Negative electrode for lithium secondary battery and lithium secondary battery containing the same
Through spherical natural graphite negative electrode material and asphalt filling technology, the problem of volume expansion/shrinkage of lithium secondary batteries during charging/discharging is solved, the durability and expansion performance of the battery are improved, side reactions are reduced, and the battery is extended Service life.
Patent Information
- Application Number
- CN202080003280.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-02-01
- Filing Date
- 2020-01-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-01-31
AI Technical Summary
The natural graphite anode material of existing lithium secondary batteries has volume expansion/shrinkage problems during charging/discharging, resulting in poor long-term durability and increased side reactions, affecting battery performance.
Spherical natural graphite is used as the negative electrode active material, and asphalt is filled on its surface to form a carbon layer. The negative electrode active material layer is formed by drying and pressing, increasing the BET specific surface area and total pore volume to reduce side reactions with the electrolyte.
It effectively suppresses the volume expansion/contraction of the lithium secondary battery during charging/discharging, improves the durability and expansion performance of the negative electrode, reduces the growth of the solid electrolyte interface, and extends the cycle life of the battery.
Smart Images

Figure BDA0002833481680000231
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode for a lithium secondary battery and a lithium secondary battery comprising the negative electrode.
[0002] This application claims the benefit of Korean Patent Application No. 10-2019-0013772 filed in the Korean Intellectual Property Office on February 1, 2019, the disclosure of which is incorporated herein by reference in its entirety. Background Art
[0003] Recently, with the rapid and widespread use of electronic devices such as mobile phones, laptop computers and electric vehicles using batteries, the demand for secondary batteries with smaller size, lighter weight and larger capacity has been growing. In particular, lithium secondary batteries have received widespread attention as power sources for portable devices due to their advantages of light weight and high energy density. In this case, many research and development attempts have been made to improve the performance of lithium secondary batteries.
[0004] At present, the negative electrode active materials of lithium secondary batteries mainly include natural graphite and artificial graphite available on the market. In particular, when compared with artificial graphite, it is known that natural graphite negative electrode active materials have higher adhesion strength, higher capacity, higher rolling performance and excellent price competitiveness. Although natural graphite negative electrode active materials have these advantages, it is known that natural graphite has poor long-term durability and expansion performance than artificial graphite due to large volume expansion / contraction during charging / discharging. Therefore, the industry has tried to combine natural graphite with artificial graphite instead of using only natural graphite for negative electrode active materials, but in this case, there is still a problem of volume expansion / contraction of natural graphite during charging / discharging of lithium secondary batteries.
[0005] In order to solve the problem of side reactions between natural graphite negative electrode active materials and electrolytes, it has been proposed to improve the life characteristics of natural graphite by spheroidizing natural graphite and coating the surfaces of natural graphite particles with asphalt or polymer resin to form a carbon layer by heat treatment. However, a carbon layer of asphalt or polymer resin is not formed in the pores of the particles of the natural graphite negative electrode active material manufactured as described above, resulting in a high specific surface area of natural graphite and exposure of natural graphite to the electrolyte, resulting in side reactions with the electrolyte. Summary of the invention
[0006] Technical issues
[0007] In order to solve the above problems, the present invention aims to provide a negative electrode for a lithium secondary battery, the negative electrode comprising a spherical natural graphite negative electrode active material that does not expand / contract during charge / discharge.
[0008] In addition, the present invention aims to provide a negative electrode for a lithium secondary battery, the negative electrode comprising a spherical natural graphite negative electrode active material that does not cause a side reaction with an electrolyte during charge / discharge of the lithium secondary battery.
[0009] The present invention also aims to provide a lithium secondary battery, wherein the lithium secondary battery comprises the negative electrode for the lithium secondary battery.
[0010] The present invention also aims to provide a method for manufacturing the negative electrode for the lithium secondary battery.
[0011] Technical Solution
[0012] According to a first embodiment of the present invention, there is provided a negative electrode for a lithium secondary battery comprising a negative electrode active material layer, wherein the negative electrode active material layer is formed by coating a negative electrode mixture slurry comprising spherical natural graphite particles as a negative electrode active material on at least one surface of a negative electrode current collector, followed by drying and pressing, and the spherical natural graphite particles comprise a plurality of pores in which pitch is inserted, and wherein the Brunauer-Emmett-Teller (BET) specific surface area of the negative electrode active material layer after pressing is greater than the BET specific surface area of the negative electrode active material layer before pressing, and the difference between the BET specific surface areas before and after pressing is within 0.9 m 2 / g to 1.2m 2 / g range.
[0013] According to a second embodiment of the present invention, in the first embodiment, a negative electrode for a lithium secondary battery is provided, wherein the BET specific surface area of the negative electrode active material layer after pressing is greater than the BET specific surface area of the negative electrode active material layer before pressing, and the difference in the BET specific surface area before and after pressing is within 0.9 m 2 / g to 1.1m 2 / g range.
[0014] According to a third embodiment of the present invention, in the first or second embodiment, there is provided a negative electrode for a lithium secondary battery, wherein the negative electrode active material is composed of spherical natural graphite including the plurality of pores in which the pitch is inserted.
[0015] According to a fourth embodiment of the present invention, in any one of the first to third embodiments, there is provided a negative electrode for a lithium secondary battery, wherein the negative electrode active material layer after compression has a thickness of 3.3 m 2 / g to 3.8m 2 / g in the range of BET specific surface area.
[0016] According to a fifth embodiment of the present invention, in any one of the first to fourth embodiments, there is provided a negative electrode for a lithium secondary battery, wherein the total pore volume of the negative electrode active material layer after pressing is greater than the total pore volume of the negative electrode active material layer before pressing, and the difference in total pore volume before and after pressing is within 8×10 -3 cm 3 / g to 9×10 -3 cm 3 / g range.
[0017] According to a sixth embodiment of the present invention, in any one of the first to fifth embodiments, there is provided a negative electrode for a lithium secondary battery, wherein the negative electrode has an orientation degree of 14 to 23 after pressing. 004 / I 110 value.
[0018] According to a seventh embodiment of the present invention, there is provided a lithium secondary battery including the negative electrode for a lithium secondary battery defined in any one of the first to sixth embodiments.
[0019] According to an eighth embodiment of the present invention, there is provided a method for manufacturing a negative electrode for a lithium secondary battery as defined in the first embodiment, the method comprising the following steps: (S1) coating spheroidized natural graphite with asphalt; (S2) forming a negative electrode active material layer comprising the spheroidized natural graphite as a negative electrode active material on at least one surface of an electrode current collector; and (S3) pressing the negative electrode active material layer obtained in step (S2) by a pressing roller at 23° C. to 25° C. to obtain a pressed negative electrode active material layer, so that the Brewer-Emmett-Teller (BET) specific surface area of the pressed negative electrode active material layer is greater than the BET specific surface area of the negative electrode active material layer before pressing, and the difference in BET specific surface area before and after pressing is within 0.9 m 2 / g to 1.2m 2 / g range.
[0020] According to a ninth embodiment of the present invention, in the eighth embodiment, a manufacturing method is provided, wherein in the step (S2), the BET specific surface area of the negative electrode active material layer before pressing is 2.4 m 2 / g to 2.6m 2 / g.
[0021] According to a tenth embodiment of the present invention, in the eighth or ninth embodiment, there is provided a manufacturing method, wherein in the step (S2), the negative electrode active material layer before pressing has a thickness of 20×10 -3 cm 3 / g to 30×10 -3 cm 3 The total pore volume is in the range of 1000 Å / g.
[0022] According to an eleventh embodiment of the present invention, in any one of the eighth to tenth embodiments, a manufacturing method is provided, wherein the step (S3) comprises pressing the negative electrode active material layer obtained in the step (S2) by a pressing roller at 23° C. to 25° C. to obtain a pressed negative electrode active material layer, so that the total pore volume of the pressed negative electrode active material layer is greater than the total pore volume of the negative electrode active material layer before pressing, and the difference in the total pore volume before and after pressing is within 8×10 -3 cm 3 / g to 9×10 - 3 cm 3 / g range.
[0023] According to a twelfth embodiment of the present invention, in any one of the eighth to eleventh embodiments, there is provided a manufacturing method, wherein in the step (S3), the BET specific surface area of the negative electrode active material layer after compression is 3.3 m 2 / g to 3.8m 2 / g.
[0024] Beneficial Effects
[0025] The negative electrode for lithium secondary battery according to the present invention uses spherical natural graphite active material particles having multiple pores in which asphalt is inserted to fill the void space of the pores as an active material, thereby reducing the side reaction between the active material and the electrolyte during charge / discharge. As a result, the growth of the solid electrolyte interface (SEI) occurring due to the side reaction can be suppressed.
[0026] In addition, the negative electrode for the lithium secondary battery according to the present invention uses spherical natural graphite active material particles having multiple pores in which asphalt is inserted to fill the void spaces of the pores as the negative electrode active material, thereby reducing the change in the total pore volume of the negative electrode before and after pressing the negative electrode and the change in the BET specific surface area of the negative electrode, and ultimately solving the problem of volume expansion / contraction of the spherical natural graphite negative electrode active material during charging / discharging of the lithium secondary battery.
[0027] Furthermore, the negative electrode for a lithium secondary battery according to the present invention has a low orientation degree of a pressed electrode and improved expansion properties. DETAILED DESCRIPTION
[0028] These and other advantages and features of the present invention and methods for achieving them will be apparent by reference to the embodiments described in detail below. However, the present invention is not limited to the embodiments disclosed below and will be implemented in many different forms, and these embodiments are provided to make the present invention complete and fully explain the scope of the present invention to those skilled in the art to which the present invention belongs, and the present invention is limited only by the scope of the appended claims.
[0029] Hereinafter, the present invention will be described in more detail.
[0030] According to the present invention, there is provided a negative electrode for a lithium secondary battery comprising a negative electrode active material layer, wherein the negative electrode active material layer is formed by coating a negative electrode mixture slurry comprising spheroidized natural graphite as a negative electrode active material on at least one surface of a negative electrode current collector, followed by drying and pressing, the spheroidized natural graphite comprising a plurality of pores in which pitch is inserted, and the negative electrode active material layer has a thickness of 0.9 m 2 / g to 1.2m 2 / g of (Brewer-Emmett-Teller (BET) specific surface area of the negative electrode active material layer after pressing)-(BET specific surface area of the negative electrode active material layer before pressing).
[0031] The BET specific surface area refers to the surface area of a powder or a bulk measured by the amount of nitrogen physically adsorbed onto the entire surface of the powder or the bulk in order to measure the specific surface area of the powder or the bulk.
[0032] According to an embodiment of the present invention, a method of measuring the BET specific surface area is as follows.
[0033] First, the completely dried negative electrode active material layer was cut into a size of 8 mm × 8 mm to prepare 30 samples. In this case, the thickness of the negative electrode active material layer can be about 80 μm, and the loading capacity can be controlled to 3.6 mAh / cm 2 . The sampled negative electrode active material layer is placed in a standard sample cell (glass) and dried at 130°C for 2 hours under vacuum conditions. In order to measure in a liquid nitrogen container at 77K, liquid nitrogen is loaded into the liquid nitrogen container. The standard cell is cooled, and in order to measure under liquid nitrogen conditions, the standard sample cell is fixed to a measuring instrument (BEL Japan, BELSORP-mino II). Subsequently, the measurement program is started to measure the BET specific surface area by adsorption / desorption on the sampled electrode surface in a nitrogen environment. When measuring the BET specific surface area, the total pore volume can be measured together.
[0034] In the negative electrode active material layer, (BET specific surface area of the negative electrode active material layer after pressing)-(BET specific surface area of the negative electrode active material layer before pressing) (i.e., the difference between the BET specific surface areas of the negative electrode active material layer before and after pressing) is 0.9 m 2 / g to 1.2m 2 / g, and according to an embodiment of the present invention, the difference in BET specific surface area can be 0.9m 2 / g to 1.1m 2 / g, or 0.9m 2 / g to 1.0m 2 / g.
[0035] When the difference in BET specific surface area between the negative electrode active material layer before and after pressing is less than 0.9 m 2 / g, too much asphalt is coated on the surface of the negative electrode active material layer, resulting in a decrease in the capacity and energy density of the lithium secondary battery using the negative electrode active material layer, and when the difference in the BET specific surface area of the negative electrode active material layer before and after pressing exceeds 1.2 m 2 / g, there are many pores in the negative electrode active material layer, the side reaction between the electrolyte and the negative electrode active material in these pores is significantly increased, the expansion of the negative electrode is sharply increased, the cycle life of the lithium secondary battery using the negative electrode active material layer is reduced, and the battery is degraded.
[0036] According to an embodiment of the present invention, the negative electrode active material of the negative electrode mixture slurry may include spheroidized natural graphite, preferably consists essentially of spheroidized natural graphite, and more preferably consists only of spheroidized natural graphite.
[0037] In the present invention, "spheroidized natural graphite" refers to natural graphite having a nearly spherical shape, and not all natural graphite particles are controlled to have an ideal spherical shape.
[0038] According to an embodiment of the present invention, the spheroidized carbon-based negative active material may have a circularity of 0.82 to 0.98, or 0.88 to 0.92.
[0039] The circularity may be a value obtained by dividing the circumference of a circle of the same area as the projected image of the negative electrode active material by the circumference of the projected image, and specifically, the circularity may be given by the following Equation 1. The circularity may be measured using a particle shape analyzer such as Malvern Sysmex FPIA3000.
[0040] [Equation 1]
[0041] Circularity = circumference of a circle with the same area as the projected image of the active material / circumference of the projected image
[0042] The spheroidized natural graphite produced as described above can have an average particle size (D) of 10 μm to 25 μm, or 12 μm to 20 μm, or 12 μm to 16 μm by rounding the edges. 50 ), but are not limited to them.
[0043] When the average particle size of spheroidized natural graphite (D 50 ) is less than 10 μm, the capacity may be low and the rolling performance may be reduced. In addition, when the average particle size (D 50) exceeds 25 μm, since the average particle size of the negative electrode active material particles increases, the insertion and extraction of Li ions may be reduced.
[0044] The average particle size can be measured, for example, using a laser diffraction method or a scanning electron microscope (SEM) image, but the present invention is not limited thereto. The laser diffraction method is generally capable of measuring particle sizes ranging from the submicron range to several millimeters, and is capable of obtaining results with high reproducibility and high resolution. Specifically, after the target powder is dispersed in a dispersion medium and introduced into a commercially available laser diffraction particle size measuring instrument (e.g., Microtrac S3500), the particle size distribution can be calculated by measuring the difference in the diffraction pattern relative to the particle size when the particles pass through the laser beam. In this case, the minimum particle size (D min ) can be measured by calculating the particle size at the minimum particle size point in the cumulative particle number distribution based on the particle size in the measuring instrument, and the average particle size (D 50 ) can be measured by calculating the particle size at the 50% point in the cumulative particle number distribution.
[0045] The spheroidized natural graphite according to the present invention is characterized in that a plurality of pores are present inside and outside the natural graphite particles, and the pores are filled with pitch.
[0046] The negative electrode for a lithium secondary battery according to an embodiment of the present invention can be manufactured using spheroidized natural graphite as a negative electrode active material by a common method widely used in the technical field to which the present invention belongs. Preferably, the negative electrode for a lithium secondary battery according to an embodiment of the present invention can be manufactured using only spheroidized natural graphite as a negative electrode active material by a common method known in the technical field to which the present invention belongs. As a non-limiting example, in an embodiment of the present invention, a negative electrode active material layer can be formed in the following manner: a negative electrode active material containing spheroidized natural graphite is mixed with a binder, a conductive material, a solvent, etc., and stirred to prepare a negative electrode mixture, and the negative electrode mixture is coated on at least one surface of a negative electrode collector, and then dried and pressed.
[0047] In an embodiment of the present invention, in addition to the spheroidized natural graphite of the present invention, the negative electrode active material may also contain at least one of the following at an impurity level: a lithium-containing titanium composite oxide (LTO); a (semi)metal (Me), including Si, Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; an alloy of a (semi)metal (Me); an oxide of a (semi)metal (Me); a composite of a (semi)metal (Me) and carbon.
[0048] The negative electrode active material may be present in an amount of 80 wt % to 99 wt % based on the total weight of the negative electrode mixture.
[0049] The negative electrode collector may generally be 3 μm to 500 μm thick. The negative electrode collector is not limited to any particular type as long as it has high conductivity while not causing a chemical reaction of the corresponding battery, and may include, for example: copper; stainless steel; aluminum; nickel; titanium; sintered carbon; copper or stainless steel treated with carbon, nickel, titanium, silver, etc. on the surface; and aluminum-cadmium alloys, etc. In addition, in the same manner as the positive electrode collector described below, the negative electrode collector may have fine concavoconvexities to enhance the bonding strength of the negative electrode active material, and may be used in various forms such as films, sheets, foils, nets, porous bodies, foams, and non-woven fabrics.
[0050] The binder is a substance that helps bind the conductive material, the active material, and the current collector together, and may generally be present in an amount of 1 wt % to 20 wt % based on the total weight of the negative electrode mixture.
[0051] Non-limiting examples of binders may include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber, and various copolymers.
[0052] The conductive material is a substance for improving conductivity of the negative electrode active material, and may be present in an amount of 1 wt % to 20 wt % based on the total weight of the negative electrode mixture.
[0053] The conductive material is not limited to any particular type as long as it has conductivity without causing a chemical reaction in the corresponding battery, and may include, for example: carbon-based materials such as carbon black (Super P), acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; carbon fluoride; metal powders such as aluminum and nickel powders; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives.
[0054] The solvent may include an organic solvent such as water or N-methyl-2-pyrrolidone (NMP), and when the negative electrode mixture includes a negative electrode active material and optionally includes a binder and a conductive material, the solvent may be present in an appropriate amount to obtain a desired viscosity. For example, the solvent may be present in an amount such that the concentration of the solid containing the negative electrode active material and optionally including a binder and a conductive material is 40% to 70% by weight, preferably 45% to 55% by weight.
[0055] According to an embodiment of the present invention, the negative electrode active material layer formed after pressing may have a thickness of 3.3 μm. 2 / g to 3.8m 2When the BET specific surface area of the negative electrode active material layer satisfies 3.3 m 2 / g to 3.8m 2 / g range, asphalt can be uniformly coated in the pores inside and outside the negative electrode active material layer and on the surface of the negative electrode active material layer, and a reduction in the capacity of a lithium secondary battery using the negative electrode active material layer due to excessive coating of asphalt on the surface of the negative electrode active material layer can be prevented.
[0056] According to an embodiment of the present invention, the total pore volume of the negative electrode active material layer after compression may be lower than the total pore volume of the negative electrode active material layer immediately before compression by 8×10 -3 cm 3 / g to 9×10 -3 cm 3 / g. When the difference in the total pore volume of the negative electrode active material layer satisfies 8×10 -3 cm 3 / g to 9×10 -3 cm 3 When the content of the negative electrode active material layer is within the range of 0.1477 W / g, it is possible to avoid an increase in processing cost exceeding the cost required for fine coating so that the pore volume difference is as described above, and to prevent the expansion performance of the negative electrode after charge / discharge cycles from being deteriorated due to the side reaction between the negative electrode active material layer and the electrolyte.
[0057] The negative electrode including the spheroidized natural graphite according to the present invention has a low orientation degree value, and its expansion performance is improved.
[0058] The orientation degree of the negative electrode can generally be measured by X-ray diffraction (XRD) after the manufactured negative electrode is pressed to a predetermined electrode density, and the obtained value can be expressed as I indicating the ratio of the 004 peak to the 110 peak. 004 / I 110 .
[0059] That is, the orientation degree of the negative electrode (I 004 / I 110 ) is the peak intensity ratio of the (004) plane to the (110) plane obtained by X-ray diffraction analysis in the electrode (I 004 / I 110 ), and the peak intensity ratio can be obtained by X-ray diffraction analysis, and the X-ray diffraction analysis in the electrode refers to the X-ray diffraction analysis performed on the electrode (negative electrode) in which the composite particles are manufactured. The X-ray diffraction analysis can be measured by using Cu-Kα radiation using an X-ray diffraction analyzer Bruker D4 Endeavor, and can be numerically corrected by the Topas3 fitting program.
[0060] I 004 / I110 The smaller the value, the better the isotropic property, and since the negative electrode does not expand in one direction but in multiple directions, the expansion rate is reduced, which can explain the improvement in expansion performance. 004 / I 110 When the value is high, the negative electrode expands only in one direction along the Y axis, and the expansion rate increases, which is not conducive to improving the expansion performance.
[0061] I indicating the orientation degree of the negative electrode containing ordinary natural graphite 004 / I 110 The value is about 40. In contrast, in the negative electrode containing only the spheroidized natural graphite of the present invention as the negative electrode active material, the voids in the spheroidized natural graphite are filled with pitch, and the spheroidized natural graphite is carbon-coated with pitch on the surface, thereby reducing the specific surface area as a whole and improving the isotropic properties of the electrode, and the orientation degree I of the negative electrode is 004 / I 110 The value is 14 to 23, or 16 to 22, or about 16, and the value of the orientation degree of the negative electrode is much lower than that of the existing negative electrode.
[0062] In the present invention, the total pore volume of the negative electrode active material layer can be obtained using a machine used when the BET specific surface area is measured in the same method under the same measurement conditions.
[0063] According to another embodiment of the present invention, there is provided a method for manufacturing a negative electrode for a lithium secondary battery, the method comprising the following steps:
[0064] (S1) coating spheroidized natural graphite with asphalt;
[0065] (S2) forming a negative electrode active material layer containing the spheroidized natural graphite as a negative electrode active material on at least one surface of an electrode current collector, so that the BET specific surface area of the negative electrode active material layer before pressing is 2.4 m 2 / g to 2.6m 2 / g; and
[0066] (S3) compressing the negative electrode active material layer obtained in step (S2) by a pressing roller at a temperature of 23° C. to 25° C. to obtain a pressed negative electrode active material layer, so that the BET specific surface area of the pressed negative electrode active material layer is greater than the BET specific surface area of the negative electrode active material layer before pressing, and the difference between the BET specific surface areas before and after pressing is in the range of 0.9 m 2 / g to 1.2m 2 / g.
[0067] In the (S1) step, the "spheroidized natural graphite" according to the present invention can be manufactured as follows. First, the raw graphite ore is processed into small particles by mechanical treatment. Strong alkali solution treatment and strong acid solution treatment are carried out at high temperature to remove impurities. After washing and drying at high temperature, screening is carried out to mine plate-like natural graphite. In order to turn the plate-like natural graphite into a sphere, primary grinding and secondary grinding, i.e., mechanical processing, are carried out. Subsequently, after acid treatment, washing and drying, purification is carried out to obtain high-purity spherical natural graphite. During mechanical crushing and grinding, the surface of the obtained spherical natural graphite will be damaged, and chemically reactive groups will be formed after strong alkali / strong acid cleaning. During spheroidization, damage occurs in natural graphite due to mechanical processing. Therefore, spherical natural graphite is obtained by carbonizing the pitch on the surface of high-purity solid phase natural graphite at 1100°C to 1500°C to form a carbon coating, and then crushing, screening and iron removal are carried out. In particular, according to an embodiment of the present invention, in order to fill the holes inside and outside the natural graphite with asphalt, the spherical natural graphite is placed in a container, a coating agent is added, and high temperature heating is performed under airtight conditions to fill the voids in the active material particles. The coating agent mainly comprises asphalt, but when the coating agent only comprises asphalt, the negative electrode active material particles finally manufactured may be too hard. In order to reduce the hardness, an auxiliary agent can be used in addition. The actual carbon ratio after carbon coating can be 3% to 10% by weight, or 4% to 10% by weight.
[0068] In this case, the actual carbon ratio can be calculated by the following equation.
[0069] Actual carbon ratio (weight %) = [{(weight of the final negative electrode active material - (weight of natural graphite particles before pitch insertion)} / (weight of the final negative electrode active material)] × 100
[0070] The actual carbon ratio is the amount of pitch inserted into spheroidized natural graphite particles as the final negative electrode active material.
[0071] In this case, the average particle size of the asphalt used as the coating agent may be about 3 μm to 5 μm. In addition, the amount of the asphalt used may be more than twice the actual carbon ratio after carbon coating.
[0072] In the (S2) step, a negative electrode active material layer including the spheroidized natural graphite as a negative electrode active material is formed on at least one surface of an electrode current collector.
[0073] According to an embodiment of the present invention, the negative electrode active material layer before pressing may have a porosity of 40% to 55%. In addition, the total pore volume of the negative electrode active material layer before pressing may be 20×10 -3 cm 3 / g to 30×10 -3 cm 3 / g, or 24×10 -3 cm 3 / g to 27×10 -3 cm 3 / g.
[0074] In step (S3), the BET specific surface area of the negative electrode active material layer after compression can be within 3.3 m 2 / g to 3.8m 2 / g, or 3.4m 2 / g to 3.7m 2 According to an embodiment of the present invention, the negative electrode active material layer may have a -3 cm 3 / g to 9×10 -3 cm 3 / g of (total pore volume of the negative electrode active material layer after compression) - (total pore volume of the negative electrode active material layer before compression), and the porosity of the negative electrode active material layer after compression can be 15% to 35%, or 20% to 33%, or 20% to 32%, or 20% to 28%, or 27% to 32%, 28% to 29%.
[0075] According to an embodiment of the present invention, the dried negative electrode active material can be pressed at least once by a roller press. The temperature of the roller press used can be in a range of, for example, between 23°C and 25°C, and the negative electrode active material layer can be pressed by a roller press. The roller press can be a tandem press, for example, a tandem press (THANK-METAL, a small precision roller press) can be used to press the negative electrode active material layer with an adjustment gap between 30 and 65. In addition, in an embodiment of the present invention, the pressing conditions can be controlled so that the negative electrode active material layer after pressing has a pressing density of 1.5g / cc to 1.6g / cc and a porosity of 15% to 35%, or 20% to 33%, or 20% to 32%, or 20% to 28%, or 27% to 32%, 28% to 29%.
[0076] In addition, an embodiment of the present invention provides a lithium secondary battery.
[0077] Specifically, the lithium secondary battery of the present invention can be manufactured by injecting the nonaqueous electrolyte of the present invention into an electrode structure comprising a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode. In this case, the positive electrode, the negative electrode and the separator constituting the electrode structure may include positive electrodes, negative electrodes and separators commonly used to manufacture lithium secondary batteries.
[0078] In this case, a positive electrode can be manufactured by coating a positive electrode mixture containing a positive electrode active material, a binder, a conductive material, and a solvent on a positive electrode current collector.
[0079] The positive electrode current collector is not limited to any specific type as long as it has conductivity while not causing a chemical reaction in the corresponding battery, and can include, for example: stainless steel; aluminum; nickel; titanium; sintered carbon; or aluminum or stainless steel treated with carbon, nickel, titanium, or silver on the surface.
[0080] The positive electrode active material is a compound capable of reversibly intercalating and deintercalating lithium. Specifically, the positive electrode active material can include, for example, a lithium composite metal oxide containing lithium and at least one of the following metals: cobalt, manganese, nickel, and aluminum. More specifically, the lithium composite metal oxide can include at least one of the following: lithium-manganese-based oxides (such as LiMnO2, LiMn2O4), lithium-cobalt-based oxides (such as LiCoO2), lithium-nickel-based oxides (such as LiNiO2), lithium-nickel-manganese-based oxides (such as LiNi 1- Y Mn Y O2(0 < Y < 1), LiMn 2-Z Ni Z O4(0 < Z < 2)), lithium-nickel-cobalt-based oxides (such as LiNi 1-Y1 Co Y1 O2(0 < Y1 < 1)), lithium-manganese-cobalt-based oxides (such as LiCo 1-Y2 Mn Y2 O2(0 < Y2 < 1), LiMn 2-Z1 Co Z1 O4(0 < Z1 < 2)), lithium-nickel-manganese-cobalt-based oxides (such as Li(Ni p Co q Mn r1 )O2(0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4(0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2)) or lithium-nickel-cobalt-transition metal (M) oxides (such as Li(Ni p2 Co q2 Mn r3 M s2)O2 (where M is selected from: Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are each independently the atomic fraction of the element, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1)). Among them, due to the ability to improve the capacity and stability of the battery, the lithium composite metal oxide can be: LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (e.g., Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2)) or lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O2), and considering the significant improvement effect obtained by controlling the type and amount of the constituent elements of the lithium composite metal oxide, the lithium composite metal oxide can be at least one of the following: Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2.
[0081] Based on the total weight of each cathode mixture, the cathode active material can be present in an amount of 80 wt% to 99 wt%.
[0082] The binder is a substance that helps the binding of the active material and the conductive material and helps the binding with the current collector, and is usually present in an amount of 1 wt% to 30 wt% based on the total weight of the cathode mixture. Examples of the binder can include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber, fluororubber, and various copolymers.
[0083] The conductive material is generally present in an amount of 1 wt % to 30 wt % based on the total weight of the positive electrode mixture.
[0084] The conductive material is not limited to any specific type as long as it has conductivity while not causing a chemical reaction of the corresponding battery, and may include, for example: graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black; conductive fibers such as carbon fibers or metal fibers; fluorinated carbon; metal powders such as aluminum, nickel powders; conductive whiskers such as zinc oxide, potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives. Specific examples of conductive materials on the market may include acetylene black-based products (Chevron Chemical Company) or Denka black (Denka Singapore Private Limited), products from Gulf Oil Company, Ketjen black, EC-based products (Armak Company), Vulcan XC-72 (Cabot Company), and Super-P (Timcal).
[0085] The solvent may include an organic solvent, such as N-methyl-2-pyrrolidone (NMP), and when the positive electrode mixture includes a positive electrode active material and optionally includes a binder and a conductive material, the solvent may be present in an appropriate amount to obtain a desired viscosity. For example, the solvent may be present in an amount such that the concentration of the solid containing the positive electrode active material and optionally including a binder and a conductive material is 50% to 95% by weight, preferably 70% to 90% by weight.
[0086] The separator may include: a porous polymer film commonly used as a separator, for example, a porous polymer film made of a polyolefin polymer such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer and ethylene / methacrylate copolymer, which are used alone or in combination; or an ordinary porous non-woven fabric, for example, a non-woven fabric made of high melting point glass fiber, polyethylene terephthalate fiber, but not limited thereto.
[0087] The electrolyte may include, for example: an organic electrolyte containing a lithium salt dissolved in a non-aqueous solvent; or a polymer electrolyte.
[0088] The non-aqueous solvent constituting the organic electrolyte may include, for example, at least one of the following: propylene carbonate, ethylene carbonate, butylene carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, cyclopentane, dichloroethane, chlorobenzene, nitrobenzene, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, ethyl butyl carbonate, dipropyl carbonate, diisopropyl carbonate, dibutyl carbonate, diethylene glycol and dimethyl ether as well as known solutions for lithium secondary batteries. In particular, the non-aqueous solvent may preferably be a combination of one of propylene carbonate, ethylene carbonate and butyl carbonate and one of dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.
[0089] The lithium salt may include, but is not limited to, lithium salts commonly used in lithium secondary battery electrolytes. For example, the cation may include Li + , and the anion may include at least one of the following: F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - 、AlO4 - 、AlCl4 - PF6 - 、SbF6 - 、AsF6 - 、BF2C2O4 - , BC4O8 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - 、C4F9SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2- 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - These lithium salts can be used alone or in combination as required.
[0090] The polymer electrolyte may include, for example, an organic electrolyte and a (co)polymer that swells well in the organic electrolyte, such as polyethylene oxide, polypropylene oxide, polyacetonitrile, polyvinylidene fluoride, polymethacrylate, polymethyl methacrylate.
[0091] The secondary battery according to the present invention has high energy density, high output, and improved safety and stability, and in particular, can be preferably used in medium and large battery modules. Therefore, the present invention also provides a medium and large battery module including the secondary battery as a unit cell.
[0092] The medium and large-sized battery modules can be preferably used as power sources for devices requiring high output and high capacity, such as electric vehicles, hybrid electric vehicles, and energy storage systems.
[0093] Meanwhile, the present invention relates to a negative electrode for a lithium secondary battery, and the negative electrode for a lithium secondary battery according to the present invention and a lithium secondary battery including the same may be manufactured using various methods known in the technical field to which the present invention pertains.
[0094] Hereinafter, embodiments of the present invention will be described in detail to help understand the present invention. However, embodiments according to the present invention may be modified in many other forms, and should not be interpreted as the scope of the present invention being limited to the following embodiments. Embodiments of the present invention are provided to fully explain the present invention to those of ordinary skill in the art to which the present invention belongs.
[0095] Example 1
[0096] Production of spheroidized natural graphite
[0097] First, the raw graphite ore is processed into small particles by mechanical treatment. Strong alkali solution treatment and strong acid solution treatment are carried out at high temperature to remove impurities. After washing and drying at high temperature, screening is carried out to mine plate-like natural graphite. In order to turn the plate-like natural graphite into a spherical shape, primary grinding and secondary grinding, i.e. mechanical processing, are carried out. Subsequently, after acid treatment, washing and drying, purification is carried out to obtain high-purity spherical natural graphite. During mechanical crushing and grinding, damage will occur on the surface of the obtained spherical natural graphite, and chemically reactive groups will be formed after strong alkali / strong acid cleaning. During spheroidization, defects occur in natural graphite due to mechanical processing. Carbon coating is carried out by solid-phase coating of asphalt (softening temperature of about 130°C) on the surface of damaged high-purity solid phase natural graphite by dry method and carbonizing at about 1200°C in an inert gas atmosphere for about 24 hours, followed by crushing, screening and iron removal to obtain D 50 It is spherical natural graphite with a size of about 16 μm and a circularity of 0.90. The actual carbon ratio after carbon coating is about 3 wt%.
[0098] Negative electrode manufacturing
[0099] The negative electrode active material prepared as above, styrene butadiene rubber (SBR) (Zeon) as a binder, carboxymethyl cellulose (Daicel, Daicel 2200) as a thickener, and carbon black (Imerys, SuperC-65) as a conductive material were prepared and dispersed in water at a weight ratio of 96.6:1.3:1.1:1.0 to prepare a negative electrode mixture slurry, which was coated on both surfaces of a copper foil and dried to obtain a preliminary negative electrode having a negative electrode active material layer before pressing. Subsequently, a negative electrode having a negative electrode active material layer on both surfaces of a copper foil (a final negative electrode having a negative electrode active material layer formed by pressing) was manufactured from the preliminary negative electrode having a negative electrode active material layer before pressing using a tandem press (THANK-METAL, a small precision roller press) at a temperature of 25° C. In this case, pressing was performed with the adjustment gap of the tandem press between 30 and 65 to obtain a target porosity of the negative electrode active material layer. The density of the negative electrode active material layer of the negative electrode obtained by pressing was about 1.57 g / cc, and the loading amount of the negative electrode active material was 3.6 mAh / cm 2 , the porosity of the negative electrode active material layer was 28%, and the thickness of the negative electrode active material layer was 80 μm.
[0100] The BET specific surface area of the negative electrode active material layer before pressing (the BET specific surface area of the negative electrode active material layer of the preliminary negative electrode) was 2.5 m 2 / g, and the BET specific surface area after pressing (the BET specific surface area of the negative electrode active material layer of the negative electrode finally obtained) is 3.5 m2 / g. In addition, the total pore volume of the negative electrode active material layer before pressing was 25.4×10 -3 cm 3 / g, and the total pore volume after pressing is 33.9×10 -3 cm 3 / g. The orientation degree of the negative electrode obtained after pressing is about 16. 004 / I 110 .
[0101] Manufacturing of lithium secondary batteries
[0102] LiCoO2 (Umicore, XD2Oa) as a positive electrode active material, styrene butadiene rubber (KUREHA, KF9706) as a binder, Denka black (Denka, FX35) as a conductive material, and an additive (ZEON, BM74 OH) were prepared and dispersed in N-methylpyrrolidone in a weight ratio of 97.68:1.2:1.0:0.12 to prepare a positive electrode mixture slurry, and the positive electrode mixture slurry was coated on both surfaces of an aluminum foil, followed by drying and pressing to manufacture a positive electrode.
[0103] A coin-cell type lithium secondary battery is manufactured by placing a polyethylene film separator (W-scope, WL20C) as a separator between the positive electrode and the negative electrode manufactured as described above and preparing an electrolyte, wherein the electrolyte contains an organic solvent with a weight ratio of ethylene carbonate / ethylmethyl carbonate of 2:8, 1M LiPF6 electrolyte salt and 0.5 weight% of vinylene carbonate additive.
[0104] Example 2
[0105] A negative electrode and a lithium secondary battery including the same were manufactured using the same spheroidized natural graphite as in Example 1, except that less expandable natural graphite with reduced inner pores was used and the actual carbon ratio after carbon coating the natural graphite was 4.5 wt %.
[0106] In this case, the BET specific surface area of the negative electrode active material layer using the obtained spheroidized natural graphite before pressing was 2.5 m 2 / g, and the BET specific surface area after pressing is 3.6m 2 / g. In addition, the total pore volume of the negative electrode active material layer before pressing is 26×10 -3 cm 3 / g, and the total pore volume after pressing is 35×10 -3 cm 3 / g.
[0107] The orientation degree of the negative electrode obtained after pressing is about 22 I 004 / I110 .
[0108] Example 3
[0109] A negative electrode and a lithium secondary battery including the same were manufactured using the same spheroidized natural graphite as in Example 1, except that less expandable natural graphite with reduced inner pores was used and the actual carbon ratio after carbon coating the natural graphite was 5.5 wt %.
[0110] In this case, the BET specific surface area of the negative electrode active material layer using the obtained spheroidized natural graphite before pressing was 2.5 m 2 / g, and the BET specific surface area after pressing is 3.4m 2 / g. In addition, the total pore volume of the negative electrode active material layer before pressing is 25×10 -3 cm 3 / g, and the total pore volume after pressing is 32.8×10 -3 cm 3 / g.
[0111] The orientation degree of the negative electrode obtained after pressing is about 18 I 004 / I 110 .
[0112] Comparative Example 1
[0113] First, the raw graphite ore is processed into small particles by mechanical treatment. Strong alkali solution treatment and strong acid solution treatment are carried out at high temperature to remove impurities. After washing and drying at high temperature, screening is carried out to mine plate-like natural graphite. In order to turn the plate-like natural graphite into a spherical shape, primary grinding and secondary grinding, i.e. mechanical processing, are carried out. Subsequently, after acid treatment, washing and drying, purification is carried out to obtain high-purity spherical natural graphite. During mechanical crushing and grinding, damage will occur on the surface of the obtained spherical natural graphite, and chemically reactive groups will be formed after strong alkali / strong acid washing. During spheroidization, damage occurs in the natural graphite due to mechanical processing. Therefore, carbon coating is carried out by carbonizing the pitch on the surface of high-purity solid phase natural graphite at about 1200°C in an inert gas atmosphere for about 24 hours, followed by crushing, screening and iron removal to obtain D 50 It is spherical natural graphite with a size of about 16 μm and a circularity of 0.90. The actual carbon ratio after carbon coating is about 3 wt%.
[0114] The spheroidized natural graphite was used to form a negative electrode active material layer, so that the BET specific surface area of the negative electrode active material layer before pressing was 2.3 m 2 / g, and the BET specific surface area after pressing is 3.9m 2 / g, and the total pore volume of the negative electrode active material layer before pressing is 26.2×10-3 cm 3 / g, and the total pore volume after pressing is 37.2×10 -3 cm 3 / g. Except for the above, a lithium secondary battery was manufactured by the same method as in Example 1. The orientation degree of the negative electrode obtained after pressing was about 40 I 004 / I 110 .
[0115] Comparative Example 2
[0116] Spheroidized natural graphite was produced by the same method as in Example 1, except that the surface of the high-purity solid phase natural graphite was coated with only crude oil instead of asphalt so that the actual carbon ratio was about 3%.
[0117] The spheroidized natural graphite was used to form a negative electrode active material layer, so that the BET specific surface area of the negative electrode active material layer before pressing was 2.3 m 2 / g, and the BET specific surface area after pressing is 3.9m 2 / g, and the total pore volume before pressing is 26.2×10 - 3 cm 3 / g, and the total pore volume after pressing is 37×10 -3 cm 3 / g. Except for the above, a lithium secondary battery was manufactured by the same method as in Example 1. The orientation degree of the negative electrode obtained after pressing was about 39 I 004 / I 110 .
[0118] Comparative Example 3
[0119] Spheroidized natural graphite was obtained by the same method as in Example 1 except that the surface of the high-purity solid phase natural graphite was coated with pitch only so that the actual carbon ratio was 4.0%. The orientation degree of the negative electrode obtained after pressing was about 39 I 004 / I 110 .
[0120] The spheroidized natural graphite was used to form a negative electrode active material layer, so that the BET specific surface area of the negative electrode active material layer before pressing was 2.3 m 2 / g, and the BET specific surface area after pressing is 3.8m 2 / g, and the total pore volume of the negative electrode active material layer before pressing is 26×10 -3 cm 3 / g, and the total pore volume after pressing is 36×10 -3 cm 3 / g. A lithium secondary battery was manufactured by the same method as in Example 1 except for the above.
[0121] Comparative Example 4
[0122] Spheroidized natural graphite was obtained by the same method as in Example 1 except that the surface of the high-purity solid phase natural graphite was coated with pitch only so that the actual carbon ratio was 5.5%. The orientation degree of the negative electrode obtained after pressing was about 39 I 004 / I 110 .
[0123] The spheroidized natural graphite was used to form a negative electrode active material layer, so that the BET specific surface area of the negative electrode active material layer before pressing was 2.3 m 2 / g, and the BET specific surface area after pressing is 3.7m 2 / g, and the total pore volume of the negative electrode active material layer before pressing is 26.6×10 -3 cm 3 / g, and the total pore volume after pressing is 36.6×10 -3 cm 3 / g. A lithium secondary battery was manufactured by the same method as in Example 1 except for the above.
[0124] Evaluation Method
[0125] Evaluation of BET specific surface area and total pore volume of negative electrode active material layer
[0126] The negative electrodes of Examples 1 to 3 and Comparative Examples 1 to 4 were completely dried, and the negative electrode active material layer was cut into a size of 8 mm × 8 mm to prepare 30 samples. The sampled negative electrode active material layer was placed in a standard sample cell (glass) and dried at 130 ° C for 2 hours under vacuum conditions. In order to measure in a liquid nitrogen container at 77K, liquid nitrogen was loaded into the liquid nitrogen container. The standard cell was cooled, and in order to measure under liquid nitrogen conditions, the standard sample cell was fixed to a measuring instrument (BEL Japan, BELSORP-mino II). Subsequently, the program of the measuring instrument was started to measure the BET specific surface area by adsorption / desorption on the surface of the sampled negative electrode active material layer in a nitrogen environment.
[0127] When measuring the BET specific surface area, the total pore volume can be measured together.
[0128] Evaluation of negative electrode orientation
[0129] The orientation degrees of the negative electrodes of Examples 1 to 3 and Comparative Examples 1 to 4 were measured by using an X-ray diffraction analyzer (X-ray diffraction (XRD), model: Bruker D4 Endeavor) using Cu-Kα radiation, and numerical correction was performed by Topas3 fitting program.
[0130] The ratio of the measured 004 peak to the 110 peak is expressed as I, which indicates the orientation degree of the negative electrode. 004 / I 110 .
[0131] Evaluation method of negative electrode thickness expansion rate during charge / discharge cycle
[0132] The negative electrode thickness expansion rate of the lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 4 in the charge / discharge cycle was evaluated. The negative electrode thickness expansion rate is a value obtained by dividing the expanded negative electrode thickness during charging by the reference negative electrode thickness, wherein the reference negative electrode thickness is the measured thickness of the negative electrode after pressing, and the expanded negative electrode thickness is the measured thickness of the negative electrode charged during charge / discharge. In this case, the charge / discharge cycle was performed under the following conditions, and the results are shown in Table 1 below.
[0133] -Charging range: SOC 0 to 95 ± 25 ℃
[0134] -1st cycle: 0.1C, 0.1C CC / CV mode 4.35V charge 0.005C cut-off, 0.1C CC mode discharge 2.75V
[0135] - Cycle 2: 0.2C CC / CV mode 4.35V charging 0.005C cut-off, 0.2C CC mode discharge 2.75V
[0136] - Cycle 3 to 30: 0.5C CC / CV mode 4.35V charging 0.005C cut-off, 0.5C CC mode discharge 2.75V
[0137] [Table 1]
[0138]
[0139] As can be seen from the above, the negative electrodes according to Examples 1 to 3 of the present invention have much lower negative electrode thickness expansion rates than the negative electrodes of Comparative Examples 1 to 4.
[0140] Although the embodiments of the present invention have been described above, those skilled in the art to which the present invention pertains will appreciate that the present invention may be implemented in other forms without departing from the technical aspects or essential features of the present invention.
[0141] Therefore, it should be understood that the disclosed embodiments are provided only as examples and are not intended to limit the present invention. The scope of the present invention is defined by the appended claims rather than the detailed description, and should be interpreted as the scope of the present invention encompasses all modifications or changes derived from the meaning and scope of the appended claims and equivalent concepts.
Claims
1. A negative electrode for a lithium secondary battery, the negative electrode comprising: A negative electrode active material layer, wherein the negative electrode active material layer is formed by coating a negative electrode mixture slurry containing spherical natural graphite particles as a negative electrode active material on at least one surface of a negative electrode current collector, followed by drying and pressing, wherein the spherical natural graphite particles contain a plurality of pores in which carbonized pitch is inserted, and The BET specific surface area of the negative electrode active material layer after pressing is greater than the BET specific surface area of the negative electrode active material layer before pressing, and the difference in BET specific surface area before and after pressing is within 0.9 m 2 / g to 1.2m 2 / g range, The negative electrode active material layer after pressing has a thickness of 3.3 μm 2 / g to 3.8m 2 / g in the range of BET specific surface area, wherein the negative electrode active material layer after compression has a compression density of 1.5 g / cc to 1.6 g / cc, The orientation degree of the negative electrode after pressing is 004 / I 110 Values range from 14 to 23.
2. The negative electrode for a lithium secondary battery according to claim 1, wherein the BET specific surface area of the negative electrode active material layer after pressing is greater than the BET specific surface area of the negative electrode active material layer before pressing, and the difference between the BET specific surface areas before and after pressing is within 0.9 m 2 / g to 1.1m 2 / g range. 3 . The negative electrode for a lithium secondary battery according to claim 1 , wherein the negative electrode active material is composed of the spheroidized natural graphite including a plurality of pores in which the carbonized pitch is inserted.
4. The negative electrode for a lithium secondary battery according to claim 1, wherein the total pore volume of the negative electrode active material layer after pressing is greater than the total pore volume of the negative electrode active material layer before pressing, and the difference in total pore volume before and after pressing is within 8×10 -3 cm 3 / g to 9×10 -3 cm 3 / g range. 5 . A lithium secondary battery, comprising the negative electrode for a lithium secondary battery according to claim 1 .
6. A method for manufacturing a negative electrode for a lithium secondary battery according to claim 1, the method comprising the following steps: (S1) coating spheroidized natural graphite with pitch and carbonizing the pitch to form a carbon coating; (S2) forming a negative electrode active material layer including the spheroidized natural graphite as a negative electrode active material on at least one surface of an electrode current collector; and (S3) compressing the negative electrode active material layer obtained in the step (S2) by a pressing roller at 23° C. to 25° C. to obtain the negative electrode active material layer after compression, so that the BET specific surface area of the negative electrode active material layer after compression is greater than the BET specific surface area of the negative electrode active material layer before compression, and the difference in BET specific surface area before and after compression is within 0.9 m 2 / g to 1.2m 2 / g range.
7. The method according to claim 6, wherein in the step (S2), the BET specific surface area of the negative electrode active material layer before the pressing is 2.4 m 2 / g to 2.6m 2 / g.
8. The method according to claim 6, wherein in the step (S2), the negative electrode active material layer before pressing has a thickness of 20×10 -3 cm 3 / g to 30×10 -3 cm 3 The total pore volume is in the range of 1000 Å / g.
9. The method according to claim 6, wherein the step (S3) include: The negative electrode active material layer obtained in the step (S2) is pressed by a pressing roller at 23° C. to 25° C. to obtain the pressed negative electrode active material layer, so that the total pore volume of the pressed negative electrode active material layer is greater than the total pore volume of the negative electrode active material layer before pressing, and the difference in the total pore volume before and after pressing is within 8×10 -3 cm 3 / g to 9×10 -3 cm 3 / g range.
10. The method according to claim 6, wherein in the step (S3), the BET specific surface area of the negative electrode active material layer after the pressing is 3.3 m 2 / g to 3.8m 2 / g.