Nanocrystalline NdFeB magnet and preparation method thereof

By refining raw material particles and introducing neodymium-rich grain boundary phases, nanocrystalline neodymium-ferrobor magnets are prepared, which solves the problem of degradation in performance of neodymium-ferrobor magnets at high temperatures, and achieves improvement in high-temperature magnetic performance and cost reduction, which is suitable for industrial production .

CN112216460BActive Publication Date: 2024-11-08SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910629057.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-07-12
Publication Date
2024-11-08
Estimated Expiration
2039-07-12

AI Technical Summary

Technical Problem

The existing neodymium iron boron magnets have severe thermal demagnetization at high temperatures, and the coercive force and maximum magnetic energy product are reduced. The cost is high when increasing the coercive force by replacing the heavy rare earth element dysprosium, and the complex operation of the grain boundary diffusion process is not conducive to industrial production.

Method used

By refining the raw material particles, introducing neodymium-rich grain boundary phase, inhibiting grain growth during the sintering process, nanocrystalline neodymium-ferrobor magnets are prepared, and hot pressing sintering and heating of the main phase alloy powder and the grain boundary alloy powder are used. Deformation treatment, control the grain size between 150nm-250nm.

Benefits of technology

It improves the high-temperature magnetic properties, coercive force temperature coefficient and maximum magnetic energy product of neodymium iron boron magnets, reduces production costs, simplifies the process flow, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112216460B_ABST
    Figure CN112216460B_ABST
Patent Text Reader

Abstract

The present invention provides a nanocrystalline NdFeB magnet and a preparation method thereof, wherein the preparation method comprises the following steps: providing a main phase alloy powder, wherein the main phase alloy powder is composed of R x Fe (100‑x‑y‑z) M y B z , wherein R is one or more of Nd, Ce, and Pr, M is one or more of Co, Ga, Cu, and Al, 12≤x≤15, 0.1≤y≤8, and 4≤z≤8; providing a grain boundary phase alloy powder, wherein the grain boundary phase alloy powder is composed of Nd in atomic percentage. a Fe (100‑a‑b‑c) Ga b Cu c , wherein 55≤a≤65, 15≤b≤25, 0≤c≤10; the main phase alloy powder and the grain boundary phase alloy powder are uniformly mixed to obtain a mixed powder; the mixed powder is hot pressed and sintered to obtain a hot pressed block; the hot pressed block is subjected to a thermal deformation treatment to orient the grains therein to obtain the nanocrystalline NdFeB magnet, wherein the grain size in the nanocrystalline NdFeB magnet is 150nm-250nm. The nanocrystalline NdFeB magnet according to the present invention has better high temperature magnetic properties, and the preparation method is simple and easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth permanent magnetic materials, and in particular to a nanocrystalline neodymium iron boron magnet and a preparation method thereof. Background Art

[0002] NdFeB permanent magnet materials are currently widely used in aerospace, power electronics, medical equipment, transportation and other fields due to their excellent permanent magnetic properties. In recent years, with the vigorous development of new energy industries such as wind power generation and electric vehicles, the demand for NdFeB magnets that can meet high temperature (>150℃) applications has increased dramatically. The coercive force and maximum magnetic energy product at 180℃ and the coercive force temperature coefficient are three important parameters for evaluating the high temperature performance of magnets.

[0003] Due to the low Curie temperature of NdFeB magnets (312°C), thermal demagnetization is serious at higher operating temperatures, resulting in a serious decrease in the maximum magnetic energy product at high temperatures. At present, in order to meet the higher coercive force requirements of NdFeB magnets at high temperatures, the industry replaces the neodymium element with the heavy rare earth element dysprosium. However, the addition of heavy rare earth elements increases the coercive force at the expense of the magnetic energy product, and the high price of dysprosium is not conducive to the production of low-cost magnets.

[0004] In recent years, domestic and foreign researchers have developed a grain boundary diffusion technology for low melting point eutectic alloys that do not contain heavy rare earth elements. This technology can transform eutectic alloys such as Nd 70 Cu 30 、Nd 90 Al 10 , Pr 70 Cu 30 The alloy is placed on the surface of the NdFeB magnet. At a certain temperature, the alloy melts and enters the interior of the magnet through the grain boundary, increasing the content of the neodymium-rich phase around the grains. The use of grain boundary diffusion technology not only improves the coercivity of the magnet but also effectively reduces the adverse effects of the reduction of remanence. At the same time, the grain boundary diffusion process can improve the temperature stability of the coercivity to a certain extent. However, the process is complicated to operate and the diffusion depth is limited, which is not conducive to industrial production. Summary of the invention

[0005] The object of the present invention is to provide a method for manufacturing a neodymium iron boron magnet which is easy to produce and has good high temperature magnetic properties.

[0006] Another object of the present invention is to provide a low-cost NdFeB magnet with good high-temperature magnetic properties.

[0007] The inventors have found through repeated studies that the high temperature magnetic properties of NdFeB magnets are closely related to the grain size, so reducing the grain size can effectively improve the high temperature magnetic properties of NdFeB magnets. At the same time, the inventors have also found that the neodymium-rich phase not only has the effect of improving the coercive force of the magnet, but also can further inhibit the growth of grains during the sintering process by introducing the neodymium-rich phase into the grain boundary phase. On this basis, the inventors have found through repeated studies that by refining the raw material particles and introducing the neodymium-rich grain boundary phase to further limit the growth of grains, the grains can be effectively refined and the high temperature magnetic properties of NdFeB magnets can be improved, and the present invention has been completed on this basis.

[0008] The method for preparing a nanocrystalline NdFeB magnet according to the first embodiment of the present invention is characterized by comprising the following steps:

[0009] Provide a main phase alloy powder, wherein the main phase alloy powder is composed of R x Fe (100-x-y-z) M y B z , wherein R is one or more of Nd, Ce, and Pr, M is one or more of Co, Ga, Cu, and Al, 12≤x≤15, 0.1≤y≤8, and 4≤z≤8;

[0010] Provide a grain boundary phase alloy powder, wherein the grain boundary phase alloy powder is composed of Nd a Fe (100-a-b-c) Ga b Cu c , where 55≤a≤65, 15≤b≤25, 0≤c≤10;

[0011] uniformly mixing the main phase alloy powder and the grain boundary phase alloy powder to obtain a mixed powder;

[0012] Hot pressing and sintering the mixed powder to obtain a hot pressed block;

[0013] The hot pressed block is subjected to thermal deformation treatment to orient the grains therein, thereby obtaining the nanocrystalline NdFeB magnet, wherein the grain size of the nanocrystalline NdFeB magnet is 150nm-250nm.

[0014] Furthermore, the content of the grain boundary phase alloy powder in the mixed powder is 6-12wt%.

[0015] Furthermore, the grain size of the main phase alloy powder is 10-100 nm.

[0016] Furthermore, the main phase alloy is prepared by the following steps:

[0017] Mixing ingredients according to the proportion of each element in the main phase alloy powder;

[0018] Mixing the ingredients and melting them under vacuum to obtain a first master alloy;

[0019] Rapidly solidifying the first master alloy in a protective atmosphere to form a first alloy sheet;

[0020] The first alloy sheet is crushed by hydrogen explosion method and pulverized by air jet mill to obtain the main phase alloy magnetic powder.

[0021] Furthermore, the particle size of the grain boundary phase alloy powder is about 150-250 μm, preferably 200 μm.

[0022] Furthermore, the grain boundary phase powder is prepared by the following steps:

[0023] Mixing the ingredients according to the proportion of each element in the grain boundary phase alloy powder;

[0024] The ingredients are mixed and melted under vacuum to obtain a second master alloy;

[0025] Rapidly solidifying the second master alloy in a protective atmosphere to form a second alloy sheet;

[0026] The second alloy sheet is pulverized by hydrogen crushing and air flow milling to obtain the grain boundary phase alloy powder.

[0027] Furthermore, the hot pressing sintering is carried out under vacuum, and the vacuum degree is 1×10- 2 Pa or less, and the hot pressing sintering temperature is 550-650°C, the pressure is 200-400MPa, and the time is 20min-1h.

[0028] Furthermore, the thermal deformation treatment is carried out under vacuum, and the vacuum degree is 1×10- 2 Below Pa, the temperature is 650-700℃, the deformation is 70-75%, and the deformation rate is 0.2-0.4mm / min.

[0029] The nanocrystalline NdFeB magnet according to the second embodiment of the present invention is characterized in that the nanocrystalline NdFeB magnet comprises a main phase and a grain boundary phase.

[0030] The main phase is composed of R x Fe (100-x-y-z) M y B z , wherein R is one or more of Nd, Ce, and Pr, M is one or more of Co, Ga, Cu, and Al, 12≤x≤15, 0.1≤y≤8, and 4≤z≤8;

[0031] The grain boundary phase is composed of Nd in atomic percentage. a Fe(100-a-b-c) Ga b Cu c , where 55≤a≤65, 15≤b≤25, 0≤c≤10,

[0032] The grain size of the nanocrystalline NdFeB magnet is 150nm-250nm.

[0033] Furthermore, the absolute value of the coercive force temperature coefficient of the nanocrystalline NdFeB magnet is 0.38-0.42% / °C, the coercive force at 180°C is 0.60-0.80T, and the maximum magnetic energy product at 180°C is 180-200kJ / m 3 .

[0034] The above technical solution of the present invention has at least one of the following beneficial effects:

[0035] According to the method for preparing the nanocrystalline NdFeB magnet of the embodiment of the present invention, by introducing an effective amount of Nd-rich alloy powder as grain boundary phase alloy powder, not only the coercive force of the NdFeB magnet can be improved, but also the effect of effectively suppressing the growth of grains can be effectively suppressed, thereby effectively improving the high temperature magnetic properties of the NdFeB magnet;

[0036] In addition, by refining the raw material particle size, the high temperature magnetic properties of NdFeB magnets can be further improved;

[0037] In addition, the grain boundary phase powder used is Nd a Fe (100-a-b-c) Ga b Cu c Alloy powders, which do not contain expensive heavy rare earth elements such as dysprosium or terbium, strategic elements such as cobalt or nickel, are low-priced, easily available and relatively inexpensive;

[0038] Moreover, the preparation method of the present invention has significantly stronger advantages than the existing methods in terms of production efficiency, production cost, preparation of large-sized magnets and uniformity of magnet performance.

[0039] The NdFeB magnet prepared by the method for preparing a nanocrystalline NdFeB magnet according to an embodiment of the present invention has an absolute value of a coercive force temperature coefficient of 0.38-0.42% / °C, a coercive force of 0.60-0.80T at 180°C, and a maximum magnetic energy product of 180-200 kJ / m at 180°C. 3 . BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Schematic diagram of the process of preparing a nanocrystalline NdFeB magnet according to an embodiment of the present invention;

[0041] Figure 2is a curve of coercive force measured at different temperatures for the NdFeB magnets according to Example 1 and the comparative example;

[0042] Figure 3 is a curve of the maximum magnetic energy product measured at different temperatures according to Example 1 and the comparative example;

[0043] Figure 4 1 and 2 are backscattered electron scanning images of NdFeB magnets, wherein (a) is a backscattered electron scanning image of the nanocrystalline NdFeB magnet of Example 1 of the present invention, and (b) is a backscattered electron scanning image of a comparative example. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0045] Let's first combine Figure 1 The method for preparing the nanocrystalline NdFeB magnet according to an embodiment of the present invention is described in detail.

[0046] like Figure 1 As shown, the method for preparing a nanocrystalline NdFeB magnet according to an embodiment of the present invention comprises the following steps:

[0047] Step S1, providing a main phase alloy powder, wherein the main phase alloy powder is composed of R x Fe (100-x-y-z) M y B z , wherein R is one or more of Nd, Ce, and Pr, M is one or more of Co, Ga, Cu, and Al, 12≤x≤15, 0.1≤y≤8, and 4≤z≤8.

[0048] Preferably, in order to control the grain size in the final NdFeB magnet, a main phase alloy powder with a grain size of 10-100 nm is selected, and more preferably a main phase alloy powder with a grain size of about 50 nm is selected.

[0049] The main phase alloy powder can be purchased from commercial channels, and preferably, prepared by the following method:

[0050] a) preparing the main phase alloy powder according to the ratio of each element in the main phase alloy powder.

[0051] The raw materials for each component may be alloys or metal oxides thereof.

[0052] b) mixing the ingredients and melting them under vacuum to obtain a first master alloy.

[0053] The specific smelting conditions can adopt existing alloy smelting technology, which will not be described in detail here.

[0054] c) rapidly solidifying the first master alloy in a protective atmosphere to form a first alloy sheet.

[0055] The protective atmosphere may be, for example, a commonly used argon atmosphere, etc. In addition, the rapid solidification method may refer to the method commonly used in preparing alloy sheets, which will not be described in detail here.

[0056] d) Thereafter, the first alloy sheet is crushed by hydrogen explosion method and pulverized by air jet mill to obtain the main phase alloy powder.

[0057] The specific conditions of the hydrogen explosion method and the air flow mill can refer to the conventional method for preparing alloy powders, which will not be described in detail here.

[0058] Step S2, providing a grain boundary phase alloy powder, wherein the grain boundary phase alloy powder is composed of Nd a Fe (100-a-b-c) Ga b Cu c , among which, 55≤a≤65, 15≤b≤25, 0≤c≤10.

[0059] In the present invention, a neodymium-rich phase is introduced as a grain boundary phase to increase the coercive force and further inhibit the grain growth to improve the high-temperature magnetic properties of the magnet.

[0060] As a neodymium-rich phase, the inventors have found through repeated research that neodymium-iron-gallium alloys have a good effect of improving the coercivity of neodymium-iron-boron magnets, inhibiting grain growth, and improving the high-temperature performance of neodymium-iron-boron magnets. In addition, adding copper also helps to improve the coercivity, so preferably, 2≤c≤10.

[0061] In addition, as a grain boundary phase, in order to be better dispersed between the main phase alloy powders so as to effectively inhibit grain growth, the particle size of the grain boundary phase alloy powder is about 150-250 μm, preferably about 200 μm.

[0062] The grain boundary phase alloy powder can be purchased through commercial channels, and preferably, is prepared by alloy pulverization. The specific method can be prepared by referring to the above-mentioned method for preparing the main phase alloy powder, which will not be described in detail here.

[0063] Step S3, mixing the main phase alloy powder and the grain boundary phase alloy powder evenly to obtain a mixed powder.

[0064] The specific method of mixing is not particularly limited, and mixing can be performed by, for example, stirring.

[0065] Step S4, hot pressing and sintering the mixed powder to obtain a hot pressed block.

[0066] After mixing, the mixed powder is hot pressed and sintered to prepare a hot pressed block.

[0067] Specifically, the hot pressing sintering is carried out under vacuum conditions, and the vacuum degree is 1×10- 2 Below Pa.

[0068] In addition, the hot pressing sintering temperature is 550-650° C., preferably 600° C.; the pressure is 200-400 MPa, preferably 300 MPa; and the time is 20 min-1 h, preferably 30 min.

[0069] Step S5, subjecting the alloy block to thermal deformation treatment to orient the grains therein to obtain the nanocrystalline NdFeB magnet.

[0070] After the hot-pressed block is obtained, in order to obtain the desired magnetic properties, it needs to be subjected to a heat deformation treatment so that the grains therein are oriented.

[0071] Specifically, the thermal deformation process is carried out under vacuum conditions, and the vacuum degree is 1×10- 2 Below Pa.

[0072] Preferably, the temperature of the thermal deformation treatment is 650-700°C, preferably 675°C; the deformation amount is 70-75%, preferably 75%; the deformation rate is 0.2-0.4 mm / min, preferably 0.3 mm / min.

[0073] By the above method, the grain size of the obtained nanocrystalline NdFeB magnet can be controlled within 150nm-250nm. The absolute value of the coercive force temperature coefficient of the nanocrystalline NdFeB magnet is 0.38-0.42% / °C, with better thermal stability, and the coercive force at 180°C is as high as 0.60-0.80T, and the maximum magnetic energy product at 180°C is as high as 180-200kJ / m 3 , compared with existing reports, it has higher high-temperature magnetic properties.

[0074] The method for preparing the nanocrystalline NdFeB magnet according to the embodiment of the present invention is further described in detail below in conjunction with specific embodiments.

[0075] Example 1

[0076] The chemical formula of the main phase alloy powder is Nd 13.6 Fe 73.6 Ga0.6 Co 6.6 B 5.6 The chemical formula of the grain boundary phase alloy powder is Nd 60 Fe 15 Ga 20 The mass fraction of Cu5.NdFeGaCu alloy powder is 8% of the mixed magnetic powder.

[0077] 1. Preparation of main phase alloy powder: Raw materials with a purity greater than 99% (raw materials are neodymium ingots, iron ingots, gallium ingots, cobalt ingots and ferroboron ingots) are prepared according to the nominal composition of Nd 13.6 Fe 73.6 Ga 0.6 Co 6.6 B 5.6 After proportioning, it is melted in a vacuum arc furnace with a vacuum degree of 1×10- 2 Below Pa, high-power electricity is sent to melt the raw materials quickly, and electromagnetic stirring is used to make the composition uniform. The current is turned off and the alloy liquid is allowed to cool. The above steps are repeated in the melting furnace for more than 5 times to obtain the main alloy ingot.

[0078] After that, the main alloy ingot is roughly crushed and rapidly solidified in a vacuum rapid quenching furnace, that is, the main alloy is melted under an argon protective atmosphere and sprayed onto a copper roller with a rotation speed of 30m / s to prepare an alloy strip with a thickness of about 20 to 50 microns.

[0079] Next, the alloy ribbon was subjected to hydrogen explosion and air flow grinding process. The specific process was to evacuate the hydrogen explosion furnace to 2×10- 3 Pa, and then filled with high-purity hydrogen to 0.4MPa, the alloy absorbed hydrogen and exploded, and then vacuumed and dehydrogenated at 600℃. The alloy powder after hydrogen explosion was jet milled under nitrogen protection to prepare magnetic powder with an average grain size of 50nm. The specific measurement method of the energy size is: in at least 5 backscattered electron scanning images at a magnification of 40,000, at least 50 grains are selected in each image, and the average grain size is calculated using the intercept method.

[0080] Preparation of grain boundary phase alloy powder: Raw materials with a purity greater than 99% (the raw materials are neodymium ingots, iron ingots, gallium ingots, and copper ingots) are prepared according to the composition of Nd 60 Fe 15 Ga 20 Cu5 is mixed in a furnace, and alloy powder particles of about 200 microns are prepared by rapid solidification and ball milling. The specific preparation process is the same as that of the main phase alloy powder, and its detailed description is omitted here.

[0081] Preparation of nanocrystalline NdFeB magnets: The main phase alloy powder and the grain boundary phase alloy powder are mixed evenly, wherein the mass fraction of the grain boundary phase alloy powder is 8wt% of the mixed powder. Thereafter, the mixed powder is loaded into a mold and first hot-pressed and sintered in a vacuum hot-pressing furnace at a temperature of 600°C, a pressure of 300MPa, and a time of 30min to obtain a dense, isotropic NdFeB permanent magnet with a size of Φ10mm×14mm. Then, a thermal deformation treatment is performed at a thermal deformation temperature of 675°C, a deformation amount of about 75%, and a deformation rate of 0.2-0.4mm / min to obtain an anisotropic NdFeB permanent magnet with a size of Φ25mm×3.5mm. Both the hot-pressing sintering and thermal deformation processes are carried out under vacuum, and the vacuum degree is not less than 1×10- 2 Pa.

[0082] The grain size of the obtained anisotropic NdFeB permanent magnet is 210 nm (the measurement method of the grain size refers to the measurement method of the main phase alloy powder mentioned above).

[0083] Example 2

[0084] Compared with the above-mentioned Example 1, except that the mass fraction of the grain boundary phase alloy powder in the mixed powder is changed to 10wt%, the rest is the same as Example 1, and the detailed description thereof is omitted here.

[0085] Example 3

[0086] Compared with the above-mentioned Example 1, in addition to changing the grain boundary phase alloy powder composition to Nd 62 Fe 15 Ga 15 Except for Cu8, the rest are the same as those in Example 1, and the detailed description thereof is omitted here.

[0087] Comparative Example

[0088] In order to further illustrate the effect of the preparation method of the present invention, as a comparison, the same main phase alloy powder as in Example 1 is used, and the same hot pressing sintering and thermal deformation treatment as in Example 1 are carried out without introducing the grain boundary phase alloy powder, to obtain an undoped anisotropic NdFeB permanent magnet.

[0089] For the permanent magnets obtained in the above-mentioned Example 1 and the comparative example, the coercive force and the maximum magnetic energy product were measured as a function of temperature. The results are shown in Figure 2 and Figure 3 .

[0090] Depend on Figure 2It can be seen that compared with the comparative example, the NdFeB magnet prepared by the preparation method of the present invention has a significantly improved temperature coefficient of coercive force, that is, the temperature stability of the magnet is improved, and its coercive force at high temperature (above about 160°C) is greatly improved, which can meet the application requirements.

[0091] Depend on Figure 3 It can be seen that compared with the comparative example, the NdFeB magnet prepared by the preparation method of the present invention has a maximum magnetic energy product at high temperature (above about 160° C.) significantly higher than that of the comparative example, and can meet the application requirements.

[0092] In addition, the magnetic properties of the permanent magnets obtained in Examples 1 to 3 and Comparative Example at 180° C. were measured. The results are shown in Table 1.

[0093] The equipment used to measure the magnetization curve of the magnet is a comprehensive physical property measurement system, model Quantum DesignPPMS-9T EC-II.

[0094] The coercivity temperature coefficient is calculated by the following formula:

[0095] β=[H T2 -H T1 ] / [H T1 ×(T2-T1)]

[0096] Where β represents the coercivity temperature coefficient, H T2 represents the coercivity at temperature T2, H T1 In the present invention, the coercive force at 180°C and 25°C is measured respectively, and the coercive force temperature coefficient is calculated by the above formula.

[0097] Table 1 Magnetic properties at 180°C

[0098]

[0099] It can be seen from Table 1 above that the NdFeB magnet prepared by the preparation method of the present invention has significantly higher high-temperature magnetic properties than undoped permanent magnets. That is to say, the present invention can effectively improve the high-temperature magnetic properties of the NdFeB magnet by introducing NdFeGCu alloy as a grain boundary phase to inhibit grain growth.

[0100] Figure 4 Figure 2 shows a backscattered electron scan of a NdFeB magnet. Figure 4It can be seen that, compared with the magnet of the comparative example shown in (b), the nanocrystalline NdFeB magnet of Example 1 of the present invention shown in (a) has a grain size controlled at about 210 nm, and a certain amount of grain boundary phase (rich in neodymium, gallium and copper elements) is dispersed between the grains. This makes the nanocrystalline NdFeB magnet of the present invention have better high-temperature magnetic properties.

[0101] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a nanocrystalline NdFeB magnet, characterized in that: The steps include: Provide a main phase alloy powder, wherein the main phase alloy powder is composed of R x Fe (100-x-y-z) M y B z , wherein R is one or more of Nd, Ce, and Pr, M is one or more of Co, Ga, Cu, and Al, 12≤x≤15, 0.1≤y≤8, and 4≤z≤8; Provide a grain boundary phase alloy powder, wherein the grain boundary phase alloy powder is composed of Nd a Fe (100-a-b-c) Ga b Cu c , where 55≤a≤65, 15≤b≤25, 0≤c≤10; The main phase alloy powder and the grain boundary phase alloy powder are uniformly mixed to obtain a mixed powder; Hot pressing and sintering the mixed powder to obtain a hot pressed block; The hot pressed block is subjected to a thermal deformation treatment to orient the grains therein, thereby obtaining the nanocrystalline NdFeB magnet, wherein the grain size of the nanocrystalline NdFeB magnet is 150nm-250nm, The grain size of the main phase alloy powder is 10-100nm.

2. The method for preparing a nanocrystalline NdFeB magnet according to claim 1, characterized in that: The content of the grain boundary phase alloy powder in the mixed powder is 6-12wt%.

3. The method for preparing a nanocrystalline NdFeB magnet according to claim 1, characterized in that: The main phase alloy powder is prepared by the following steps: Mixing ingredients according to the proportion of each element in the main phase alloy powder; Mixing the ingredients and melting them under vacuum to obtain a first master alloy; Rapidly solidifying the first master alloy in a protective atmosphere to form a first alloy sheet; The first alloy sheet is crushed by hydrogen explosion method and pulverized by air jet mill to obtain the main phase alloy powder.

4. The method for preparing a nanocrystalline NdFeB magnet according to claim 1, characterized in that: The grain size of the grain boundary phase alloy powder is 150-250 μm.

5. The method for preparing a nanocrystalline NdFeB magnet according to claim 4, characterized in that: The grain boundary phase powder is prepared by the following steps: Mixing the ingredients according to the proportion of each element in the grain boundary phase alloy powder; The ingredients are mixed and melted under vacuum to obtain a second master alloy; Rapidly solidifying the second master alloy in a protective atmosphere to form a second alloy sheet; The second alloy sheet is pulverized by hydrogen crushing and air flow milling to obtain the grain boundary phase alloy powder.

6. The method for preparing a nanocrystalline NdFeB magnet according to claim 1, characterized in that: The hot pressing sintering is carried out under vacuum, and the vacuum degree is 1×10 -2 Pa or less, and the hot pressing sintering temperature is 550-650°C, the pressure is 200-400MPa, and the time is 20min to 1h.

7. The method for preparing a nanocrystalline NdFeB magnet according to claim 1, characterized in that: The thermal deformation treatment is carried out under vacuum, and the vacuum degree is 1×10 -2 Below Pa, the temperature is 650-700℃, the deformation is 70~75%, and the deformation rate is 0.2-0.4mm / min.

8. A nanocrystalline NdFeB magnet obtained by the method for preparing a nanocrystalline NdFeB magnet according to claim 1, characterized in that: The nanocrystalline NdFeB magnet includes a main phase and a grain boundary phase. The main phase is composed of R x Fe (100-x-y-z) M y B z , wherein R is one or more of Nd, Ce, and Pr, M is one or more of Co, Ga, Cu, and Al, 12≤x≤15, 0.1≤y≤8, and 4≤z≤8; The grain boundary phase is composed of Nd in atomic percentage. a Fe (100-a-b-c) Ga b Cu c , where 55≤a≤65, 15≤b≤25, 0≤c≤10, The grain size of the nanocrystalline NdFeB magnet is 150nm-250nm.

9. The nanocrystalline NdFeB magnet according to claim 8, characterized in that: The absolute value of the coercive force temperature coefficient of the nanocrystalline NdFeB magnet is 0.38-0.42% / °C, the coercive force at 180°C is 0.60-0.80 T, and the maximum magnetic energy product at 180°C is 180-200 kJ / m 3 .