Binder aqueous solution for lithium ion battery electrode, slurry for lithium ion battery electrode, lithium ion battery electrode and lithium ion battery

CN112447973BActive Publication Date: 2024-11-22ARAKAWA CHEM IND LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202010909021.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-05
Filing Date
2020-09-02
Publication Date
2024-11-22
Estimated Expiration
2040-09-02

AI Technical Summary

Technical Problem

然而,取决于电极活性物质,伴随充放电容易产生膨胀和收缩

Benefits of technology

[0033] By using the binder aqueous solution for lithium ion battery electrodes of the present disclosure, it is possible to produce a slurry with good storage stability, a non-curling, high-adhesion, and soft electrode, and a first-time Coulombic efficiency, capacity maintenance rate, and durability. Lithium-ion battery with good resilience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

[Technical Problem] Provide an aqueous binder solution for lithium-ion battery electrodes, a slurry for lithium-ion battery electrodes, a lithium-ion battery electrode, and a lithium-ion battery. [Technical Means] The present disclosure provides an aqueous binder solution for lithium-ion battery electrodes, the aqueous binder solution for lithium-ion battery electrodes containing a water-soluble polymer (A), the water-soluble polymer (A) being a polymer of a monomer group, relative to 100 mol % of the monomer group, the monomer group contains 5 mol % to 80 mol % of a hydroxyl-containing vinyl ether (a). In one embodiment, the monomer group contains 20 mol % to 95 mol % of a (meth)acrylamide-containing compound (b).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a binder aqueous solution for lithium ion battery electrodes, a slurry for lithium ion battery electrodes, a lithium ion battery electrode, and a lithium ion battery. Background Art

[0002] Lithium-ion batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and have been used in a wide range of applications. Therefore, in recent years, research has been conducted on improving battery components such as electrodes in order to further improve the performance of lithium-ion batteries.

[0003] The positive and negative electrodes of lithium-ion batteries are manufactured by the following method: a slurry formed by dispersing an electrode active material and a binder resin in a solvent is applied to both sides of a current collector (such as a metal foil), the solvent is dried and removed to form an electrode layer, and then the electrode layer is compression-molded using a roller press or the like.

[0004] In recent years, various electrode active materials have been proposed in lithium ion battery electrodes from the viewpoint of increasing battery capacity. However, depending on the electrode active material, expansion and contraction are easily generated with charge and discharge. Therefore, the lithium ion battery electrode that is easily expanded and contracted with charge and discharge undergoes volume changes (resilience) compared to the initial stage due to repeated charge and discharge, and the electrical characteristics such as the cycle characteristics of the lithium ion battery using the lithium ion battery electrode are easily reduced.

[0005] Therefore, in this field, attempts are being made to use binder resins to solve the above technical problems. For example, it is proposed to obtain good charge and discharge characteristics by using polyacrylamide as a binder of a water-soluble resin (Patent Documents 1 and 2). In addition, for the expansion and contraction accompanying the charge and discharge of the active material, it is proposed to suppress the expansion by adding a crosslinking agent to the particulate resin as a binder resin (Patent Document 3). The crosslinking agent usually undergoes a crosslinking reaction in the drying step after applying the slurry composition to the collector, and forms crosslinks between particles of the particulate resin.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2015-118908

[0009] Patent Document 2: Japanese Patent Application Publication No. 2015-106488

[0010] Patent Document 3: International Publication No. 2015 / 098507 Summary of the invention

[0011] Technical problem to be solved by the invention

[0012] However, from the viewpoint of ensuring solubility in water, the polyacrylamides of Patent Documents 1 and 2 cannot achieve a high molecular weight to the extent that the binder resin is insoluble in water. As a result, there is a technical problem that the resistance to rebound resilience caused by swelling of the active material is insufficient.

[0013] Depending on the situation, the combined use of the cross-linking agent described in Patent Document 3 sometimes does not show an effect even if a large amount is added. In this case, when a large amount of cross-linking agent is added in order to show the effect of the cross-linking agent (such as resistance to rebound), the adhesion (adhesion) of the electrode active material layer to the collector is reduced, and the desired effect such as high temperature cycle characteristics cannot be obtained, so there is room for further improvement.

[0014] When the neutralization rate of the polymer containing an unsaturated organic acid is low, the initial coulombic efficiency and the capacity retention rate may decrease. In addition, when the neutralization rate of the polymer containing an acrylate and an unsaturated organic acid exceeds 95%, the amount of unneutralized unsaturated organic acid increases due to the hydrolysis of the acrylate. This leads to a decrease in the initial coulombic efficiency and the capacity retention rate.

[0015] Therefore, the technical problem to be solved by the present invention is to provide a good aqueous solution of binder for lithium ion battery electrodes, which imparts good initial coulombic efficiency, capacity retention rate and resilience resistance to lithium ion batteries, good anti-curling properties, electrode softness and electrode adhesion to electrodes, and good storage stability to slurry.

[0016] Technical means to solve technical problems

[0017] The present inventors have conducted intensive studies and have found that the above-mentioned technical problems can be solved by using a water-soluble polymer having a predetermined unsaturated monomer as a constituent component.

[0018] The following items are provided according to the present disclosure.

[0019] (Item 1)

[0020] A binder aqueous solution for lithium ion battery electrodes, the binder aqueous solution for lithium ion battery electrodes containing a water-soluble polymer (A), the water-soluble polymer (A) being a polymer of a monomer group, and the monomer group containing 5 mol% to 80 mol% of a hydroxyl-containing vinyl ether (a) relative to 100 mol% of the monomer group.

[0021] (Item 2)

[0022] The aqueous binder solution for lithium ion battery electrodes as described in the above item, wherein the monomer group contains 20 mol % to 95 mol % of the (meth)acrylamide group-containing compound (b).

[0023] (Item 3)

[0024] The aqueous binder solution for lithium ion battery electrodes according to any one of the above items, wherein the monomer group contains 0.01 mol % to 50 mol % of an unsaturated organic acid or an inorganic salt thereof (c).

[0025] (Item 4)

[0026] A slurry for lithium ion battery electrodes comprising the binder aqueous solution for lithium ion battery electrodes as described in any one of the above items and an electrode active material (B).

[0027] (Item 5)

[0028] A lithium ion battery electrode obtained by applying the slurry for lithium ion battery electrodes as described in the above item on a current collector and drying and solidifying it.

[0029] (Item 6)

[0030] A lithium-ion battery comprising the lithium-ion battery electrode as described in the above item.

[0031] In the present disclosure, in addition to the combinations explicitly described, one or more of the above features may be provided in further combinations.

[0032] Beneficial Effects

[0033] By using the aqueous binder solution for lithium ion battery electrodes disclosed in the present invention, a slurry with good storage stability can be produced, a non-curling, highly adhesive and flexible electrode can be produced, and a lithium ion battery with good initial coulombic efficiency, capacity retention rate and resilience resistance can be produced. DETAILED DESCRIPTION

[0034] In the entire scope of the present disclosure, the range of the numerical values ​​of each physical property value, content, etc. can be appropriately set (for example, selected from the upper and lower limit values ​​described in each of the following items). Specifically, with respect to the numerical value α, when A4, A3, A2, A1 (A4>A3>A2>A1) and the like are exemplified as the upper and lower limits of the numerical value α, the range of the numerical value α is exemplified as less than A4, less than A3, less than A2, more than A1, more than A2, more than A3, A1-A2, A1-A3, A1-A4, A2-A3, A2-A4, A3-A4, etc.

[0035] [Aqueous binder solution for lithium-ion battery electrodes: also called aqueous solution]

[0036] The present disclosure provides an aqueous binder solution for lithium ion battery electrodes, wherein the aqueous binder solution for lithium ion battery electrodes contains a water-soluble polymer (A), wherein the water-soluble polymer (A) is a polymer of a monomer group, and relative to 100 mol % of the monomer group, the monomer group contains 5 mol % to 80 mol % of a hydroxyl-containing vinyl ether (a).

[0037] <Water-soluble polymer (A): also referred to as component (A)>

[0038] In the present disclosure, "water-soluble" means that when 0.5 g of the compound is dissolved in 100 g of water at 25°C, the insoluble component is less than 0.5% by mass (less than 2.5 mg).

[0039] <Hydroxyl-containing vinyl ether (a): also referred to as component (a)>

[0040] In the present disclosure, hydroxyl-containing vinyl ether refers to a vinyl ether consisting of H2C=CH-OR OH (Where R OH It refers to a compound represented by a group having a hydroxyl group).

[0041] In one embodiment, the hydroxyl-containing vinyl ether is represented by the general formula (1) H2C=CH-R-OH, wherein R represents:

[0042] a substituted or unsubstituted oxyalkylene group having 1 to 5 carbon atoms;

[0043] Polyoxyalkylene represented by general formula (2)

[0044] [Chemistry 1]

[0045] (wherein, q is an integer of 1 to 3, and n is an integer greater than 1. In addition, n is preferably an integer of 1 to 10);

[0046] [Chemistry 2]

[0047]

[0048] or a combination thereof.

[0049] Examples of the alkylene group include a linear alkylene group, a branched alkylene group, and a cycloalkylene group.

[0050] A straight chain alkylene group can be represented by the general formula -(CH2) n - (n is an integer greater than or equal to 1). Examples of the linear alkylene group include a methylene group, an ethylene group, a propylene group, an n-butylene group, and an n-pentylene group.

[0051] The branched alkylene group is a group in which at least one hydrogen of the straight chain alkylene group is replaced by an alkyl group. Examples of the branched alkylene group include methylmethylene, ethylmethylene, propylmethylene, butylmethylene, methylethylene, ethylethylene, propylethylene, methylpropylene, 2-ethylpropylene, dimethylpropylene, and methylbutylene.

[0052] Examples of the cycloalkylene group include a monocyclic cycloalkylene group, a bridged ring cycloalkylene group, and a condensed ring cycloalkylene group.

[0053] In the present disclosure, a monocyclic ring refers to a ring structure formed by a covalent bond of carbon and having no internal bridge structure. In addition, a fused ring refers to a ring structure in which two or more monocyclic rings share two atoms (i.e., each ring only shares (condenses) one side with each other). A bridged ring refers to a ring structure in which two or more monocyclic rings share three or more atoms.

[0054] Examples of the monocyclic cycloalkylene group include cyclopentylene and the like.

[0055] Examples of the substituent of the oxyalkylene group include a hydroxyl group, an amino group, an acetyl group, and a sulfonic acid group.

[0056] Examples of the hydroxyl group-containing vinyl ether include hydroxyalkyl vinyl ether and polyalkylene glycol monovinyl ether.

[0057] Examples of the hydroxyalkyl vinyl ether include hydroxy linear alkyl vinyl ether, hydroxy branched alkyl vinyl ether, and hydroxy cycloalkyl vinyl ether.

[0058] Examples of the hydroxy linear alkyl vinyl ether include 2-hydroxyethyl vinyl ether, 3-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, and 5-hydroxypentyl vinyl ether.

[0059] Examples of the hydroxy branched alkyl vinyl ether include 2-hydroxypropyl vinyl ether, 2-hydroxy-2-methylpropyl vinyl ether, and 4-hydroxy-2-methylbutyl vinyl ether.

[0060] Examples of the hydroxycycloalkyl vinyl ether include 4-hydroxycyclopentyl vinyl ether and the like.

[0061] Examples of the polyalkylene glycol monovinyl ether include polymethylene glycol monovinyl ether, polyethylene glycol monovinyl ether, and polypropylene glycol monovinyl ether.

[0062] Examples of the polymethylene glycol monovinyl ether include dimethylene glycol monovinyl ether, trimethylene glycol monovinyl ether, tetramethylene glycol monovinyl ether, pentamethylene glycol monovinyl ether, hexamethylene glycol monovinyl ether, heptamethylene glycol monovinyl ether, octamethylene glycol monovinyl ether, nonamethylene glycol monovinyl ether and decamethylene glycol monovinyl ether.

[0063] Examples of the polyethylene glycol monovinyl ether include diethylene glycol monovinyl ether, triethylene glycol monovinyl ether, tetraethylene glycol monovinyl ether, pentaethylene glycol monovinyl ether, hexaethylene glycol monovinyl ether, heptaethylene glycol monovinyl ether, octaethylene glycol monovinyl ether, nonaethylene glycol monovinyl ether, and decaethylene glycol monovinyl ether.

[0064] Examples of the polypropylene glycol monovinyl ether include dipropylene glycol monovinyl ether, tripropylene glycol monovinyl ether, tetrapropylene glycol monovinyl ether, pentapropylene glycol monovinyl ether, hexapropylene glycol monovinyl ether, heptapropylene glycol monovinyl ether, octapropylene glycol monovinyl ether, nonapropylene glycol monovinyl ether and decapropylene glycol monovinyl ether.

[0065] The upper and lower limits of the content of the hydroxyl-containing vinyl ether relative to 100 mol% of the monomer group are exemplified by 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 9 mol%, 5 mol%, etc. In one embodiment, the content of the hydroxyl-containing vinyl ether is 5 mol% to 80 mol% relative to 100 mol% of the monomer group.

[0066] The upper and lower limits of the content of the hydroxyl-containing vinyl ether relative to 100 mass % of the monomer group are exemplified by 85 mass %, 80 mass %, 75 mass %, 70 mass %, 65 mass %, 60 mass %, 55 mass %, 50 mass %, 45 mass %, 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 5 mass %, etc. In one embodiment, the content of the hydroxyl-containing vinyl ether is 5 mass % to 85 mass % relative to 100 mass % of the monomer group.

[0067] <(Meth)acrylamide group-containing compound (b): also referred to as component (b)>

[0068] In the present disclosure, "a (meth)acrylamide group-containing compound" refers to a compound having a (meth)acrylamide group. The (meth)acrylamide group-containing compound can be any known compound without particular limitation, and can be used alone or in combination of two or more.

[0069] In the present disclosure, “(meth)acrylic acid” means “at least one selected from the group consisting of acrylic acid and methacrylic acid”. Similarly, “(meth)acrylate” means “at least one selected from the group consisting of acrylate and methacrylate”. Furthermore, “(meth)acryloyl” means “at least one selected from the group consisting of acryloyl and methacryloyl”.

[0070] In one embodiment, the (meth)acrylamide-containing compound is represented by the following structural formula:

[0071] [Chemistry 1]

[0072]

[0073] (Where R 1 is a hydrogen atom or a methyl group; R 2 and R 3 are each independently a hydrogen atom, a substituted or unsubstituted alkyl group, or an acetyl group, or R 2 and R 3 are groups that together form a ring structure; R 4 and R 5 are each independently a hydrogen atom, a substituted or unsubstituted alkyl group, a hydroxyl group, an amino group (-NR a R b (R a and R b Each independently represents a hydrogen atom or a substituted or unsubstituted alkyl group) or an acetyl group. Examples of substituents of the substituted alkyl group include hydroxyl, amino, acetyl, and the like. 2 and R 3 Examples of the groups that form a ring structure together include morpholino and the like. )

[0074] Examples of the alkyl group include a linear alkyl group, a branched alkyl group, and a cycloalkyl group.

[0075] Straight chain alkyl is composed of the general formula -C n H 2n+1 (n is an integer greater than or equal to 1). Examples of the linear alkyl group include methyl, ethyl, propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl.

[0076] The branched alkyl group is a group in which at least one hydrogen atom of a linear alkyl group is substituted by an alkyl group. Examples of the branched alkyl group include isopropyl, isobutyl, sec-butyl, tert-butyl, diethylpentyl, trimethylbutyl, trimethylpentyl, and trimethylhexyl.

[0077] Examples of the cycloalkyl group include a monocyclic cycloalkyl group, a bridged ring cycloalkyl group, and a condensed ring cycloalkyl group.

[0078] Examples of the monocyclic cycloalkyl group include cyclopentyl, cyclohexyl, cycloheptyl, cyclodecyl, and 3,5,5-trimethylcyclohexyl.

[0079] Examples of the bridged cycloalkyl group include tricyclodecanyl, adamantyl, and norbornyl.

[0080] Examples of the fused ring cycloalkyl group include bicyclodecanyl and the like.

[0081] The number of carbon atoms in the alkyl group is not particularly limited, and the upper and lower limits thereof are exemplified by 40, 35, 30, 29, 25, 20, 15, 12, 10, 9, 8, 7, 6, 5, 4, 3, 2, and 1.

[0082] Examples of the (meth)acrylamide group-containing compound include (meth)acrylamide, N-isopropyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, diacetone (meth)acrylamide, maleic acid amide (maleic acid amide), (meth)acryloyl morpholine, hydroxyethyl (meth)acrylamide and salts thereof; examples of the salt include dimethylaminopropyl (meth)acrylamide methyl chloride quaternary salt (Methyl quaternary salt), dimethylaminoethyl (meth)acrylate benzyl chloride quaternary salt (benzyl chloride quaternary salt) and the like. Among them, when (meth)acrylamide, particularly acrylamide, is used, a binder having high water solubility, high interaction with the electrode active material, high dispersibility in the slurry and high adhesion between the electrode active materials in the electrode can be produced.

[0083] The upper and lower limits of the content of the (meth)acrylamide group-containing compound relative to 100 mol% of the monomer group are exemplified by 95 mol%, 90 mol%, 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, etc. In one embodiment, the range of the above content is preferably 20 mol% to 95 mol%.

[0084] The upper and lower limits of the content of the (meth)acrylamide group-containing compound relative to 100 mass% of the monomer group are exemplified by 95 mass%, 90 mass%, 85 mass%, 80 mass%, 75 mass%, 70 mass%, 65 mass%, 60 mass%, 55 mass%, 50 mass%, 45 mass%, 40 mass%, 35 mass%, 30 mass%, 25 mass%, 20 mass%, 15 mass%, 10 mass%, etc. In one embodiment, the content of the (meth)acrylamide group-containing compound relative to 100 mass% of the monomer group is preferably 10 to 95 mass%.

[0085] <Unsaturated organic acid or inorganic salt thereof (c): also referred to as component (c)>

[0086] As the component (c), various known substances can be used without particular limitation, and the component (c) can be used alone or in combination of two or more.

[0087] Examples of the unsaturated organic acid include unsaturated carboxylic acid, unsaturated sulfonic acid, and unsaturated phosphoric acid.

[0088] Examples of the unsaturated carboxylic acid include (meth)acrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid.

[0089] Examples of the unsaturated sulfonic acid include α,β-ethylenically unsaturated sulfonic acids such as vinylsulfonic acid, styrylsulfonic acid, and (meth)allylsulfonic acid; (meth)acrylamide-tert-butylsulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, 2-(meth)acrylamide-2-hydroxypropanesulfonic acid, 3-sulfopropane (meth)acrylate, and bis-(3-sulfopropyl)itaconate.

[0090] Examples of the unsaturated phosphoric acid include vinylphosphonic acid, vinyl phosphate, bis((meth)acryloyloxyethyl)phosphate, diphenyl-2-(meth)acryloyloxyethyl phosphate, dibutyl-2-(meth)acryloyloxyethyl phosphate, dioctyl-2-(meth)acryloyloxyethyl phosphate, monomethyl-2-(meth)acryloyloxyethyl phosphate, and 3-(meth)acryloyloxy-2-hydroxypropanephosphoric acid.

[0091] In the present disclosure, a compound that belongs to both the (meth)acrylamide group-containing compound and the unsaturated organic acid is an unsaturated organic acid.

[0092] In the present disclosure, the inorganic salt of an unsaturated organic acid refers to a salt whose cation part is a metal cation. Examples of the inorganic salt include alkali metal salts, alkaline earth metal salts, and the like.

[0093] Examples of the alkali metal include lithium, sodium, and potassium.

[0094] Examples of the alkaline earth metal include magnesium and calcium.

[0095] The upper and lower limits of the content of the unsaturated organic acid or its inorganic salt relative to 100 mol% of the monomer group are exemplified by 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 9 mol%, 5 mol%, 4 mol%, 1 mol%, 0.9 mol%, 0.5 mol%, 0.3 mol%, 0.1 mol%, 0.09 mol%, 0.05 mol%, 0.03 mol%, 0.01 mol%, etc. In one embodiment, the content of the unsaturated organic acid or its inorganic salt relative to 100 mol% of the monomer group is preferably 0.01 mol% to 50 mol%.

[0096] The upper and lower limits of the content of the unsaturated organic acid or its inorganic salt relative to 100 mass% of the monomer group are exemplified by 75 mass%, 70 mass%, 65 mass%, 60 mass%, 55 mass%, 50 mass%, 45 mass%, 40 mass%, 35 mass%, 30 mass%, 25 mass%, 20 mass%, 15 mass%, 10 mass%, 9 mass%, 5 mass%, 4 mass%, 1 mass%, 0.9 mass%, 0.5 mass%, 0.3 mass%, 0.1 mass%, 0.09 mass%, 0.05 mass%, 0.03 mass%, 0.01 mass%, etc. In one embodiment, the content of the unsaturated organic acid or its inorganic salt is preferably 0.01 mass% to 75 mass% relative to 100 mass% of the monomer group.

[0097] The upper and lower limits of the content of the unsaturated carboxylic acid or its inorganic salt relative to 100 mol% of the monomer group are exemplified by 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 1 mol%, 0 mol%, etc. In one embodiment, the content of the unsaturated carboxylic acid or its inorganic salt relative to 100 mol% of the monomer group is preferably 0 mol% to 50 mol%.

[0098] The upper and lower limits of the content of the unsaturated carboxylic acid or its inorganic salt relative to 100 mass % of the monomer group are exemplified by 60 mass %, 55 mass %, 50 mass %, 45 mass %, 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 5 mass %, 1 mass %, 0 mass %, etc. In one embodiment, the content of the unsaturated carboxylic acid or its inorganic salt is preferably 0 mass % to 60 mass % relative to 100 mass % of the monomer group.

[0099] The upper and lower limits of the content of the unsaturated sulfonic acid or its inorganic salt relative to 100 mol% of the monomer group are exemplified by 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 1 mol%, 0 mol%, etc. In one embodiment, the content of the unsaturated sulfonic acid or its inorganic salt relative to 100 mol% of the monomer group is preferably 0 mol% to 50 mol%.

[0100] The upper and lower limits of the content of the unsaturated sulfonic acid or its inorganic salt relative to 100 mass% of the monomer group are exemplified by 75 mass%, 70 mass%, 65 mass%, 60 mass%, 55 mass%, 50 mass%, 45 mass%, 40 mass%, 35 mass%, 30 mass%, 25 mass%, 20 mass%, 15 mass%, 10 mass%, 5 mass%, 1 mass%, 0 mass%, etc. In one embodiment, the content of the unsaturated sulfonic acid or its inorganic salt is preferably 0 mass% to 75 mass% relative to 100 mass% of the monomer group.

[0101] The upper and lower limits of the content of the unsaturated phosphoric acid or its inorganic salt relative to 100 mol% of the monomer group are exemplified by 50 mol%, 45 mol%, 40 mol%, 35 mol%, 30 mol%, 25 mol%, 20 mol%, 15 mol%, 10 mol%, 5 mol%, 1 mol%, 0 mol%, etc. In one embodiment, the content of the unsaturated phosphoric acid or its inorganic salt relative to 100 mol% of the monomer group is preferably 0 mol% to 50 mol%.

[0102] The upper and lower limits of the content of the unsaturated phosphoric acid or its inorganic salt relative to 100 mass % of the monomer group are exemplified by 75 mass %, 70 mass %, 65 mass %, 60 mass %, 55 mass %, 50 mass %, 45 mass %, 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 5 mass %, 1 mass %, 0 mass %, etc. In one embodiment, the content of the unsaturated phosphoric acid or its inorganic salt is preferably 0 mass % to 75 mass % relative to 100 mass % of the monomer group.

[0103] <Relative Ratio of Components (a) to (c) in the Monomer Group>

[0104] The upper and lower limits of the molar ratio of the component (a) to the component (b) contained in the monomer group [the amount of the substance of the component (a) / the amount of the substance of the component (b)] are exemplified by 4, 3, 2, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0.09, 0.07, 0.05, etc. In one embodiment, the molar ratio of the component (a) to the component (b) contained in the monomer group [the amount of the substance of the component (a) / the amount of the substance of the component (b)] is preferably 0.05 to 4.

[0105] The upper and lower limits of the molar ratio of the component (a) to the component (c) contained in the monomer group [the amount of the substance of the component (a) / the amount of the substance of the component (c)] are exemplified by 8000, 7500, 5000, 2500, 1000, 750, 500, 250, 100, 90, 75, 50, 25, 10, 9, 7, 5, 3, 1, 0.9, 0.7, 0.5, 0.3, 0.1, etc. In one embodiment, the molar ratio of the component (a) to the component (c) contained in the monomer group [the amount of the substance of the component (a) / the amount of the substance of the component (c)] is preferably 0.1 to 8000.

[0106] The upper and lower limits of the molar ratio of the component (b) to the component (c) contained in the monomer group [the amount of the substance of the component (b) / the amount of the substance of the component (c)] are exemplified by 9500, 9000, 8000, 7500, 5000, 2500, 1000, 750, 500, 250, 100, 90, 75, 50, 25, 10, 9, 7, 5, 3, 1, 0.9, 0.7, 0.5, 0.4, etc. In one embodiment, the molar ratio of the component (b) to the component (c) contained in the monomer group [the amount of the substance of the component (b) / the amount of the substance of the component (c)] is preferably 0.4 to 9500.

[0107] The upper and lower limits of the mass ratio of the component (a) to the component (b) contained in the monomer group [mass of the component (a) / mass of the component (b)] are exemplified by 8.5, 8, 7.5, 5, 3, 1, 0.9, 0.5, 0.3, 0.1, 0.09, 0.06, etc. In one embodiment, the mass ratio of the component (a) to the component (b) contained in the monomer group [mass of the component (a) / mass of the component (b)] is preferably 0.06 to 8.5.

[0108] The upper and lower limits of the mass ratio of the component (a) to the component (c) contained in the monomer group [mass of the component (a) / mass of the component (c)] are exemplified by 8500, 8000, 7500, 5000, 2500, 1000, 750, 500, 250, 100, 90, 75, 50, 25, 10, 9, 7, 5, 3, 1, 0.9, 0.7, 0.5, 0.3, 0.1, 0.09, 0.06, etc. In one embodiment, the mass ratio of the component (a) to the component (c) contained in the monomer group [mass of the component (a) / mass of the component (c)] is preferably 0.06 to 8500.

[0109] The upper and lower limits of the mass ratio of the component (b) to the component (c) contained in the monomer group [mass of the component (b) / mass of the component (c)] are exemplified by 8000, 7500, 5000, 2500, 1000, 750, 500, 250, 100, 90, 75, 50, 25, 10, 9, 7, 5, 3, 1, 0.9, 0.7, 0.5, 0.3, 0.13, etc. In one embodiment, the mass ratio of the component (b) to the component (c) contained in the monomer group [mass of the component (b) / mass of the component (c)] is preferably 0.13 to 8000.

[0110] <Monomers other than any of the above: also referred to as other components>

[0111] The monomer group may contain monomers other than components (a) to (c) as long as the desired effects of the present invention are not impaired. As the other components, various known components may be used alone or in combination of two or more.

[0112] Examples of other components include unsaturated carboxylic acid esters not containing a hydroxyl group, conjugated dienes, and aromatic vinyl compounds.

[0113] The hydroxyl-free unsaturated carboxylic acid ester is preferably a hydroxyl-free (meth)acrylate. Examples of the hydroxyl-free (meth)acrylate include a hydroxyl-free linear (meth)acrylate, a hydroxyl-free branched (meth)acrylate, a hydroxyl-free alicyclic (meth)acrylate, and a hydroxyl-free substituted (meth)acrylate.

[0114] Examples of the hydroxyl-free linear (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, hexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, and decyl (meth)acrylate.

[0115] Examples of the branched (meth)acrylate not containing a hydroxyl group include isopropyl (meth)acrylate, isobutyl (meth)acrylate, isoamyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate.

[0116] Examples of the alicyclic (meth)acrylate not containing a hydroxyl group include cyclohexyl (meth)acrylate and the like.

[0117] Examples of the substituted (meth)acrylate not containing a hydroxyl group include glycidyl (meth)acrylate, allyl (meth)acrylate, and ethylene di(meth)acrylate.

[0118] The unsaturated carboxylic acid ester containing no hydroxyl group can be suitably used for the purpose of imparting flexibility to the electrode. From the above viewpoint, the content of the unsaturated carboxylic acid ester containing no hydroxyl group is preferably less than 40 mol% (e.g., less than 30 mol%, less than 20 mol%, less than 19 mol%, less than 15 mol%, less than 10 mol%, less than 5 mol%, less than 1 mol%, 0 mol%) relative to 100 mol% of the above monomer group.

[0119] In addition, the content of the unsaturated carboxylic acid ester not containing a hydroxyl group is preferably 90 mass% or less (for example, less than 80 mass%, less than 70 mass%, less than 60 mass%, less than 50 mass%, less than 40 mass%, less than 30 mass%, less than 20 mass%, less than 19 mass%, less than 15 mass%, less than 10 mass%, less than 5 mass%, less than 1 mass%, or 0 mass%) relative to 100 mass% of the above-mentioned monomer group.

[0120] Examples of the conjugated diene include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted straight-chain conjugated pentadiene, and substituted side-chain conjugated hexadiene (substituted and side-chain conjugated hexadiene).

[0121] From the viewpoint of the cycle characteristics of the lithium ion battery, the content of the conjugated diene is preferably less than 10 mol %, more preferably 0 mol %, based on 100 mol % of the monomer group.

[0122] The upper and lower limits of the content of the conjugated diene relative to 100 mass % of the monomer group are exemplified by 30 mass %, 20 mass %, 10 mass %, 5 mass %, 1 mass %, 0 mass %, etc. In one embodiment, the content is preferably 0 mass % to 30 mass %.

[0123] Examples of the aromatic vinyl compound include styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, chlorostyrene, and divinylbenzene.

[0124] From the viewpoint of the cycle characteristics of the lithium ion battery, the content of the aromatic vinyl compound is preferably less than 10 mol %, more preferably 0 mol %, based on 100 mol % of the monomer group.

[0125] The upper and lower limits of the content of the aromatic vinyl compound relative to 100 mass % of the monomer group are exemplified by 30 mass %, 20 mass %, 10 mass %, 5 mass %, 1 mass %, 0 mass %, etc. In one embodiment, the content is preferably 0 mass % to 30 mass %.

[0126] As for the ratio of the above-mentioned unsaturated carboxylic acid ester not containing hydroxyl group, the above-mentioned conjugated diene, and other components other than the above-mentioned aromatic vinyl compound in the above-mentioned monomer group, examples thereof include less than 10 mol%, less than 5 mol%, less than 2 mol%, less than 1 mol%, less than 0.1 mol%, less than 0.01 mol%, and 0 mol%, relative to 100 mol% of the above-mentioned monomer group. In addition, examples thereof include less than 10 mass%, less than 9 mass%, less than 7 mass%, less than 5 mass%, less than 4 mass%, less than 2 mass%, less than 1 mass%, less than 0.9 mass%, less than 0.5 mass%, less than 0.3 mass%, less than 0.1 mass%, less than 0.05 mass%, less than 0.01 mass%, and 0 mass%, relative to 100 mass% of the above-mentioned monomer group.

[0127] <Method for producing component (A)>

[0128] The component (A) can be synthesized using various known polymerization methods, preferably using a free radical polymerization method. Specifically, it is preferred to add a free radical polymerization initiator and, if necessary, a chain transfer agent to a monomer mixture containing the above components, and perform a polymerization reaction at a reaction temperature of 50° C. to 100° C. while stirring. The reaction time is not particularly limited, but is preferably 1 to 10 hours.

[0129] The free radical polymerization initiator is not particularly limited, and various known free radical polymerization initiators can be used. Examples of free radical polymerization initiators include persulfates such as potassium persulfate and ammonium persulfate; redox polymerization initiators in which the above persulfates are combined with reducing agents such as sodium bisulfite; azo initiators such as 2,2′-azobis-2-amidinopropane dihydrochloride, etc. The amount of the free radical polymerization initiator used is not particularly limited, and is preferably 0.05% to 5.0% by mass, and more preferably 0.1% to 3.0% by mass, relative to 100% by mass of the monomer group providing component (A).

[0130] Before the free radical polymerization reaction and / or when the obtained component (A) is dissolved in water, the pH of the reaction solution may be adjusted using a common neutralizing agent such as ammonia and organic amines, potassium hydroxide, sodium hydroxide, lithium hydroxide, etc., for the purpose of improving the manufacturing stability. In this case, the pH is preferably 2 to 11. In addition, ethylenediaminetetraacetic acid (EDTA) or its salts may be used as metal ion sealants for the same purpose.

[0131] When component (A) has an acid group (acid group), it can be used by adjusting the appropriate neutralization rate according to the application (a neutralization rate of 100% means neutralization with a base of the same molar number as the acid component contained in component (A); a neutralization rate of 50% means neutralization with a base of half the molar number of the acid component contained in component (A)). The neutralization rate when dispersing the electrode active material is not particularly limited. In one embodiment, it is preferably 95% to 100% after the formation of a coating, etc. From the viewpoint of preventing the initial capacity from decreasing, it is preferably 95% or more; from the viewpoint of preventing hydrolysis, it is preferably less than 100%. Examples of neutralizing salts include Li salts, Na salts, K salts, ammonium salts, Mg salts, Ca salts, Zn salts, Al salts, and the like.

[0132] In one embodiment, the component (A) is preferably an inorganic salt. The inorganic salt of the component (A) refers to a salt whose cation part is a metal cation. Examples of the inorganic salt include the above-mentioned inorganic salts.

[0133] <(A) Physical properties of components>

[0134] The upper limit and lower limit of the glass transition temperature of the component (A) are exemplified by 160°C, 155°C, 150°C, 145°C, 140°C, 135°C, 130°C, 125°C, 120°C, 115°C, 110°C, 105°C, 100°C, 95°C, 90°C, 85°C, 80°C, 75°C, 70°C, 65°C, 60°C, 55°C, 50°C, 45°C, 40°C, 35°C, 30°C, 25°C, 20°C, 15°C, 10°C, 5°C, 0°C, etc. In one embodiment, it is preferably 0°C or higher, and more preferably 30°C or higher from the viewpoint of mechanical strength and heat resistance.

[0135] The glass transition temperature of the component (A) can be adjusted by the combination of monomers. The glass transition temperature of the component (A) can be determined from the glass transition temperature (Tg, absolute temperature: K) of the homopolymer of the monomers and their mass fractions according to the Fox equation shown below.

[0136] 1 / Tg=(W1 / Tg1)+(W2 / Tg2)+(W3 / Tg3)+…+(W n / Tg n )

[0137] [Wherein, Tg represents the glass transition temperature (K) of the polymer to be determined, W1~W n Indicates the mass fraction of each monomer, Tg1~Tg n represents the glass transition temperature (K) of each monomer homopolymer].

[0138] For example, the glass transition temperature is 165°C for acrylamide homopolymers, 106°C for acrylic acid homopolymers, -15°C for hydroxyethyl acrylate homopolymers, and 105°C for acrylonitrile homopolymers. In order to obtain the (A) component having the desired glass transition temperature, the composition of the monomers constituting it can be determined. In addition, the glass transition temperature of the homopolymer of the monomer can be measured by DSC (differential scanning calorimeter), DTA (differential thermal analyzer), TMA (thermomechanical measuring device), etc., for example, under conditions of heating from -100°C to 300°C (heating rate 10°C / min.). In addition, the values ​​recorded in the literature can also be used. The literature exemplifies "Chemical Handbook (Chemical Handbook) Basics II Edited by the Chemical Society of Japan (Revised 5th Edition)", p325, etc.

[0139] The gel fraction of the cured product of component (A) is not particularly limited, and the upper and lower limits of the gel fraction of the cured product of component (A) are exemplified by 99.9%, 95%, 90%, 85%, 80%, 75%, 70%, 65%, 60%, 55%, 50%, 45%, 40%, 35%, 30%, 25%, 20%, etc. In one embodiment, from the viewpoint of the effect of anti-rebound accompanying charge and discharge cycles, it is preferably 20% or more, and more preferably 25% or more.

[0140] The gel fraction of the cured product of the component (A) is a value calculated by the following formula:

[0141] Gel fraction (%) = {insoluble residue in water (g) / mass of solid resin (g)} × 100

[0142] In one embodiment, the curing conditions of the cured product are exemplified by 120° C. for 4 hours.

[0143] The gel fraction is measured, for example, as follows. An appropriate amount (e.g., 10 g) of an aqueous solution of a binder for lithium-ion battery electrodes containing the component (A) is added to an appropriate container (e.g., an ointment jar (manufactured by Souichi Glass Co., Ltd., product name "Tinplate ointment jar (Ointment Can Brick)")) and dried under appropriate drying conditions (e.g., at 120°C for 4 hours using a circulating air dryer (manufactured by ADVANTECH Toyo Co., Ltd., product name "Air Supply Constant Temperature Dryer DSR420DA")) to obtain a heat-crosslinked solid resin. The mass of the solid resin is accurately measured at 25°C using an appropriate mass meter (e.g., manufactured by Sartorius Japan Co., Ltd., product name "Standard Balance CPA324S"). The solid resin to be measured is transferred to a suitable container (e.g., a 300 mL beaker) containing an appropriate amount (e.g., 150 mL) of pure water, and immersed in the water under stirring conditions (e.g., 3 hours at 25°C) using a suitable magnetic stirrer (e.g., manufactured by Tokyo Rikaki Co., Ltd., product name "Powerful Magnetic Stirrer RCX-1000D"), and then filtered under reduced pressure using a suitable apparatus (e.g., using a Kiriyama funnel (Kiriyama Route) (manufactured by Kiriyama Manufacturing Co., Ltd., product name "Kiriyama Funnel SB-60") and a suction bell (suction bell) (manufactured by Kiriyama Manufacturing Co., Ltd., product name "suction bell VKB-200") through filter paper (manufactured by Kiriyama Manufacturing Co., Ltd., "No. 50B")). Then, the insoluble residue remaining on the filter paper is dried under appropriate conditions (e.g., 3 hours at 120°C) using an appropriate dryer (e.g., the above-mentioned circulating air dryer), and the mass of the insoluble residue is accurately measured using an appropriate mass meter (e.g., the above-mentioned mass meter) at an appropriate temperature (e.g., 25°C), and the gel fraction of the resin after thermal crosslinking of the water-soluble battery binder is calculated using the above formula.

[0144] It is believed that the thermal crosslinking of component (A) is caused by the hydroxyl group derived from the hydroxyl-containing vinyl ether (a) and the amide group derived from the (meth)acrylamide-containing compound (b). In component (A), the molar ratio of hydroxyl group to amide group (hydroxyl group / amide group) is not particularly limited, and preferably the amide group is in excess. The upper and lower limits of the molar ratio of hydroxyl group to amide group (hydroxyl group / amide group) are exemplified as 2.0, 1.5, 1.0, 0.9, 0.7, 0.5, 0.3, 0.1, 0.09, 0.07, 0.05, etc. In one embodiment, preferably hydroxyl group / amide group = 0.05 to 2.0, more preferably 0.1 to 2.0. By satisfying the above conditions, it is believed that the effect of anti-rebound resilience accompanying charge and discharge cycles can be obtained without damaging the adhesion between the active material layer and the collector, but it does not mean that the present invention is limited thereto.

[0145] The weight average molecular weight (Mw) of the component (A) is not particularly limited, and the upper and lower limits thereof are exemplified by 7 million, 6.5 million, 6 million, 5.5 million, 5 million, 4.5 million, 4 million, 3.5 million, 3 million, 2.5 million, 2 million, 1.5 million, 1 million, 950,000, 900,000, 850,000, 800,000, 750,000, 700,000, 650,000, 600,000, 550,000, 500,000, 450,000, 400,000, 350,000, 300,000, 250,000, 200,000, 150,000, 100,000, etc. In one embodiment, from the viewpoint of the dispersion stability of the slurry, it is preferably 100,000 to 7 million, and more preferably 350,000 to 6 million.

[0146] The number average molecular weight (Mn) of the component (A) is not particularly limited, and the upper and lower limits thereof are exemplified by 6,000,000, 5,500,000, 5,000,000, 4,500,000, 4,000,000, 3,500,000, 3,000,000, 2,500,000, 2,000,000, 1,500,000, 950,000, 900,000, 850,000, 800,000, 750,000, 700,000, 650,000, 600,000, 550,000, 500,000, 450,000, 400,000, 300,000, 200,000, 100,000, 50,000, 10,000, etc. In one embodiment, the number average molecular weight (Mn) of the component (A) is preferably 10,000 or more.

[0147] The weight average molecular weight and the number average molecular weight can be determined as polyacrylic acid-equivalent values ​​measured by gel permeation chromatography (GPC) in an appropriate solvent, for example.

[0148] The upper and lower limits of the molecular weight distribution (Mw / Mn) of the component (A) are exemplified by 15, 14, 13, 11, 10, 9, 7.5, 5, 4, 3, 2.9, 2.5, 2, 1.5, 1.1, etc. In one embodiment, the molecular weight distribution (Mw / Mn) of the component (A) is preferably 1.1-15.

[0149] The B-type viscosity of the aqueous solution containing 13% by mass of the component (A) is not particularly limited, and the upper and lower limits thereof are exemplified by 100,000 mPa·s, 90,000 mPa·s, 80,000 mPa·s, 70,000 mPa·s, 60,000 mPa·s, 50,000 mPa·s, 45,000 mPa·s, 40,000 mPa·s, 30,000 mPa·s, 20,000 mPa·s, 10,000 mPa·s, 9000 mPa·s, 8000 mPa·s, 7000 mPa·s, 6000 mPa·s, 5000 mPa·s, 4000 mPa·s, 3000 mPa·s, 2000 mPa·s, 1000 mPa·s, 900 mPa·s, 700 mPa·s, 500 mPa·s, 300 mPa·s, 200 mPa·s, and 100 mPa·s. In one embodiment, the B-type viscosity is preferably in the range of 100 mPa·s to 100,000 mPa·s.

[0150] The B-type viscosity is measured using a B-type viscometer such as "B-type Viscometer BM" manufactured by Toki Sangyo Co., Ltd.

[0151] The upper and lower limits of the pH of the aqueous solution of the binder for lithium ion battery electrodes are exemplified by 9, 8.9, 8.5, 8, 7.9, 7.5, 7, 6.9, 6.5, 6, 5.9, 5.6, 5.5, 5.4, 5.2, 5.1, 5, etc. In one embodiment, the pH of the aqueous solution of the binder for lithium ion battery electrodes is preferably pH 5 to 9 from the viewpoint of solution stability.

[0152] The pH can be measured at 25° C. using a glass electrode pH meter (for example, manufactured by Horiba, Ltd., product name “pH meter D-52”).

[0153] The upper and lower limits of the content of the component (A) relative to 100% by mass of the aqueous solution of the binder for lithium ion battery electrodes are exemplified by 25% by mass, 23% by mass, 21% by mass, 20% by mass, 19% by mass, 15% by mass, 14% by mass, 12% by mass, 10% by mass, 9% by mass, 7% by mass, 6% by mass, 5% by mass, etc. In one embodiment, the content of the component (A) is preferably 5% to 25% by mass relative to 100% by mass of the aqueous solution of the binder for lithium ion battery electrodes.

[0154] The upper and lower limits of the water content relative to 100 mass % of the lithium ion battery electrode binder aqueous solution are exemplified by 95 mass %, 90 mass %, 85 mass %, 80 mass %, etc. In one embodiment, the water content relative to 100 mass % of the lithium ion battery electrode binder aqueous solution is preferably 80 mass % to 95 mass %.

[0155] The upper and lower limits of the mass ratio of the component (A) contained in the aqueous solution of the lithium ion battery electrode binder to water are 0.25, 0.2, 0.15, 0.1, 0.05, etc. In one embodiment, the mass ratio of the component (A) contained in the aqueous solution of the lithium ion battery electrode binder to water is preferably 0.05 to 0.25.

[0156] <Additives>

[0157] The aqueous binder solution for lithium ion battery electrodes may contain a substance which is neither the component (A) nor water as an additive.

[0158] Examples of the additive include a dispersant, a leveling agent, an antioxidant, a thickener, and a dispersion (emulsion).

[0159] The content of the additive relative to 100 mass % of the component (A) is exemplified by 5 mass % or less, less than 5 mass %, less than 4 mass %, less than 2 mass %, less than 1 mass %, less than 0.9 mass %, less than 0.5 mass %, less than 0.4 mass %, less than 0.2 mass %, less than 0.1 mass %, less than 0.09 mass %, less than 0.05 mass %, less than 0.04 mass %, less than 0.02 mass %, less than 0.01 mass %, 0 mass %, etc. In one embodiment, from the viewpoint of generating HAZE in the adhesive when exceeding 5 mass %, the content of the additive relative to 100 mass % of the component (A) is preferably 5 mass % or less.

[0160] In addition, the content of the additive relative to 100 mass % of the above-mentioned aqueous solution is exemplified as less than 5 mass %, less than 4 mass %, less than 2 mass %, less than 1 mass %, less than 0.9 mass %, less than 0.5 mass %, less than 0.4 mass %, less than 0.2 mass %, less than 0.1 mass %, less than 0.09 mass %, less than 0.05 mass %, less than 0.04 mass %, less than 0.02 mass %, less than 0.01 mass %, 0 mass %, etc.

[0161] Examples of the dispersant include anionic dispersants, cationic dispersants, nonionic dispersants, and polymer dispersants.

[0162] Examples of the leveling agent include surfactants such as alkyl surfactants, silicon surfactants, fluorine surfactants, and metal surfactants. By using a surfactant, craters generated during coating can be prevented, and the smoothness of the slurry layer (coating) can be improved.

[0163] Examples of the antioxidant include phenol compounds, hydroquinone compounds, organic phosphine compounds, sulfur compounds, phenylenediamine compounds, polymer phenol compounds, etc. The polymer phenol compound is a polymer having a phenol structure in the molecule. The weight average molecular weight of the polymer phenol compound is preferably 200 to 1000, more preferably 600 to 700.

[0164] Examples of thickeners include cellulose polymers such as carboxymethyl cellulose, methyl cellulose, hydroxypropyl cellulose, and their ammonium salts and alkali metal salts; (modified) poly(meth)acrylic acid and their ammonium salts and alkali metal salts; (modified) polyvinyl alcohol, copolymers of acrylic acid or acrylic acid salts and vinyl alcohol, polyvinyl alcohols such as copolymers of maleic anhydride or maleic acid or fumaric acid and vinyl alcohol; polyethylene glycol, polyethylene oxide, polyvinyl pyrrolidone, modified polyacrylic acid, oxidized starch, starch phosphate, casein, various modified starches, acrylonitrile-butadiene copolymer hydrogenates, etc.

[0165] Examples of the dispersion (emulsion) include styrene-butadiene copolymer latex, polystyrene polymer latex, polybutadiene polymer latex, acrylonitrile-butadiene copolymer latex, polyurethane polymer latex, polymethyl methacrylate polymer latex, methyl methacrylate-butadiene copolymer latex, polyacrylate polymer latex, vinyl chloride polymer latex, vinyl acetate polymer emulsion, vinyl acetate-ethylene copolymer emulsion, polyethylene emulsion, carboxyl-modified styrene-butadiene copolymer resin emulsion, acrylic resin emulsion, polyethylene, polypropylene, polyethylene terephthalate, polyamide (PA), polyimide (PI), polyamideimide (PAI), aromatic polyamide, alginic acid and its salts, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), etc.

[0166] In addition, about dispersion (emulsion), it is also possible to contain in an amount more than the content of the above-mentioned additive. Relative to (A) component 100 mass%, the upper and lower limits of the content of dispersion (emulsion) are exemplified as 20 mass%, 19 mass%, 17 mass%, 15 mass%, 13 mass%, 10 mass%, 9 mass%, 7 mass%, 5 mass%, 4 mass%, 2 mass%, 1 mass%, 0 mass%, etc. In one embodiment, from the viewpoint of resilience resistance and discharge capacity retention rate, relative to (A) component 100 mass%, the addition amount of dispersion (emulsion) is preferably less than 5 mass%.

[0167] The aqueous binder solution for lithium ion battery electrodes can be used as an aqueous binder solution for lithium ion battery negative electrodes and an aqueous binder solution for lithium ion battery positive electrodes.

[0168] [Lithium-ion battery electrode slurry: also called slurry]

[0169] The present disclosure provides a slurry for lithium ion battery electrodes, comprising the above-mentioned aqueous binder solution for lithium ion battery electrodes and an electrode active material (B).

[0170] In this disclosure, "slurry" refers to a suspension of liquid and solid particles.

[0171] The upper and lower limits of the content of the component (A) relative to 100 mass % of the slurry are exemplified by 99.9 mass %, 95 mass %, 90 mass %, 85 mass %, 80 mass %, 75 mass %, 70 mass %, 65 mass %, 60 mass %, 55 mass %, 50 mass %, 45 mass %, 40 mass %, 35 mass %, 30 mass %, 25 mass %, 20 mass %, 15 mass %, 10 mass %, 5 mass %, 4 mass %, 2 mass %, 1 mass %, 0.9 mass %, 0.5 mass %, 0.2 mass %, 0.1 mass %, etc. In one embodiment, the content is preferably 0.1 mass % to 99.9 mass %.

[0172] Examples of water include ultrapure water, pure water, distilled water, ion-exchanged water, and tap water.

[0173] The upper and lower limits of the water content relative to 100 mass % of the slurry are exemplified by 70 mass %, 65 mass %, 60 mass %, 55 mass %, 50 mass %, 45 mass %, 40 mass %, 35 mass %, 30 mass %, etc. In one embodiment, the water content is preferably 30 mass % to 70 mass %.

[0174] <Electrode Active Material (B)>

[0175] The electrode active material may be used alone or in combination of two or more. Examples of the electrode active material include a negative electrode active material and a positive electrode active material.

[0176] As long as it is a material that can reversibly absorb and release lithium, the negative electrode active material is not particularly limited, and a suitable material can be appropriately selected according to the type of the target lithium ion battery, and can be used alone or in combination of two or more. Examples of the negative electrode active material include carbon materials and silicon materials, oxides containing lithium atoms, lead compounds, tin compounds, arsenic compounds, antimony compounds, and aluminum compounds that are alloyed with lithium.

[0177] Examples of the above-mentioned carbon materials include graphite (also called black lead, examples include natural graphite, artificial graphite, etc.) as highly crystalline carbon, low-crystalline carbon (soft carbon, hard carbon), carbon black (ketjen black, acetylene black, channel black, lamp black, oil furnace black, thermal black, etc.), fullerenes, carbon nanotubes, carbon nanofibers, carbon nanohorns, carbon fibrils, mesophase carbon microbeads (MCMB), pitch-based carbon fibers, etc.

[0178] The silicon material includes SiC, SiO x C y (0<x≤3, 0<y≤5); Si3N4; Si2N2O; with SiO xSilicon oxide composites represented by (0<x≤2) (for example, materials described in Japanese Patent Publication No. 2004-185810 and Japanese Patent Publication No. 2005-259697); silicon materials described in Japanese Patent Publication No. 2004-185810, etc. In addition, silicon materials described in Japanese Patent No. 5390336 and Japanese Patent No. 5903761 can also be used.

[0179] The silicon oxide is preferably of the composition formula SiO x Silicon oxide represented by (0<x<2, preferably 0.1≤x≤1).

[0180] The silicon alloy is preferably an alloy of silicon and at least one transition metal, and the transition metal is selected from the group consisting of titanium, zirconium, nickel, copper, iron and molybdenum. These transition metal silicon alloys have high electronic conductivity and high strength, so they are preferred. The silicon alloy is more preferably a silicon-nickel alloy or a silicon-titanium alloy, and is particularly preferably a silicon-titanium alloy. Relative to 100 mol% of the metal element in the silicon alloy, the content of silicon in the silicon alloy is preferably 10 mol% or more, and more preferably 20 mol% to 70 mol%. In addition, the silicon material can be any of single crystal, polycrystalline and amorphous.

[0181] In addition, when using silicon materials as electrode active materials, electrode active materials other than silicon materials may be used in combination. Examples of such electrode active materials include the above-mentioned carbon materials; conductive polymers such as polyphenylene; X B Y O Z (A represents an alkali metal or a transition metal; B represents at least one transition metal selected from cobalt, nickel, aluminum, tin, manganese, etc.; O represents an oxygen atom; X, Y and Z are numbers in the range of 0.05<X<1.10, 0.85<Y<4.00, 1.5<Z<5.00, respectively); and other metal oxides, etc. When a silicon material is used as an electrode active material, the volume change accompanying the absorption and release of lithium is small, so it is preferably used in combination with a carbon material.

[0182] Examples of the above-mentioned oxides containing lithium atoms include ternary nickel cobalt manganese oxide, lithium-manganese composite oxides (LiMn2O4, etc.), lithium-nickel composite oxides (LiNiO2, etc.), lithium-cobalt composite oxides (LiCoO2, etc.), lithium-iron composite oxides (LiFeO2, etc.), lithium-nickel-manganese composite oxides (LiNi 0.5 Mn 0.5 O2, etc.), lithium-nickel-cobalt composite oxide (LiNi 0.8 Co 0.2O2, etc.), lithium-transition metal phosphate compounds (LiFePO4, etc.) and lithium-transition metal sulfate compounds (Li x Fe2(SO4)3), lithium-titanium composite oxide (lithium titanate: Li4Ti5O 12 ) and other lithium-transition metal composite oxides and other previously known electrode active materials.

[0183] From the viewpoint of significantly exerting the effects of the present invention, the carbon material and / or the material alloying with lithium contained in the electrode active material is preferably 50 mass % or more, more preferably 80 mass % or more, further preferably 90 mass % or more, and particularly preferably 100 mass %.

[0184] In one embodiment, the electrode active material (B) is preferably a negative electrode active material containing 1 mass % or more (2 mass % or more, 5 mass % or more, 10 mass % or more, 25 mass % or more, 50 mass % or more, 75 mass % or more, 90 mass % or more, 100 mass %) of silicon and / or silicon oxide covered with a carbon layer.

[0185] Positive electrode active materials can be roughly divided into active materials containing inorganic compounds and active materials containing organic compounds. Examples of inorganic compounds contained in positive electrode active materials include metal oxides. Examples of metal oxides include transition metal oxides, composite oxides of lithium and transition metals, transition metal sulfides, etc. Examples of the above transition metals include Fe, Co, Ni, Mn, Al, etc. Examples of inorganic compounds used in positive electrode active materials include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiFePO4, LiNi 1 / 2 Mn 3 / 2 O4、LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2、LiCo 0.3 Ni 0.5 Mn 0.2 O2、LiCo 0.2 Ni 0.6 Mn 0.2 O2、LiCo 0.1 Ni 0.8 Mn 0.1 O2、LiCo 0.15 Ni 0.8 Al 0.05 O2, Li[Li 0.1 Al 0.1 Mn 1.8]O4, LiFeVO4 and other lithium-containing composite metal oxides; TiS2, TiS3, amorphous MoS2 and other transition metal sulfides; Cu2V2O3, amorphous V2O-P2O5, MoO3, V2O5, V6O 13 Transition metal oxides, etc. These compounds may also be compounds with partial element substitution. Examples of organic compounds contained in the positive electrode active material include conductive polymers such as polyacetylene and polyparaphenylene. By allowing the carbon source to be present during reduction calcination, iron-based oxides with poor conductivity may also be used as electrode active materials covered with carbon materials. In addition, these compounds may also be compounds with partial element substitution. Among them, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiFePO4, LiNi 1 / 2 Mn 3 / 2 O4、LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3O2、LiCo 0.3 Ni 0.5 Mn 0.2 O2、LiCo 0.2 Ni 0.6 Mn 0.2 O2、LiCo 0.1 Ni 0.8 Mn 0.1 O2、LiCo 0.15 Ni 0.8 Al 0.05 O2, Li[Li 0.1 Al 0.1 Mn 1.8 ]O4.

[0186] In one embodiment, the electrode active material (B) is preferably a positive electrode active material containing iron phosphate and / or a metal oxide.

[0187] The shape of the electrode active material is not particularly limited, and can be any shape such as microparticles and thin films, preferably microparticles. The average particle size of the electrode active material is not particularly limited, and its upper and lower limits are exemplified by 50μm, 45μm, 40μm, 35μm, 30μm, 25μm, 20μm, 15μm, 10μm, 5μm, 4μm, 3μm, 2.9μm, 2μm, 1μm, 0.5μm, 0.1μm, etc. More specifically, in one embodiment, from the viewpoint of uniformly forming a thin coating film, if it is above 0.1μm, the operability is good, and if it is below 50μm, it is easy to apply the electrode, so the average particle size of the electrode active material is preferably 0.1μm to 50μm, more preferably 0.1μm to 45μm, further preferably 1μm to 10μm, and particularly preferably 5μm.

[0188] In the present disclosure, "particle size" refers to the maximum distance between any two points on the contour line of a particle (the same below). In addition, in the present disclosure, unless otherwise specified, "average particle size" refers to a value calculated as the average value of the particle sizes of particles observed in several to dozens of fields of view using an observation method such as a scanning electron microscope (SEM) and a transmission electron microscope (TEM) (the same below).

[0189] In the above-mentioned slurry, relative to 100 mass % of the electrode active material (B), the upper and lower limits of the content of the (A) component are exemplified as 15 mass %, 14 mass %, 13 mass %, 12 mass %, 11 mass %, 10 mass %, 9 mass %, 8 mass %, 7 mass %, 6 mass %, 5 mass %, 4 mass %, 3 mass %, 2 mass %, 1.5 mass %, 1 mass %, 0.5 mass %, etc. In one embodiment, relative to 100 mass % of the electrode active material (B), the content of the (A) component is preferably 0.5 mass % to 15 mass %.

[0190] <Conductive additive>

[0191] In one embodiment, the slurry may contain a conductive aid. Examples of the conductive aid include fibrous carbon such as vapor grown carbon fiber (VGCF), carbon nanotube (CNT), carbon nanofiber (CNF); graphite particles; carbon black such as acetylene black, Ketjen black, furnace black; Cu, Ni, Al, Si or their alloys having an average particle size of less than 10 μm, etc. The content of the conductive aid is not particularly limited, and is preferably 0% to 10% by mass, more preferably 0.5% to 6% by mass, relative to the electrode active material component.

[0192] <Slurry Viscosity Adjusting Solvent>

[0193] The slurry viscosity adjusting solvent is not particularly limited, and may include a non-aqueous medium having a normal boiling point of 80° C. to 350° C. The slurry viscosity adjusting solvent may be used alone or in combination of two or more. Examples of the slurry viscosity adjusting solvent include amide solvents such as N-methylpyrrolidone, dimethylformamide, and N,N-dimethylacetamide; hydrocarbon solvents such as toluene, xylene, n-dodecane, and tetralin; alcohol solvents such as methanol, ethanol, 2-propanol, isopropanol, 2-ethyl-1-hexanol, 1-nonanol, and lauryl alcohol; ketone solvents such as acetone, methyl ethyl ketone, cyclohexanone, phorone, acetophenone, and isophorone; ether solvents such as dioxane and tetrahydrofuran (THF); ester solvents such as benzyl acetate, isoamyl butyrate, methyl lactate, ethyl lactate, and butyl lactate; amine solvents such as o-toluidine, m-toluidine, and p-toluidine; lactones such as γ-butyrolactone and δ-butyrolactone; sulfoxide / sulfone solvents such as dimethyl sulfoxide and sulfolane; water, etc. Among them, N-methylpyrrolidone is preferred from the viewpoint of coating workability. The content of the non-aqueous medium is not particularly limited, but is preferably 0% by mass to 10% by mass relative to 100% by mass of the slurry.

[0194] The slurry may contain, as an additive, a component other than component (A), component (B), water, a conductive additive, or a slurry viscosity adjusting solvent, within a range not impairing the effects of the present invention. Examples of the additive include the above-mentioned additives.

[0195] The content of the additives relative to 100 mass % of the component (A) is exemplified by 0 mass % to 5 mass %, less than 1 mass %, less than 0.1 mass %, less than 0.01 mass %, 0 mass %, and the like.

[0196] The content of the additive relative to 100 mass % of the component (B) is exemplified by 0 mass % to 5 mass %, less than 1 mass %, less than 0.1 mass %, less than 0.01 mass %, 0 mass %, and the like.

[0197] In addition, about dispersion (emulsion), it is also possible to contain in an amount more than the content of the above-mentioned additive. Relative to 100% by mass of slurry for lithium ion battery electrodes, the upper and lower limits of the content of dispersion (emulsion) are exemplified as 20% by mass, 19% by mass, 17% by mass, 15% by mass, 13% by mass, 10% by mass, 9% by mass, 7% by mass, 5% by mass, 4% by mass, 2% by mass, 1% by mass, 0% by mass, etc. In one embodiment, from the viewpoint of resilience resistance and discharge capacity retention rate, relative to 100% by mass of the above-mentioned aqueous solution or the above-mentioned slurry for lithium ion battery electrodes, the addition amount of dispersion (emulsion) is preferably less than 5% by mass.

[0198] The slurry for lithium ion battery electrodes can be used as a slurry for lithium ion battery negative electrodes or a slurry for lithium ion battery positive electrodes.

[0199] The slurry is produced by mixing the component (A), the component (B), and water, and, if necessary, a conductive additive and a slurry viscosity adjusting solvent.

[0200] Examples of the mixing means for the slurry include a ball mill, a sand mill, a pigment disperser, a pounder, an ultrasonic disperser, a homogenizer, a planetary mixer, and a Hobart mixer.

[0201] [Lithium-ion battery electrodes]

[0202] The present disclosure provides a lithium ion battery electrode, which is obtained by applying the above-mentioned lithium ion battery electrode slurry on a current collector and drying and curing it. The above-mentioned lithium ion battery electrode has a cured product of the above-mentioned lithium ion battery electrode slurry on the surface of the current collector.

[0203] The current collector may be any of various known current collectors without particular limitation. The material of the current collector is not particularly limited, and examples thereof include metal materials such as copper, iron, aluminum, nickel, stainless steel, and nickel-plated steel; and carbon materials such as carbon cloth and carbon paper. The shape of the current collector is also not particularly limited, and in the case of metal materials, examples thereof include metal foil, metal cylinder, metal coil, and metal plate; and in the case of carbon materials, examples thereof include carbon plate, carbon film, and carbon cylinder. Among them, in the case of using the electrode active material for the negative electrode, copper foil is preferably used as the current collector because it is currently used in industrial products.

[0204] The coating means is not particularly limited, and examples thereof include conventionally known coating devices such as a comma coater, a gravure coater, a micro gravure coater, a die coater, and a bar coater.

[0205] The drying means is not particularly limited, but the temperature is preferably 60° C. to 200° C., more preferably 100° C. to 195° C. The atmosphere may be dry air or an inert atmosphere.

[0206] The thickness of the electrode (cured product) is not particularly limited, but is preferably 5 μm to 300 μm, more preferably 10 μm to 250 μm. Within the above range, a sufficient Li absorption and release function for a high-density current value can be easily obtained.

[0207] The lithium-ion battery electrode can be used as a positive electrode or a negative electrode of a lithium-ion battery.

[0208] [Lithium-ion battery]

[0209] The present disclosure provides a lithium ion battery comprising the lithium ion battery electrode. The battery also comprises an electrolyte and a packaging material, which are not particularly limited.

[0210] (Electrolyte)

[0211] Examples of the electrolyte include a non-aqueous electrolyte solution in which a supporting electrolyte is dissolved in a non-aqueous solvent. The non-aqueous electrolyte solution may contain a film-forming agent.

[0212] The non-aqueous solvent may be any known non-aqueous solvent without particular limitation, and may be used alone or in combination of two or more. Examples of the non-aqueous solvent include chain carbonate solvents such as diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate; cyclic carbonate solvents such as ethylene carbonate, propylene carbonate, and butylene carbonate; chain ether solvents such as 1,2-dimethoxyethane; cyclic ether solvents such as tetrahydrofuran, 2-methyltetrahydrofuran, sulfolane, and 1,3-dioxolane; chain ester solvents such as methyl formate, methyl acetate, and methyl propionate; cyclic ester solvents such as γ-butyrolactone and γ-valerolactone; acetonitrile, etc. Among them, a combination of mixed solvents containing cyclic carbonates and chain carbonates is preferred.

[0213] A lithium salt may be used as the supporting electrolyte. Various known lithium salts may be used as the lithium salt without particular limitation, and may be used alone or in combination of two or more. Examples of the supporting electrolyte include LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. Among them, LiPF6, LiClO4, and CF3SO3Li, which are easily soluble in a solvent and show a high degree of dissociation, are preferred. The higher the degree of dissociation of the supporting electrolyte used, the higher the lithium ion conductivity, and therefore, the lithium ion conductivity can be adjusted by the type of supporting electrolyte.

[0214] The film forming agent can use various known film forming agents without particular limitation, and can be used alone or in combination of two or more. The film forming agent exemplifies carbonate compounds such as vinylene carbonate, vinyl ethylene carbonate, vinyl ethyl carbonate, methyl phenyl carbonate, fluoroethylene carbonate, and difluoroethylene carbonate; cyclosulfide hydrocarbons such as ethylene sulfide and propylene sulfide; sultone compounds such as 1,3-propane sultone and 1,4-butane sultone; anhydrides such as maleic anhydride and succinic anhydride. The content of the film forming agent in the electrolyte solution is not particularly limited, and is preferably in the order of less than 10% by mass, less than 8% by mass, less than 5% by mass, and less than 2% by mass. By making the content less than 10% by mass, the advantage of the film forming agent is that it is easy to achieve the suppression of the initial irreversible capacity, the improvement of low temperature characteristics and rate characteristics, etc.

[0215] The form of the lithium-ion battery is not particularly limited. Examples of the lithium-ion battery include a cylindrical type in which the electrode sheet and the separator are spirally shaped; a cylindrical type in which the plate electrode and the separator are combined with an inside-out structure; and a button type in which the plate electrode and the separator are stacked. In addition, by placing these batteries in any outer packaging box, they can be used in any shape such as a button type, a cylindrical type, or a square type.

[0216] The manufacturing method of the lithium ion battery is not particularly limited, and can be assembled by taking appropriate procedures according to the structure of the battery. The manufacturing method of the lithium ion battery is exemplified by the method described in Japanese Patent Publication No. 2013-089437. The battery can be manufactured by installing a negative electrode on an outer packaging box, setting an electrolyte and a diaphragm thereon, and then installing a positive electrode so that the positive electrode and the negative electrode are opposite to each other, and fixing them with a gasket and a sealing plate.

[0217] Example

[0218] The present invention is described in detail below by way of examples and comparative examples. However, the description in the above preferred embodiments and the following examples are provided only for the purpose of illustration and are not provided for the purpose of limiting the present invention. Therefore, the scope of the present invention is not limited to the embodiments or examples specifically described in this specification, but is limited only by the scope of the claims. In addition, in each example and comparative example, unless otherwise specified, the numerical values ​​of parts, % and the like are based on mass.

[0219] 1. (A) Production of ingredients

[0220] Production Example 1

[0221] Into a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube, 1450 g of ion exchange water, 137.3 g (1.5580 mol) of hydroxyethyl vinyl ether, 188.6 g (1.3266 mol) of a 50% aqueous acrylamide solution, and 0.09 g (0.0006 mol) of sodium methallyl sulfonate were added, and oxygen in the reaction system was removed by nitrogen gas, and then the temperature was raised to 50°C. 2.3 g of 2,2′-azobis-2-amidinopropane dihydrochloride (2,2′-azobis-2-amidinopropane dihydrochloride) (manufactured by Nihon Chemical Co., Ltd., product name “NC-32”) and 50 g of ion exchange water were added thereto, and the mixture was heated to 80° C. and reacted for 3 hours to obtain an aqueous solution containing a water-soluble polymer.

[0222] Production Example 2

[0223] 550 g of ion exchange water was added to a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube. After removing oxygen in the reaction system with nitrogen, the temperature was raised to 80°C. A mixed solution of 99.0 g (1.1236 mol) of hydroxyethyl vinyl ether, 870.8 g (6.1241 mol) of a 50% acrylamide aqueous solution, 0.2 g (0.0014 mol) of sodium methallyl sulfonate, 100 g of ion exchange water, and a mixed solution of 5.3 g of 2,2′-azobis-2-amidinopropane dihydrochloride (manufactured by Nihon Ho Chemical Co., Ltd., product name "NC-32") and 170 g of ion exchange water were added dropwise simultaneously. The addition was continued dropwise over 3 hours while being kept at 80°C to obtain an aqueous solution containing a water-soluble polymer.

[0224] Production Examples 3 and 4

[0225] Except having changed the monomer composition in the said Production Example 1 into the thing shown in Table 1, it carried out similarly to Production Example 1, and prepared the aqueous solution containing a water-soluble polymer.

[0226] Production Example 5

[0227] 1340 g of ion exchange water, 68.8 g (0.7806 mol) of hydroxyethyl vinyl ether, 237.0 g (1.6669 mol) of 50% acrylamide aqueous solution, 55.2 g (0.6123 mol) of 80% acrylic acid, and 0.24 g (0.0015 mol) of sodium methallyl sulfonate were added to a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet pipe. After removing oxygen in the reaction system with nitrogen, the temperature was raised to 50° C. 2.3 g of 2,2′-azobis-2-amidinopropane dihydrochloride (manufactured by Nihon Kagaku Co., Ltd., product name “NC-32”) and 50 g of ion exchange water were added thereto, and the temperature was raised to 80° C. to carry out a reaction for 3 hours. Then, 51.0 g (0.6123 mol) of a 48% sodium hydroxide aqueous solution was added as a neutralizing agent and stirred, and ion-exchanged water was added so that the solid content concentration became 13%, thereby obtaining an aqueous solution containing a water-soluble polymer.

[0228] Production Example 6 and Production Example 7

[0229] Except having changed the monomer composition in the said Production Example 5 into the thing shown in Table 1, it carried out similarly to Production Example 5, and prepared the aqueous solution containing a water-soluble polymer.

[0230] Comparative Manufacturing Example 1

[0231] 1310 g of ion exchange water, 462.9 g (3.2549 mol) of 50% acrylamide aqueous solution, and 0.26 g (0.0016 mol) of sodium methallyl sulfonate were added to a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet tube. After removing oxygen in the reaction system with nitrogen, the temperature was raised to 50° C. 2.3 g of 2,2′-azobis-2-amidinopropane dihydrochloride (manufactured by Nihon Chemical Co., Ltd., product name “NC-32”) and 50 g of ion exchange water were added thereto, and the temperature was raised to 80° C. for 3 hours to react to obtain an aqueous solution containing a water-soluble polymer.

[0232] Comparative Manufacturing Example 2

[0233] Except having changed the monomer composition in the said comparative production example 1 into the thing shown in Table 1, it carried out similarly to the comparative production example 1, and prepared the aqueous solution containing a water-soluble polymer.

[0234] Comparative Manufacturing Example 3

[0235] 1400 g of ion exchange water, 200.9 g (1.4129 mol) of 50% acrylamide aqueous solution, 46.8 g (0.5194 mol) of 80% acrylic acid, 76.9 g (0.6623 mol) of 2-hydroxyethyl acrylate, and 0.41 g (0.0026 mol) of sodium methallyl sulfonate were added to a reaction apparatus equipped with a stirrer, a thermometer, a reflux condenser, and a nitrogen inlet pipe. After removing oxygen in the reaction system with nitrogen, the temperature was raised to 50° C. 2.2 g of 2,2′-azobis-2-amidinopropane dihydrochloride (manufactured by Nihon Chemical Co., Ltd., product name “NC-32”) and 50 g of ion exchange water were added thereto, and the temperature was raised to 80° C. to carry out a reaction for 3 hours. Then, 34.6 g (0.4156 mol) of a 48% sodium hydroxide aqueous solution was added as a neutralizing agent and stirred, and ion-exchanged water was added so that the solid content concentration became 13%, thereby obtaining an aqueous solution containing a water-soluble polymer.

[0236] Comparative Manufacturing Example 4

[0237] An aqueous solution containing a water-soluble polymer was prepared in the same manner as in Comparative Production Example 3 except that the monomer composition and the amount of the neutralizing agent in the above Comparative Production Example 3 were changed as shown in Table 1.

[0238] B-type viscosity

[0239] The viscosity of each binder aqueous solution was measured at 25° C. under the following conditions using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd., product name “B-type viscometer BM”).

[0240] When the viscosity is 100,000mPa·s to 20,000mPa·s: use No.4 rotor and rotate at 6rpm. When the viscosity is less than 20,000mPa·s: use No.3 rotor and rotate at 6rpm.

[0241] Weight average molecular weight

[0242] The weight average molecular weight was determined as a polyacrylic acid conversion value measured by gel permeation chromatography (GPC) in a 0.2 M phosphate buffer / acetonitrile solution (90 / 10, pH 8.0). The GPC apparatus used was HLC-8220 (manufactured by Tosoh Corporation) and the column used was SB-806M-HQ (manufactured by SHODEX).

[0243] Gel fraction

[0244] 10 g of the binder aqueous solution for lithium ion battery electrodes containing component (A) was placed in an ointment can (manufactured by Sogo Rikagaku Glass Co., Ltd., product name "tinplate ointment can"), and dried at 120°C for 4 hours using a circulating air dryer (manufactured by ADVANTECH Toyo Co., Ltd., product name "air supply constant temperature dryer DSR420DA") to obtain a heat-crosslinked solid resin. The mass of the solid resin was accurately measured at 25°C using a mass meter (manufactured by Sartorius Japan Co., Ltd., product name "standard balance CPA324S"). The solid resin to be measured was transferred to a container (300 mL beaker) filled with 150 mL of pure water, immersed in water at 25° C. for 3 hours under stirring conditions using a magnetic stirrer (manufactured by Tokyo Rikakii Co., Ltd., product name "Powerful Magnetic Stirrer RCX-1000D"), and then filtered under reduced pressure through filter paper (manufactured by Kiriyama Seisakusho Co., Ltd., "No. 50B") using a Kiriyama funnel (manufactured by Kiriyama Seisakusho Co., Ltd., product name "Kiriyama Funnel SB-60") and a suction bell (manufactured by Kiriyama Seisakusho Co., Ltd., product name "Suction Bell VKB-200") Then, the insoluble residue remaining on the filter paper was dried at 120° C. for 3 hours using the above-mentioned circulating air dryer, and the mass of the insoluble residue was accurately measured at 25° C. using the above-mentioned mass meter, and the gel fraction of the resin after thermal crosslinking of the water-soluble battery binder was calculated by the following formula.

[0245] Gel fraction (%) = {insoluble residue (g) / mass of solid resin (g)} × 100

[0246] Curl Evaluation

[0247] Curl was evaluated as follows.

[0248] The two adjacent sides of the aluminum foil cut into 50mm×50mm were fixed on the glass plate with tape, and the adhesive aqueous solution was evenly applied on the surface of the aluminum foil with a thickness of 400μm by the scraper method (ドクターブレード method), and dried for 5 minutes in a 120℃ circulating air dryer (manufactured by ADVANTEC, product name "DRS420DA"). After taking it out of the dryer and letting it stand for 2 minutes, the height of the corner not fixed by the tape and the glass surface was measured. The greater the height, the greater the curl. The curl of the adhesive film is related to the curl when the electrode is made. The greater the curl of the adhesive film, the greater the curl when the electrode is made, and there is a possibility of causing problems such as peeling during the electrode manufacturing process.

[0249] Based on the numerical value of the height, the evaluation was performed as follows.

[0250] A: Less than 10mm

[0251] B: 10mm or more and less than 20mm

[0252] C: 20mm or more

[0253] [Table 1]

[0254]

[0255] ·HEVE: Hydroxyethyl Vinyl Ether

[0256] ·DEGV: Diethylene glycol monovinyl ether

[0257] AM: Acrylamide (manufactured by Mitsubishi Chemical Co., Ltd., “50% Acrylamide”)

[0258] DMAA: N,N-dimethyl(meth)acrylamide (manufactured by KJ Chemikals Co., Ltd., “DMAA”)

[0259] AA: Acrylic acid (manufactured by Osaka Organic Chemical Industry Co., Ltd., "80% acrylic acid")

[0260] ·AN: Acrylonitrile (manufactured by Mitsubishi Micron Co., Ltd., "Acrylonitrile")

[0261] HEA: 2-Hydroxyethyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., “HEA”)

[0262] SMAS: Sodium methallyl sulfonate

[0263] ·NaOH: Sodium hydroxide (manufactured by Kanto Chemical Co., Ltd., “48% sodium hydroxide solution”)

[0264] 2. Manufacture of electrode slurry and battery production and evaluation

[0265] Example 1-1: Electrode Evaluation

[0266] <Manufacture of Electrode Paste

[0267] Using a commercially available planetary mixer (product name "Awatori Rentaro", manufactured by Shinchi Co., Ltd.), in a container dedicated to this mixer, 3 parts by mass of the aqueous solution obtained in Production Example 1, 91 parts of lithium cobaltate LCO (LiCoO2, manufactured by Nippon Chemical Industry Co., Ltd., product name "Cellseed C-5H") as the electrode active material, and 6 parts of acetylene black were mixed. Ion-exchanged water was added thereto to make the solid component concentration 50%, and the container was set in the above-mentioned mixer. Then, after kneading at 2000 rpm for 10 minutes, defoaming was carried out for 1 minute to obtain an electrode paste.

[0268] <Manufacture of Electrode

[0269] On the surface of a current collector made of aluminum foil, the above-mentioned lithium-ion battery electrode paste was uniformly coated by a doctor blade method so that the dried film thickness was 100 μm, dried at 60 °C for 30 minutes, and then heat-treated at 150 °C / vacuum for 120 minutes. Then, pressing was carried out using a roll press so that the density of the film (electrode active material layer) was 3.0 g / cm 3 , thereby obtaining an electrode.

[0270] <Assembly of Lithium Half-Cell

[0271] Inside a glove box purged with argon, the material obtained by punching the above-mentioned electrode into a diameter of 16 mm was loaded inside a gasket on the Al lower cover of a test cell (manufactured by Nippon Tomcell Co., Ltd.). Next, a separator formed of a polypropylene porous film punched into a diameter of 24 mm (manufactured by CS TECH CO., LTD., product name "SelionP2010") was loaded, and further 500 μL of electrolyte was injected so that air could not enter, and then a material obtained by punching a commercially available metallic lithium foil into 16 mm was loaded, and the outer package of the aforementioned test cell was sealed with screws, thereby assembling a lithium half-cell. The electrolyte used here is a solution in which LiPF6 is dissolved at a concentration of 1 mol / L in a solvent of ethylene carbonate / ethyl methyl carbonate = 1 / 1 (mass ratio).

[0272] Example 1-2 to Example 1-8, Comparative Example 1-1 to Comparative Example 1-5

[0273] Except that the composition in the above Example 1-1 was changed as shown in Table 2, a lithium half-cell was obtained in the same manner as in Example 1-1.

[0274] Example 2-1: Electrode Evaluation

[0275] <Manufacture of Electrode Paste>

[0276] Using a commercially available planetary mixer (product name "Awatori Ren Tarou", manufactured by Shinchi Co., Ltd.), in a container dedicated to this mixer, 5 parts by mass of the aqueous solution obtained in Production Example 1, 20 parts by mass of silicon monoxide particles with a D50 of 5 μm ("CC powder", manufactured by Osaka Titanium Technologies Co., Ltd.), and 80 parts by mass of natural graphite (manufactured by Ito Graphite Industry Co., Ltd., product name "Z-5F") were mixed. Ion-exchanged water was added thereto to make the solid content concentration 40%, and the container was placed in the above-mentioned mixer. Then, after kneading at 2000 rpm for 10 minutes, defoaming was carried out for 1 minute to obtain an electrode paste.

[0277] <Manufacture of Electrode>

[0278] On the surface of a current collector composed of a copper foil, the above-mentioned lithium-ion battery electrode paste was uniformly coated by the doctor blade method so that the dried film thickness was 80 μm, dried at 150 °C for 30 minutes, and then heat-treated at 150 °C / vacuum for 120 minutes. Then, rolling press processing was carried out to make the density of the film (electrode active material layer) 1.5 g / cm 3 , thereby obtaining an electrode.

[0279] <Assembly of Lithium Half-Cell>

[0280] A lithium half-cell was manufactured according to the same procedure as in Example 1-1.

[0281] Comparative Example 2-1

[0282] A lithium half-cell was obtained in the same manner as in Example 2-1, except that the composition in the above-mentioned Example 2-1 was changed as shown in Table 2.

[0283] <Storage Stability Test of Electrode Paste>

[0284] After measuring the viscosity (unit: mPa·s) of the electrode paste with a B-type viscometer, it was stored in an oven heated to 40 °C for 3 days. After storage, the viscosity was measured again with a B-type viscometer, and the viscosity change was calculated using the following formula and evaluated according to the following evaluation criteria.

[0285] Viscosity change (%) = (viscosity of the electrode paste after storage) / (viscosity of the electrode paste before storage) × 100

[0286] A: Less than 110%

[0287] B: 110% or more and less than 120%

[0288] C: 120% or more and less than 130%

[0289] D: Above 130%

[0290] <Electrode flexibility evaluation>

[0291] Cut the electrode into a width of 10 mm × a length of 70 mm, and wind it around a Teflon (registered trademark) rod with a diameter with the active material layer on the outside, observe the surface condition of the active material layer, and evaluate it according to the following criteria. of the Teflon (registered trademark) rod, observe the surface condition of the active material layer, and evaluate it according to the following criteria.

[0292] A: There are no cracks and peeling in the active material layer bonded to the current collector.

[0293] B: Cracks are found in the active material layer bonded to the current collector, but no peeling is found.

[0294] C: Cracks and peeling are found in the active material layer bonded to the current collector.

[0295] <Electrode adhesion evaluation>

[0296] Evaluate the electrode adhesion as follows.

[0297] Cut out a test piece with a width of 2 cm × a length of 10 cm from the electrode and fix it with the coating surface facing up. Then, press and paste a 15-mm-wide adhesive tape ("Cellotape" (registered trademark), manufactured by Nichiban Co., Ltd.) (specified in JIS Z1522) on the surface of the active material layer of this test piece, and then use a tensile testing machine (manufactured by A&D Co., Ltd., "TENSILON RTM-100") at 25 °C to measure the stress when peeling this adhesive tape from one end of the test piece at a speed of 30 mm / minute in the 180° direction. The measurement is carried out 5 times, converted into a value per 15-mm width, and the average value is calculated as the peel strength. The greater the peel strength, the higher the adhesion strength between the current collector and the active material layer or the adhesion between the active materials, indicating that the active material layer is difficult to peel from the current collector or the active materials are difficult to peel from each other.

[0298] Based on the value of the peel strength, evaluate as follows.

[0299] A: The peel strength is greater than 5 N / m.

[0300] B: The peel strength is 1 N / m to 5 N / m.

[0301] C: The peel strength is less than 1 N / m.

[0302] <Charge and discharge measurement>

[0303] The lithium half-cell was placed in a thermostatic chamber at 25°C, and charging was started at a constant current (0.1C), and charging was completed (cut off) when the voltage reached 5.0 V. Next, discharging was started at a constant current (0.1C), and discharging was completed (cut off) when the voltage reached 3.0 V. This charging and discharging cycle was repeated 30 times.

[0304] In addition, under the above measurement conditions, "1C" means the current value at which a battery with a certain capacitance is discharged at a constant current within 1 hour. For example, "0.1C" means the current value at which the discharge is completed after 10 hours, and "10C" means the current value at which the discharge is completed after 0.1 hours.

[0305] Example 2-1, Comparative Example 2-1

[0306] <Charge and discharge measurement>

[0307] The lithium half-cell was placed in a thermostatic chamber at 25°C, and charging was started at a constant current (0.1C), and charging was completed (cut off) when the voltage reached 0.01 V. Next, discharging was started at a constant current (0.1C), and discharging was completed (cut off) when the voltage reached 1.0 V. This charging and discharging cycle was repeated 30 times.

[0308] <First Coulombic Efficiency Measurement>

[0309] The first coulombic efficiency was calculated from the first charge capacity (mAh) and the first discharge capacity (mAh) in the charge-discharge cycle test at room temperature (25° C.) using the following formula.

[0310] First coulombic efficiency = {(first discharge capacity) / (first charge capacity)}×100

[0311] <Measurement of Rebound Rate>

[0312] After 30 cycles of charge and discharge cycle testing at room temperature (25° C.), the lithium half cell was disassembled and the thickness of the electrode was measured. The springback rate of the electrode was calculated by the following formula.

[0313] Resilience = {(electrode thickness after 30 cycles - collector thickness) / (electrode thickness before charge and discharge - collector thickness)}×100-100(%)

[0314] <Discharge Capacity Retention Rate>

[0315] The discharge capacity retention rate was calculated by the following formula.

[0316] Discharge capacity retention rate = {(discharge capacity at the 30th cycle) / (discharge capacity at the 1st cycle)}×100 (%)

[0317] [Table 2]

[0318]

[0319] LCO: Lithium cobalt oxide (LiCoO2)

[0320] NMC: Lithium Nickel Manganese Cobalt Oxide (Li[Ni 1 / 3 Mn 1 / 3 Co 1 / 3 ]O2)

Claims

1. An aqueous solution of a binder for lithium ion battery electrodes, the aqueous solution of the binder for lithium ion battery electrodes containing a water-soluble polymer (A), the water-soluble polymer (A) being a polymer of a monomer group, the monomer group containing 5 mol% to 80 mol% of a hydroxyl-containing vinyl ether (a) and 20 mol% to 95 mol% of a (meth)acrylamide-containing compound (b) relative to 100 mol% of the monomer group, wherein the (meth)acrylamide-containing compound (b) is (meth)acrylamide and / or N,N-dimethyl (meth)acrylamide.

2. The binder aqueous solution for lithium ion battery electrodes according to claim 1, in, The monomer group contains 0.01 mol % to 50 mol % of an unsaturated organic acid or an inorganic salt thereof (c).

3. A slurry for lithium ion battery electrodes comprising the binder aqueous solution for lithium ion battery electrodes according to claim 1 or 2 and an electrode active material (B).

4. A lithium ion battery electrode obtained by applying the slurry for lithium ion battery electrodes according to claim 3 onto a current collector and drying and solidifying the slurry.

5. A lithium ion battery comprising the lithium ion battery electrode according to claim 4.

Citation Information

Patent Citations

  • Electrode material for lithium secondary battery, electrode structural body with the electrode material, secondary battery with the electrode structure, manufacturing method of the electrode material, manufacturing method of the electrode structural body, and manufacturing method of the secondary battery

    JP2004185810A

  • Anode active material and cathode active material for lithium secondary battery, and lithium secondary battery

    JP2005259697A

  • Binder for lithium ion battery electrode, paste for lithium ion battery negative electrode using the same and manufacturing method of lithium ion battery negative electrode

    JP2013089437A

  • Slurry for electricity storage device negative electrode and electricity storage device negative electrode, slurry for electricity storage device positive electrode and electricity storage device positive electrode, and electricity storage device

    JP2015106488A

  • Binder composition for electricity storage device, slurry for electricity storage device, electricity storage device electrode, separator, and electricity storage device

    JP2015118908A