing system comprises an amplifier (19) and a recorder (20), wherein the recorder (20) is a data acquisition on-line / off-line workstation installed by a computer.
5. A method for measuring the intracrystalline diffusion coefficient of a porous material using the device described in claim 1, comprising the following steps: (1). Spreading the accurately weighed porous material between the carrier sheets (31) and placing it in the measuring chamber (16), tightening it to form a thin layer, and placing the adsorbate in the vaporization chamber (11); (2). Turning on the gas source of the gas chamber system, connecting the adsorption and desorption system and the power supply of the data acquisition and processing system; (3). Adjusting the set temperature of the adsorption and desorption system to the temperature to be measured, opening the detection chamber, adjusting the device to the adsorption state, measuring the blank chamber (15) and the measuring chamber (16) in turn, and starting data acquisition; (4). After the adsorption is stable, measuring the carrier gas flow rate; (5). After achieving complete adsorption, adjusting the device to the desorption state, and when the vertical coordinate of the time response curve returns to zero or approaches zero and is a stable straight line, it means that the desorption is complete; (6). Obtaining the time-voltage response data on the data acquisition and processing system, normalizing the time-voltage response data, and using MATLAB to establish a mathematical model to obtain the measured intracrystalline diffusion coefficient value.
6. The method for measuring the intracrystalline diffusion coefficient of porous materials according to claim 5, characterized in that: The method of step (6) comprises the following specific steps: (1) Normalization of time-voltage response data: Taking the desorption separation mutation point as the time point 0, the voltage data is normalized. The processing formula is as follows: Where X0 is the voltage value at time 0, X1 is the voltage value at the end of desorption, and X m is the voltage value at a certain point in time, and the unit of the above voltage value is mV; X is the dimensionless value after the voltage value is normalized, and its value is between 0 and 1; (2) After normalization, select 30-50 groups of data and import them into the MATLAB program, and use nonlinear least squares fitting to perform parameter fitting on equations (1) to (3); in The relative concentration of the effluent, i.e., X in step (1); D is the intracrystalline diffusion coefficient; β n Determined by the following equation: β n how much n +L-1=0 (2) L is determined by the following formula: Where F is the carrier gas flow rate, mL / min; K is the Henry coefficient, dimensionless; V s is the volume of adsorbent, m 3 ; R is the adsorbent particle size, m; Diffusion time coefficient and L as fitting parameters, given and the initial value of L, substitute L into formula (2) to obtain a series of β1, β2, …, βn, and then convert the experimental data Substitute t and L and β1, β2, …, βn into equation (1) and use lsqcurvefit function to fit the parameters to obtain the diffusion time constant and L value; (3) The obtained diffusion time constant Substitute the L value and the experimental data time t back into formula (1) to calculate the relative concentration The relative concentrations were calculated based on the fitted values. A graph of experimental values and fitted values versus time t is used to test the fit of the fitted curve to the experimental curve until the set standard is met.