Water-based silica sol gel inorganic zinc-rich primer and preparation method thereof
A sol-gel, inorganic zinc-rich technology
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2021-01-08
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 1
Abstract
Description
technical field
[0001] The invention relates to a coating paint, in particular to a steel anticorrosion protective paint which can be used in harsh and harsh marine environments and an anticorrosion protective paint which can be used for the inner wall of a solvent storage tank, and a preparation method and a construction method thereof. Background technique
[0002] Steel is one of the most important industrial materials. Among the many measures to prevent and delay the corrosion of steel, the most economical and effective is to use coatings for anti-corrosion protection. For offshore and coastal bridges, ships, storage tanks, drilling platforms, pipe racks, oil pipelines, tanks and other large steel structures and steel equipment, coatings are almost the only effective protective measures available. As an important variety of steel anti-corrosion coatings, zinc-rich coatings use the active energy of zinc powder to form electrochemical cathodic protection to effectively pro...
Examples
Embodiment 1
[0045] The components of water-based silica sol gel inorganic zinc-rich paint are:
[0046] Component A
[0047] Aqueous silica sol gel: 36.7g (14.7%)
[0048] Deionized water: 24.2g (9.7%)
[0049] Auxiliary 3.1g (1.2%) - specifically composed of 0.1g bactericide, 0.2g defoamer, 0.5g dispersant, 2.2g anti-settling thixotropic agent: 0.1g wetting and leveling agent;
[0050] Zinc oxide: 1.5g (0.6%)
[0051] Zinc chloride: 3.0g (1.2%)
[0052] Silica powder: 28.5g (12.6%)
[0053] Component B:
[0054] 500 mesh spherical active zinc powder: 150g
[0055] Put 36.7g of water-based silica sol gel liquid and 1.8g of organosilane polymer into 24.2g of deionized water, add 0.1g of bactericide, 0.2g of defoamer, 0.5g of dispersant, 2.2g of anti-sedimentation thixotropic agent, 0.1g Wetting and leveling agent, after uniform mixing, put in 1.5g of zinc oxide, 1.5g of zinc chloride, 30.0g of silicon micropowder, disperse evenly through high-speed shearing, and prepare a paint to o...
Embodiment 2
[0058] The components of water-based silica sol gel inorganic zinc-rich paint are:
[0059] Component A
[0060] Aqueous silica sol gel: 34.7g (15.2%)
[0061] Deionized water: 18.3g (8.0%)
[0062] Auxiliary 4.1g (1.8%) - specifically composed of 0.1g bactericide, 0.2g defoamer, 1.5g dispersant, 2.2g anti-settling thixotropic agent: 0.1g wetting and leveling agent;
[0063] Zinc oxide: 3.5g (1.5%)
[0064] Zinc chloride: 2.3g (1.0%)
[0065] Feldspar powder: 5.8g (2.5%)
[0066] Component B:
[0067] 500 mesh spherical active zinc powder: 160g
[0068] Put 34.7g of aqueous silica sol gel liquid and 2.0g of organosilane polymer into 18.3g of deionized water, add 0.1g of bactericide, 0.2g of defoamer, 1.5g of dispersant, 2.2g of anti-sedimentation thixotropic agent, 0.1g Wetting and leveling agent, after mixing evenly, put in 3.5g zinc oxide, 2.3g zinc oxide, 5.8g feldspar powder, disperse evenly through high-speed shearing, blend into paint, and obtain component A;
[...