Schottky diode preparation method and Schottky diode

By using boron ion implantation and metal structure design in GaN Schottky diodes, the performance problems caused by electric field non-uniformity when vertical GaN Schottky diodes are reverse biased are solved and the reverse breakdown voltage is significantly improved. Compared with the switch, the leakage current is suppressed and the output power is improved.

CN112086353BActive Publication Date: 2024-10-01NANJING NANZHI INST OF ADVANCED OPTOELECTRONIC INTEGRATION NANJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011106984.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-16
Publication Date
2024-10-01
Estimated Expiration
2040-10-16

AI Technical Summary

Technical Problem

When the vertical GaN Schottky diode is reverse biased, the uneven distribution of the electric field under the anode causes avalanche breakdown, resulting in a drop in breakdown voltage and an increase in leakage current, which reduces device performance.

Method used

By processing the GaN sample, spin-coating photoresist and etching, PECVD deposits silicon dioxide, performs RIE etching and boron ion implantation to form a field plate structure, and evaporates a Ni/Au metal structure on its surface as an anode and backside The evaporated Ti/Al/Ti/Au metal structure is used as the cathode, and boron ion implantation is used to improve device performance.

Benefits of technology

It significantly improves the reverse breakdown voltage and switching ratio, effectively suppresses leakage current, and improves output power and overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112086353B_ABST
    Figure CN112086353B_ABST
Patent Text Reader

Abstract

The present application discloses a method for preparing a Schottky diode and a Schottky diode, wherein the method for preparing a Schottky diode comprises: processing a GaN sample to obtain a GaN sample; then spin coating a photoresist on the surface of the GaN sample and etching it; PECVD depositing silicon dioxide on the surface of the etched GaN sample, and performing photolithography and RIE etching on it; performing boron ion implantation on the etched GaN sample; depositing a silicon dioxide layer on the surface of the GaN sample after the boron ion implantation, and etching the silicon dioxide layer to form a field plate structure; evaporating a Ni / Au metal structure on the surface of the field plate structure as the anode of the Schottky diode; evaporating a Ti / Al / Ti / Au metal structure on the back side of the GaN sample as the cathode of the Schottky diode. By adopting the above-mentioned scheme, the reverse breakdown voltage and the switching ratio of the Schottky diode treated by boron ion implantation are significantly improved, and the leakage current can be effectively suppressed, the output power can be improved, and the overall performance of the Schottky diode can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to a method for preparing a Schottky diode and a Schottky diode. Background Art

[0002] Power semiconductor devices are electronic devices used in power conversion and control circuits of power equipment. Traditional power semiconductor devices are mainly silicon-based power devices with semiconductor silicon as the substrate. However, with the continuous development of science and technology, new technological products (such as power switches, smart phones, electric vehicles, renewable energy generation and other products) have higher and higher requirements for the performance of power semiconductor devices, so that traditional silicon-based power devices can no longer meet current needs. Therefore, the third-generation semiconductors GaN and SiC, which are known for their high performance, have come into people's view. Compared with silicon, SiC and GaN have wide bandgap (3.43eV), high electron mobility (1245cm 2 / V·s) and high electron saturation rate (2.5×10 7 cm / s), etc., which can theoretically achieve higher breakdown voltage and lower on-resistance, making it more suitable for manufacturing power semiconductor devices.

[0003] Schottky diodes are one of the more commonly used semiconductor power devices. The performance of Schottky diodes based on SiC and GaN is much better than that of silicon-based Schottky diodes. Therefore, more and more research is being done on Schottky diodes based on SiC and GaN. Generally, GaN Schottky diode devices are divided into lateral devices and vertical devices. Compared with lateral Schottky diodes, vertical Schottky diodes can improve the breakdown characteristics of the device by simply increasing the thickness of the drift region of the device without sacrificing the lateral size of the chip, so they have higher power density.

[0004] However, when the vertical GaN Schottky diode is reverse biased, the electric field below the anode is not uniformly distributed in the horizontal direction, that is, the closer to the electrode edge, the denser the distribution of the electric field lines, which makes the electric field maximum appear at the edge below the anode, making avalanche breakdown prone to occur here, resulting in a decrease in the actual breakdown voltage and output power of the vertical GaN Schottky diode and an increase in the reverse leakage current, reducing the performance of the Schottky diode. Summary of the invention

[0005] The present application provides a Schottky diode preparation method and a Schottky diode to solve the problem of low performance of existing Schottky diodes.

[0006] In a first aspect, an embodiment of the present application provides a method for preparing a Schottky diode, the method comprising:

[0007] Process GaN samples and obtain GaN samples;

[0008] Spin coating photoresist on the surface of the GaN sample and etching it;

[0009] PECVD deposits silicon dioxide on the surface of the etched GaN sample, and then performs photolithography and RIE etching on it;

[0010] Performing boron ion implantation on the etched GaN sample;

[0011] A silicon dioxide layer is deposited on the surface of the GaN sample after the boron ion implantation, and the silicon dioxide layer is etched to form a field plate structure;

[0012] A Ni / Au metal structure is evaporated on the surface of the field plate structure to serve as the anode of the Schottky diode;

[0013] A Ti / Al / Ti / Au metal structure was evaporated on the back side of the GaN sample to serve as the cathode of the Schottky diode.

[0014] In combination with the first aspect, in one implementation, processing a GaN sample includes:

[0015] Cleaning the GaN sample by organic cleaning and inorganic cleaning in sequence;

[0016] The organic cleaning is to ultrasonically clean the GaN sample in acetone and isopropanol solutions for 5 minutes respectively, rinse with deionized water, and blow dry with N2;

[0017] The inorganic cleaning is to place the GaN sample in a mixed solution of concentrated hydrochloric acid: water = 1:1 and soak for 10 minutes to remove the surface oxide layer.

[0018] In combination with the first aspect, in one implementation, photoresist is spin-coated on the surface of the GaN sample and during the etching process, the spin coating speed is 4000rad / s-4500rad / s, the spin coating time is 30s-35s, the exposure time is 6s-6.5s, and the etching is ICP etching.

[0019] In combination with the first aspect, in one implementation, before the etched GaN sample is implanted with boron ions, the method further includes:

[0020] Silicon dioxide is deposited on the surface of the GaN sample, and is then coated with silicon and subjected to RIE etching.

[0021] In combination with the first aspect, in one implementation, after the etched GaN sample is implanted with boron ions, the method further includes:

[0022] The GaN sample after boron ion implantation was cleaned and then annealed by rapid thermal annealing. The GaN sample after ion implantation was subjected to rapid thermal annealing treatment in a nitrogen atmosphere at 450° C. for 10 minutes.

[0023] In combination with the first aspect, in one implementation, after evaporating the Ni / Au metal structure on the surface of the field plate structure, the method further includes: stripping off excess metal.

[0024] In combination with the first aspect, in one implementation, the implantation energy of the boron ions is 40keV-45keV, and the implantation dose is 0.4×10 13 at / cm 2 -0.5×10 13 at / cm 2 .

[0025] In combination with the first aspect, in one implementation, the etching of the silicon dioxide layer is performed by selective etching using a mixed solution of NH4F:HF=7:1, and the etching time is 40s-45s.

[0026] In combination with the first aspect, in one implementation, the thickness of the silicon dioxide layer is 100 nm-200 nm.

[0027] In a second aspect, the embodiments of the present application provide a Schottky diode, characterized in that the Schottky diode is prepared by the preparation method described in any one of the first aspects.

[0028] The present application discloses a method for preparing a Schottky diode and a Schottky diode, wherein the method for preparing a Schottky diode comprises: firstly processing a GaN sample to obtain a GaN sample; then spin coating a photoresist on the surface of the GaN sample and etching it; PECVD depositing silicon dioxide on the surface of the etched GaN sample, and performing photolithography and RIE etching on it; then performing boron ion implantation on the etched GaN sample; then depositing a silicon dioxide layer on the surface of the GaN sample after the boron ion implantation, and etching the silicon dioxide layer to form a field plate structure; finally, evaporating a Ni / Au metal structure on the surface of the field plate structure as the anode of the Schottky diode; evaporating a Ti / Al / Ti / Au metal structure on the back side of the GaN sample as the cathode of the Schottky diode. By adopting the above-mentioned scheme, the reverse breakdown voltage and the switching ratio of the Schottky diode treated by boron ion implantation are significantly improved, and the leakage current can be effectively suppressed, the output power can be improved, and the overall performance of the Schottky diode can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0030] Figure 1 It is a schematic flow chart of a method for preparing a Schottky diode provided in an embodiment of the present application;

[0031] Figure 2 It is a schematic diagram of a complete preparation process of another Schottky diode provided in an embodiment of the present application. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0033] From the description of the background technology, it can be seen that the performance of the traditional vertical GaN Schottky diode is relatively low. In order to improve the performance of the vertical GaN Schottky diode, the prior art has a diode using a junction Schottky structure, usually by implanting Mg ions into the n-type GaN epitaxial layer. However, the Mg-doped GaN formed by ion implantation is very difficult to activate and has a low activation rate if it is to be converted into p-type GaN.

[0034] There are also Schottky diodes with ion implantation structures in the prior art, which use Ar+ implantation process and F+ implantation process, but there are still some disadvantages. For example, Ar+ itself has a large ion radius, and the ion implantation process requires the injection of accelerated high-energy Ar+, so this process is very destructive; and although the F+ ion itself has a strong electronegativity, its ion radius is small. The device optimized by this process may experience F ion diffusion at high temperature, resulting in a decrease in device performance.

[0035] Therefore, in order to solve the above problems, the present application provides a method for preparing a Schottky diode, referring to Figure 1 , the preparation method comprises:

[0036] S11, processing the GaN sample to obtain a GaN sample.

[0037] The purpose of pre-treating the GaN sample in this step is to remove the oxide layer on the surface of the GaN sample and obtain a usable GaN sample.

[0038] The specific treatment process includes: cleaning the GaN sample by organic cleaning and inorganic cleaning in sequence.

[0039] The organic cleaning is to place the GaN sample in acetone and isopropanol solutions for ultrasonic cleaning for 5 minutes respectively; each solution is cleaned twice, and then rinsed with deionized water and dried with N2.

[0040] The inorganic cleaning is to place the GaN sample in a mixed solution of concentrated hydrochloric acid: water = 1:1 and soak for 10 minutes to remove the surface oxide layer.

[0041] S12, spin coating photoresist on the surface of the GaN sample and etching it.

[0042] This step is the Schottky diode mesa isolation process, and its main purpose is to isolate the area that does not need to be implanted with boron ions.

[0043] The photoresist selected in the photolithography process of this step is AZ5214, and the spin coating method is adopted for uniform coating, the rotation speed is 4000rad / s-4500rad / s, the time is 30s-35s, the exposure time is 6.0s-6.5s, and the etching adopts ICP etching (Inductively Couple Plasma Etch).

[0044] S13, depositing silicon dioxide on the surface of the GaN sample, and performing resist coating and RIE etching on the surface of the GaN sample.

[0045] The silicon dioxide (SiO2) is used as a protective layer to eliminate the electric field in the edge area and improve the withstand voltage of the Schottky diode.

[0046] This step is to first deposit a layer of silicon dioxide using the PECVD process, then spin-coat the silicon dioxide layer with photoresist, and etch to expose the surface of the GaN sample and the specific area where boron ions need to be injected.

[0047] S14, implanting boron ions into the etched GaN sample.

[0048] The ion selected for the Schottky diode ion implantation of the present application is B+. Boron itself is an element of the same main group as Ga, has similar chemical properties and has a higher electronegativity than Ga ions, so boron ions can be implanted into GaN as implanted ions to combine with free carriers at the boundary.

[0049] This step is to implant boron ions into a specific area on the surface of the GaN sample, wherein the specific area is the area formed after etching in step S13.

[0050] The boron ion implantation energy is 40keV-45keV, and the implantation dose is 0.4×10 13 at / cm 2 -0.5×10 13 at / cm2 .

[0051] S15, cleaning the GaN sample after the boron ion implantation, and then annealing it by rapid thermal annealing. The annealing process is a rapid thermal annealing process in a nitrogen atmosphere at 450°C for 10 minutes.

[0052] In this step, BOE solution is used to clean the GaN sample after boron ion implantation. BOE solution is a buffered oxide etching solution, usually a mixture of hydrofluoric acid (49%) and water or ammonium fluoride and water. After cleaning, it is annealed. The purpose of annealing is to repair lattice damage, move boron ions to lattice sites, and activate them.

[0053] S16, depositing a silicon dioxide layer on the surface of the GaN sample after the boron ion implantation, and etching the silicon dioxide layer to form a field plate structure.

[0054] In this step, silicon dioxide is deposited again as a dielectric layer of the field plate structure. After spin coating the photoresist, etching is performed to form a field plate structure. The thickness of the silicon dioxide layer is 100nm-200nm. The silicon dioxide layer is selectively etched using a mixed solution of NH4F:HF=7:1, and the etching time is 40s-45s.

[0055] S17, vapor-depositing a Ni / Au metal structure on the surface of the field plate structure as an anode of the Schottky diode.

[0056] This step is an anode metal evaporation process, specifically, evaporating a Ni / Au (40nm / 200nm) metal structure on one side of the field plate structure formed in step S16 as the anode of the Schottky diode.

[0057] After evaporating the Ni / Au metal structure on the surface of the field plate structure, the process also includes: stripping off the excess metal. During evaporation, the entire surface is usually covered, and there will be excess metal. Therefore, the excess metal needs to be stripped off. The specific method of stripping the metal can be dissolving with a solvent, for example, dissolving with acetone.

[0058] S18, evaporating a Ti / Al / Ti / Au metal structure on the back side of the GaN sample as the cathode of the Schottky diode.

[0059] This step is the cathode metal evaporation process, specifically, Ti / Al / Ti / Au (20nm / 130nm / 50nm / 150nm) is evaporated on the back surface of the GaN sample by magnetron sputtering to form a multi-layer metal structure to prepare an ohmic contact as the cathode of the Schottky diode.

[0060] Reference Figure 2 , Figure 2This is the complete preparation process of the Schottky diode disclosed in this application. First, the GaN sample is cleaned, coated, photolithographic, and ICP etched; then PECVD is used to grow SiO2, coated and photolithographic again, and etched with RIE; then B ion implantation is performed, followed by BOE cleaning, and then repaired by rapid thermal annealing; then PECVD is used to grow SiO2, coated and photolithographic again, and etched with BOE; then coated and photolithographically evaporated Ni / Au as the anode, the excess metal is stripped, the N side is ICP etched, and finally Ti / Al / Ti / Au is evaporated as the cathode, and the prepared device (Schottky diode) is tested to complete the preparation. For the specific operations and parameters involved in the above process, please refer to the relevant description in the above preparation method, which will not be described in detail here.

[0061] Based on the above disclosed method for preparing a Schottky diode, the present application further discloses a Schottky diode, and the Schottky diode is prepared by the above preparation method.

[0062] For specific details about the Schottky diode, please refer to the above preparation method, which is not specifically limited in this section.

[0063] In order to make the solution of the present application more clear, the present application also discloses specific embodiments.

[0064] Example 1

[0065] a. Cleaning process of GaN samples: This process firstly carries out organic cleaning, using immersion in acetone and immersion in isopropanol solution for ultrasonic cleaning for 5 minutes, and then two cleanings are carried out respectively. After organic cleaning, inorganic cleaning process is carried out, and the main method is to immerse the GaN sample in a mixed solution of concentrated hydrochloric acid: water = 1:1 for 10 minutes, in order to remove the oxide layer on the surface of GaN.

[0066] b Schottky diode mesa isolation process: The photoresist selected in the photolithography process is AZ5214, and the spin coating method is used for uniform coating, with a rotation speed of 4000 rad / s, a time of 30s, and an exposure time of 6.5s.

[0067] c. Preparation of a silicon dioxide protective layer: depositing silicon dioxide on the surface of the GaN sample, and performing glue coating and RIE etching on the surface of the GaN sample.

[0068] d Boron ion implantation process: B + The ion implantation energy is 40 keV and the implantation dose is 0.4×10 13 at. / cm 2 Perform the injection.

[0069] e The GaN sample after boron ion implantation is cleaned with a BOE solution (49% hydrofluoric acid mixed with water in a ratio of 1:1), and then annealed by rapid thermal annealing.

[0070] f Field plate structure preparation process: PECVD grows a 100nm thick SiO2 film on the surface of the GaN sample, and then photolithography is used to selectively etch the SiO2 on the GaN surface using a mixed solution of NH4F:HF=7:1, with a processing time of 40s.

[0071] g Anode metal evaporation process: The anode mainly adopts Ni / Au (40nm / 200nm) metal structure.

[0072] h Cathode metal evaporation process: A multilayer metal structure of Ti / Al / Ti / Au (20nm / 130nm / 50nm / 150nm) was evaporated on the N-side of the GaN sample by magnetron sputtering to prepare an ohmic contact.

[0073] Example 2

[0074] a. Cleaning process of GaN samples: This process firstly carries out organic cleaning, using immersion in acetone and immersion in isopropanol solution for ultrasonic cleaning for 5 minutes, and then two cleanings are carried out respectively. After organic cleaning, inorganic cleaning process is carried out, and the main method is to immerse the GaN sample in a mixed solution of concentrated hydrochloric acid: water = 1:1 for 10 minutes, in order to remove the oxide layer on the surface of GaN.

[0075] b Schottky diode mesa isolation process: The photoresist selected in the photolithography process is AZ5214, and the spin coating method is used for uniform coating, with a rotation speed of 4500 rad / s, a time of 35s, and an exposure time of 6s.

[0076] c. Preparation of a silicon dioxide protective layer: depositing silicon dioxide on the surface of the GaN sample, and performing glue coating and RIE etching on the surface of the GaN sample.

[0077] d Boron ion implantation process: B + The ion implantation energy is 45 keV and the implantation dose is 0.5×10 13 at. / cm 2 Perform the injection.

[0078] e The GaN sample after boron ion implantation is cleaned with a BOE solution (49% ammonium fluoride mixed with water in a ratio of 1:1), and then annealed by rapid thermal annealing.

[0079] f Field plate structure preparation process: PECVD grows a 200nm thick SiO2 film on the surface of the GaN sample, and then photolithography is used to selectively etch the SiO2 on the GaN surface using a mixed solution of NH4F:HF=7:1, with a processing time of 40s.

[0080] g Anode metal evaporation process: The anode mainly adopts Ni / Au (40nm / 200nm) metal structure.

[0081] h Cathode metal evaporation process: A multilayer metal structure of Ti / Al / Ti / Au (20nm / 130nm / 50nm / 150nm) was evaporated on the N-side of the GaN sample by magnetron sputtering to prepare an ohmic contact.

[0082] In order to further clarify the performance of the vertical structure Schottky diode prepared by the preparation method disclosed in this application, the performance of the Schottky diode (B+ implanted device) prepared in Example 1 combining the field plate structure and the boron ion implantation process is compared with the existing field plate structure Schottky diode (single field plate device). The specific experimental operation can be implemented by existing technology and is not specifically limited in this application. The results show that the reverse breakdown voltage of the Schottky diode implanted by boron ions is increased to 585V, the reverse leakage current is reduced by 5 orders of magnitude, and the switching ratio is increased to 10 8 In addition, the boron ion implantation technology increases the Schottky barrier of the diode from 0.68eV to 0.82eV. The specific results are shown in Table 1:

[0083] Table 1

[0084] <![CDATA[I on / I off ]]> SBH n <![CDATA[V on ]]> <![CDATA[R on ]]> Single field plate device <![CDATA[10 5 ]]> 0.68eV 1.78 0.51V <![CDATA[68.8mΩ·cm 2 ]]> B+ injected devices <![CDATA[10 8 ]]> 0.82eV 1.07 0.49V <![CDATA[71.2mΩ·cm 2 ]]>

[0085] As can be seen from the above, the Schottky barrier height (SBH) of the Schottky diode treated with boron ion implantation is 0.82eV, which is 0.14eV higher than that of the Schottky diode with a single field plate structure (0.68eV). This shows that the reverse rectification characteristics of the Schottky diode have been greatly improved. In addition, the ideal factor n of the device with a single field plate structure is 1.78, which indicates that there are a large number of recombination centers in the barrier region of the device, resulting in serious leakage, while the ideal factor n of the Schottky diode structure treated with boron ion implantation is 1.07, which is very close to 1, which shows that the physical mechanism of the Schottky diode is very consistent with the thermal electron emission theory and has better device rectification characteristics. The switching ratio (I on / I off ) is 10 5 , while the device switching ratio of boron ion implantation increased to 10 8 It can be seen that the boron ion implantation technology has increased the switching ratio of the Schottky diode by 10 3 times, and the two devices have a on ) and forward turn-on voltage (V on This shows that the boron ion implantation method optimizes the performance of GaN-based Schottky diodes without significantly reducing their forward conduction characteristics.

[0086] In addition, the reverse breakdown voltage of the device with a single field plate is 189 V, while the reverse breakdown voltage of the device treated with boron ion implantation is 585 V, and the reverse breakdown voltage is increased by 396 V. Therefore, the vertical structure Schottky diode with boron ion implantation disclosed in the present application can effectively increase the reverse breakdown voltage, suppress leakage current, and improve output efficiency.

[0087] In this specification, the same or similar parts between the various embodiments can be referred to each other. In particular, for the device embodiment, since it is implemented by adopting a preparation method, the description is relatively simple, and the relevant parts can be referred to the description in the method embodiment.

[0088] The present application is described in detail above in conjunction with specific implementation methods and exemplary examples, but these descriptions cannot be understood as limiting the present application. Those skilled in the art understand that, without departing from the spirit and scope of the present application, a variety of equivalent replacements, modifications or improvements can be made to the technical solution of the present application and its implementation methods, all of which fall within the scope of the present application. The scope of protection of the present application shall be subject to the attached claims.

Claims

1. A method for preparing a Schottky diode, characterized in that: The preparation method comprises: Process GaN samples and obtain GaN samples; Spin-coating photoresist on the surface of the GaN sample and etching it; the spin-coating speed is 4000rad / s-4500rad / s, the spin-coating time is 30s-35s, the exposure time is 6s-6.5s, and the etching is ICP etching; Silicon dioxide is deposited on the surface of the etched GaN sample by PECVD, and then subjected to photolithography and RIE etching; The etched GaN sample is implanted with boron ions; wherein the implantation energy of the boron ions is 40keV-45keV, and the implantation dose is 0.4×10 13 at / cm 2 -0.5×10 13 at / cm 2 ; The GaN sample after boron ion implantation was cleaned and then annealed by rapid thermal annealing. The GaN sample after ion implantation was subjected to rapid thermal annealing treatment in a nitrogen atmosphere at 450°C for 10 minutes. A silicon dioxide layer is deposited on the surface of the GaN sample after the boron ion implantation, and the silicon dioxide layer is etched to form a field plate structure; A Ni / Au metal structure is evaporated on the surface of the field plate structure to serve as the anode of the Schottky diode; A Ti / Al / Ti / Au metal structure is evaporated on the back side of the GaN sample as the cathode of the Schottky diode to obtain a boron ion-implanted vertical structure GaN-based Schottky diode.

2. The preparation method according to claim 1, characterized in that: Processing of GaN samples, including: Cleaning the GaN sample by organic cleaning and inorganic cleaning in sequence; The organic cleaning is to ultrasonically clean the GaN sample in acetone and isopropanol solutions for 5 minutes respectively, rinse with deionized water, and blow dry with N2; The inorganic cleaning is to place the GaN sample in a mixed solution of concentrated hydrochloric acid: water = 1:1 and soak for 10 minutes to remove the surface oxide layer.

3. The preparation method according to claim 1, characterized in that: Before the boron ion implantation of the etched GaN sample, it also includes: Silicon dioxide is deposited on the surface of the GaN sample, and is subjected to resist coating and RIE etching.

4. The preparation method according to claim 1, characterized in that: After evaporating the Ni / Au metal structure on the surface of the field plate structure, the method further includes: stripping off excess metal.

5. The preparation method according to claim 1, characterized in that: The silicon dioxide layer is selectively etched using a mixed solution of NH4F:HF=7:1, and the etching time is 40s-45s.

6. The preparation method according to claim 5, characterized in that: The thickness of the silicon dioxide layer is 100nm-200nm.

7. A Schottky diode, characterized in that: The Schottky diode is prepared by the preparation method according to any one of claims 1 to 6.