A black optical decorative film with nano-laminated structure

Through the black optical decorative film with nano-laminated structure, combined with the principles of optical absorption and refractive, the durability and conductivity of the black optical decorative film in the prior art in high temperature and salt spray environments is solved, and low reflectivity and resistance are achieved Oil stains and impact resistance, suitable for a variety of application scenarios.

CN112026426BActive Publication Date: 2024-12-06DONGGUAN DEPAI PRECISION MACHINERY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011132619.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-21
Publication Date
2024-12-06
Estimated Expiration
2040-10-21

AI Technical Summary

Technical Problem

The existing black optical decorative film is not durable in high temperature and salt spray environments, and has electrical conductivity, which makes it impossible to be used in 5G mobile phones and other fields. It has insufficient oil stain resistance and impact resistance, which affects its service life and optical performance.

Method used

A black optical decorative film with a nano-laminated structure, including substrate, nano-laminated film, impermeable module layer and oil-resistant and stain-resistant anti-fingerprint film layer, is prepared through the principle of optical absorption and refractive. The nano-laminated film is made of induced metal The film layer and the silicon oxide film layer are composed of a magnesium fluoride layer, and the oil-resistant and stain-resistant anti-fingerprint film layer is composed of specific materials, with good self-cleaning performance and anti-bacterial and sterilization capabilities.

Benefits of technology

It has achieved the advantages of low reflectivity in the visible light range, strong oil stain resistance and impact resistance, long service life, suitable for mobile phones, automobiles, hardware, etc., and is non-conductive in the 5G industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112026426B_ABST
    Figure CN112026426B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of optical decorative films, and in particular to a black optical decorative film with a nano-laminated structure, wherein the black optical decorative film with a nano-laminated structure comprises a substrate, a nano-laminated film, an anti-reflection module layer, and an oil-proof, stain-resistant, and anti-fingerprint film layer arranged in sequence from bottom to top. The black optical decorative film has the advantages of low reflectivity in the visible light range, strong resistance to oil stains and impacts, and a long service life, and can be widely used in mobile phone battery back covers, black low-light decorative rings for mobile phone camera protection glasses, mobile phone middle frames, automobiles, various instrument panels, and various hardware parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical decorative films, and in particular to a black optical decorative film with a nano-laminated structure. Background Art

[0002] Black is a popular color in the decoration industry, especially in the mobile phone industry. Although there are many different colored mobile phones, black still accounts for a large proportion of sales. Black exterior accessories are also the mainstream color in life. In addition to chrome plating, the most mainstream color of metal hardware such as stainless steel is also black.

[0003] Black is also the dominant color for decorative parts in the vacuum coating field. Most of the black is made by reactive magnetron sputtering PVD or multi-arc ion plating and chemical vapor deposition (PECVD) of various metals and carbon-containing gases such as methane acetylene. However, the black formed by carbides is due to the use of methane acetylene in the coating process. The film layer contains carbon and hydrogen bonds. It will react chemically with oxygen and water molecules under high temperature and salt spray environments and cannot pass high and low temperature and salt spray tests. Its application in industries with high requirements such as mobile phones and automobiles is limited. In addition, carbides prepared by vacuum coating have a certain conductivity due to the presence of carbon, which will shield radio microwave signals and cannot be used in the field of 5G mobile phones, which have high requirements for radio transmission. The existing black optical decorative films are not resistant to oil and impact, which affects their service life, and their optical properties need to be further improved. Summary of the invention

[0004] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a nano-laminated structure black optical decorative film, which has the advantages of low reflectivity in the visible light range, strong oil resistance and impact resistance, and a long service life. It can be widely used in mobile phone battery back covers, black low-light decorative rings for mobile phone camera protection glass, mobile phone middle frames, automobiles and various instrument panels, and various hardware parts.

[0005] The object of the present invention is achieved through the following technical solution: a nano-laminated structure black optical decorative film, comprising a substrate, a nano-laminated film, an anti-reflection module layer and an oil-proof, stain-resistant and anti-fingerprint film layer arranged in sequence from bottom to top.

[0006] Furthermore, the nano-laminated film includes an induced metal film layer and a silicon oxide film layer arranged in sequence from bottom to top, and the upper surface of the silicon oxide film layer is connected to the lower surface of the anti-reflection module layer.

[0007] Furthermore, there are multiple nano-laminated films, and the multiple nano-laminated films are stacked in sequence.

[0008] Furthermore, the substrate is a glass substrate, a PMMA substrate, a PC plastic substrate or a stainless steel substrate.

[0009] Furthermore, the transition hardening layer is a primer layer or a UV paint layer adhered to the substrate.

[0010] Furthermore, the anti-reflection module layer is a magnesium fluoride layer.

[0011] Furthermore, the anti-reflection module layer includes 2-6 anti-reflection layers stacked sequentially from bottom to top.

[0012] Furthermore, the thickness of the induced metal film layer is 3-6 nm, and the thickness of the silicon oxide film layer is 70-90 nm.

[0013] Furthermore, the thickness of the oil-proof, stain-resistant and anti-fingerprint film layer is 30-100 nm.

[0014] Furthermore, the nano-laminated structure black optical decorative film also includes a transition hardening layer, the lower surface of the transition hardening layer is connected to the upper surface of the substrate, and the upper surface of the transition hardening layer is connected to the lower surface of the nano-laminated film.

[0015] Furthermore, the oil-proof, stain-resistant and anti-fingerprint film layer includes a base layer and a protective layer coated on the upper surface of the base layer, and the material for the protective layer includes the following raw materials in parts by weight:

[0016] 20-26 parts of butyl acrylate, 12-16 parts of acrylic acid, 6-14 parts of lauryl methacrylate, 6-10 parts of melamine formaldehyde resin, 18-26 parts of nano titanium dioxide, 5-9 parts of nano calcium fluoride, 3-5 parts of vinyl trimethoxy silane, 12-18 parts of isopropyl alcohol, 2-4 parts of perfluoropolyether, 0.5-1 part of dimethyl azobisisobutyrate. The perfluoropolyether is preferably, but not limited to, DuPont krytox GPL 227. The melamine formaldehyde resin is preferably, but not limited to, CYMEL 1123 highly alkyl etherified benzoguanamine resin. The substrate layer is preferably, but not limited to, a PET layer.

[0017] The materials used in the oil-proof, stain-resistant and anti-fingerprint film layer of the present invention are prepared by combining PET resin, melamine formaldehyde resin, butyl acrylate, acrylic acid, lauryl methacrylate, 14-22 parts of nano titanium dioxide, nano oxide, vinyl trimethoxysilane, etc., and the raw materials have good compatibility, which can prevent the nano titanium dioxide particles from settling and agglomerating with the pure water contact angle of the present embodiment, so as to form a stable oil-proof, stain-resistant and anti-fingerprint film layer. The prepared oil-proof, stain-resistant and anti-fingerprint film layer has excellent self-cleaning performance, stain resistance and antibacterial and bactericidal ability, good light transmittance, good bonding with the substrate layer, and good hydrophobicity. The pure water contact angle θ>100° can further prevent the polluting particles from being deposited or adsorbed on the surface of the oil-proof, stain-resistant and anti-fingerprint film layer, so as to have a long service life and good scratch resistance.

[0018] Furthermore, a packaging protective film is attached to the upper surface of the oil-proof, stain-resistant and anti-fingerprint film layer.

[0019] The beneficial effects of the present invention are as follows: the nano-laminated structure black optical decorative film of the present invention is prepared by the principle of optical absorption and refraction, has the advantages of low reflectivity in the visible light range, strong oil resistance and impact resistance, long service life, and can be widely used in mobile phone battery back covers, mobile phone camera protection glass black low-light decorative rings, mobile phone middle frames, automobiles and various instrument panels and various hardware, etc., and has strong practicality. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a partial cross-sectional schematic diagram of Example 1.

[0021] Figure 2 This is the visible light reflection characteristic curve of the black optical decorative film with nano-laminated structure without packaging protection film in Example 5.

[0022] The accompanying drawings are marked as follows: 1—substrate, 2—transition hardening layer, 3—nano-laminated film, 4—anti-reflection module layer, 5—oil-proof, stain-resistant and anti-fingerprint film layer, and 6—packaging protective film. DETAILED DESCRIPTION

[0023] In order to facilitate the understanding of those skilled in the art, the following embodiments and attached Figure 1 The present invention is further described, and the contents mentioned in the implementation modes are not intended to limit the present invention.

[0024] In a typical embodiment of the present application, a nano-laminated structure black optical decorative film comprises a substrate 1, a nano-laminated film 3, an anti-reflection module layer 4 and an oil-proof, stain-resistant and anti-fingerprint film layer 5 arranged in sequence from bottom to top. The nano-laminated structure black optical decorative film of the present invention is prepared by the principle of optical absorption and refraction, and is not the black color of traditional vacuum sputtering PVD. It has the advantages of adjustable transmittance, low reflectivity in the visible light range, strong resistance to oil stains and impact, and is non-conductive and can be widely used in mobile phone battery back covers, mobile phone camera protection glass black low-light decorative rings, mobile phone middle frames, automobiles and various instrument panels, and various hardware parts.

[0025] In one embodiment, the nano-laminated film 3 includes an induced metal film layer and a silicon oxide film layer arranged in sequence from bottom to top, and the upper surface of the silicon oxide film layer is connected to the lower surface of the anti-reflection module layer 4. The thickness of the induced metal film layer is 3-6nm, and the physical structure is a discontinuous island structure showing non-conductive characteristics. The thickness of the silicon oxide film layer is 70-90nm. The induced metal film layer material of the nano-laminated film 3 can be metals such as chromium, silicon, nickel, gold, tungsten or copper, among which chromium, silicon and germanium have greater absorption of short-wavelength visible light; nickel has greater absorption of long-wavelength visible light, and this characteristic can also be used to manufacture a film layer with color cast characteristics. The silicon oxide film layer can improve the mechanical properties of the nano-laminated film 3 and improve the micro-wear performance of the nano-laminated film 3.

[0026] In one embodiment, the number of the nano-laminated films 3 is multiple, and the multiple nano-laminated films 3 are stacked in sequence. According to the transmittance or the material of the substrate 1, the number of the nano-laminated films 3 in this embodiment is 2-20, and the optical transmittance of the number of the nano-laminated films 3 can select different numbers of film stacks according to the transmittance requirements, so as to meet the requirements of different transmittances. The more the number, the lower the transmittance, and the transmittance of 1.5-25% can be achieved, which can be used to plate a light-reducing film (ND film).

[0027] The nano-laminated structure black optical decorative film of the present invention adopts nanotechnology, has non-conductive properties, and can withstand a voltage of more than 5000 volts. It can be used in the 5G industry with extremely high requirements for conductivity and signal shielding, and can also be used in various home appliances and automobile instrument panels with relevant conductivity and voltage resistance requirements.

[0028] In one embodiment, the substrate 1 is a glass substrate 1, a PMMA (acrylic) substrate 1, a PC plastic substrate 1 or a stainless steel substrate 1. The thickness of the substrate 1 is 1-15 mm. Further, the glass substrate 1 is a K9 optical glass or a Corning glass substrate 1.

[0029] In one embodiment, the nano-laminated structure black optical decorative film further includes a transition hardening layer 2, the lower surface of the transition hardening layer 2 is connected to the upper surface of the substrate 1, and the upper surface of the transition hardening layer 2 is connected to the lower surface of the nano-laminated film 3. The transition hardening layer 2 can improve the adhesion between the substrate 1 and the nano-laminated film 3, and further improve the impact resistance of the nano-laminated structure black optical decorative film, making it less likely to be damaged and extending its service life.

[0030] In one embodiment, the substrate 1 is a PMMA substrate 1, and the transition hardening layer 2 is covered on the upper surface of the substrate 1 by a flow coating or dipping process, and the thickness of the transition hardening layer 2 is 3-10 mm.

[0031] In one embodiment, the transition hardening layer 2 is a primer layer or UV paint layer attached to the substrate 1. This can improve the adhesion between the substrate 1 and the nano-laminated film 3. The primer layer and UV paint layer are commercially available primer layers and UV paint layers, which are used here.

[0032] In one embodiment, the anti-reflection module layer 4 is a single-layer magnesium fluoride layer or includes 2-6 anti-reflection layers stacked sequentially from bottom to top.

[0033] In one embodiment, the anti-reflection module layer 4 is a single-layer magnesium fluoride layer, and the thickness of the magnesium fluoride layer is 90-100nm. The single-layer magnesium fluoride film used in the present invention can be set on the surface of the nano-laminated film 3 as an anti-reflection film, and by setting the thickness of the magnesium fluoride layer, the transmission enhancement is formed, so that the reflectivity is greatly reduced, and the magnesium fluoride layer can be prevented from being too thick to affect the overall performance of the black optical decorative film.

[0034] In one embodiment, the anti-reflection module layer 4 is composed of 2-6 anti-reflection layers stacked in sequence from bottom to top. The anti-reflection layer is made of a high-refractive or low-refractive material. The primer layer and UV paint layer are commercially available primer layers and UV paint layers, which are used here. Through the above arrangement, the transmittance can be enhanced and the reflectivity can be greatly reduced.

[0035] The present invention can obtain products with different transmission colors and reflection colors by adopting the anti-reflection module, the nano-laminated film 3 and the substrate 1 structure and controlling the thickness of each layer.

[0036] In one embodiment, the thickness of the oil-proof, stain-resistant and anti-fingerprint film layer 5 is 30-100nm. The oil-proof, stain-resistant and anti-fingerprint film layer 5 has good acid and alkali resistance and can pass the rigorous high and low temperature resistance and salt spray tests in industries such as mobile phones and automobiles. The oil-proof, stain-resistant and anti-fingerprint film layer 5 can adopt the oil-proof, stain-resistant and anti-fingerprint film layer 5 available on the market, which is only used here. The oil-proof, stain-resistant and anti-fingerprint film layer 5 has been coated on the substrate 1 and covered with the nano-laminated film 3 and the anti-reflection module layer 4, which can avoid oil stains and fingerprints that affect the appearance of the panel during use, and can increase the wear resistance and acid, alkali and salt spray resistance of the film layer.

[0037] In one embodiment, the upper surface of the oil-proof, stain-resistant and anti-fingerprint film layer 5 is attached with a packaging protective film 6. The packaging protective film 6 is retained until the user uses and installs it, mainly to prevent the nano-laminated structure black optical decorative film from being scratched during installation and transportation. Furthermore, the packaging protective film 6 has a thickness of 0.01-0.05 mm, which plays a good protective role.

[0038] Example 1

[0039] In this embodiment, a nano-laminated structure black optical decorative film includes a substrate 1, a nano-laminated film 3, an anti-reflection module layer 4 and an oil-proof, stain-resistant and anti-fingerprint film layer 5 which are arranged in sequence from bottom to top.

[0040] Furthermore, the nano-laminated film 3 includes an induced metal film layer and a silicon oxide film layer arranged in sequence from bottom to top, and the upper surface of the silicon oxide film layer is connected to the lower surface of the anti-reflection module layer 4. The thickness of the induced metal film layer is 4nm, and the thickness of the silicon oxide film layer is 80nm.

[0041] Furthermore, the number of the nano-laminated films 3 is 2, and the two nano-laminated films 3 are stacked in sequence.

[0042] Furthermore, the nano-laminated black optical decorative film also includes a transition hardening layer 2 , the lower surface of the transition hardening layer 2 is connected to the upper surface of the substrate 1 , and the upper surface of the transition hardening layer 2 is connected to the lower surface of the nano-laminated film 3 .

[0043] Furthermore, the substrate 1 is a PMMA substrate 1 , and the transition hardening layer 2 is a UV paint layer adhered to the substrate 1 .

[0044] Furthermore, the anti-reflection module layer 4 is a single-layer magnesium fluoride layer.

[0045] Furthermore, the thickness of the oil-proof, stain-resistant and anti-fingerprint film layer 5 is 50 nm. The upper surface of the oil-proof, stain-resistant and anti-fingerprint film layer 5 is attached with a packaging protective film 6. The thickness of the packaging protective film 6 is 0.04 mm.

[0046] Example 2

[0047] In this embodiment, a nano-laminated structure black optical decorative film includes a substrate 1, a nano-laminated film 3, an anti-reflection module layer 4 and an oil-proof, stain-resistant and anti-fingerprint film layer 5 which are arranged in sequence from bottom to top.

[0048] Furthermore, the nano-laminated film 3 includes an induced metal film layer and a silicon oxide film layer arranged in sequence from bottom to top, and the upper surface of the silicon oxide film layer is connected to the lower surface of the anti-reflection module layer 4. The thickness of the induced metal film layer is 3nm, and the thickness of the silicon oxide film layer is 70nm.

[0049] Furthermore, the number of the nano-laminated films 3 is 3, and the three nano-laminated films 3 are stacked in sequence.

[0050] Furthermore, the substrate 1 is a stainless steel substrate 1. The anti-reflection module layer 4 is a single-layer magnesium fluoride layer.

[0051] Furthermore, the thickness of the oil-proof, dirt-resistant and anti-fingerprint film layer 5 is 100 nm.

[0052] Furthermore, the nano-laminated black optical decorative film also includes a transition hardening layer 2 , the lower surface of the transition hardening layer 2 is connected to the upper surface of the substrate 1 , and the upper surface of the transition hardening layer 2 is connected to the lower surface of the nano-laminated film 3 .

[0053] Furthermore, the upper surface of the oil-proof, stain-resistant and anti-fingerprint film layer 5 is attached with a packaging protection film 6. The packaging protection film 6 has a thickness of 0.03 mm.

[0054] The rest of the contents of this embodiment are the same as those of Embodiment 1 and will not be described again here.

[0055] Example 3

[0056] In this embodiment, a nano-laminated structure black optical decorative film includes a substrate 1, a nano-laminated film 3, an anti-reflection module layer 4 and an oil-proof, stain-resistant and anti-fingerprint film layer 5 which are arranged in sequence from bottom to top.

[0057] Furthermore, the nano-laminated film 3 includes an induced metal film layer and a silicon oxide film layer arranged in sequence from bottom to top, and the upper surface of the silicon oxide film layer is connected to the lower surface of the anti-reflection module layer 4. The thickness of the induced metal film layer is 3nm, and the thickness of the silicon oxide film layer is 70nm.

[0058] Furthermore, the number of the nano-laminated films 3 is 4, and the plurality of nano-laminated films 3 are stacked in sequence.

[0059] Furthermore, the substrate 1 is K9 optical glass. The nano-laminated structure black optical decorative film further comprises a transition hardening layer 2, the lower surface of the transition hardening layer 2 is connected to the upper surface of the substrate 1, and the upper surface of the transition hardening layer 2 is connected to the lower surface of the nano-laminated film 3.

[0060] Furthermore, the transition hardening layer 2 is a base oil layer adhered to the substrate 1 .

[0061] Furthermore, the anti-reflection module layer 4 includes three anti-reflection layers stacked sequentially from bottom to top.

[0062] Furthermore, the thickness of the oil-proof, dirt-resistant and anti-fingerprint film layer 5 is 100 nm.

[0063] Furthermore, the upper surface of the oil-proof, stain-resistant and fingerprint-resistant film layer 5 is attached with a packaging protection film 6. The packaging protection film 6 has a thickness of 0.05 mm.

[0064] The rest of the contents of this embodiment are the same as those of Embodiment 1 and will not be described again here.

[0065] Example 4

[0066] The difference between this embodiment and embodiment 1 is that the induced metal film layer material of the nano-laminated film 3 includes the following elements in parts by weight: 10 parts of copper, 0.2 parts of chromium, 0.1 parts of silicon, 0.25 parts of germanium and 0.2 parts of nickel.

[0067] Further, the oil-proof, stain-resistant and anti-fingerprint film layer 5 includes a base layer and a protective layer coated on the upper surface of the base layer, and the protective layer material includes the following raw materials in parts by weight: 24 parts of butyl acrylate, 14 parts of acrylic acid, 12 parts of lauryl methacrylate, 8 parts of melamine formaldehyde resin, 23 parts of nano titanium dioxide, 6 parts of nano calcium fluoride, 4 parts of vinyl trimethoxysilane, 15 parts of isopropanol, 3 parts of perfluoropolyether, and 0.8 parts of dimethyl azobisisobutyrate. The perfluoropolyether is preferably, but not limited to, DuPont krytox GPL 227. The melamine formaldehyde resin is preferably, but not limited to, CYMEL 1123 highly alkyl etherified benzoguanamine resin. The base layer is preferably, but not limited to, a PET layer.

[0068] The visible light reflection characteristic curve of this embodiment is as follows: Figure 2 As shown, the reflectivity in the visible light range of 400nm-700nm is less than 1%.

[0069] The pure water contact angle of the oil-proof, stain-resistant and anti-fingerprint film layer 5 of this embodiment is 109°, and the contact angle of n-hexadecane is 67°.

[0070] The rest of the contents of this embodiment are the same as those of Embodiment 1 and will not be described again here.

[0071] Example 5

[0072] The difference between this embodiment and embodiment 4 is that the induced metal film layer material of the nano-laminated film 3 includes the following elements in parts by weight: 12 parts of copper, 0.3 parts of chromium, 0.2 parts of silicon, 0.1 parts of germanium and 0.1 parts of nickel.

[0073] Furthermore, the oil-proof, stain-resistant and anti-fingerprint film layer 5 includes a base layer and a protective layer coated on the upper surface of the base layer, and the material of the protective layer includes the following raw materials in parts by weight: 20-26 parts of butyl acrylate, 12-16 parts of acrylic acid, 6-14 parts of lauryl methacrylate, 6-10 parts of melamine formaldehyde resin, 18-26 parts of nano titanium dioxide, 5-9 parts of nano calcium fluoride, 3-5 parts of vinyl trimethoxy silane, 12-18 parts of isopropyl alcohol, 2-4 parts of perfluoropolyether, and 0.5-1 part of dimethyl azobisisobutyrate.

[0074] The rest of the contents of this embodiment are the same as those of Embodiment 4 and will not be described again here.

[0075] The pure water contact angle of the oil-proof, stain-resistant and anti-fingerprint film layer 5 of this embodiment is 111°, and the contact angle of n-hexadecane is 70°.

[0076] Example 6

[0077] The difference between this embodiment and embodiment 1 is that the induced metal film layer material of the nano-laminated film 3 includes the following elements in parts by weight: 10 parts of silver, 0.2 parts of chromium, 0.5 parts of silicon, 0.3 parts of germanium and 0.1 parts of nickel.

[0078] Furthermore, the oil-proof, stain-resistant and anti-fingerprint film layer 5 includes a base layer and a protective layer coated on the upper surface of the base layer, and the material of the protective layer includes the following raw materials in parts by weight: 20-26 parts of butyl acrylate, 12-16 parts of acrylic acid, 6-14 parts of lauryl methacrylate, 6-10 parts of melamine formaldehyde resin, 18-26 parts of nano titanium dioxide, 5-9 parts of nano calcium fluoride, 3-5 parts of vinyl trimethoxy silane, 12-18 parts of isopropyl alcohol, 2-4 parts of perfluoropolyether, and 0.5-1 part of dimethyl azobisisobutyrate.

[0079] The rest of the contents of this embodiment are the same as those of Embodiment 4 and will not be described again here.

[0080] The pure water contact angle of the oil-proof, stain-resistant and anti-fingerprint film layer 5 of this embodiment is 105°, and the contact angle of n-hexadecane is 63°.

[0081] Example 7

[0082] The difference between this embodiment and embodiment 4 is that the oil-proof, stain-resistant and anti-fingerprint film layer 5 includes a base layer and a protective layer coated on the upper surface of the base layer, and the material for the protective layer includes the following raw materials in parts by weight: 20-26 parts of butyl acrylate, 12-16 parts of acrylic acid, 6-14 parts of lauryl methacrylate, 6-10 parts of melamine formaldehyde resin, 18-26 parts of nano titanium dioxide, 5-9 parts of nano calcium fluoride, 3-5 parts of vinyl trimethoxy silane, 12-18 parts of isopropyl alcohol, 2-4 parts of perfluoropolyether, and 0.5-1 part of dimethyl azobisisobutyrate.

[0083] The rest of the contents of this embodiment are the same as those of Embodiment 4 and will not be described again here.

[0084] The pure water contact angle of the oil-proof, dirt-resistant and anti-fingerprint film layer 5 of this embodiment is 114°, and the contact angle of n-hexadecane is 68°.

[0085] Comparative Example 1

[0086] The difference between this comparative example and Example 4 is that the oil-proof, stain-resistant and anti-fingerprint film layer 5 of this comparative example includes a base layer and a protective layer coated on the upper surface of the base layer, and the protective layer material includes the following raw materials in parts by weight: 20-26 parts of butyl acrylate, 12-16 parts of acrylic acid, 6-14 parts of lauryl methacrylate, 6-10 parts of melamine formaldehyde resin, 18-26 parts of nano titanium dioxide, 12-18 parts of isopropyl alcohol, and 0.5-1 parts of dimethyl azobisisobutyrate. The pure water contact angle of the oil-proof, stain-resistant and anti-fingerprint film layer 5 of Comparative Example 1 is 94°, and the contact angle of n-hexadecane is 58°.

[0087] The anti-fingerprint performance of Examples 4-7 was determined by laying the nano-laminated black optical decorative film without the packaging protective film 6 flat, with the 5 layers of the oil-proof, stain-resistant and anti-fingerprint film facing upward, slowly pressing the hard coating surface with a finger, observing the obviousness of the fingerprint, and then wiping it with a non-woven fabric, recording the following four grades, of which A and B were qualified: (A) basically invisible fingerprints; (B) very shallow fingerprints, easy to wipe clean; (C) obvious fingerprints, easy to wipe clean; (D) obvious fingerprints, not easy to wipe clean. Taking a certain black optical decorative film on the market as comparative example 2, for comparison, Examples 4-7 were A, A, B and A respectively; Comparative example 1 was C; Comparative example 2 was C.

[0088] The black optical decorative film of the present invention has the advantages of low reflectivity in the visible light range, strong oil and impact resistance, and long service life. It can be widely used in mobile phone battery back covers, black low-light decorative rings for mobile phone camera protection glass, mobile phone middle frames, automobiles and various instrument panels, and various hardware parts.

[0089] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A black optical decorative film with a nano-laminated structure, characterized in that: It includes a substrate, a nano-laminated film, an anti-reflection module layer, and an oil-proof, stain-resistant, and anti-fingerprint film layer arranged in sequence from bottom to top; The nano-laminated structure black optical decorative film further comprises a transition hardening layer, the lower surface of the transition hardening layer is connected to the upper surface of the substrate, and the upper surface of the transition hardening layer is connected to the lower surface of the nano-laminated film; The nano-laminated film comprises an induced metal film layer and a silicon oxide film layer arranged in sequence from bottom to top, the lower surface of the induced metal film layer is connected to the upper surface of the transition hardening layer, and the upper surface of the silicon oxide film layer is connected to the lower surface of the anti-reflection module layer; the number of the nano-laminated films is multiple, and the multiple nano-laminated films are stacked in sequence; The thickness of the induced metal film layer is 3-6 nm, and the thickness of the silicon oxide film layer is 70-90 nm; The oil-proof, stain-resistant and anti-fingerprint film layer comprises a base layer and a protective layer coated on the upper surface of the base layer. The material for the protective layer comprises the following raw materials in parts by weight: 20-26 parts of butyl acrylate, 12-16 parts of acrylic acid, 6-14 parts of lauryl methacrylate, 6-10 parts of melamine formaldehyde resin, 18-26 parts of nano titanium dioxide, 5-9 parts of nano calcium fluoride, 3-5 parts of vinyl trimethoxy silane, 12-18 parts of isopropyl alcohol, 2-4 parts of perfluoropolyether, and 0.5-1 part of dimethyl azobisisobutyrate.

2. The nano-laminated black optical decorative film according to claim 1, characterized in that: The substrate is a glass substrate, a PMMA substrate, a PC plastic substrate or a stainless steel substrate.

3. The nano-laminated black optical decorative film according to claim 1, characterized in that: The transition hardening layer is a primer layer or a UV paint layer adhered to the substrate.

4. The nano-laminated structure black optical decorative film according to claim 1, characterized in that: The anti-reflection module layer is a magnesium fluoride layer.

5. The nano-laminated black optical decorative film according to claim 1, characterized in that: The anti-reflection module layer includes 2-6 anti-reflection layers stacked sequentially from bottom to top.

6. The nano-laminated black optical decorative film according to claim 1, characterized in that: A packaging protective film is attached to the upper surface of the oil-proof, dirt-resistant and fingerprint-resistant film layer.