A method for preparing in-situ nitrogen-doped epitaxial oxide single crystal thin film
By introducing a mixture of oxygen and nitrogen into the pulsed laser deposition device, in-situ nitrogen doping is achieved, and the problem of difficult to regulate the nitrogen doping content and damaged film quality in the prior art is solved, and high-quality nitrogen doping is obtained The oxide film regulates the transition temperature and switching ratio of the metal insulator.
Patent Information
- Application Number
- CN202211083022.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to achieve in-situ nitrogen doping to grow high-quality functional oxide films, and the nitrogen doping content is difficult to continuously regulate. The post-treatment method may destroy the crystal quality of the film and is costly.
By introducing a mixture of oxygen and nitrogen into the pulsed laser deposition device, the atmosphere in the cavity is regulated, and the plasma generated by bombarding the target surface with pulsed lasers collides with nitrogen, thereby achieving in-situ doping of nitrogen, avoiding post-treatment, and achieving high quality Growth of single crystal oxide films.
The preparation of high-quality nitrogen-doped oxide film is realized, the transition temperature of metal insulator is regulated, the crystal quality and switching ratio are improved, the preparation process is simplified, and the cost is reduced.
Smart Images

Figure CN115506009B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of material technology, and in particular to a method for preparing an in-situ nitrogen-doped epitaxial oxide single crystal film. Background Art
[0002] Oxide thin film materials have played an important role in the development of modern science and technology. At present, many technologies have been developed for the preparation of functional oxide thin films, such as solution method, spin coating method, magnetron sputtering, molecular beam deposition, pulsed laser deposition, etc. Among them, pulsed laser deposition technology (PLD), as a popular thin film epitaxial growth method, has many advantages, such as high film crystal quality and stable stoichiometric ratio. Nitrogen doping has a significant effect on regulating the functional behavior of oxide thin films, such as regulating the phase transition temperature and switching ratio of vanadium dioxide thin films. Since PLD technology is often used for the epitaxial growth of thin films in an oxygen environment, nitrogen doping of thin films is often used, that is, the method of selecting nitrogen-doped targets, or some post-processing methods, such as ion implantation and ammoniation treatment. Among them, the nitrogen-doped target method is to pre-sinter the target doped with nitrogen and then perform epitaxial growth. Ion implantation mainly uses the prepared oxide thin film sample, places it in a high vacuum, and then bombards it with N ion beams to achieve nitrogen doping; ammoniation treatment is to place the prepared oxide film in an ammonia atmosphere and high temperature conditions to achieve nitrogen doping.
[0003] Although the doped epitaxial growth of oxide thin films can be achieved by bombarding nitrogen-doped targets, there are two problems. First, the nitrogen doping content is the same as the target material. Therefore, different targets need to be fired for different contents, and continuous adjustment cannot be achieved during the epitaxial growth process. Second, some targets are not easy to fire after nitrogen doping, and the cost is higher than before doping. Post-treatment methods for nitrogen doping are simple and effective, but post-treatment methods often destroy the crystal quality of the original epitaxial growth film and affect the functional performance of the film. The current bottleneck in the preparation of high-epitaxial quality nitrogen-doped functional oxide thin film materials is that there is no preparation method that can achieve in-situ nitrogen doping growth. Compared with oxygen, nitrogen has lower activity and stronger bond energy. Conventional vapor deposition preparation methods make it difficult to separate nitrogen into nitrogen ions and participate in the film deposition process. At present, there is no public information on the introduction of nitrogen to regulate film performance in PLD technology. Summary of the invention
[0004] In response to the above technical problems, the present invention discloses a method for preparing an in-situ nitrogen-doped epitaxial oxide single crystal film. The obtained film has high epitaxial quality and achieves a certain content of doping, thereby realizing the performance regulation of the functional oxide film and meeting its needs in materials science research and engineering applications.
[0005] To this end, the technical solution adopted by the present invention is:
[0006] A method for preparing an in-situ nitrogen-doped epitaxial oxide single crystal film comprises: cleaning a substrate, placing the substrate in a pulse laser deposition device cavity, introducing a mixture of oxygen and nitrogen, and after the atmosphere in the cavity is uniform and stable, performing pulse laser deposition on the substrate with a pure oxide target material, and after the deposition is completed, performing annealing in the same atmosphere environment.
[0007] This technical solution is used to control the gas environment in the PLD cavity during epitaxial growth, so that nitrogen doping can be achieved while epitaxially growing high-quality single-crystalline oxide films. Since the pulsed laser bombards the surface of the target material, the plasma plume emitted has extremely high energy. When it collides with the nitrogen gas molecules in the cavity, it can ionize the gas molecules into a mixture of atoms, ions, and electrons, and transmit them to the surface of the substrate material, thereby participating in the epitaxial growth of the film. Since this is an in-situ growth technology, there is no need for post-doping treatment, which effectively guarantees the crystal quality of the film. In addition, by reasonably controlling the atmosphere in the cavity, the same target material can be continuously adjusted with different nitrogen doping concentrations.
[0008] As a further improvement of the present invention, the oxide is vanadium dioxide. With this technical solution, the metal-insulator transition temperature of the vanadium dioxide film is reduced by nitrogen doping, and the higher the doping concentration, the greater the reduction in the phase transition temperature.
[0009] As a further improvement of the present invention, the substrate is made of titanium dioxide.
[0010] As a further improvement of the present invention, the condition parameters of pulsed laser deposition are: temperature 380-420°C, total gas pressure in the cavity 15-25 mTorr, laser energy density 1.0-1.2 J / cm2, and pulse frequency 10 Hz. Further preferably, the condition parameters of pulsed laser deposition are: temperature 400°C, total gas pressure in the cavity 20 mTorr, laser energy density 1.1 J / cm2, and pulse frequency 10 Hz.
[0011] As a further improvement of the present invention, after the deposition is completed, the original epitaxial atmosphere is kept warm for 5 minutes and then annealed.
[0012] As a further improvement of the present invention, the volume ratio of oxygen and nitrogen introduced into the mixture is 1: 1. By adopting this technical solution, by controlling the volume ratio of oxygen and nitrogen to be 1: 1, an ideal metal-insulator transition performance can be obtained.
[0013] Compared with the prior art, the present invention has the following beneficial effects:
[0014] First, by adopting the technical solution of the present invention, nitrogen doping is achieved by regulating the atmosphere during epitaxial growth, and the preparation of doped oxide films can be achieved without selecting specific target materials. The method is simple and effective; it does not involve secondary processing of the film and will not cause damage to the prepared high-quality film.
[0015] Second, compared with other existing technologies, the nitrogen-doped vanadium dioxide film prepared by the technical solution of the present invention not only regulates the metal-insulator transition temperature, but also effectively improves the crystal quality. This effect comes from the introduction of nitrogen, which not only provides a nitrogen source for doping, but also provides internal forces for the film growth process, so that it can reduce lattice mismatch. In particular, under the optimized nitrogen and oxygen atmosphere conditions, nitrogen-doped vanadium dioxide has a lower transition temperature and maintains a higher switching ratio, and is expected to be applied to high-performance intelligent switching devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is an XRD comparison diagram of the thin films deposited in Examples 1-3 of the present invention and Comparative Examples 1-2.
[0017] Figure 2 It is a microscopic morphology picture of the thin film deposited in Examples 1-3 of the present invention and Comparative Examples 1-2.
[0018] Figure 3 It is an XPS comparison chart of the thin films deposited in Examples 1-3 of the present invention and Comparative Examples 1-2.
[0019] Figure 4 It is a comparison chart of the N content of the thin films deposited in Examples 1-3 of the present invention and Comparative Examples 1-2.
[0020] Figure 5 1 and 2 are the temperature resistance curves of the thin films deposited in Examples 1 to 3 of the present invention and Comparative Examples 1 to 2.
[0021] Figure 6 It is an XRD comparison diagram of the thin films deposited in Example 1 of the present invention and Comparative Example 3.
[0022] Figure 7 3 are the resistance-temperature curves of the thin films deposited in Example 1 of the present invention and Comparative Example 3. DETAILED DESCRIPTION
[0023] The preferred embodiments of the present invention are described in further detail below.
[0024] Example 1
[0025] Titanium dioxide was selected as the substrate and cleaned and dried. Before depositing the film, the atmosphere was introduced into the PLD chamber, and the ratio of oxygen and nitrogen entering the chamber was regulated by a flow meter, and the volume ratio of oxygen and nitrogen was controlled to be 1:1, which was maintained for 10 minutes. After the atmosphere in the chamber was uniform and stable, the pure target of vanadium dioxide was pulsed laser deposited on the titanium dioxide substrate by pulse laser deposition technology, and after the film deposition was completed, it was kept warm in the atmosphere for 5 minutes and then annealed in the same atmosphere.
[0026] Example 2
[0027] Based on Example 1, in this example, the volume ratio of oxygen to nitrogen is 2:1.
[0028] Example 3
[0029] Based on Example 1, in this example, the volume ratio of oxygen to nitrogen is 1:2.
[0030] Comparative Example 1
[0031] On the basis of Example 1, in this comparative example, the gas introduced is pure nitrogen.
[0032] Comparative Example 2
[0033] On the basis of Example 1, in this comparative example, the gas introduced is pure oxygen.
[0034] The XRD comparison diagrams of the films obtained in Examples 1 to 3 and Comparative Examples 1 to 2 are shown in FIG. Figure 1 As shown, SEM comparison diagram is as follows Figure 2 As shown in the energy spectrum comparison diagram Figure 3 As shown in the figure, the comparison of N content is as follows Figure 4 As shown, it can be seen that under the same nitrogen-oxygen ratio environment, the method of the embodiment can achieve effective regulation of the nitrogen doping content from about 0% to 4%.
[0035] The temperature resistance curves of the films obtained in Examples 1 to 3 and Comparative Examples 1 to 2 are as follows: Figure 5 As shown, it can be seen that the metal-insulator transition temperature of the vanadium dioxide film is reduced by nitrogen doping, and the higher the doping concentration, the greater the reduction in phase transition temperature. Under the condition of a nitrogen and oxygen volume ratio of 1:1, an ideal metal-insulator transition performance can be obtained.
[0036] Comparative Example 3
[0037] Based on Example 1, the difference of this comparative example is that the ratio of oxygen to nitrogen changes during the deposition process. Specifically, during the deposition process, the flow ratio of nitrogen to oxygen into the chamber changes instantly, and the nitrogen ratio is first reduced to a volume ratio of nitrogen to oxygen of 0.5:1, and then restored after 2 minutes.
[0038] The XRD comparison diagrams of the films deposited in Example 1 and Comparative Example 3 are as follows: Figure 6 As shown, the resistance-temperature curve is Figure 7 As shown, it can be seen that the fluctuation of the nitrogen and oxygen gas ratio in Comparative Example 1 shows that the obtained sample is not a single-phase structure, and the metal-insulator transition performance of the obtained film is worse, which is specifically manifested in that the transition is not sharp, the temperature range is more relaxed, there are multiple transitions, and the transition switching ratio is reduced. It can be seen that the fluctuation of gas pressure can easily cause the composition of the film to be uneven, which in turn greatly affects the metal-insulator transition performance.
[0039] During the epitaxial growth of a single crystal substrate, the crystal structure and lattice parameters of the single crystal substrate are the same or similar to those of the epitaxial film, making it easier to obtain a high-quality single crystal epitaxial film. Titanium dioxide and vanadium dioxide both have a rutile structure and similar structures, but the lattice parameters of the two are quite different (the unit cell volume of vanadium dioxide is smaller than that of titanium dioxide). Therefore, under normal circumstances, vanadium dioxide single crystals can be epitaxially grown in PLD technology, but the general crystal quality is poor. The doping of nitrogen in the embodiment of the present invention, on the one hand, nitrogen ions are slightly larger than cations, causing a certain lattice expansion, and during epitaxial growth, reducing the lattice mismatch between the substrate and the substrate, is conducive to the preparation of high-quality single crystal vanadium dioxide thin films; on the other hand, nitrogen doping introduces hole carriers, inhibits VV dimerization in the vanadium dioxide structure, plays a role in stabilizing the rutile phase, and is also conducive to maintaining its high crystal quality.
[0040] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing an in-situ nitrogen-doped epitaxial oxide single crystal thin film, characterized in that: include: Clean the substrate, place the substrate in the chamber of the pulse laser deposition equipment, introduce a mixture of oxygen and nitrogen, and after the atmosphere in the chamber is uniform and stable, perform pulse laser deposition on the substrate with a pure oxide target material. After the deposition is completed, annealing is performed in the same atmosphere; The conditions for pulsed laser deposition are: temperature 380~420℃, total pressure in the chamber 15~25mTorr, laser energy density 1.0~1.2J / cm 2 , pulse frequency is 10 Hz; the oxide is vanadium dioxide, and the material of the substrate is titanium dioxide.
2. The method for preparing an in-situ nitrogen-doped epitaxial oxide single crystal thin film according to claim 1, characterized in that: The pulse laser deposition conditions are as follows: temperature 400°C, total pressure in the chamber 20 mTorr, laser energy density 1.1 J / cm 2 , pulse frequency 10 Hz.
3. The method for preparing an in-situ nitrogen-doped epitaxial oxide single crystal thin film according to claim 2, characterized in that: After the deposition is completed, the substrate is kept warm for 5 min in the original epitaxial atmosphere and then annealed.
4. The method for preparing an in-situ nitrogen-doped epitaxial oxide single crystal thin film according to any one of claims 1 to 3, characterized in that: A mixture of oxygen and nitrogen was introduced, with the volume ratio of oxygen to nitrogen being 1:1.