Industrial-grade alumina continuous fiber winding and sintering device and process method
By using a winding sintering device with uniform through holes and multi-layer structural grids in the alumina fiber sintering process, the problem of breakage caused by fiber shrinkage is solved, and fiber continuity and molding quality are improved.
Patent Information
- Application Number
- CN202011370075.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-11-30
AI Technical Summary
During the sintering process, the liquid phase shrinkage of the gel skeleton of the alumina fiber causes the fiber to break, which affects the continuity and molding quality. The existing winding and sintering device cannot adapt to the fiber shrinkage, resulting in excessive tension and breakage.
A winding sintering device is designed that includes uniform through holes in the cylindrical wall and a multi-layer structure grid. The five-layer structure grid is bonded with an adhesive. The cylindrical wall is made of stainless steel or ceramics. The through holes and grids are The optimized design is to adapt to fiber shrinkage, combined with reasonable heating rate control, to ensure uniform fiber sintering.
It significantly reduces the breakage rate of alumina fibers, ensures the continuity and molding quality of the fibers, ensures the uniformity of the sintering process and the high-quality output of the fibers.
Smart Images

Figure CN112442744B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an industrial-grade alumina continuous fiber winding and sintering device and a process method, belonging to the field of alumina spinning equipment. Background Art
[0002] Alumina fiber is a polycrystalline inorganic fiber whose main component is alumina. The main component is Al2O3, and some also contain a small amount of metal oxides such as SiO2 and B2O3. The heat resistance of alumina fiber is better than some other fibers. It can withstand ultra-high temperatures of 1450℃~1600℃, has high tensile strength, good elastic modulus and good electrical insulation performance, good chemical stability, and also has excellent properties such as low thermal conductivity and thermal expansion coefficient, and good thermal shock resistance. Alumina continuous fiber is usually used as a structural reinforcement material to prepare composite materials. Composite materials as high-temperature thermal insulation materials have been widely used in weapons, aviation, aerospace and automobiles.
[0003] The sol-gel method has become a common method for preparing alumina fibers because of its simple production process and the ability to obtain alumina fibers with uniform components, high purity and uniform performance. The main production steps of the sol-gel method are: 1. The alkoxide or inorganic salt of aluminum is used as a raw material and mixed evenly with a spinning aid, and after hydrolysis or alcoholysis reaction, a sol with uniform properties is obtained after concentration, and the sol has good rheological properties and suitable viscosity so that it can be spun; 2. Precursor gel fibers are obtained by centrifugation, spinning, dry spinning, electrospinning and other methods; 3. A reasonable heat treatment system is formulated to dry and sinter to obtain the final polycrystalline lead oxide continuous fiber. Under normal circumstances, during the sintering process of alumina fibers, due to the presence of a large amount of liquid phase in the gel skeleton, shrinkage occurs during drying, and the shrinkage rate can reach more than 30%, which can easily cause cracking of the product and fiber breakage, resulting in a decrease in the mechanical properties of the fiber, affecting the continuity of the alumina fiber, and reducing the fiber molding quality. The winding surface of the ordinary winding and sintering device cannot reduce the winding diameter accordingly as the alumina fiber shrinks, causing the alumina fiber to break due to excessive tension.
[0004] When alumina fiber is sintered at 200-400℃, the fiber shrinkage can reach 20%. In this temperature range, the organic synthetic fiber additives decompose, lose water and carbonize, the water vapor in the molecules overflows, and the physical and chemical reactions in the fiber are complex and intense, resulting in fiber quality loss and length shrinkage. The fiber is very easy to break. Therefore, 200-400℃ is the period when the fiber blank strength is the weakest, and it is the critical moment for the molding quality of alumina fiber.
[0005] Therefore, how to design a winding and sintering device that can shrink along with the shrinkage of alumina fibers is a technical problem that urgently needs to be solved. Summary of the invention
[0006] In order to solve at least one of the above problems, the present invention provides an industrial-grade alumina continuous fiber winding and sintering device and process method. The alumina continuous fiber winding and sintering device of the present invention can ensure that when the alumina fiber is sintered, the yarn will not break due to fiber shrinkage and the sintering device cannot change the shrinkage size accordingly. Compared with other alumina continuous fiber sintering devices, the present invention can greatly reduce the breakage of alumina fibers during the sintering process, ensure the continuous winding of the fibers, and improve the quality of alumina continuous fibers. During the sintering process, the through holes of the middle device can also ensure the uniformity of fiber sintering.
[0007] The first object of the present invention is to provide a winding and sintering device, which includes two parts. One part is a cylindrical cylinder with uniform through holes in the cylindrical wall; the other part is a cylindrical cylinder with uniform grids in the cylindrical wall. The grid is a multi-layer structure, which includes a sponge layer, a polypropylene PP layer, a polyamide PA layer, a polyimide PI layer and an aramid layer from the outside to the inside, and the thickness ratio of the five layers is 4:6:10:9:3; the cylindrical cylinder with uniform grids in the cylindrical wall is nested outside the cylindrical cylinder with uniform through holes in the cylindrical wall.
[0008] In one embodiment of the present invention, the multilayer structure of the grid is bonded together by an adhesive, and the preparation method of the grid is to coat a polypropylene PP resin on a sponge layer and solidify it; then coat a polyamide PA resin and solidify it; then coat a polyimide PI resin and solidify it; then bond an aramid fabric thereon by an adhesive to obtain a grid; the aramid can be a needle-punched aramid fabric, a woven aramid fabric, etc.
[0009] In one embodiment of the present invention, the cylindrical cylinder having uniform through holes in its wall is made of stainless steel, ceramic or silicon carbide.
[0010] In one embodiment of the present invention, the radius of the cylindrical cylinder with uniform through holes in the cylindrical wall is 100 mm, and the length is 200-600 mm; more preferably 400 mm.
[0011] In one embodiment of the present invention, the diameter of the through holes in the cylindrical cylinder having uniform through holes on the cylindrical wall is 3-10 mm, more preferably 5 mm; the interval between two rows of through holes is 3-10 mm, more preferably 10 mm.
[0012] In one embodiment of the present invention, the width of the grid in the cylindrical cylinder with a cylindrical wall containing uniform grids is 5-20 mm, more preferably 10 mm; and the gap between two grids is 15 mm.
[0013] In one embodiment of the present invention, the number of grids in the cylindrical barrel having a cylindrical wall containing uniform grids is 3-30, and more preferably 24.
[0014] In one embodiment of the present invention, a cylindrical cylinder having a cylindrical wall with uniform through holes and a cylindrical cylinder having a cylindrical wall with uniform grids are connected by bolts.
[0015] In one embodiment of the present invention, the height of the grid (cylinder wall) in the cylinder having a cylinder wall containing a uniform grid is 32% of the cylinder wall thickness of the cylinder having a cylinder wall containing uniform through holes.
[0016] The second object of the present invention is a process method for winding and sintering industrial-grade alumina continuous fibers, wherein the method adopts the winding and sintering device described in the present invention.
[0017] In one embodiment of the present invention, the winding sintering process is tube sintering, and each tube is an axis.
[0018] In one embodiment of the present invention, in the winding and sintering process, the winding and sintering device is placed in a sintering box at a certain angle for sintering, and the inclination angle is 15-30° to facilitate subsequent unwinding; more preferably 15°.
[0019] In one embodiment of the present invention, the winding sintering process is specifically as follows: at 0-300°C, the heating rate range is 0.1-1°C / min, at 300°C-700°C, the heating rate range is 0.5-1.5°C / min, at 700°C-1000°C, the heating rate is 1.0-2°C / min, and at 1000°C-1300°C, the heating rate is 1.5-2.5°C / min.
[0020] In one embodiment of the present invention, the industrial-grade alumina continuous fiber is a precursor fiber prepared by a sol-gel method, a centrifugal spinning method or an electrospinning process.
[0021] The working principle of the present invention is:
[0022] The precursor fiber (industrial-grade alumina continuous fiber) prepared by the sol-gel method, centrifugal spinning method or electrospinning process is evenly laid on the surface of a cylindrical tube with a uniform grid on the cylindrical wall. After the whole tube is covered, the entire winding and sintering device is placed in a sintering box, and the inclination angle of the winding and sintering device is controlled to be 15-30°, and then sintering is started. The sintering process is: at 0-300°C, the heating rate range is 0.1-1°C / min, 300°C-700°C, the heating rate range is 0.5-1.5°C / min, 700°C-1000°C, the heating rate is 1.0-2°C / min, and the heating rate at 1000°C-1300°C is 1.5-2.5°C / min; after sintering is completed, cool to room temperature and unwind.
[0023] Beneficial effects of the present invention:
[0024] (1) The winding and sintering device of the present invention has through holes on the cylindrical cylinder with uniform through holes on the cylinder wall, which can ensure uniform sintering of the alumina precursor fibers and avoid the situation where the outer fibers are sintered but the inner fibers are not sintered.
[0025] (2) The cylindrical wall of the winding sintering device contains a cylindrical tube with a uniform grid. The grid can reduce the outer diameter of the grid as the alumina fiber shrinks during the sintering process, thereby adapting to the tension of the alumina fiber, reducing fiber breakage, ensuring the continuous production of the alumina fiber, and ensuring the fiber quality.
[0026] (3) The melting rate of polyamide and polyimide grids is about 1 mm / 10°C, which can coordinate the reduction of the winding radius with the shrinkage rate of the alumina fiber with temperature. It can ensure that at this temperature stage, the winding radius of the sintering device decreases evenly with the fiber shrinkage, thereby reducing fiber breakage and ensuring the quality of fiber molding.
[0027] (4) The winding sintering process method of the present invention has a reasonable setting of the heating rate. In the initial sintering stage, the heating is slow, which can allow the generated volatile gases to escape slowly, avoid the generation of microcracks on the fiber surface, and reduce the breakage in the subsequent sintering process. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram of the assembly of the industrial-grade alumina continuous fiber winding and sintering device of the present invention; wherein 1 is a cylindrical cylinder with uniform through holes on the cylindrical wall, and 2 is a cylindrical cylinder with uniform grids on the cylindrical wall.
[0029] Figure 2 It is a schematic structural diagram of a cylindrical drum 1 having uniform through holes in the cylindrical wall in the industrial-grade alumina continuous fiber winding and sintering device of the present invention.
[0030] Figure 3 It is a schematic structural diagram of a cylindrical drum 2 having a uniform grid on the cylindrical wall in the industrial-grade alumina continuous fiber winding and sintering device of the present invention. DETAILED DESCRIPTION
[0031] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0032] Example 1
[0033] A winding sintering device (structure as Figure 1 ), the winding and sintering device includes two parts, one part is a cylindrical tube 1 with uniform through holes in the cylindrical wall; the other part is a cylindrical tube 2 with uniform grid in the cylindrical wall, and the cylindrical tube 2 with uniform grid in the cylindrical wall is nested outside the cylindrical tube 1 with uniform through holes in the cylindrical wall.
[0034] Furthermore, the grid in the cylindrical tube 2 whose cylindrical wall contains a uniform grid is a multi-layer structure, which includes a sponge layer, a polypropylene PP layer, a polyamide PA layer, a polyimide PI layer and an aramid layer from the outside to the inside, and the thickness ratio of the five layers is 4:6:10:9:3.
[0035] Furthermore, the multi-layer structure of the grid is bonded together by an adhesive, and the preparation method of the grid is to coat a polypropylene PP resin on a sponge layer and solidify it; then coat a polyamide PA resin and solidify it; then coat a polyimide PI resin and solidify it; then bond an aramid fabric thereon by an adhesive to obtain a grid; the aramid can be a needle-punched aramid fabric, a woven aramid fabric, etc.
[0036] Furthermore, the cylindrical tube 1 having uniform through holes in the cylindrical wall is made of stainless steel, ceramic or silicon carbide.
[0037] Furthermore, the radius of the cylindrical barrel 1 with uniform through holes in the cylindrical wall is 100 mm, and the length is 200-600 mm; more preferably 400 mm.
[0038] Furthermore, the diameter of the through holes in the cylindrical barrel 1 having uniform through holes on the cylindrical wall is 3-10 mm, and more preferably 5 mm; the interval between two rows of through holes is 3-10 mm, and more preferably 10 mm.
[0039] Furthermore, the width of the grid on the cylindrical barrel 2 with a uniform grid on the cylindrical wall is 5-20 mm, and more preferably 10 mm; the gap between two grids is 15 mm.
[0040] Furthermore, the number of grids on the cylindrical barrel 2 having uniform grids on the cylindrical wall is 3-30, and more preferably 24.
[0041] Furthermore, the cylindrical barrel 1 whose cylindrical wall contains uniform through holes and the cylindrical barrel 2 whose cylindrical wall contains uniform grids are connected by bolts.
[0042] Furthermore, the height of the grid (cylindrical wall) on the cylindrical barrel 2 whose cylindrical wall contains uniform grids is 32% of the thickness of the cylindrical barrel 1 whose cylindrical wall contains uniform through holes.
[0043] Example 2
[0044] A winding and sintering process for industrial-grade alumina continuous fibers, wherein the method uses the winding and sintering device described in Example 1, specifically:
[0045] The cylindrical cylinder 1 ( Figure 2 ) has a length of 400mm, a radius of 100mm, a through hole radius of 5mm, and a distance between two rows of through holes of 10mm.
[0046] The cylindrical cylinder 2 ( Figure 3 ) has a grid width of 10mm, a gap of 15mm between two grids, and a number of 24; a grid height of 32mm, a sponge height of 4mm, a polypropylene height of 6mm, a polyamide height of 10mm, a polyimide height of 9mm, and a polyurethane foam height of 5mm.
[0047] The precursor fiber (industrial-grade alumina continuous fiber) prepared by the sol-gel method is evenly wound on the surface of a cylindrical tube 2 with a uniform grid on the cylindrical wall. After the entire tube is fully laid, the entire winding and sintering device is placed in a sintering box. The inclination angle of the winding and sintering device is controlled to be 15°, and then sintering is started. The sintering process is: at 0-300°C, the heating rate range is 0.5°C / min, 300°C-700°C, the heating rate range is 1°C / min, 700°C-1000°C, the heating rate is 1.5°C / min, 1000°C-1300°C The heating rate is 2°C / min; after sintering is completed, cool to room temperature and unwind.
[0048] The breakage rate during the sintering process using the winding sintering process is less than 5%.
[0049] Comparative Example 1
[0050] The grid in the winding sintering device in Example 2 is adjusted to be made of stainless steel so that it does not melt with the temperature. Other things remain the same as in Example 2.
[0051] The test results show that the fiber breakage rate reaches 60%.
[0052] Comparative Example 2
[0053] The polypropylene in Example 2 was adjusted to polyethylene wax, and the rest was the same as Example 2.
[0054] The test results show that the fiber breakage rate reaches 20%.
[0055] Comparative Example 3
[0056] The polypropylene in Example 2 is adjusted to aramid fiber and polyurethane foam, and the rest is the same as Example 2.
[0057] The test results show that the fiber breakage rate reaches 10%, but the fibers are easy to stick together.
[0058] Comparative Example 4
[0059] The sintering process in Example 2 is adjusted as follows: at 0-300°C, the heating rate range is 1.5°C / min, at 300°C-700°C, the heating rate range is 2°C / min, at 700°C-1000°C, the heating rate is 2.5°C / min, and at 1000°C-1300°C, the heating rate is 3°C / min. The rest remains consistent with Example 2.
[0060] The test results show that the fiber breakage rate reaches 55%.
[0061] Comparative Example 5
[0062] The grid height in Example 2 was adjusted to 32 mm, the sponge height to 5 mm, the polypropylene height to 5 mm, the polyamide height to 6 mm, the polyimide height to 9 mm, the polyurethane foam height to 7 mm, and the rest remained the same as in Example 2.
[0063] The test results show that the fiber breakage rate reaches 55%.
[0064] By comparing the above-mentioned Example 2 with the control examples 1-5, it can be seen that the material and height of the grid in the present application need to be completely consistent with the sintering process, and the adjustment of any one parameter may not achieve the effect of reducing the breakage rate of the present application.
[0065] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the technology and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A process for winding and sintering industrial-grade alumina continuous fibers, characterized in that: The process method adopts a winding sintering device to sinter the tubes, each tube being an axis; The winding sintering device comprises two parts, one part is a cylindrical cylinder (1) whose cylindrical wall contains uniform through holes; the other part is a cylindrical cylinder (2) whose cylindrical wall contains uniform grids, wherein the grids are multi-layer structures, and from the outside to the inside, they are respectively a sponge layer, a polypropylene PP layer, a polyamide PA layer, a polyimide PI layer and an aramid layer, and the thickness ratio of the five layers is 4:6:10:9:3; the cylindrical cylinder (2) whose cylindrical wall contains uniform grids is nested outside the cylindrical cylinder (1) whose cylindrical wall contains uniform through holes; The winding sintering device is placed in the sintering box at a certain angle for sintering, and the angle of inclination is 15-30°; The sintering process of the winding sintering device is: At 0-300℃, the heating rate range is 0.1-1℃ / min, at 300℃-700℃, the heating rate range is 0.5-1.5℃ / min, at 700℃-1000℃, the heating rate is 1.0-2℃ / min, and at 1000℃-1300℃, the heating rate is 1.5-2.5℃ / min.
2. The process according to claim 1, characterized in that: The industrial-grade alumina continuous fiber is a precursor fiber prepared by a sol-gel method, a centrifugal spinning method or an electrostatic spinning process.
3. The process according to claim 1, characterized in that: The cylindrical drum (1) in the winding sintering device has a cylindrical wall with uniform through holes, a radius of 100 mm, and a length of 200-600 mm.
4. The process according to claim 1, characterized in that: The diameter of the through holes in the cylindrical drum (1) having uniform through holes in the cylindrical wall of the winding sintering device is 3-10 mm.
5. The process according to claim 1, characterized in that: The cylindrical drum (2) in the winding sintering device has a cylindrical wall with a uniform grid, and the grid width is 5-20 mm.
6. The process according to claim 1, characterized in that: In a winding sintering device, a cylindrical drum (2) whose cylindrical wall contains uniform grids and a cylindrical drum (1) whose cylindrical wall contains uniform through holes are connected by bolts.
7. The process according to claim 1, characterized in that: The height of the grid in the cylindrical drum (2) with a uniform grid on the cylindrical wall in the winding sintering device is 32% of the thickness of the cylindrical drum (1) with a uniform through-hole on the cylindrical wall.