A micro oxygen sensor chip
By optimizing the thickness symmetry of the zirconia matrix layer and the control of the printing layer, the problem of long response time of the micro oxygen sensor chip is solved, rapid response and ignition are achieved, and internal resistance of the sensitive electrode is reduced.
Patent Information
- Application Number
- CN202011479412.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-15
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-12-15
AI Technical Summary
The existing micro oxygen sensor chips have problems such as long response time and slow ignition, which are mainly due to the high internal resistance caused by the large thickness of the sensitive electrode layer.
By optimizing the structural design, including providing the thickness symmetry of the first zirconia matrix layer, the second zirconia matrix layer and the third zirconia matrix layer, and reducing sensitivity through stacked isostatic pressure and printed screen latex layer thickness control, Extreme internal resistance ensures heater thickness and insulation layer thickness, achieving rapid heating and response.
It effectively reduces the response time of the oxygen sensor, ensuring that the response time of the micro oxygen sensor is significantly shortened and the ignition speed is accelerated while ensuring other functions.
Smart Images

Figure CN112432984B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sensor chips, and more particularly to a concentration difference battery type micro oxygen sensor chip. Background Art
[0002] At present, the chip-type concentration cell oxygen sensor has a three-layer structure: heater layer, air channel layer and sensitive electrode layer. And the electrode material of the zirconium oxide oxygen sensor is platinum, which plays a catalytic role and electrode role. In order to ensure the thick film printing effect, the current manufacturing process mainly adopts the method of stacking and co-firing three layers of equal thickness zirconium oxide cast sheets after printing on the front and back sides. The thicker the sensitive electrode layer, the greater its internal resistance and the longer the oxygen sensor response time. Therefore, the current micro oxygen sensor chip has problems such as long response time and slow ignition.
[0003] Therefore, how to provide an oxygen sensor chip with a short response time is a problem that those skilled in the art need to solve urgently. Summary of the invention
[0004] In view of this, the present invention provides a micro oxygen sensor chip, which ensures that the internal resistance of the sensitive electrode is reduced without affecting other functions, so as to shorten the response time of the oxygen sensor.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A micro oxygen sensor chip, comprising in sequence a protective layer, a sensitive electrode outer electrode layer, a first zirconium oxide substrate layer, a sensitive electrode inner electrode layer, an air channel layer, a second zirconium oxide substrate layer, a first insulating layer, a heating electrode layer, a second insulating layer, a third zirconium oxide substrate layer, a third insulating layer and a heating electrode pin layer;
[0007] The first zirconia substrate layer, the second zirconia substrate layer and the third zirconia substrate layer are bonded and connected at both sides, and the sensitive electrode inner electrode layer and the air channel layer are arranged in the middle of the first zirconia substrate layer and the second zirconia substrate layer, the first insulating layer, the heating electrode layer and the second insulating layer are arranged in the middle of the second zirconia substrate layer and the third zirconia substrate layer, one end of the heating electrode layer is connected to the pin of the heating electrode pin layer, and one end of the sensitive electrode inner electrode layer is connected to the pin of the sensitive electrode outer electrode layer;
[0008] The thickness of the first zirconia matrix layer and the third zirconia matrix layer are symmetrical, both of which are 80-120 μm, and the thickness ratio of the first zirconia matrix layer, the second zirconia matrix layer and the third zirconia matrix layer is 1:8:1-1:11:1, and the thickness of the second zirconia matrix layer is 800-900 μm.
[0009] Preferably, the thickness of the protective layer is 20 to 40 μm, the thickness of the sensitive electrode outer electrode layer and the heating electrode pin layer is 10 to 15 μm, the thickness of the sensitive electrode inner electrode layer is 8 to 12 μm, the thickness of the first insulating layer, the second insulating layer and the third insulating layer is 10 to 20 μm, the thickness of the heating electrode layer is 10 to 15 μm, and the thickness of the air channel layer is 40 to 80 μm.
[0010] Preferably, a third through hole is provided at one end of the third zirconia substrate layer, and the heating electrode layer is connected to the pins of the heating electrode pin layer through the third through hole.
[0011] Preferably, the third through hole is formed from the center outwards by a third platinum slurry layer, an insulating layer and a third zirconium oxide matrix layer.
[0012] Preferably, a first through hole is provided at one end of the first zirconia substrate layer, and the sensitive electrode inner electrode layer is connected to a pin of the sensitive electrode outer electrode layer through the first through hole.
[0013] Preferably, the first through hole is formed from the center outwards by a first platinum slurry layer and a first zirconium oxide matrix layer.
[0014] Preferably, the insulating wall of the third zirconia matrix layer has an outer diameter of 300-500 μm and an inner diameter of 200-300 μm, the outer diameter of the third platinum slurry layer is 200-300 μm, and the thickness of the third platinum slurry layer is the same as that of the third zirconia matrix layer.
[0015] Preferably, the thickness of the substrate layer is achieved by controlling the thickness of the cast sheet, specifically, the thickness of the cast sheet with a thickness of 30-60 μm is prepared and then the thickness is controlled by lamination isostatic pressing.
[0016] The thickness of the first zirconia substrate layer and the third zirconia substrate layer is controlled by isostatic pressing of 2-3 layers of tape-cast sheets, and the thickness of the second zirconia substrate layer is controlled by isostatic pressing of 15-30 layers of tape-cast sheets.
[0017] Preferably, the printing layer is controlled by controlling the thickness of the printing screen latex layer.
[0018] The thickness of the screen latex used for printing the protective layer, the first insulating layer, the second insulating layer and the third insulating layer is controlled at 18-22 μm, and the printing thickness is controlled by controlling the scraper pressure of the printing machine. The insulating layer at the through hole is printed by screen printing, and the first platinum paste layer and the third platinum paste layer are printed by SMT steel mesh, and the thickness is consistent with the thickness of the corresponding substrate layer.
[0019] Preferably, the material of the heating electrode layer is metal platinum.
[0020] The first insulating layer, the second insulating layer and the third insulating layer are made of aluminum oxide.
[0021] It can be seen from the above technical solutions that, compared with the prior art, the present invention discloses a micro oxygen sensor chip, which ensures that the internal resistance of the sensitive electrode is as small as possible by controlling the thickness; and ensures that there is no stress concentration inside the chip by controlling the thickness of the third zirconia substrate layer (constituting the heating layer) and the first zirconia substrate layer (constituting the sensitive electrode layer) to be symmetrical.
[0022] Since the thickness of the sensitive electrode of the chip of the present invention is very small, the internal resistance is very small at the same temperature. When it is applied to an actual oxygen sensor, the internal resistance is very small at the same temperature. At the same time, after the thickness of the heater is reduced, the cold resistance increases accordingly. After the external voltage is applied, the sensitive electrode is quickly heated, and the internal resistance of the sensitive electrode is further reduced. The micro oxygen sensor reaches the optimal temperature and starts to work, and the ignition response is completed.
[0023] The beneficial effect of the present invention is that the response time of the oxygen sensor is reduced while ensuring other functions. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0025] Figure 1 The accompanying drawing is a schematic diagram of the structure of a micro oxygen sensor chip provided by the present invention.
[0026] in:
[0027] 1. Protective layer, 2. Sensitive electrode outer electrode layer, 3. First zirconia substrate layer, 4. Sensitive electrode inner electrode layer, 5. Air channel layer, 6. Second zirconia substrate layer, 7. First insulating layer, 8. Heating electrode layer, 9. Second insulating layer, 10. Third zirconia substrate layer, 11. Third insulating layer, 12. Heating electrode pin layer, 13. Third through hole, 14. First through hole. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The embodiment of the present invention discloses a micro oxygen sensor chip, such as Figure 1 As shown, it includes a protective layer 1, a sensitive electrode outer electrode layer 2, a first zirconia substrate layer 3, a sensitive electrode inner electrode layer 4, an air channel layer 5, a second zirconia substrate layer 6, a first insulating layer 7, a heating electrode layer 8, a second insulating layer 9, a third zirconia substrate layer 10, a third insulating layer 11 and a heating electrode pin layer 12 in sequence; the protective layer 1, the sensitive electrode outer electrode layer 2, the first zirconia substrate layer 3, the sensitive electrode inner electrode layer 4 together constitute the sensitive electrode layer, and the second zirconia substrate layer 6, the first insulating layer 7, the heating electrode layer 8, the second insulating layer 9, the third zirconia substrate layer 10, the third insulating layer 11 and the heating electrode pin layer 12 together constitute the heating electrode layer.
[0030] The protective layer 1 covers the surface of the outer electrode layer of the sensitive electrode, but does not cover the pin. Its main function is to protect the outer electrode from being contaminated by the outside world. Figure 1 The structure includes two upper and lower rectangles, which are respectively attached to the corresponding positions of the surface of the outer electrode layer 2 of the sensitive electrode; the air channel 5 is connected to the outside; the inner electrode layer 4 of the sensitive electrode is in contact with the air channel, and the outer electrode layer 2 of the sensitive electrode is in contact with the tail gas end of the application body. Since the oxygen concentrations at the two electrodes are different, their electrode potentials are different, and the electrode potentials change with the oxygen concentration difference on both sides. The inner electrode layer 4 of the sensitive electrode is connected to the external detection circuit through the lower end pin of the outer electrode layer of the sensitive electrode; the first zirconia matrix layer 3, the second zirconia matrix layer 6, The third zirconia substrate layer 10 is substrate zirconia, and both sides of the substrate layer are directly connected by overlapping, the first zirconia substrate layer 3 and the third zirconia substrate layer 10 are symmetrical in thickness, and the thickness ratio of the first zirconia substrate layer, the second zirconia substrate layer and the third zirconia substrate layer is 1:8:1 to 1:11:1; the first insulating layer 7, the second insulating layer 9, and the third insulating layer 11 mainly function to ensure that the substrate layer is completely insulated from the platinum paste layer to avoid leakage; the heating electrode layer 8 plays a heating role, and the heating electrode pin layer is connected to the external circuit.
[0031] A third through hole 13 is provided at one end of the third zirconia substrate layer 10, and the heating electrode layer 8 is connected to the pin of the heating electrode pin layer through the third through hole 13. At the same time, the third through hole 13 must be insulated from the third zirconia substrate. During the printing process, the insulating latex has fluidity, so an insulating layer is printed in the third through hole, and the heating electrode and the pin are connected through platinum paste, that is, a platinum paste layer is also printed on the insulating layer. Therefore, the third through hole 13 is respectively a third platinum paste layer, an insulating layer and a third zirconia substrate layer from the center of the circle to the outside.
[0032] At the same time, a first through hole 14 is provided at one end of the first zirconium oxide substrate layer 3 , and the sensitive electrode inner electrode layer 4 is connected to the pin of the sensitive electrode outer electrode layer through the first through hole 14 .
[0033] In order to minimize the thickness of the base zirconia layer, i.e., the first zirconia base layer 3 and the third zirconia base layer 10, which is specifically 80μm-120μm in this embodiment, while ensuring the symmetry of the thickness of the first zirconia base layer 3 and the third zirconia base layer 10; increase the thickness of the second zirconia base layer 6, which is 800-900μm in this embodiment; in order to ensure the insulation effect at the through hole and ensure connectivity, there are at least 6 third through holes 13 at one end of the third zirconia base layer, and the diameter is 300-500μm; in order to avoid stress concentration caused by the reduction of the base layer thickness, the thickness of the printed layer should be reduced accordingly. The specific implementation results are: in order to avoid the influence of the printed layer thickness on the base layer, the internal sensitive The electrode thickness is as small as possible, so the thickness of the inner electrode layer 4 of the sensitive electrode is 8-12μm. At the same time, in order to ensure that the heating wire can be connected, the thickness of the heating electrode layer 8 is 10-15μm. In order to ensure good contact between the chip and the lead terminal, the thickness of the outer electrode layer 2 of the sensitive electrode and the heating electrode pin layer 12 is 10-15μm; in order to ensure the insulation effect, the thickness of the first insulating layer, the second insulating layer and the third insulating layer is 10-20μm. In order to ensure the insulation effect at the through hole and the heating wire can be connected with the outer pin, the inner diameter of the insulating wall is between 200-300μm, and the outer diameter of the through hole platinum paste is between 200-300μm; at the same time, in order to ensure the protective effect of the electrode protective layer, the thickness of the protective layer is 20μm-40μm.
[0034] Among them, the thickness control mode is as follows: the thickness of the substrate layer is achieved by controlling the thickness of the cast sheet, specifically, after preparing a cast sheet with a thickness of 30-60μm, the thickness is controlled by isostatic pressing after lamination, the thickness of the first zirconia substrate layer and the third zirconia substrate layer is controlled by laminating 2-3 layers of cast sheets, and the thickness of the second zirconia substrate layer is controlled by laminating 15-30 layers; the printing layer is controlled by controlling the thickness of the printed screen latex layer, such as the thickness of the screen latex used for printing the protective layer, the first insulating layer, the second insulating layer and the third insulating layer is controlled at 18-22μm, and the insulating layer at the through hole is screen printed, the first platinum paste layer and the third platinum paste layer are through-hole printed by SMT steel mesh, and the aperture size is designed by two screen film drawings to achieve aperture control. At the same time, when the rest of the chip is bonded by platinum paste, the printing thickness of the platinum paste layer is controlled to be 8-15μm.
[0035] In the above operation, the printing method is a multiple printing and one drying method of not less than 3 times and not more than 5 times. The substrate layer is decomposed into two sides for printing to reduce the shrinkage of the single-layer substrate caused by excessive printing and drying times.
[0036] The present invention ensures that the internal resistance of the sensitive pole is as small as possible by controlling the thickness; ensures that there is no stress concentration inside the chip by controlling the symmetry of the third zirconia substrate layer and the first zirconia substrate layer; and avoids the problem of difficulty in printing too thin a substrate layer by limiting the thickness and number of printing layers. The printed layer is printed on both sides to reduce the shrinkage of the single-layer substrate caused by too many printing and drying times. The method of multiple printings and one drying is adopted to ensure that the printed pattern is printed completely at one time, avoiding the problems of warping caused by multiple dryings and errors caused by multiple alignments. The air channel is realized by printing, avoiding stress concentration caused by through holes.
[0037] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0038] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A micro oxygen sensor chip, It is characterized in that It includes a protective layer, a sensitive electrode outer electrode layer, a first zirconia substrate layer, a sensitive electrode inner electrode layer, an air channel layer, a second zirconia substrate layer, a first insulating layer, a heating electrode layer, a second insulating layer, a third zirconia substrate layer, a third insulating layer and a heating electrode pin layer in sequence; The first zirconia substrate layer, the second zirconia substrate layer and the third zirconia substrate layer are bonded and connected at both sides, and the sensitive electrode inner electrode layer and the air channel layer are arranged in the middle of the first zirconia substrate layer and the second zirconia substrate layer, the first insulating layer, the heating electrode layer and the second insulating layer are arranged in the middle of the second zirconia substrate layer and the third zirconia substrate layer, one end of the heating electrode layer is connected to the pin of the heating electrode pin layer, and one end of the sensitive electrode inner electrode layer is connected to the pin of the sensitive electrode outer electrode layer; The first zirconia matrix layer and the third zirconia matrix layer have symmetrical thicknesses, both of which are between 80 and 120 μm, and the thickness ratio of the first zirconia matrix layer, the second zirconia matrix layer and the third zirconia matrix layer is 1:8:1 to 1:11:1, and the thickness of the second zirconia matrix layer is between 800 and 900 μm; The thickness of the protective layer is 20-40 μm, the thickness of the sensitive electrode outer electrode layer and the heating electrode pin layer is 10-15 μm, the thickness of the sensitive electrode inner electrode layer is 8-12 μm, the thickness of the first insulating layer, the second insulating layer and the third insulating layer is 10-20 μm, the thickness of the heating electrode layer is 10-15 μm, and the thickness of the air channel layer is 40-80 μm; The thickness of the first zirconia substrate layer and the third zirconia substrate layer is controlled by isostatic pressing of 2-3 layers of tape-cast sheets, and the thickness of the second zirconia substrate layer is controlled by isostatic pressing of 15-30 layers of tape-cast sheets, and the thickness of the tape-cast sheets is 30-60 μm; The thickness of the screen latex used for printing the protective layer, the first insulating layer, the second insulating layer and the third insulating layer is controlled at 18-22 μm, and the printing thickness is controlled by controlling the scraper pressure of the printing machine. The insulating layer at the through hole is printed by screen printing, and the first platinum paste layer and the third platinum paste layer are printed by SMT steel mesh, and the thickness is consistent with the thickness of the corresponding substrate layer.
2. A micro oxygen sensor chip according to claim 1, It is characterized in that A third through hole is provided at one end of the third zirconia substrate layer, and the heating electrode layer is connected to the pins of the heating electrode pin layer through the third through hole.
3. A micro oxygen sensor chip according to claim 2, It is characterized in that The third through hole is provided with a third platinum slurry layer, an insulating layer and a third zirconium oxide matrix layer in sequence from the center outward.
4. A micro oxygen sensor chip according to claim 3, It is characterized in that A first through hole is provided at one end of the first zirconia substrate layer, and the sensitive electrode inner electrode layer is connected to the pin of the sensitive electrode outer electrode layer through the first through hole.
5. A micro oxygen sensor chip according to claim 4, It is characterized in that The first through hole is provided with a first platinum slurry layer and a first zirconium oxide matrix layer in order from the center outward.
6. A micro oxygen sensor chip according to claim 3, It is characterized in that The outer diameter of the insulating wall of the third zirconia matrix layer is 300-500 μm, the inner diameter of the insulating wall is between 200-300 μm, the outer diameter of the third platinum slurry layer is between 200-300 μm, and the thickness of the third platinum slurry layer is the same as that of the third zirconia matrix layer.
7. A micro oxygen sensor chip according to claim 1, It is characterized in that The material of the heating electrode layer is metal platinum. The first insulating layer, the second insulating layer and the third insulating layer are made of aluminum oxide.
Citation Information
Patent Citations
Chip oxygen sensor
CN102411018A
Switch type zirconium-based oxygen core body
CN111307910A
Miniature oxygen sensor chip
CN214097254U
Oxygen concentration detecting element and method of producing same
US20050158458A1
Oxygen sensor element
US5707503A