Bismuth telluride-based thin film thermoelectric module manufacturing method, thermoelectric module and thermoelectric generator

The manufacturing of short-planar bismuth telluride-based film thermoelectric modules without cavity structures through MEMS micromachining technology and thin film deposition technology has solved the problems of lack of materials and structural complexity of existing thermoelectric modules, and achieved efficient thermoelectric conversion and reduced manufacturing costs. , suitable for a variety of application fields.

CN112038472BActive Publication Date: 2024-11-12SUZHOU UNIV OF SCI & TECH +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202010835425.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-19
Publication Date
2024-11-12
Estimated Expiration
2040-08-19

AI Technical Summary

Technical Problem

The existing thermoelectric modules have problems with lack of material types and structural complexity in improving the thermoelectric conversion efficiency, resulting in high manufacturing costs, insufficient mechanical strength, and difficult to mass production.

Method used

Planar bismuth telluride-based film thermoelectric modules are manufactured using MEMS micromachining technology and thin film deposition technology. By depositing a silicon dioxide film layer, a metal strip on the heat sink substrate and alternately deposition of P-type and N-type bismuth telluride-based films, combined with heat conduction The design of the insulating layer forms a short-planar thin-film thermoelectric generator without a cavity structure.

Benefits of technology

It improves the thermoelectric power density, reduces manufacturing costs, is suitable for the synthetic and preparation of a variety of material systems, and is suitable for portable, wearable and distributed sensor network systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112038472B_ABST
    Figure CN112038472B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for manufacturing a bismuth telluride-based thin film thermoelectric module, a thermoelectric module and a thermoelectric generator. The manufacturing method comprises the following steps: depositing a silicon dioxide film layer on a heat sink substrate; preparing a plurality of spaced metal strips on the silicon dioxide film layer; alternately depositing P-type and N-type bismuth telluride-based thin films on the upper surface of the silicon dioxide film layer between different metal strips to obtain a first semi-finished product; coating a photoresist on the upper surface of the first semi-finished product, and removing the photoresist on part of the metal strips, so that the metal strips from which the photoresist is removed and the metal strips from which the photoresist is not removed are arranged alternately; depositing a metal layer on the metal strips from which the photoresist is removed to obtain a second semi-finished product; coating a photoresist on the upper surface of the second semi-finished product, and removing the photoresist on the metal layer; and depositing a heat-conducting insulating layer on the metal layer from which the photoresist is removed. The present invention realizes the scalability of a planar bismuth telluride-based thin film thermoelectric generator by using MEMS micromachining technology and thin film deposition technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of thermoelectric material power generation, and in particular to a method for manufacturing a planar bismuth telluride-based thin-film thermoelectric module, a thermoelectric module and a thermoelectric generator. Background Art

[0002] Ambient energy harvesting technology is expected to realize the application of portable, wearable and distributed sensor network systems in the Internet of Things society. The available energy sources include sunlight, indoor lighting, radio waves, mechanical vibration and heat. The effective use of thermal energy has been a long-awaited issue, and thermoelectric (TE) generators that use the Seebeck effect to convert temperature differences into electrical energy have also received widespread attention. The energy conversion efficiency generated by TE mainly depends on the advantages of TE materials, ZT = S 2 σT k -1 , where S represents the Seebeck coefficient, σ and k represent the electrical and thermal conductivity, respectively, and T represents the average temperature of the cold and hot sources. Increasing ZT can improve the conversion efficiency, but the correlation between S, σ, and k prevents this. Only a few materials, such as bismuth-telluride and lead-telluride, are known to achieve high conversion efficiency.

[0003] The past two decades have seen an improvement in the fundamental understanding of electrical and thermal transport. This understanding has led to substantial performance enhancements in TE materials with the help of micro- and nano-technologies. Bismuth telluride-based low-dimensional materials have emerged as promising TE candidates due to their ability to maintain low thermal conductivity and high electrical conductance. Bismuth telluride-based TE generators that are highly compatible with MEMS processes and low in contamination (unlike Pb) have also been increasingly fabricated and reported.

[0004] Thermoelectric (TE) phenomenon is also called thermoelectric phenomenon. In 1822, Thomas Seebeck discovered the thermoelectric effect (the principle of power generation of TE materials); in 1834, Jean Peltier discovered the cooling effect at the interface of two conductors of different materials in a current loop (the principle of refrigeration of TE materials). Some good semiconductor TE materials were discovered in the 1950s. Materials with ZT ≥ 0.5 are usually called TE materials. The larger the ZT, the higher the efficiency of the TE device. In order to overcome the obstacle of the lack of high ZT value TE materials, people turned to the structural design of natural TE materials and the development of artificial synthetic TE materials - low-dimensional thermoelectric materials. Mesoscopic physics theoretical research shows that under the same working conditions, low-dimensional thin film structure TE materials have higher ZT values ​​than other bulk materials.

[0005] So far, there are three typical types of low-dimensional thin film TE materials: (1) quantum-dot structures, which use quantum-confinement effects to increase the density of states near the Fermi level, thereby improving the conductivity of the material; (2) phonon-blocking / electron-transmitting superlattices, which reduce the lattice thermal conductivity (kL) of the material by introducing the so-called "acoustic-mismatch" between the superlattice components. Unlike conventional TE alloy materials, materials of this type of structure usually have significantly reduced carrier scattering rates, that is, high conductivity; (3) thin film structure materials that use the thermonic effects in semiconductor heterojunctions to improve the ZT value of the material. Hicks and Dresslhaus proposed that quantum well superlattices can significantly improve the ZT value of the material, and quantum wire superlattices can even bring a greater improvement.

[0006] So far, the main materials are bismuth intermetallic compounds such as bismuth telluride (Bi2Te3), lead telluride (PtTe), zinc antimonide (ZnSb), germanium, iron silicide (FeSi2), etc. Among them, Bi2Te3-based compounds have a large ZT value at relatively low temperatures, which continues to rise from room temperature to about 450K, and are currently the most widely used thermoelectric conversion materials. The research on new low-dimensional TE structural materials has great theoretical and application value. The discovery of high ZT value materials (ZT>4) will trigger a technological revolution in the refrigeration industry, energy industry and semiconductor microelectronics industry. Although quantum dots or superlattice materials can obtain thermoelectric materials with dimensionless merit factors of more than 2, the complex process, high cost and difficulty in mass production of such structural materials limit their application. Therefore, the development of thermoelectric devices with micro-nano structures may be a more realistic way to industrialize the application of thermoelectric materials. In the traditional structure of a planar bismuth telluride-based TE generator, the bismuth telluride-based film is usually suspended on the cavity to cut off the bypass. Although the cavity ensures the temperature difference across the film, its structure weakens the mechanical strength of the device and greatly increases the manufacturing cost. Summary of the invention

[0007] In order to overcome the shortcomings of the prior art, the present invention provides a method for manufacturing a planar bismuth telluride-based thin film thermoelectric module, a thermoelectric module and a thermoelectric generator. The technical solution is as follows:

[0008] In one aspect, the present invention provides a method for manufacturing a planar bismuth telluride-based thin film thermoelectric module, comprising the following steps:

[0009] S1, depositing a silicon dioxide film layer on a heat sink substrate;

[0010] S2, preparing a plurality of metal strips arranged at intervals on the silicon dioxide film layer;

[0011] S3, alternately depositing a P-type bismuth telluride-based film and an N-type bismuth telluride-based film on the upper surface of the silicon dioxide film layer between different metal strips, so that a P-type bismuth telluride-based film is deposited on one side of each metal strip and an N-type bismuth telluride-based film is deposited on the other side, to obtain a first semi-finished product;

[0012] S4, coating a photoresist on the upper surface of the first semi-finished product, and removing the photoresist on a portion of the metal strips, so that the metal strips from which the photoresist is removed and the metal strips from which the photoresist is not removed are arranged alternately;

[0013] S5, depositing a metal layer on the metal strip from which the photoresist has been removed, to obtain a second semi-finished product;

[0014] S6, coating a photoresist on the upper surface of the second semi-finished product, and removing the photoresist on the metal layer deposited in step S5;

[0015] S7. Depositing a thermally conductive insulating layer on the metal layer from which the photoresist has been removed.

[0016] Furthermore, after executing step S7, the method further includes removing the thermally conductive insulating layer deposited outside the metal layer.

[0017] Furthermore, before step S1, the method further includes: performing micro-arc oxidation treatment on the upper and lower surfaces of the heat sink substrate to obtain a ceramic oxide layer, wherein the thickness of the ceramic oxide layer is in the range of 5-15 μm.

[0018] Furthermore, the metal strip has a thickness range of 10-30 μm, a length range of 15-30 mm, and a width range of 0.8-1.2 μm; the P-type bismuth telluride-based film and the N-type bismuth telluride-based film have a thickness range of 30-80 nm, a length range of 0.8-1.2 μm, and a width range of 0.6-0.8 μm.

[0019] Furthermore, the thickness of the silicon dioxide film layer deposited in step S1 is in the range of 80-120 μm, and is obtained by rapidly depositing an amorphous silicon film using a PECVD method and then subjecting the film to wet oxygen high-temperature oxidation; the thickness of the photoresist coated in step S4 and the photoresist coated in step S6 are both in the range of 50-100 μm; the thickness of the metal layer deposited in step S5 is in the range of 50-100 μm; the thickness of the thermally conductive insulating layer in step S7 is in the range of 50-100 μm, and the thermally conductive insulating layer is made of aluminum nitride.

[0020] On the other hand, the present invention provides a planar bismuth telluride-based thin film thermoelectric module, comprising a heat sink substrate, a silicon dioxide film layer, a plurality of first metal strips, a plurality of second metal strips, a bismuth telluride-based thin film, a photoresist and a thermally conductive insulating layer, wherein the silicon dioxide film layer is arranged on the upper surface of the heat sink substrate, and the first metal strips and the second metal strips are alternately arranged on the upper surface of the silicon dioxide film layer; adjacent first metal strips and second metal strips are connected and conducted through bismuth telluride-based thin films deposited on the silicon dioxide film layer, and the bismuth telluride-based thin films include P-type bismuth telluride-based thin films and N-type bismuth telluride-based thin films, different types of bismuth telluride-based thin films are distributed on both sides of the first metal strips and the second metal strips, and one or more bismuth telluride-based thin films of the same type are distributed between adjacent first metal strips and second metal strips;

[0021] The surface of the second metal strip is covered by the thermally conductive insulating layer, and the surface except the surface covered by the thermally conductive insulating layer is covered by the photoresist, and the height of the thermally conductive insulating layer is greater than the height of the photoresist.

[0022] Furthermore, adjacent first metal strips and second metal strips are arranged at equal intervals, the width of the first metal strip is the same as the width of the second metal strip, and the lengths of the P-type bismuth telluride-based film and the N-type bismuth telluride-based film are both equal to the distance between adjacent first metal strips and second metal strips.

[0023] Furthermore, the thickness of the second metal strip is not less than the thickness of the first metal strip, the thickness range of the first metal strip is 10-30 μm, the length range of the first metal strip and the second metal strip are both 15-30 mm, and the width range is both 0.8-1.2 μm. The first metal strip and the second metal strip are made of the same or different materials, and the first metal strip and the second metal strip are made of aluminum, gold or silver.

[0024] Further, the P-type bismuth telluride-based thin films and the N-type bismuth telluride-based thin films are arranged in rows at staggered intervals on the upper surface of the silicon dioxide film layer;

[0025] A longitudinal spacing between a plurality of bismuth telluride-based thin films of the same type between adjacent first metal strips and second metal strips is equal to a width of the bismuth telluride-based thin films of the same type.

[0026] In yet another aspect, the present invention provides a thermoelectric generator, comprising the above-mentioned planar bismuth telluride-based thin film thermoelectric module.

[0027] The beneficial effects brought by the technical solution provided by the present invention are as follows:

[0028] a. Using MEMS micromachining technology and thin film deposition technology, planar bismuth telluride-based thin film thermoelectric modules and thermoelectric generators have good scalability;

[0029] b. By shortening the length of bismuth telluride-based NWs to submicrometer scale, the thermoelectric power density is effectively improved;

[0030] c. Suitable for the synthesis and preparation of planar thin film TE generators of various material systems, with strong applicability;

[0031] d. It has a wide range of uses and can be widely used in fields such as portable, wearable and distributed sensor network systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 is a front cross-sectional view of a planar bismuth telluride-based thin-film thermoelectric generator provided by an embodiment of the present invention;

[0034] Figure 2 Schematic diagram of the top structure of a planar bismuth telluride-based thin-film thermoelectric generator provided by an embodiment of the present invention;

[0035] Figure 3 It is a structural diagram of a planar bismuth telluride-based thin-film thermoelectric generator unit provided in an embodiment of the present invention.

[0036] Among them, the figure marks include: 1-heat sink substrate, 2-silicon dioxide film layer, 3-first metal belt, 4-second metal belt, 5-P-type bismuth telluride-based film, 6-N-type bismuth telluride-based film, 7-thermal conductive insulation layer, 8-photoresist. DETAILED DESCRIPTION

[0037] In order to enable those skilled in the art to better understand the scheme of the present invention, and to more clearly understand the purpose, technical scheme and advantages of the present invention, the technical scheme in the embodiment of the present invention is clearly and completely described below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be noted that the implementation methods not shown or described in the accompanying drawings are forms known to those skilled in the art. In addition, although demonstrations of parameters containing specific values ​​may be provided herein, it should be understood that the parameters do not need to be exactly equal to the corresponding values, but may be approximated to the corresponding values ​​within an acceptable error tolerance or design constraint. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work should belong to the scope of protection of the present invention. In addition, the terms "including" and "having" in the specification and claims of the present invention and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, device, product or equipment containing a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or equipment.

[0038] In one embodiment of the present invention, a method for manufacturing a planar bismuth telluride-based thin film thermoelectric module is provided, characterized in that it comprises the following steps:

[0039] S1, depositing a silicon dioxide film layer on a heat sink substrate;

[0040] S2, preparing a plurality of metal strips arranged at intervals on the silicon dioxide film layer;

[0041] S3, alternately depositing a P-type bismuth telluride-based film and an N-type bismuth telluride-based film on the upper surface of the silicon dioxide film layer between different metal strips, so that a P-type bismuth telluride-based film is deposited on one side of each metal strip and an N-type bismuth telluride-based film is deposited on the other side, to obtain a first semi-finished product;

[0042] S4, coating a photoresist on the upper surface of the first semi-finished product, and removing the photoresist on a portion of the metal strips, so that the metal strips from which the photoresist is removed and the metal strips from which the photoresist is not removed are arranged alternately;

[0043] S5, depositing a metal layer on the metal strip from which the photoresist has been removed, to obtain a second semi-finished product;

[0044] S6, coating a photoresist on the upper surface of the second semi-finished product, and removing the photoresist on the metal layer deposited in step S5;

[0045] S7. Depositing a thermally conductive insulating layer on the metal layer from which the photoresist has been removed.

[0046] Before step S1, the method further includes: performing micro-arc oxidation treatment on the upper and lower surfaces of the heat sink substrate to obtain a ceramic oxide layer, wherein the thickness of the ceramic oxide layer is in the range of 5-15 μm; after performing step S7, the method further includes removing the thermally conductive insulating layer deposited outside the metal layer, specifically removing the excess thermally conductive insulating layer by electron beam evaporation;

[0047] Specifically, the thickness of the silicon dioxide film layer deposited in step S1 is in the range of 80-120 μm, and is obtained by rapidly depositing a loosely structured amorphous silicon film by PECVD method and then oxidizing it by wet oxygen at high temperature, wherein the density of the amorphous silicon film is less than 2.2 g / cm 3 ; The metal strip prepared in step S2 has a thickness range of 10-30 μm, preferably 20 μm, a length range of 15-30 mm, preferably 20 mm, and a width range of 0.8-1.2 μm, preferably 1 μm; the P-type bismuth telluride-based film and the N-type bismuth telluride-based film deposited in step S3 have a thickness range of 30-80 nm, preferably 50 nm, a length range of 0.8-1.2 μm, preferably 1 μm, and a width range of 0.6-0.8 μm, preferably 0.7 μm; the optical film coated in step S4 The photoresist coated in the photoresist and step S6 are both spin-coated by a photoresist spreader, and the thickness range is 50-100μm, and SU8 photoresist is preferred; the thickness range of the metal layer deposited in step S5 is 50-100μm; the thickness range of the thermally conductive insulating layer in step S7 is 50-100μm, and the thermally conductive insulating layer is made of aluminum nitride; in steps S3 to S7, the metal strip, P-type bismuth telluride-based film, N-type bismuth telluride-based film, and metal layer are deposited, and the photoresist and thermally conductive insulating layer are removed by processes such as masking, electron beam evaporation and photolithography. It should be noted that the silicon dioxide film layer deposited on the heat sink substrate in this embodiment is mainly to facilitate the above-mentioned metal strip and bismuth telluride-based film lithography and other processes, and has certain electrical insulation and thermal insulation properties. Based on the function of the silicon dioxide film layer, if the silicon dioxide film layer material is simply replaced, it is also within the protection scope of this embodiment. For example, the silicon dioxide film layer can be doped to form a silicon oxynitride film layer, which has similar functions to the silicon dioxide film layer and has better electrical insulation and thermal insulation properties.

[0048] In one embodiment of the present invention, the heat sink substrate is an aluminum substrate that has been subjected to surface micro-arc oxidation treatment. The micro-arc oxidation can modulate the thickness, density and thermal conductivity of the oxide layer by controlling the plasma electrolysis process parameters. The aluminum substrate can also be replaced with a copper substrate for surface micro-arc oxidation treatment as required. The upper and lower surfaces of the heat sink substrate are both ceramic oxide layers, and the thickness of the ceramic oxide layer ranges from 5 to 15 μm, preferably 10 μm. The material of the metal layer can be the same as or different from the material of the corresponding deposited metal strip. For example, when the metal strip is preferably an aluminum strip, the deposited metal layer can be an aluminum layer, or a gold layer or a silver layer can be deposited. Under the premise of cost permission, the aluminum strip can be replaced by a silver strip or a gold strip. The present invention is not limited to aluminum, gold and silver. Metal materials with a thermal conductivity greater than or equal to 200 W / (m·K) or an electrical conductivity greater than or equal to 3E+07S / m can be selected to achieve the technical solution of the present invention. The higher the thermal conductivity / electrical conductivity, the higher the thermoelectric conversion efficiency and output power density of the TE generator under the same working conditions.

[0049] In one embodiment of the present invention, a planar bismuth telluride-based thin film thermoelectric module is provided. Figure 1 and Figure 2 , comprising a heat sink substrate 1, a silicon dioxide film layer 2, a plurality of first metal strips 3, a plurality of second metal strips 4, a bismuth telluride-based film, a photoresist 8 and a thermally conductive insulating layer 7; the heat sink substrate 1 is an aluminum substrate or a copper substrate, preferably an aluminum substrate; the silicon dioxide film layer 2 is arranged on the upper surface of the heat sink substrate 1; the first metal strips 3 and the second metal strips 4 are alternately arranged on the upper surface of the silicon dioxide film layer 2, the first metal strips 3 and the second metal strips 4 are made of the same or different materials, the first metal strips 3 and the second metal strips 4 are made of aluminum, gold or silver, and for economic considerations, the first metal strips 3 and The second metal strips 4 are preferably aluminum strips; the adjacent first metal strips 3 and second metal strips 4 are connected and conducted through a bismuth telluride-based film deposited on the silicon dioxide film layer 2, the bismuth telluride-based film includes a P-type bismuth telluride-based film 5 and an N-type bismuth telluride-based film 6, the P-type bismuth telluride-based film 5 and the N-type bismuth telluride-based film 6 are thermoelectric materials with opposite Seebeck coefficients and deposited in the direction of planar heat flow transmission, different types of bismuth telluride-based films are distributed on both sides of the first metal strip 3 and the second metal strip 4, and one or more bismuth telluride-based films of the same type are distributed between the adjacent first metal strips 3 and the second metal strips 4;

[0050] The surface of the second metal strip 4 is covered by the thermally conductive insulating layer 7, which is preferably made of aluminum nitride. The thermally conductive insulating layer is used as a heat source interface for heat injection. Except for the surface covered by the thermally conductive insulating layer 7, the surface is covered by the photoresist 8, and the height of the thermally conductive insulating layer 7 is greater than the height of the photoresist 8.

[0051] In one embodiment of the present invention, the adjacent first metal strips 3 and second metal strips 4 are arranged at equal intervals, the width of the first metal strip 3 is the same as the width of the second metal strip 4, the thickness of the second metal strip 4 is not less than the thickness of the first metal strip 3, preferably, the thickness of the second metal strip 4 is 60 μm greater than the thickness of the first metal strip 3, the thickness of the first metal strip 3 is 10-30 μm, the length of the first metal strip 3 and the second metal strip 4 are both in the range of 15-30 mm, preferably 20 mm, and the width is both in the range of 0.8-1.2 μm, preferably 1 μm;

[0052] The P-type bismuth telluride-based films 5 and the N-type bismuth telluride-based films 6 are arranged in rows at staggered intervals on the upper surface of the silicon dioxide film layer 2, and the lengths of the P-type bismuth telluride-based films 5 and the N-type bismuth telluride-based films 6 are both equal to the distance between the adjacent first metal strips 3 and the second metal strips 4, and the longitudinal spacing of multiple bismuth telluride-based films of the same type between the adjacent first metal strips 3 and the second metal strips 4 is equal to the width of the bismuth telluride-based films of the same type.

[0053] In one embodiment of the present invention, the length and width of the P-type bismuth telluride-based film and the N-type bismuth telluride-based film can be reduced to below 100 nm on a higher resolution processing platform to obtain higher thermoelectric material performance and energy conversion efficiency; the coordinated control between the film layer size parameters in steps S1 to S5 can modulate the heat flow transport and current transport characteristics to obtain the highest electrical transfer performance and the lowest thermal transfer performance. The process flow is also applicable to the preparation of gradient thermoelectric material energy conversion TE planar thin film generators. It should be noted that the manufacturing method of this embodiment is also applicable to the preparation of short planar thin film thermoelectric material TE generators with cavity-free structures of different components. The bismuth telluride-based film in this embodiment can be replaced with similar high-quality thermoelectric materials such as lead telluride-based and germanium silicon-based materials. These equivalent replacement materials are also within the protection scope of this embodiment.

[0054] In one embodiment of the present invention, a thermoelectric generator is provided, comprising the planar bismuth telluride-based thin film thermoelectric module as described above.

[0055] In one embodiment of the present invention, see Figure 3 The second metal strip 4 directly contacts the heat source through the heat-conducting insulating layer 7 on its surface to transfer heat, thereby forming a high-temperature end at its bottom. The first metal strip 3 forms a low-temperature end at its bottom through heat transfer from the cold source. The first metal strip 3 is connected to the second metal strip 4 on one side through the P-type bismuth telluride-based film 5. A temperature difference occurs at both ends of the P-type bismuth telluride-based film 5. Figure 2, a bismuth telluride-based thin film generator without a cavity structure, as shown by the thick arrow, the heat flow is perpendicular to the silicon substrate, as shown by the thin arrow, the heat flux will form a steep temperature gradient in the bismuth telluride-based thin film, and a shorter bismuth telluride-based thin film generator array can obtain a steeper temperature gradient. Due to the Seebeck effect, the carriers on the P-type bismuth telluride-based thin film 5 move from the high-temperature end to the low-temperature end to form a potential difference, and the potential of the first metal strip 3 is less than the potential of the second metal strip 4 connected to the same P-type bismuth telluride-based thin film 5. Similarly, the first metal strip 3 is connected to the second metal strip 4 on the other side through the N-type bismuth telluride-based thin film 6. The N-type telluride A potential difference is also formed at both ends of the bismuth-based film 6, but since the Seebeck coefficients of the N-type bismuth telluride-based film 6 and the P-type bismuth telluride-based film 5 have opposite signs, the potential of the first metal strip 3 is higher than the potential of the second metal strip 4 connected to the same N-type bismuth telluride-based film 6. The currents formed by the above two potential differences are in the same direction, so that there is a larger potential difference between the second metal strips 4 at both ends of the first metal strip 3. In addition, there are multiple bismuth telluride-based films between adjacent first metal strips 3 and second metal strips 4. In addition, there are multiple groups of the above-mentioned first metal strips 3 and second metal strips 4, and finally the potential difference is further expanded to increase higher power generation. It should be noted that the Seebeck effect belongs to the prior art. The cause of the Seebeck effect can be simply explained as the carriers in the conductor move from the hot end to the cold end under the temperature gradient and accumulate at the cold end, thereby forming an electric potential difference inside the material. At the same time, a reverse charge flow is generated under the action of the potential difference. When the charge flow of thermal motion reaches a dynamic equilibrium with the internal electric field, a stable thermoelectric potential is formed at both ends of the semiconductor. There are two types of carriers in the semiconductor, namely electrons and holes.

[0056] The present invention relates to a design method of a semiconductor device, in particular to a design method of a semiconductor thermoelectric generator, more specifically, to a design and preparation method of a planar bismuth telluride-based thin film thermoelectric (TE) generator designed and prepared by combining MEMS micromachining technology and thin film deposition technology. In order to solve the problems of low efficiency and difficulty in realizing large temperature difference and high energy density heat sources of existing semiconductor thermoelectric devices, the present invention provides a preparation method of a planar bismuth telluride-based thin film thermoelectric (TE) generator to overcome the shortcomings of the prior art; the present invention obtains an effective temperature gradient maintenance structure through novel heat source and heat sink material selection and structural design, and then utilizes the opposite sign of the Seebeck coefficient of P-type / N-type thermoelectric materials to deposit P-type / N-type thermoelectric materials in the planar heat flow transmission direction, so as to obtain a power density of 20mW / cm at a temperature difference of 5°C. 2 Thermoelectric (TE) generators.

[0057] The planar bismuth telluride-based thin film thermoelectric module manufacturing method, thermoelectric module and thermoelectric generator proposed in the present invention use MEMS micromachining technology and thin film deposition technology to design and prepare a short planar thin film bismuth telluride-based thermoelectric generator without a cavity structure. This novel design concept utilizes the steep temperature gradient formed near the main heat flow. By shortening the bismuth telluride-based-NW to a sub-micron length, the power density of the generator of the present invention is more scalable compared to traditional planar bismuth telluride-based thermoelectric generators. The thermoelectric device designed by the present invention for heat flow and current transmission in parallel to the thin film plane has a huge contribution to improving the performance of semiconductor thermoelectric devices, and can be widely used in portable, wearable and distributed sensor network systems and other fields.

[0058] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for manufacturing a planar bismuth telluride-based thin film thermoelectric module, It is characterized in that The following steps are involved: S1, depositing a silicon dioxide film layer on a heat sink substrate; S2, preparing a plurality of metal strips arranged at intervals on the silicon dioxide film layer; S3, alternately depositing a P-type bismuth telluride-based film and an N-type bismuth telluride-based film on the upper surface of the silicon dioxide film layer between different metal strips, so that a P-type bismuth telluride-based film is deposited on one side of each metal strip and an N-type bismuth telluride-based film is deposited on the other side, to obtain a first semi-finished product; S4, coating a photoresist on the upper surface of the first semi-finished product, and removing the photoresist on a portion of the metal strips, so that the metal strips from which the photoresist is removed and the metal strips from which the photoresist is not removed are arranged alternately; S5, depositing a metal layer on the metal strip from which the photoresist has been removed, to obtain a second semi-finished product; S6, coating a photoresist on the upper surface of the second semi-finished product, and removing the photoresist on the metal layer deposited in step S5; S7, depositing a thermally conductive insulating layer on the metal layer from which the photoresist has been removed; After executing step S7, the method further includes removing the thermally conductive insulating layer deposited outside the metal layer.

2. The method for manufacturing a planar bismuth telluride-based thin film thermoelectric module according to claim 1, It is characterized in that Before step S1, the method further includes: performing micro-arc oxidation treatment on the upper and lower surfaces of the heat sink substrate to obtain a ceramic oxide layer, wherein the thickness of the ceramic oxide layer is in the range of 5-15 μm.

3. The method for manufacturing a planar bismuth telluride-based thin film thermoelectric module according to claim 1, It is characterized in that The thickness of the metal strip is in the range of 10-30 μm, the length is in the range of 15-30 mm, and the width is in the range of 0.8-1.2 μm; the thickness of the P-type bismuth telluride-based film and the N-type bismuth telluride-based film are both in the range of 30-80 nm, the length is both in the range of 0.8-1.2 μm, and the width is both in the range of 0.6-0.8 μm.

4. The method for manufacturing a planar bismuth telluride-based thin film thermoelectric module according to claim 1, It is characterized in that The thickness of the silicon dioxide film layer deposited in step S1 is in the range of 80-120 μm, and is obtained by rapidly depositing an amorphous silicon film by the PECVD method and then subjecting it to wet oxygen high-temperature oxidation; the thickness of the photoresist coated in step S4 and the photoresist coated in step S6 are both in the range of 50-100 μm; the thickness of the metal layer deposited in step S5 is in the range of 50-100 μm; the thickness of the thermally conductive insulating layer in step S7 is in the range of 50-100 μm, and the thermally conductive insulating layer is made of aluminum nitride.

5. A planar bismuth telluride-based thin film thermoelectric module, It is characterized in that The heat sink substrate comprises a heat sink substrate (1), a silicon dioxide film layer (2), a plurality of first metal strips (3), a plurality of second metal strips (4), a bismuth telluride-based film, a photoresist (8) and a thermally conductive insulating layer (7), wherein the silicon dioxide film layer (2) is arranged on the upper surface of the heat sink substrate (1), and the first metal strips (3) and the second metal strips (4) are arranged alternately and spaced apart on the upper surface of the silicon dioxide film layer (2); adjacent first metal strips (3) and second metal strips (4) are deposited on the silicon dioxide film layer to form a heat sink substrate. The bismuth telluride-based films on the silicon dioxide film layer (2) are connected and conductive, the bismuth telluride-based films comprising a P-type bismuth telluride-based film (5) and an N-type bismuth telluride-based film (6), the P-type bismuth telluride-based film (5) and the N-type bismuth telluride-based film (6) being arranged in rows at staggered intervals on the upper surface of the silicon dioxide film layer (2); the longitudinal spacing of a plurality of bismuth telluride-based films of the same type between adjacent first metal strips (3) and second metal strips (4) is equal to the width of the bismuth telluride-based films of the same type; Different types of bismuth telluride-based thin films are distributed on both sides of the first metal strip (3) and the second metal strip (4), and one or more bismuth telluride-based thin films of the same type are distributed between adjacent first metal strips (3) and second metal strips (4); The surface of the second metal strip (4) is covered by the thermally conductive insulating layer (7), and the surface other than the surface covered by the thermally conductive insulating layer (7) is covered by the photoresist (8), and the height of the thermally conductive insulating layer (7) is greater than the height of the photoresist (8).

6. The planar bismuth telluride-based thin film thermoelectric module according to claim 5, It is characterized in that Adjacent first metal strips (3) and second metal strips (4) are arranged at equal intervals, the width of the first metal strip (3) is the same as the width of the second metal strip (4), and the lengths of the P-type bismuth telluride-based film (5) and the N-type bismuth telluride-based film (6) are both equal to the distance between adjacent first metal strips (3) and second metal strips (4).

7. The planar bismuth telluride-based thin film thermoelectric module according to claim 6, It is characterized in that The thickness of the second metal strip (4) is not less than the thickness of the first metal strip (3), the thickness of the first metal strip (3) is in the range of 10-30 μm, the length of the first metal strip (3) and the second metal strip (4) are both in the range of 15-30 mm, and the width is both in the range of 0.8-1.2 μm, the first metal strip (3) and the second metal strip (4) are made of the same or different materials, and the first metal strip (3) and the second metal strip (4) are made of aluminum, gold or silver.

8. A thermoelectric generator, It is characterized in that A planar bismuth telluride-based thin film thermoelectric module comprising any one of claims 5 to 7.

Citation Information

Patent Citations

  • Thin film thermoelectric devices having favorable crystal tilt

    CN105051924A

  • Planar bismuth telluride-based thin film thermoelectric module and thermoelectric generator

    CN212542474U

  • Thermoelectric energy converters with reduced interface losses and maunfacturing method thereof

    US20140360545A1