Residue removal

Through the combination of chemical mechanical polishing and etching processes, the problem of residual material contamination in the selective deposition process is solved, and residues at undesired locations on the semiconductor substrate are efficiently removed, improving the electrical performance and structural accuracy of the device.

CN112136204BActive Publication Date: 2024-10-11APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980031899.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-06-21
Filing Date
2019-05-03
Publication Date
2024-10-11
Estimated Expiration
2039-05-03

AI Technical Summary

Technical Problem

When forming small-sized, high-aspect-ratio semiconductor device structures using existing technology, the selective deposition process is difficult to limit to designated locations, resulting in residual material forming in undesired locations, contaminating the substrate and affecting the electrical performance of the device.

Method used

A chemical mechanical polishing (CMP) process is used to remove residues on the substrate after selective deposition, and an etching process is used to selectively remove residual material in undesired locations while protecting material formed in desired locations.

Benefits of technology

Effectively removes residues on the substrate, improves the electrical performance and reliability of the device, and ensures accuracy and high density of small-size structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112136204B_ABST
    Figure CN112136204B_ABST
Patent Text Reader

Abstract

A method for removing residue after a selective deposition process is provided. In one embodiment, the method includes performing a selective deposition process to form a metal-containing dielectric material at a first location on a substrate, and performing a residue removal process to remove residue from a second location on the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments generally relate to methods for removing defects from a semiconductor substrate at certain locations on the substrate. More particularly, embodiments relate to methods for selectively forming desired materials on a substrate (with different materials at different locations on the substrate) by a selective deposition process utilizing local passivation deposition. Background Art

[0002] Reliably producing sub-half-micron and smaller features is one of the key technical challenges for the next generation of very large scale integration (VLSI) and ultra large scale integration (ULSI) of semiconductor devices. However, the reduced dimensions of VLSI and ULSI technology have placed additional demands on processing capabilities as the limits of circuit technology are pushed. Reliably forming gate structures on substrates is important to the success of VLSI and ULSI and the ongoing efforts to increase circuit density and quality of the respective substrates and dies.

[0003] As the geometric limits of structures used to form semiconductor devices are pushed toward the limits of technology, the need for accurately forming structures with small critical dimensions and high aspect ratios, as well as structures with different materials, with the desired materials has become increasingly difficult to meet. Conventional methods for selective deposition can be performed to form a layer of material only at certain locations on a flat surface on a substrate, the layer of material being made of a material different from the substrate material. However, as the geometric limits of structures continue to be pushed, the selective deposition process may not be effectively limited and formed on the substrate at a specified small size, resulting in the formation of undesirable materials at undesirable locations on the substrate. In addition, when the selectivity of the deposition process is not high enough, some residual materials are often formed at undesirable locations. Retaining these residual materials at undesirable locations may contaminate the device structure on the substrate, degrade the electrical performance of the device, and ultimately cause the device to fail.

[0004] Therefore, there is a need for improved methods for removing residues after a selective deposition process suitable for next generation semiconductor chips or other semiconductor devices. Summary of the invention

[0005] Embodiments of the present disclosure provide methods for removing residues from undesired locations on a substrate in semiconductor applications. In one embodiment, the method includes performing a selective deposition process to form a metal-containing dielectric material at a first location on a substrate, and performing a residue removal process to remove residues from a second location on the substrate.

[0006] In another example, a method for removing residue from a substrate includes: performing a selective deposition process to form a metal-containing dielectric material on a metal material on a substrate and leaving residue on the dielectric material on the substrate, wherein the metal-containing dielectric material is a high dielectric constant material having a dielectric constant greater than 12; and performing a residue removal process to remove the residue from the substrate.

[0007] In yet another example, a method for removing residue from a substrate includes: performing a selective deposition process by an atomic layer deposition process to form a metal-containing dielectric material on a metal material on a substrate, and leaving residue on the dielectric material on the substrate; and performing a residue removal process to remove the residue from the substrate, wherein the residue has a diameter less than 30 nm but greater than 2 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] In order that the manner in which the above-recited features of the present disclosure are obtained and can be understood in detail, a more particular description of the disclosure, briefly summarized above, may be had by reference to embodiments of the disclosure illustrated in the appended drawings.

[0009] Figure 1 is a schematic cross-sectional view of a processing chamber configured to perform an etching process according to one or more embodiments of the present disclosure.

[0010] Figure 2 is a schematic cross-sectional view of a polishing system configured to perform a chemical mechanical polishing (CMP) process.

[0011] Figure 3 is a flow chart of a method for performing a residue removal process according to one or more embodiments of the present disclosure.

[0012] FIG. 4A to FIG. 4C The picture is Figure 3 Cross-sectional view of a substrate during a patterning process.

[0013] Figure 5 Depicted in Figure 3 Cross-sectional view of a substrate during a patterning process.

[0014] To facilitate understanding, identical reference numerals have been used, where possible, to designate identical elements that are common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.

[0015] It is to be noted, however, that the appended drawings illustrate only exemplary embodiments of this disclosure and are therefore not to be considered limiting of its scope, for the disclosure may admit to other equally effective embodiments. DETAILED DESCRIPTION

[0016] A method for removing residue from a substrate is provided. The method utilizes a chemical mechanical polishing process after the selective deposition process to remove residue from a selective deposition process. Alternatively, the method utilizes an etching process that can selectively remove residue from undesired locations of the substrate without damaging or removing material formed at desired locations. After removing the residue, an additional chemical mechanical polishing process can be optionally performed to remove residue from the substrate if residue is present, if necessary.

[0017] As used herein, the term "substrate" refers to a material layer that serves as a base for subsequent processing operations and includes a surface to be cleaned. For example, the substrate may include one or more materials including silicon-containing materials, Group IV or Group III-V containing compounds such as Si, polycrystalline silicon, amorphous silicon, Ge, SiGe, GaAs, InP, InAs, GaAs, GaP, InGaAs, InGaAsP, GaSb, InSb, and the like, or a combination of the foregoing compounds. In addition, the substrate may also include dielectric materials such as silicon dioxide, organosilicates, and carbon-doped silicon oxides. The substrate may also include one or more conductive metals such as nickel, titanium, platinum, molybdenum, rhenium, osmium, chromium, iron, aluminum, copper, tungsten, or a combination thereof. In addition, the substrate may include any other materials such as metal nitrides, metal oxides, and metal alloys depending on the application. In one or more embodiments, the substrate may form a contact structure, a metal silicide layer, or a gate structure, wherein the gate structure includes a gate dielectric layer and a gate electrode layer to facilitate connection with interconnect features (such as plugs, vias, contacts, wiring, and conductive lines) subsequently formed thereon or suitable structures for use in semiconductor devices.

[0018] In addition, the substrate is not limited to any particular size or shape. The substrate may be a circular wafer having a diameter of 200 mm, a diameter of 300 mm, a diameter of 450 mm, or other diameters. The substrate may also be any polygonal, square, rectangular, curved, or otherwise non-circular workpiece, such as a polygonal glass or plastic substrate used to manufacture a flat panel display.

[0019] Figure 1 is a simplified cross-sectional view of an exemplary processing chamber 100 that is suitable for etching residue from a substrate in the processing chamber 100. The exemplary processing chamber 100 is suitable for performing a patterning process. One example of a processing chamber 100 that may be suitable for benefiting from the present disclosure is the EMBODIMENT® available from Applied Materials, Inc. located in Santa Clara, California. Sym3 TM Etch Processing Chamber. It is contemplated that other processing chambers, including those from other manufacturers, may be suitable for practicing embodiments of the present disclosure.

[0020] The plasma processing chamber 100 includes a chamber body 105 having a chamber volume 101 defined therein. The chamber body 105 has sidewalls 112 and a bottom 118 coupled to a ground 126. The sidewalls 112 have liners 115 that protect the sidewalls 112 and extend the time between maintenance cycles of the plasma processing chamber 100. The size of the chamber body 105 and related components of the plasma processing chamber 100 is not limited and is typically proportionally larger than the size of the substrate 210 to be processed therein. Examples of substrate sizes include 200 mm diameter, 250 mm diameter, 300 mm diameter, and 450 mm diameter, among other diameters.

[0021] The chamber body 105 supports a chamber lid assembly 110 to enclose the chamber volume 101. The chamber body 105 may be fabricated from aluminum or other suitable materials. A substrate access port 113 is formed through a sidewall 112 of the chamber body 105 to facilitate transfer of substrates 210 into and out of the plasma processing chamber 100. The access port 113 may be coupled to a transfer chamber and / or other chambers of a substrate processing system (not shown).

[0022] A pumping port 145 is formed through the sidewall 112 of the chamber body 105 and connected to the chamber volume 101. A pumping device (not shown) is coupled to the chamber volume 101 via the pumping port 145 to evacuate and control the pressure in the chamber volume 101. The pumping device may include one or more pumps and throttle valves.

[0023] The gas plate 160 is coupled to the chamber body 105 via a gas line 167 to supply process gases into the chamber volume 101. The gas plate 160 may include one or more process gas sources 161, 162, 163, 164, and may additionally include inert gases, non-reactive gases, and reactive gases as desired. Examples of process gases that may be provided by the gas plate 160 include, but are not limited to, hydrocarbon-containing gases including methane (CH4), sulfur hexafluoride (SF6), carbon tetrafluoride (CF4), hydrogen bromide (HBr), hydrocarbon-containing gases, argon (Ar), chlorine (Cl2), nitrogen (N2), helium (He), and oxygen (O2). In addition, the process gas may include a gas containing chlorine, fluorine, oxygen, and hydrogen, such as BCl3, C2F4, C4F8, C4F6, CHF3, CH2F2, CH3F, NF3, CO2, SO2, CO, and H2, among others.

[0024] Valve 166 controls the flow of process gases from sources 161, 162, 163, 164 from gas plate 160 and is governed by controller 165. The flow of gases supplied from gas plate 160 to chamber body 105 may include a combination of gases.

[0025] The lid assembly 110 may include a nozzle 114. The nozzle 114 has one or more ports for introducing a process gas from a source 161, 162, 164, 163 of a gas plate 160 into the chamber volume 101. After the process gas is introduced into the plasma processing chamber 100, the gas is excited to form a plasma. An antenna 148, such as one or more inductor coils, may be disposed adjacent to the plasma processing chamber 100. An antenna power supply 142 may power the antenna 148 via a matching circuit 141 to inductively couple energy, such as RF energy, to the process gas to maintain a plasma formed by the process gas in the chamber volume 101 of the plasma processing chamber 100. Alternatively, or in addition to the antenna power supply 142, a process electrode below the substrate 210 and / or above the substrate 221001 may be used to capacitively couple RF power to the process gas to maintain a plasma within the chamber volume 101. The operation of the power supply 142 may be controlled by a controller, such as the controller 165 , which also controls the operation of other components in the plasma processing chamber 100 .

[0026] A substrate support pedestal 135 is disposed in the chamber volume 101 to support the substrate 210 during processing. The substrate support pedestal 135 may include an electrostatic chuck 122 for holding the substrate 301 during processing. The electrostatic chuck (ESC) 122 holds the substrate 210 to the substrate support pedestal 135 using electrostatic attraction. The ESC 122 is powered by an RF power supply 125 integrated with a matching circuit 124. The ESC 122 includes an electrode 121 embedded in a dielectric body. The electrode 121 is coupled to the RF power supply 125 and provides a bias that attracts plasma ions formed from the process gas in the chamber volume 101 to the ESC 122 and the substrate 210 positioned thereon. During processing of the substrate 210, the RF power supply 125 may be cycled on and off, or pulsed. The ESC 122 has an isolator 128 for reducing the attraction of plasma to the sidewall of the ESC 122 so as to extend the maintenance life cycle of the ESC 122. In addition, the substrate support pedestal 135 may have a cathode liner 136 for protecting the sidewall of the substrate support pedestal 135 from the plasma gas and extending the maintenance interval of the plasma processing chamber 100.

[0027] Additionally, the electrode 121 is coupled to a power supply 150. The power supply 150 provides a clamping voltage of about 200 volts to about 2000 volts to the electrode 121. The power supply 150 may also include a system controller for controlling the operation of the electrode 121 by directing a DC current to the electrode 121 to clamp or unclamp the substrate 210.

[0028] The ESC 122 may include a heater disposed therein and connected to a power source (not shown) for heating the substrate, and a cooling base 129 supporting the ESC 122 may include conduits for circulating a heat transfer fluid to maintain the temperature of the ESC 122 and the substrate 210 disposed thereon. The ESC 122 is configured to perform within a temperature range required by the thermal budget of the device fabricated on the substrate 210. For example, for some embodiments, the ESC 122 may be configured to maintain the substrate 210 at a temperature of about -25 degrees Celsius to about 500 degrees Celsius.

[0029] A cooling base 129 is provided to assist in controlling the temperature of the substrate 210. To reduce process drift and time, the temperature of the substrate 210 may be maintained substantially constant throughout the time that the substrate 210 is in the cleaning chamber by the cooling base 129. In one embodiment, the temperature of the substrate 210 is maintained at approximately 30 degrees Celsius to 120 degrees Celsius during subsequent cleaning processes.

[0030] A cover ring 130 is disposed on the ESC 122 and along the perimeter of the substrate support pedestal 135. The cover ring 130 is configured to confine etching gas to a desired portion of the exposed top surface of the substrate 210 while shielding the top surface of the substrate support pedestal 135 from the plasma environment inside the plasma processing chamber 100. Lift pins (not shown) are selectively moved through the substrate support pedestal 135 to lift the substrate 210 above the substrate support pedestal 135 to facilitate access to the substrate 210 by a transfer robot (not shown) or other suitable transfer mechanism.

[0031] The controller 165 may be used to control the process sequence and adjust the gas flow from the gas plate 160 to the plasma processing chamber 100 and other process parameters. The software program, when executed by the CPU, transforms the CPU into a dedicated computer (controller) that controls the plasma processing chamber 100 so that processes according to the present disclosure are performed. The software program may also be stored and / or executed by a second controller (not shown) in parallel with the plasma processing chamber 100.

[0032] Figure 2Schematic cross-sectional view of an exemplary polishing system 200. Typically, the polishing pad 205 is fixed to the platen 202 of the polishing system 200 using an adhesive (such as a pressure sensitive adhesive) disposed between the polishing pad 205 and the platen 202. A substrate carrier 208 facing the platen 202 and the polishing pad 205 mounted on the platen 202 includes a flexible membrane 211, which is configured to apply different pressures on different areas of the substrate 210 when forcing the substrate 210 to be polished against the polishing surface of the polishing pad 205. The substrate carrier 208 includes a carrier ring 209 surrounding the substrate 210. During polishing, the downward pressure on the carrier ring 209 forces the carrier ring 209 against the polishing pad 205, thereby preventing the substrate 210 from sliding off the substrate carrier 208. The substrate carrier 208 rotates around a carrier axis 214 while the flexible membrane 211 forces the surface to be polished of the substrate 210 against the polishing surface of the polishing pad 205. The platen 202 rotates about the platen axis 204 in a rotation direction opposite to the rotation direction of the substrate carrier 208, while the substrate carrier 208 sweeps back and forth from the central area of ​​the platen 202 to the outer diameter of the platen 202, so as to partially reduce the uneven wear of the polishing pad 205. Herein, the platen 202 and the polishing pad 205 have a surface area larger than the area of ​​the surface to be polished of the substrate 210, however, in some polishing systems, the polishing pad 205 has a surface area smaller than the area of ​​the surface to be polished of the substrate 210. An endpoint detection (EPD) system 230 directs light to the substrate 210 through the platen opening 222 and further through the optically transparent window feature 206 of the polishing pad 205 disposed above the platen opening 222.

[0033] During polishing, a fluid 216 is introduced to the polishing pad 205 by a fluid dispenser 218 positioned above the platen 202. Typically, the fluid 216 is a polishing fluid (including water as part of the polishing fluid or polishing material), a polishing slurry, a cleaning fluid, or a combination thereof. In some embodiments, the fluid 216 is a polishing fluid including a pH adjuster and / or a chemically active component (such as an oxidizing agent) to enable chemical mechanical polishing of the material surface of the substrate 210 in combination with the abrasive of the polishing pad 205.

[0034] Figure 3 3 is a flow chart of an example of a method 300 for removing residue from a substrate. The method 300 begins with operation 302, performing a substrate having an interconnect structure 450 formed thereon, such as Figure 4A In one example, the interconnect structure 450 may be utilized in a back-end or front-end structure for forming a semiconductor device. Figure 4AIn the example depicted in , the interconnect structure 450 may include a glue material 405 and a capping layer 406 formed in the insulating material 402 and the interface layer 404. It should be noted that the interconnect structure 450 may be any structure, including a front-end structure or a gate structure for forming a semiconductor device.

[0035] In one example, the substrate 401 may include a material selected from the group consisting of: crystalline silicon (eg, Si <100> or Si <111> ), silicon oxide, strained silicon, silicon germanium, doped or undoped polysilicon, doped or undoped silicon wafers and patterned or unpatterned silicon on insulator wafers (SOI), carbon-doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire. Substrate 401 may have various sizes, such as 200mm, 300mm, 450mm or other diameters, and may also be a rectangular or square panel. Unless otherwise specified, the embodiments and examples described herein are performed on a substrate having a 200mm diameter, a 300mm diameter, or a 450mm diameter substrate. In embodiments in which an SOI structure is used for substrate 401, substrate 401 may include a buried dielectric layer disposed on a silicon crystalline substrate. In the embodiments depicted herein, substrate 401 may be a crystalline silicon substrate. In addition, substrate 401 is not limited to any particular size or shape. Substrate 401 may be a circular substrate having (among others) a 200mm diameter, a 300mm diameter, or other diameters (such as 450mm). The substrate 401 may also be any polygonal, square, rectangular, curved or otherwise non-circular workpiece, such as a polygonal glass substrate used in manufacturing flat panel displays.

[0036] although Figure 4A The example depicted in FIG. 4 shows that the interconnect structure 450 is formed on the substrate 401, but it should be noted that there may be additional structures formed between the interconnect structure 450 and the substrate 401 as needed. In one example, a front-end structure such as a gate structure and / or a contact structure may be formed between the interconnect structure 450 and the substrate 401 to implement the functions of the semiconductor device.

[0037] In one example, the insulating material 402 included in the interconnect structure 450 may be a dielectric material, such as a silicon oxide material, a silicon-containing material, a doped silicon material, a low-k material (such as a carbon-containing material). Suitable carbon-containing materials include amorphous carbon, SiC, SiOC, doped carbon materials, or any suitable material. Suitable examples of low-k insulating dielectric materials include SiO-containing materials, SiN-containing materials, SiOC-containing materials, SiC-containing materials, SiOCN-containing materials, carbon-based materials, or other suitable materials. In one example, the insulating material 402 is a SiN layer.

[0038] The insulating material 402 may be formed by plasma enhanced chemical vapor deposition (CVD), flowable chemical vapor deposition (CVD), high density plasma (HDP) chemical vapor deposition (CVD) process, atomic layer deposition (ALD), cyclic layer deposition (CLD), physical vapor deposition (PVD), or the like, as desired.

[0039] The interface layer 404 is disposed on the insulating material 402 adjacent to the cover layer 406, wherein the glue material 405 surrounds the cover layer 406. The interface layer 404 is also an insulating material, for example, a dielectric material, such as a silicon-containing material. Suitable examples of the interface layer 404 include SiN, SiON, SiO2, SiOC, SiOCN, SiCN and the like. In one example, the interface layer 404 is a SiON layer.

[0040] The paste material 405 may be formed of a metal-containing material (such as TiN, TaN, WN, or the like) in the insulating material 402 and vertically extends to the interface layer 404. The capping layer 406 is a metal material, such as tungsten (W), tantalum (Ta), titanium (Ti), copper (Cu), ruthenium (Ru), nickel (Ni), cobalt (Co), chromium (Cr), iron (Fe), manganese (Mn), aluminum (Al), hafnium (Hf), vanadium (V), molybdenum (Mo), palladium (Pd), gold (Au), silver (Au), platinum (Pt), alloys thereof, and combinations thereof. In a specific example, the capping layer 406 is a ruthenium (Ru), cobalt (Co), or tungsten (W) layer. In a specific example, the capping layer 406 is a ruthenium (Ru) layer.

[0041] The capping layer 406 and the interfacial layer 404 are exposed in preparation for receiving another material to be formed thereon.

[0042] At operation 304, a selective deposition process is performed on the substrate 401. The selective deposition process is performed at operation 304 to form a metal-containing dielectric material 407 on the capping layer 406, such as Figure 4B A selective deposition process is performed to selectively form a metal-containing dielectric material 407 on the capping layer 406, as shown in FIG. Figure 4B The selective deposition process performed is performed to mainly form a metal-containing dielectric material 407 having a film quality and characteristics that are compatible with the material from the capping layer 406 but not compatible with the interface layer 404 on the insulating material 402. Therefore, the metal-containing dielectric material 407 is selectively and mainly formed on the capping layer 406, but not on the interface layer 404 or generally on the entire substrate 401 (including some surfaces of the insulating material at other locations (if any)).

[0043] The metal-containing dielectric material 407 may be a high dielectric contact material having a dielectric constant greater than 10. Suitable examples of the metal-containing dielectric material 407 include metal dielectric materials: hafnium oxide (HfO x ), AlN, WSiO2, WSi, AlON, TiN, TaN, TiON, TaON, zirconia (ZrO x ), titanium oxide (TiO x ), tantalum oxide (TaO x ), niobium oxide (NbO x ), iron oxide (FeO x ), yttrium oxide (YO x ), aluminum oxide (AlO x ) and the like. In one specific example, the metal-containing dielectric material 407 is a hafnium oxide (HfO x ) or Al2O3.

[0044] In one example, the selective deposition process can be an ALD process, a CVD process, or any suitable deposition process. In one example depicted herein, the selective deposition process is an atomic layer deposition process (ALD).

[0045] In some cases, some residues 408 and / or remnants of the metal-containing dielectric material 407 may undesirably remain at undesirable locations, such as on the surface 409 of the interface layer 404. These residues 408 may contaminate the substrate surface and ultimately cause device failure. Therefore, in most cases, the metal-containing dielectric material 407 and the residue 408 are similar or identical materials. In one example, the residue 408 is also a high dielectric contact material having a dielectric constant greater than 10. Suitable examples of the metal-containing dielectric material 407 include metal dielectric materials: hafnium oxide (HfO x ), AlN, WSiO2, WSi, AlON, TiN, TaN, TiON, TaON, zirconia (ZrO x ), titanium oxide (TiO x ), tantalum oxide (TaO x ), niobium oxide (NbO x ), iron oxide (FeO x ), yttrium oxide (YO x ), aluminum oxide (AlO x ) and the like. In one specific example, the metal-containing dielectric material 407 and the residue 408 are both hafnium-containing oxide (HfO x ) or Al2O3.

[0046] At optional operation 306, a CMP process may be performed to remove residue 408 from surface 409 of interface layer 404, such as Figure 4C. The CMP process performed can remove the residue 408 from the surface 409 of the interface layer 404 without adversely damaging or over-grinding the nearby metal-containing dielectric material 407. The residue 408 remaining on the substrate 401 has a relatively loose bonding structure with the surface 409 of the interface layer 404 compared to the bonding structure in the metal-containing dielectric material 407. Therefore, by using a relatively minimal grinding down force, the residue 408 on the substrate 401 can be removed without damaging or grinding away material from the metal-containing dielectric material 407.

[0047] In one example, a CMP apparatus (such as Figure 2 408. The polishing system 200 may perform chemical mechanical polishing at a relatively reduced / mild removal rate to prevent excessive metal removal of the metal-containing dielectric material 407, thereby selectively removing the residue 408 from the substrate 401.

[0048] The chemical mechanical polishing process can remove or polish residue 408 from substrate 401 by using a specific fluid supplied during the polishing process, or by DI water. A relatively soft polishing pad, such as a pad having an elasticity greater than 90%, can be used during the chemical mechanical polishing process. During polishing, since the selected polishing pad has a relatively soft surface, slurry or other chemical fluids can be omitted as needed. In one example, DI water can be used during the chemical mechanical polishing process. The chemical mechanical polishing process is followed by an optional cleaning process to enhance the cleanliness of the substrate surface.

[0049] At operation 308, an etching process is performed to remove residue 408 from substrate 401, such as Figure 4C , regardless of whether the optional CMP process is performed at operation 306. An etching process is performed to selectively remove residue 408 from substrate 401 without damaging metal-containing dielectric material 407. The etching process is performed in a processing chamber (such as Figure 1 The process is performed in a processing chamber 100) to mainly and selectively remove the residue 408.

[0050] The etching process at operation 308 is performed by supplying an etching gas mixture to the substrate 401 in the processing chamber 100 to primarily and selectively remove the residue 408 without damaging the metal-containing dielectric material 407. In one example, the etching gas mixture includes at least a halogen-containing gas. Suitable examples of halogen-containing gases include BCl3, Cl2, NF3, CF4, HCl, HBr, Br2, combinations thereof, and the like. Inert gases such as He and Ar may also be supplied to the etching gas mixture. In some examples, carrier gases such as N2, O2, CO2, N2O, NO2, and the like may also be supplied to the etching gas mixture. In a specific example, the etching gas mixture includes BCl3, Cl2 and Ar or BCl3, NF3 and Ar.

[0051] It is believed that the different geometric configurations between the residue 408 and the metal-containing dielectric material 407 provide different etching mechanisms and behaviors during the etching process at operation 308. Therefore, by utilizing structures with different geometric configurations on the substrate, a selective etching process can be obtained. The different geometric configurations between the residue 408 and the metal-containing dielectric material 407 provide different etching surface areas, which allow different amounts of etching species to contact the residue 408 and the metal-containing dielectric material 407, respectively. For example, the residue 408 generally has an arc, oval, circular, or irregular shape, while the metal-containing dielectric material 407 generally has a vertical bulk structure. Figure 5 One embodiment of the reaction mechanism of the etching gas mixture with the residue 408 and with the metal-containing dielectric material 407 is depicted. Because the arcuate, elliptical, or circular shape of the residue 408 provides a larger surface area than the metal-containing dielectric material 407, more reactive species from the etching gas mixture are able to react with and be exposed to the residue 408, thereby forming volatile byproducts that are removed from the substrate surface (e.g., pumped out of the processing chamber). The larger surface area to react with the residue 408 provides a relatively high etch / removal rate, and thus the residue 408 can be removed from the substrate 401 at a greater etch / removal rate than the metal-containing dielectric material 407. Therefore, a selective etching process is obtained to selectively remove the residue 408 from the substrate 401 without damaging or excessively attacking the metal-containing dielectric material 407. As shown in FIG. Figure 5As shown in , the arcuate, elliptical, circular shape of the residue 408 allows the reactive etchant to move around the periphery of the residue 408, as indicated by arrows 502. In contrast, the bulk structure of the metal-containing dielectric material 407 has a relatively strong bonding structure, and only the top surface 506 is exposed for reaction. Therefore, the reactive species from the etching gas mixture preferentially react with the dangling bonds or residues 504 (which are relatively weak bonding structures) from the top surface 506 of the metal-containing dielectric material 407. Therefore, the etching / removal rate at the top surface 506 of the metal-containing dielectric material 407 is relatively slower than the etching / removal rate at the outer periphery of the residue 408, thereby providing a desired selective etching process mainly on the area where the residue 408 is located.

[0052] In one example, the etching gas mixture includes BCl3, Cl2, and Ar. During etching, the BCl3 gas and the Cl2 gas are dissociated into B* and Cl* reactive species, such as ions or radicals, for reaction. It is believed that the chlorine reactive species (e.g., Cl*) can react with the residue 408 from the substrate 401 (which is also a metal-containing dielectric material) without aggressively attacking the metal-containing dielectric material 407. In one example, the residue 408 includes hafnium oxide (HfO x ), such as HfO2 materials. Chlorine reactive species (e.g., Cl*) can efficiently react with HfO2 materials to remove residue 408 from the substrate. In another example, the etching gas mixture includes BCl3, NF3, and Ar. Fluorine reactive species (e.g., F*) can also efficiently react with HfO2 materials to remove residue 408 from the substrate. Therefore, both chlorine reactive species and fluorine reactive species (e.g., Cl* and F*) are good species to react with HfO2 materials to efficiently remove residue 408 from substrate 401.

[0053] In one example, the residue 408 has a diameter 510 less than 30 nm but greater than 2 nm, such as between about 12 nm and about 25 nm, or between about 9 nm and about 10 nm. The metal-containing dielectric material 407 has a width 512 greater than 50 nm, such as between about 80 nm and about 90 nm.

[0054] During the supply of the etching gas mixture at operation 308, several process parameters may be controlled. In one embodiment, an RF source power between about 100 watts and about 3000 watts (such as about 300 watts) may be supplied to the plasma processing chamber 100, with or without RF bias power. When RF bias power is utilized, the RF bias power may be controlled between about 1 watt and about 500 watts. The pressure of the processing chamber may be controlled within a pressure range greater than 2 mTorr but less than 500 mTorr, such as between about 5 mTorr and about 200 mTorr, such as about 150 mTorr. The substrate pedestal may be maintained at a temperature from 0 degrees Celsius up to 250 degrees Celsius, such as between 50 degrees Celsius and about 100 degrees Celsius, for example about 90 degrees Celsius.

[0055] After the residue 408 is removed from the substrate 401, a relatively clean surface is obtained after the selective deposition process to selectively form a metal-containing dielectric material 407 on the substrate, wherein the residue 408 is relatively absent on the substrate 401, such as Figure 4C as shown in .

[0056] At optional operation 310, after the etching process at operation 308, if there is still any residue or leftover that needs to be removed from the substrate 401, an additional CMP process may be performed to enhance removal efficiency and performance. The CMP process performed at operation 310 is similar to the CMP process performed at operation 306.

[0057] Therefore, a method for removing residues after a selective deposition process is provided. The method removes the residues using an etching gas mixture including at least one halogen-containing gas. The residues may include hafnium oxide (HfO x ), such as HfO2 material. A CMP process may be performed before or after the etching process as appropriate to enhance the residue removal performance and efficiency.

[0058] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope of the present disclosure, which is to be determined by the claims that follow.

Claims

1. A method for removing residue from a substrate, comprising: performing a selective deposition process to form a metal-containing dielectric material at a first location on a substrate, the first location including a surface of a capping layer and a surface of an adhesive layer, the capping layer being embedded in the adhesive layer, the adhesive layer being embedded in an insulating layer disposed on the substrate; as well as A residue removal process is performed to remove residue from a second location on the substrate without damaging the metal-containing dielectric material, wherein the residue removal process comprises a chemical mechanical polishing process.

2. The method of claim 1, wherein the residue removal process further comprises: An etching process is performed.

3. The method of claim 2, wherein performing an etching process further comprises: An etching gas mixture is supplied onto the surface of the substrate, wherein the etching gas mixture includes at least a halogen-containing gas.

4. The method of claim 3, wherein the halogen-containing gas is selected from the group consisting of: BCl3, Cl2, NF3, CF4, HCl, HBr, Bt2, and combinations thereof.

5. The method of claim 4, wherein the etching gas mixture comprises BCl3, Cl2 or NF3. The method of claim 1 , wherein the residue has a diameter less than 30 nm but greater than 2 nm.

7. The method of claim 1, wherein the metal-containing dielectric material and the residue comprise the same material.

8. The method of claim 1, wherein the metal-containing dielectric layer is a high dielectric constant material having a dielectric constant greater than 12.

9. The method of claim 1, wherein the metal-containing dielectric layer is made of a material selected from the group consisting of: a hafnium oxide (HfO x ), AlN, WSiO2, WSi, AlON, TiN, TaN, TiON, TaON, zirconia (ZrO x ), titanium oxide (TiO x ), tantalum oxide (TaO x ), niobium oxide (NbO x ), iron oxide (FeO x ), yttrium oxide (YO x ) and aluminum oxide (AlO x ).

10. The method of claim 7, wherein the metal-containing dielectric material and the residue are both hafnium-containing oxides.

11. The method of claim 1, wherein the capping layer is selected from the group consisting of: ruthenium (Ru), cobalt (Co), and tungsten (W).

12. The method of claim 1, wherein the second location of the substrate comprises a dielectric material.

13. A method for removing residue from a substrate, comprising: performing a selective deposition process to form a metal-containing dielectric material on a metal material on a substrate and leaving a residue on the dielectric material on the substrate, the metal-containing dielectric material being formed on a surface of a cover layer and a surface of an adhesive layer, the cover layer being embedded in the adhesive layer, the adhesive layer being embedded in an insulating layer disposed on the substrate, wherein the metal-containing dielectric material is a high dielectric constant material having a dielectric constant greater than 12; as well as A residue removal process is performed to remove residue from the substrate without damaging the metal-containing dielectric material, wherein the residue removal process includes a chemical mechanical polishing process.

14. The method of claim 13, wherein the metal-containing dielectric material is made of a material selected from the group consisting of: a hafnium oxide (HfO x ), AlN, WSiO2, WSi, AlON, TiN, TaN, TiON, TaON, zirconia (ZrO x ), titanium oxide (TiO x ), tantalum oxide (TaO x ), niobium oxide (NbO x ), iron oxide (FeO x ), yttrium oxide (YO x ) and aluminum oxide (AlO x ).

15. The method of claim 13, wherein the residue removal process further comprises an etching process.

16. The method of claim 13, wherein the residue has a diameter less than 30 nm but greater than 2 nm.

17. A method for removing residue from a substrate, comprising: performing a selective deposition process by an atomic layer deposition process to form a metal-containing dielectric material on a metal material on a substrate and leaving a residue on the dielectric material on the substrate, the metal-containing dielectric material being formed on a surface of a cover layer and a surface of an adhesive layer, the cover layer being embedded in the adhesive layer, and the adhesive layer being embedded in an insulating layer disposed on the substrate; as well as A residue removal process is performed to remove residue from the substrate without damaging the metal-containing dielectric material, wherein the residue has a diameter less than 30 nm but greater than 2 nm, and wherein the residue removal process comprises a chemical mechanical polishing process. The method of claim 17 , wherein the residue removal process further comprises an etching process.