Cationic dye-dyed napped artificial leather and method for producing the same

By using a combination technology of 0.07 to 0.9 dtex cationic dye-dyeable polyester fiber and anionic surfactant, the problem of fiber strength reduction and color transfer after cationic dye dyeing is solved, and the firmness and color of ultra-fine fibers are achieved. Stability, achieving high mechanical strength and dark color that is not easy to transfer.

CN112538764BActive Publication Date: 2024-10-08KURARAY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011497420.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2015-03-17
Filing Date
2016-03-17
Publication Date
2024-10-08
Estimated Expiration
2036-03-17

AI Technical Summary

Technical Problem

The polyester fiber that can be dyed with cationic dyes will reduce the fiber strength during the dyeing process, the very fine fibers will easily fall off, and the dyed nappy artificial leather will easily transfer color to other items.

Method used

Non-woven fabrics are made of polyester fibers with cationic dyeability of 0.07 to 0.9 dtex, and anionic surfactants are used in the dyeing and cleaning processes. Hot water bath cleaning at 50 to 100°C, combined with fluffing treatment, ensures Fiber firmness and color stability.

Benefits of technology

It effectively inhibits the shedding and color transfer of ultra-fine fibers, improves the tear strength and peel strength of napped artificial leather, and ensures that the dyed material is not prone to color transfer when it comes into contact with other items, achieving a color transfer evaluation of level 4 or above.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0002842614660000022
    Figure BDA0002842614660000022
  • Figure BDA0002842614660000032
    Figure BDA0002842614660000032
Patent Text Reader

Abstract

The present invention provides a napped artificial leather dyed with a cationic dye, comprising a nonwoven fabric of a polyester fiber dyeable with a cationic dye having a fineness of 0.07 to 0.9 dtex, and a polymer elastic body imparted to the inside of the nonwoven fabric, wherein the napped artificial leather has an L* value of ≤50, a color difference level of 4 or more in a color transferability evaluation of PVC under a load of 0.75 kg / cm, 50° C., and 16 hours, a tear strength of 30 N or more per 1 mm thickness, and a peel strength of 3 kg / cm or more.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present application is a divisional application of an application with application number 201680013899.8, filed on March 17, 2016, and invention name “Napped artificial leather dyed with cationic dyes and method for producing the same”. Technical Field

[0002] The present invention relates to napped artificial leather dyed with cationic dyes. Background Art

[0003] Currently, there are known napped artificial leathers with dense velvety texture, such as suede-like artificial leather and nubuck-like artificial leather. The napped artificial leather has been used as a surface material for clothing, shoes, furniture, car seats, sundry products, etc., and as a surface material for mobile phones, mobile devices, and housings of home appliances, etc. Such napped artificial leather is usually dyed before use.

[0004] The napped artificial leather is obtained by raising the surface of an artificial leather substrate obtained by containing a high molecular weight elastic body such as polyurethane inside an ultrafine fiber nonwoven fabric. As an ultrafine fiber nonwoven fabric, it is preferred to use a napped artificial leather using an entangled body of polyester ultrafine fibers from the viewpoint of excellent balance between mechanical properties and hand feel.

[0005] Conventionally, disperse dyes have been widely used to dye napped artificial leathers made of nonwoven fabrics containing ultrafine polyester fibers, due to their excellent color development. However, disperse dyes have the problem of easily transferring color to other objects in contact with them due to heat and pressure.

[0006] In order to solve such problems, dyeing with cationic dyes has been attempted. For example, the following patent document 1 discloses a cationic dye-dyable leather sample, which is formed of a polyurethane and a fiber structure, wherein the polyurethane is obtained by reacting an intermediate diol (D) having an OH terminal, a low molecular diol (E), and diphenylmethane-4,4'-diisocyanate (C2), wherein the intermediate diol (D) having an OH terminal is obtained by reacting a sulfo-containing diol (A) obtained by substantially replacing the acid component of sulfoisophthalic acid with a specific diol, a polymer diol (B) having a number average molecular weight of 500 to 3000 selected from polyesters, polycarbonates, polycaprolactones, and polyethers, and an organic diisocyanate (C1).

[0007] In addition, for example, the following patent document 2 is a technology related to synthetic leather, which discloses a synthetic leather obtained by forming a resin layer on the surface of a double-layer Raschel warp knitted fabric; the double-layer Raschel warp knitted fabric of the synthetic leather is composed of a surface knitted fabric, a back knitted fabric and a loop layer connecting them, the fiber constituting the surface knitted fabric is a polyester fiber dyed with a cationic dye, and the resin layer is formed on the surface knitted fabric side. Patent document 2 discloses a synthetic leather, as a polyester fiber, comprising a polyester formed of a dicarboxylic acid component with terephthalic acid as the main component and a diol component with ethylene glycol as the main component, wherein the dicarboxylic acid component contains the following formula (III) [wherein X represents a metal ion, a quaternary ions or quaternary ammonium ions].

[0008] [Chemical formula 1]

[0009]

[0010] In addition, for example, Patent Document 3 below discloses a deodorizing fabric dyed with a cationic dye, which is a deodorizing fabric obtained by subjecting the deodorizing fabric to a deodorizing treatment, wherein as a copolymer component, the copolyester fiber a contains a metal salt (A) of sulfoisophthalic acid and a quaternary salt of sulfoisophthalic acid. Salt or quaternary ammonium salt (B) such that 3.0≤A+B≤5.0 (mol %), 0.2≤B / (A+B)≤0.7.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Laid-Open No. 6-192968

[0014] Patent Document 2: Japanese Patent Application Publication No. 2014-29050

[0015] Patent Document 3: Japanese Patent Application Publication No. 2010-242240 Summary of the invention

[0016] Problems to be solved by the invention

[0017] The polyester fiber dyeable with cationic dyes has a copolymerization unit as a dyeing site for dyeing with cationic dyes, which reduces the strength of the fiber. Therefore, when manufacturing napped artificial leather containing such fibers, there is a problem that the ultrafine fibers are easily detached when the surface is rubbed. In addition, for napped artificial leather containing nonwoven fabric of polyester ultrafine fibers dyed with cationic dyes to a darker color, there is also a problem that the color is easily transferred to other objects in contact.

[0018] The present invention aims to provide a napped artificial leather and a stable manufacturing method thereof, wherein the napped artificial leather can suppress the shedding of ultrafine fibers forming the napped leather in the napped artificial leather dyed with a cationic dye and the color is not easily transferred to other contacting articles.

[0019] Methods for solving problems

[0020] One aspect of the present invention is a napped artificial leather dyed with a cationic dye, comprising a non-woven fabric of cationic dye-dyeable polyester fibers having a fineness of 0.07 to 0.9 dtex, and a polymer elastomer imparted to the interior of the non-woven fabric, wherein the napped artificial leather has an L* value of ≤50, and in a color transferability evaluation of PVC under a load of 0.75 kg / cm, 50°C, and 16 hours, the color difference level is judged to be 4 or above, the tear strength per 1 mm thickness is 30 N or above, and the peel strength is 3 kg / cm or above.

[0021] In addition, another aspect of the present invention is a method for producing a napped artificial leather dyed with a cationic dye, the method comprising: a step of preparing an artificial leather substrate, the artificial leather substrate comprising a nonwoven fabric of ultrafine fibers of a cationic dye-dyeable polyester of 0.07 to 0.9 dtex and a polymer elastomer impregnated into the nonwoven fabric; a step of dyeing the artificial leather substrate with a cationic dye and then washing it in a hot water bath of 50 to 100° C. containing an anionic surfactant; and a step of raising at least one side of the artificial leather substrate before or after the dyeing and washing steps, wherein the cationic dye-dyeable polyester comprises a polyester containing a dicarboxylic acid unit having a terephthalic acid unit as a main component and a diol unit having an ethylene glycol unit as a main component, and as the dicarboxylic acid unit, 1.5 to 3 mol % of the following formula (I b ) represented by the unit [Formula (I b ), X represents the season ions or quaternary ammonium ions].

[0022] [Chemical formula 2]

[0023]

[0024] Effects of the Invention

[0025] According to the present invention, it is possible to obtain a napped artificial leather dyed with a cationic dye in which ultrafine fibers are unlikely to fall off and whose color is unlikely to transfer to other articles in contact. DETAILED DESCRIPTION

[0026] An embodiment of the napped artificial leather dyed with a cationic dye of the present invention will be described in detail according to an example of its production method.

[0027] In the method for producing napped artificial leather of the present embodiment, first, an artificial leather substrate is prepared, the artificial leather substrate comprising an entangled body of ultrafine fibers including 0.07 to 0.9 dtex cationic dye-dyeable polyester ultrafine fibers and a polymer elastic body impregnated with the entangled body of ultrafine fibers.

[0028] As a specific example of the method for producing the artificial leather substrate, for example, the following method can be mentioned.

[0029] First, an entangled body of ultrafine fiber-forming fibers capable of forming dyeable polyester ultrafine fibers of 0.07 to 0.9 dtex is produced.

[0030] In the manufacture of an entangled body of ultrafine fiber-generating fibers, a fiber web of ultrafine fiber-generating fibers is first manufactured. As a method for manufacturing a fiber web, for example, a method of melt-spinning ultrafine fiber-generating fibers and directly capturing them in the state of long fibers without intentionally cutting them, and a method of implementing a known entanglement treatment after cutting them into short fibers. It should be noted that long fibers refer to fibers that are not short fibers and have not been cut at a given length. As for their length, from the perspective of being able to fully improve the fiber density, for example, they are preferably 100 mm or more, and more preferably 200 mm or more. The upper limit of the long fibers is not particularly limited, and can be a fiber length of several meters, hundreds of meters, several kilometers or more obtained by continuous spinning. Among them, from the perspective of not being easy to produce fiber disintegration, so that the ultrafine fibers are not easy to fall off, and a napped artificial leather with excellent mechanical properties can be obtained, it is particularly preferred to manufacture a long fiber web. In this embodiment, as a representative example, the situation of manufacturing a long fiber web is described in detail.

[0031] It should be noted that the ultrafine fiber generating type fiber refers to a fiber that forms an ultrafine fiber with a small fineness by subjecting the spun fiber to a chemical post-treatment or a physical post-treatment. As specific examples thereof, for example: in the fiber cross section, a polymer of an island component as a micro-region of a different type from the sea component is dispersed in a polymer of a sea component as a matrix, and then the sea component is removed to form an island-type composite fiber of a fiber bundle of ultrafine fibers with the polymer of the island component as the main body; a plurality of different resin components are alternately arranged on the periphery of the fiber to form a petal shape and an overlapping shape, and each resin component is peeled off by a physical treatment, thereby splitting to form a stripping and splitting composite fiber of a bundle of ultrafine fibers, etc. According to the island-type composite fiber, when performing an entanglement treatment such as a needle punching treatment described later, fiber damage such as breakage, bending, and cutting can be suppressed. In this embodiment, as a representative example, the case of using an island-type composite fiber to form an ultrafine fiber is described in detail.

[0032] The sea-island composite fiber is a multi-component composite fiber formed of at least two polymers, and has a cross section formed by dispersing the island component polymer in a matrix formed of the sea component polymer. The long fiber web of the sea-island composite fiber is formed by melt-spinning the sea-island composite fiber and directly capturing it on the web in the form of long fibers without cutting it.

[0033] In this embodiment, as the island component polymer, it is preferred to use a dyeable polyester obtained by copolymerizing a dicarboxylic acid component and a diol component, wherein the dicarboxylic acid component contains 1.5 to 3 mol % of a component represented by the following formula (II) and has terephthalic acid as a main component, and the diol component has ethylene glycol as a main component.

[0034] [Chemical formula 3]

[0035]

[0036] [In the above formula (II), R represents hydrogen, an alkyl group having 1 to 10 carbon atoms or a 2-hydroxyethyl group, and X represents a quaternary ions or quaternary ammonium ions.]

[0037] Examples of the compound represented by formula (II) include tetrabutyl isophthalate-5-sulfonate 5-Sulfonic acid ethyl tributyl isophthalate Tetraalkyl 5-sulfonate isophthalic acid Tetraalkylammonium 5-sulfonate isophthalic acid, such as tetrabutylammonium 5-sulfonate isophthalic acid and ethyltributylammonium 5-sulfonate isophthalic acid. The compound represented by formula (II) can be used alone or in combination of two or more. By copolymerizing a dicarboxylic acid component preferably containing 1.5 to 3 mol% of the compound represented by formula (II) and having terephthalic acid as the main component with a diol component having ethylene glycol as the main component, a dyeable polyester having excellent dyeability, mechanical properties and high-speed spinning properties brought by cationic dyes can be obtained.

[0038] The proportion of the unit represented by formula (I) derived from formula (II) in the dyeable polyester is preferably 1.5 to 3 mol%, and more preferably 1.6 to 2.5 mol%. When the proportion of the unit represented by formula (I) is less than 1.5 mol%, there is a tendency that the color development when dyed with a cationic dye is reduced. On the other hand, when the proportion of the unit represented by formula (I) exceeds 3 mol%, there is a tendency that it is difficult to obtain ultrafine fibers due to reduced high-speed spinning properties, and the mechanical properties such as the tear strength of the obtained napped artificial leather are significantly reduced.

[0039] Here, terephthalic acid as the main component means that more than 50 mol% of the dicarboxylic acid component is a terephthalic acid component. The content ratio of the terephthalic acid component in the dicarboxylic acid component is preferably more than 75 mol%. In addition, in order to improve the dyeability brought by cationic dyes, improve high-speed spinning properties, and improve the excipient properties when the napped artificial leather is used for molding purposes, in order to reduce the glass transition temperature, as a dicarboxylic acid component, in addition to the components shown in formula (II), other dicarboxylic acid components may also be contained. As specific examples of other dicarboxylic acid components, for example, other dicarboxylic acid components such as aromatic dicarboxylic acids such as isophthalic acid, cyclohexane dicarboxylic acid components such as 1,4-cyclohexane dicarboxylic acid, and aliphatic dicarboxylic acid components such as adipic acid may be contained. Among them, from the viewpoint of excellent mechanical properties and high-speed spinning properties, it is particularly preferred to contain isophthalic acid or a combination of 1,4-cyclohexane dicarboxylic acid and adipic acid.

[0040] As a dicarboxylic acid component, the copolymerization ratio of other dicarboxylic acid components is preferably 2 to 12 mol%, and more preferably 3 to 10 mol%. When the copolymerization ratio of other dicarboxylic acid components is less than 2 mol%, the glass transition temperature is not sufficiently reduced, and there is a tendency to reduce dyeability due to the increased orientation of the amorphous part inside the fiber. On the other hand, when the copolymerization ratio of other dicarboxylic acid components exceeds 12 mol%, the glass transition temperature is excessively reduced, and there is a tendency to reduce fiber strength due to the reduced orientation of the amorphous part inside the fiber. It should be noted that, in the case of containing isophthalic acid as other dicarboxylic acid units, from the viewpoint of excellent mechanical properties and high-speed spinning properties, as a dicarboxylic acid unit, it is preferred to contain 1 to 6 mol% of isophthalic acid, and more preferably 2 to 5 mol%. In addition, in the case of containing 1,4-cyclohexanedicarboxylic acid and adipic acid, from the viewpoint of excellent mechanical properties and high-speed spinning properties, it is preferred to contain 1 to 6 mol% of 1,4-cyclohexanedicarboxylic acid and adipic acid, respectively, and more preferably 2 to 5 mol%.

[0041] It should be noted that, as other dicarboxylic acid components, alkali metal salt units such as sodium salt of sulfoisophthalic acid may be contained. However, when the proportion of alkali metal salt units of sulfoisophthalic acid is too high, there is a tendency that high-speed spinning properties are reduced and mechanical properties such as tear strength of the obtained artificial leather substrate are significantly reduced. Therefore, when alkali metal salt units such as sodium salt of sulfoisophthalic acid are contained, it is preferably contained in an amount of 0 to 0.2 mol% as dicarboxylic acid units, and more preferably not contained.

[0042] In addition, the term "ethylene glycol as the main component" means that 50 mol% or more of the glycol component is the ethylene glycol component. The content of the ethylene glycol component in the glycol component is preferably 75 mol% or more, and more preferably 90 mol% or more. In addition, other components include, for example, diethylene glycol, polyethylene glycol, etc.

[0043] The glass transition temperature (Tg) of the dyeable polyester is not particularly limited, but is preferably 60 to 70° C., more preferably 60 to 65° C. When Tg is too high, high-speed stretchability decreases, and when the obtained napped artificial leather is used by thermoforming, shapeability tends to decrease.

[0044] Furthermore, the dyeable polyester may be blended with a colorant such as carbon black, a weathering agent, a mildewproofing agent, etc. as necessary within a range not impairing the effects of the present invention.

[0045] In addition, from the perspective of high-speed spinning properties, the physical properties of the resulting napped artificial leather, and excellent shapeability when used by thermoforming, the melt viscosity of the dyeable polyester at a shear rate of 1220 (1 / s) at 270°C is preferably 80 to 220 Pa / s.

[0046] As the sea component polymer, a polymer having higher solubility in solvent or decomposition by decomposing agent than the dyeable polyester can be selected. In addition, from the viewpoint of excellent spinning stability of the sea-island type composite fiber, a polymer having low affinity with the dyeable polyester and lower melt viscosity and / or surface tension than the island component polymer under spinning conditions is preferred. Specific examples of sea component polymers that meet such conditions include: water-soluble polyvinyl alcohol resins (water-soluble PVA), polyethylene, polypropylene, polystyrene, ethylene-propylene copolymers, ethylene-vinyl acetate copolymers, styrene-ethylene copolymers, styrene-acrylic acid copolymers, etc. Among them, since it can be dissolved and removed by aqueous solvents without using organic solvents, water-soluble PVA is preferred from the viewpoint of low environmental burden.

[0047] The sea-island type composite fiber can be produced by melt spinning by melt-extruding the sea component polymer and the dyeable polyester as the island component polymer from a composite spinning nozzle. The nozzle temperature of the composite spinning nozzle is not particularly limited as long as it is a temperature higher than the melting point of each polymer constituting the sea-island type composite fiber and can be melt-spinned, and is usually selected in the range of 180 to 350°C.

[0048] The fineness of the sea-island type composite fiber is not particularly limited, but is preferably 0.5 to 10 dtex, and more preferably 0.7 to 5 dtex. In addition, the average area ratio of the sea component polymer to the island component polymer in the cross section of the sea-island type composite fiber is preferably 5 / 95 to 70 / 30, and more preferably 10 / 90 to 50 / 50. In addition, the number of micro-domains of the island component in the cross section of the sea-island type composite fiber is not particularly limited, but is preferably 5 to 1000, and more preferably about 10 to 300, from the viewpoint of industrial productivity.

[0049] The molten island-type composite fibers ejected from the nozzle are cooled by a cooling device, and then pulled and thinned by a suction device such as a jet nozzle to achieve the target fineness. Specifically, the pulling and thinning is performed using a high-speed airflow, preferably to a high spinning speed equivalent to a pulling speed of 1000 to 6000 m / min, and more preferably to a high spinning speed equivalent to a pulling speed of 2000 to 5000 m / min. Then, a long fiber web can be obtained by accumulating the pulled and thinned long fibers on a collecting surface such as a movable net. It should be noted that, as needed, in order to stabilize the shape, the long fiber web can be partially crimped by further pressing the long fiber web. The unit area weight of the long fiber web thus obtained is not particularly limited, and is preferably 10 to 1000 g / m 2 range.

[0050] Then, the obtained long-fiber web is subjected to an entanglement treatment to produce an entangled web.

[0051] As a specific example of the entanglement treatment of the long fiber web, for example, a plurality of long fiber webs are stacked in the thickness direction using a stacking device, and then needle punched under the condition that at least one hook is penetrated from both sides simultaneously or alternately.

[0052] In addition, for the long fiber web, oil and antistatic agent can be added in any stage from the spinning process of the island-in-sea composite fiber to the entanglement treatment. Moreover, as needed, the entanglement state of the long fiber web can be made dense in advance by performing a shrinkage treatment by immersing the long fiber web in warm water at about 70 to 150°C. In addition, by performing a hot pressing treatment after acupuncture, the fiber density can be further made dense and the shape can be given stability. The unit area weight of the entangled web obtained in this way is preferably 100 to 2000 g / m 2 The range of left and right.

[0053] In addition, the fiber density and degree of entanglement can be increased by subjecting the entangled web to heat shrinkage as required. Specific examples of heat shrinkage include a method of contacting the entangled web with water vapor, a method of applying water to the entangled web and then heating the water applied to the entangled web by heated air, infrared or other electromagnetic waves. In addition, in order to further densify the entangled web densified by the heat shrinkage treatment, fix the morphology of the entangled web, smoothen the surface, etc., the fiber density can be further increased by performing a heat press treatment as required.

[0054] The change in the weight per unit area of ​​the entangled web in the heat shrinking treatment step is preferably 1.1 times (mass ratio) or more, more preferably 1.3 times or more, preferably 2 times or less, and more preferably 1.6 times or less, compared to the weight per unit area before the shrinking treatment. It should be noted that the entangled state affects the mechanical properties of the obtained napped artificial leather. In this embodiment, it is preferred that the napped artificial leather after cationic dyeing is densely entangled to a degree that the tear strength per 1 mm thickness is 30 N or more and the peel strength is 3 kg / cm or more.

[0055] Then, by removing the sea component polymer from the island-in-sea type composite fibers in the entangled web obtained by densification, an ultrafine long fiber nonwoven fabric which is an entangled body of ultrafine long fibers in the form of fiber bundles of dyeable polyester can be obtained. As a method for removing the sea component polymer from the island-in-sea type composite fibers, a conventionally known ultrafine fiber forming method in which the entangled web is treated with a solvent or a decomposing agent that can selectively remove only the sea component polymer can be used without particular limitation. Specifically, for example, when water-soluble PVA is used as the sea component polymer, hot water can be used as the solvent, and when a modified polyester that is easily decomposed by alkali is used as the sea component polymer, an alkaline decomposing agent such as an aqueous sodium hydroxide solution can be used.

[0056] When water-soluble PVA is used as the sea component polymer, it is preferably extracted and removed by treating it in hot water at 85 to 100° C. for 100 to 600 seconds, so that the removal rate of the water-soluble PVA is about 95 to 100% by mass. It should be noted that the water-soluble PVA can be effectively extracted and removed by repeatedly implementing the immersion clamping treatment. When water-soluble PVA is used, since the sea component polymer can be selectively removed without using an organic solvent, water-soluble PVA is preferred from the viewpoint of low environmental burden and suppression of VOC generation.

[0057] The fineness of the ultrafine fibers formed as described above is 0.07 to 0.9 dtex, preferably 0.07 to 0.3 dtex.

[0058] The nonwoven fabric of the ultrafine long fibers thus obtained preferably has a weight per unit area of ​​140 to 3000 g / m 2 , more preferably 200 to 2000 g / m 2 In addition, from the viewpoint of obtaining a nonwoven fabric having excellent mechanical strength and a full feeling by forming a dense nonwoven fabric, the apparent density of the nonwoven fabric of ultrafine long fibers is preferably 0.45 g / cm 3 More preferably, 0.55 g / cm 3 The upper limit is not particularly limited, but is preferably 0.70 g / cm from the viewpoint of obtaining a smooth feel and excellent productivity.3 the following.

[0059] In the manufacture of the napped artificial leather of the present embodiment, either or both before or after ultrafine fiber-generating fibers such as sea-island type composite fibers are ultrafinely fiberized, in order to impart morphological stability and a sense of fullness to the nonwoven fabric, a polymer elastomer such as a polyurethane elastomer is impregnated into the internal voids of the nonwoven fabric.

[0060] Specific examples of the polymer elastomer include polyurethane, acrylonitrile elastomer, olefin elastomer, polyester elastomer, polyamide elastomer, acrylic elastomer, etc. Among them, polyurethane is preferred, and water-based polyurethane is particularly preferred.

[0061] Aqueous polyurethane refers to a polyurethane obtained by solidifying a polyurethane emulsion or a polyurethane dispersion dispersed in an aqueous solvent. It is generally poorly soluble in organic solvents and forms a cross-linked structure after solidification. In addition, when the polyurethane emulsion has thermosensitive gelation, the emulsion particles undergo thermosensitive gelation without migration, so that the polymer elastic body can be uniformly provided to the fiber entanglement body.

[0062] As a method for impregnating a nonwoven fabric with a high molecular weight elastic body, there can be cited a method of impregnating an emulsion, dispersion or solution containing a polyurethane elastomer into an entangled web before ultrafine fiberization or a nonwoven fabric after ultrafine fiberization, and then coagulating it by a dry method or a wet method, etc. It should be noted that when a high molecular weight elastic body that forms a cross-linked structure after coagulation, such as an aqueous polyurethane, is used, an aging treatment by heat treatment after coagulation and drying can be performed as needed to promote crosslinking.

[0063] Examples of the impregnation method of the emulsion, dispersion or solution of the polymer elastic body include a dip-nip method in which a pressing treatment is performed once or more with a pressure roller or the like to achieve a predetermined impregnation state, a rod coating method, a knife coating method, a roll coating method, a comma coating method, a spray coating method, and the like.

[0064] It should be noted that, within the scope of not impairing the effects of the present invention, the polymer elastomer may further contain pigments such as carbon black, colorants such as dyes, coagulation regulators, antioxidants, ultraviolet absorbers, fluorescent agents, mildew inhibitors, penetrants, defoamers, lubricants, waterproofing agents, oil-proofing agents, thickeners, extenders, curing accelerators, foaming agents, water-soluble polymer compounds such as polyvinyl alcohol and carboxymethyl cellulose, inorganic microparticles, conductive agents, etc.

[0065] From the viewpoint of achieving an excellent balance between the fullness and the softness of the obtained napped artificial leather, the content of the polymer elastic body is preferably 0.1 to 50% by mass, more preferably 0.1 to 40% by mass, particularly preferably 5 to 25% by mass, and particularly preferably 10 to 15% by mass relative to the total amount of the ultrafine fibers. When the content of the polymer elastic body is too high, the color of the dyed napped artificial leather tends to be easily transferred to other objects in contact.

[0066] In this way, an artificial leather substrate can be obtained, which is a non-woven fabric of 0.07-0.9 dtex ultrafine fibers impregnated with a high molecular weight elastic body. The artificial leather substrate thus obtained is sliced ​​into multiple pieces in a direction perpendicular to the thickness direction and ground to adjust the thickness as needed. Then, at least one side is further polished using sandpaper or emery paper preferably with a grit number of 120-600, more preferably about 320-600, thereby performing a raising treatment. In this way, a raised-hair artificial leather can be obtained, wherein the raised-hair artificial leather forms a raised-hair surface on one or both sides of the artificial leather substrate.

[0067] The thickness of the napped artificial leather is not particularly limited, but is preferably 0.2 to 4 mm, more preferably 0.5 to 2.5 mm.

[0068] The length of the napped fibers of the napped artificial leather is not particularly limited, but is preferably 1 to 500 μm, more preferably 30 to 200 μm, from the viewpoint of obtaining a napped artificial leather having a fine short-hair feel like natural nubuck leather.

[0069] The napped artificial leather of the present embodiment is dyed with a cationic dye. When dyeing with a cationic dye, the cationic dye is fixed to the following formula (I) by an ionic bond. a ) contains sulfonium ions, which are dyeing sites of dyeable polyester to cationic dyes, and thus can obtain excellent dyeing fastness. As the cationic dye, any currently known cationic dye can be used without particular limitation. It should be noted that the cationic dye dissolves in the dye solution to form dye ions such as quaternary ammonium groups that show cationicity, thereby ionically bonding with the fiber. Such cationic dyes usually form salts with anions such as chloride ions. Such anions such as chloride ions are contained in cationic dyes, but are rinsed out by washing after dyeing.

[0070] [Chemical formula 4]

[0071]

[0072] The dyeing method is not particularly limited, and examples thereof include dyeing methods using dyeing machines such as a liquid jet dyeing machine, a beam dyeing machine, and a jigger. As dyeing processing conditions, dyeing can be performed under high pressure, but since the ultrafine polyester fiber of the present embodiment can be dyed under normal pressure, it is preferred to dye under normal pressure from the viewpoint of low environmental burden and reduced dyeing cost. When dyeing is performed under normal pressure, the dyeing temperature is preferably 60 to 100° C., and more preferably 80 to 100° C. In addition, dyeing auxiliaries such as acetic acid and sodium sulfate can be used during dyeing.

[0073] In this embodiment, the napped artificial leather dyed with a cationic dye is cleaned in a hot water bath containing an anionic surfactant to remove the cationic dye with low bonding strength. By such a cleaning treatment, in particular, by fully removing the cationic dye absorbed by the polymer elastic body, the color transfer of the obtained dyed napped artificial leather can be fully suppressed. Specific examples of the anionic surfactant include SORUJIN R manufactured by Niksei Chemicals Co., Ltd., SENKANOL A-900 manufactured by SENKA, and Meisanol KHM manufactured by Meisei Chemical Industry Co., Ltd.

[0074] The washing treatment in the hot water bath containing anionic surfactant is preferably performed in a hot water bath at 50 to 100° C., more preferably in a hot water bath at 60 to 80° C. In addition, a dyeing machine that has been subjected to dyeing treatment is preferably used as the hot water bath tank from the viewpoint of simplifying the production process.

[0075] As the washing time, it is preferably the time when the cotton contamination of the water fastness specified in the JIS method (JIS L 0846) is judged to be above level 4-5, specifically, it is preferably 10 to 30 minutes, and more preferably about 15 to 20 minutes. In addition, the washing can be repeated more than once. The napped artificial leather thus dyed and washed is dried. It should be noted that, by using the above-mentioned washing method, the washable chlorine in the cationic dye is fully washed to about 90ppm or less relative to the weight of the dyed napped artificial leather, thereby the color transfer of the cationic dye can be fully suppressed.

[0076] The napped artificial leather may be subjected to various finishing treatments as required, such as kneading and softening treatment, reverse seal brushing treatment, antifouling treatment, hydrophilization treatment, lubricant treatment, softener treatment, antioxidant treatment, ultraviolet absorber treatment, fluorescent agent treatment, flame retardant treatment, etc.

[0077] In this way, the napped artificial leather dyed with the cationic dye of the present embodiment can be obtained. The napped artificial leather dyed with the present embodiment is not easily color-transferred to other objects even if it is a dark color such as L* value ≤ 50.

[0078] In addition, when the napped artificial leather dyed with a cationic dye contains ultrafine fibers derived from ultrafine fibers containing polyester, the ultrafine fibers having high mechanical strength as continuous long fibers produced without reducing the high-speed spinnability of the ultrafine fibers can be contained, wherein the polyester contains a dicarboxylic acid unit mainly composed of a terephthalic acid unit and a diol unit mainly composed of an ethylene glycol unit, and the dicarboxylic acid unit contains 1.5 to 3 mol% of a quaternary In addition, after dyeing the artificial leather substrate with a cationic dye, washing it in a hot water bath containing an anionic surfactant can fully wash the cationic dye from the polymer elastomer, thereby fully suppressing color transfer caused by the cationic dye remaining in the polymer elastomer.

[0079] Specifically, the napped artificial leather dyed with a cationic dye of the present embodiment comprises a nonwoven fabric of a polyester fiber dyeable with a cationic dye having a fineness of 0.07 to 0.9 dtex, and a high molecular weight elastic body applied to the inside of the nonwoven fabric, and the L* value of the napped artificial leather is ≤50, and the color difference level is preferably adjusted to 4 or more in the color transferability evaluation of PVC under a load of 0.75 kg / cm, 50° C., and 16 hours. By adjusting to have such characteristics, a napped artificial leather can be obtained in which the ultrafine fibers of the napped leather are not easy to fall off, and the color is not easy to transfer to other contacting articles even if it is dyed with a cationic dye to a darker color.

[0080] The napped artificial leather dyed with a cationic dye according to the present embodiment preferably has L * A darker hue with a value of ≤50, further preferably having L * A darker hue with a value of ≤35. It should be noted that for L * For a value of ≤35, not only dyeing but also color transfer can be easily achieved by including a pigment such as carbon black in a cationic dye-dyeable polyester fiber or a polymer elastomer. Even if such a napped artificial leather is dark in color, color transfer can be suppressed by using the cationic dye-dyeable polyester fiber as described above and washing it in a hot water bath containing an anionic surfactant. Specifically, a dyed napped artificial leather can be obtained in which the color difference level is judged to be 4 or more in the color transfer evaluation of PVC under a load of 0.75 kg / cm, 50°C, and 16 hours.

[0081] Furthermore, by adjusting the napped artificial leather dyed with a cationic dye of the present embodiment to have a high mechanical strength of 30 N or more per 1 mm thickness and a peel strength of 3 kg / cm or more, it is possible to suppress the falling of the ultrafine fibers.

[0082] From the viewpoint that the ultrafine fibers of the napped leather are not easy to fall off, the tear strength per 1 mm thickness of the napped artificial leather dyed with a cationic dye is preferably 30N or more, preferably 35N or more, and further preferably 40N or more, and the peel strength is 3kg / cm or more, preferably 3.5kg / cm or more, and especially 4kg / cm or more.

[0083] It should be noted that the ease with which the nap of the napped artificial leather is generated can be evaluated, for example, by Martindale abrasion loss. The napped artificial leather dyed with a cationic dye can be obtained, in which the ultrafine fibers are not easily detached when the surface is rubbed at a Martindale abrasion loss of 100 mg / 35,000 times or less, and further at a Martindale abrasion loss of 95 mg / 35,000 times or less.

[0084] Example

[0085] The present invention will be further described in detail below by way of examples. It should be noted that the scope of the present invention is not limited by the examples.

[0086] [Example 1]

[0087] The sea component thermoplastic resin of ethylene-modified polyvinyl alcohol (ethylene unit content 8.5 mol%, polymerization degree 380, saponification degree 98.7 mol%) and the island component thermoplastic resin of tetrabutyl sulfoisophthalic acid were used. Polyethylene terephthalate (PET) modified with sulfoisophthalic acid: (tetrabutyl Salt unit 1.7 mol%, 1,4-cyclohexane dicarboxylic acid unit 5 mol%, adipic acid unit 5 mol%; glass transition temperature 62°C) are melted separately. Then, each molten resin is supplied to a composite spinning nozzle, wherein the composite spinning nozzle is provided with a plurality of spinnerets in parallel, and a cross section of 25 island components with uniform cross-sectional areas distributed in the sea component can be formed. At this time, the pressure is adjusted so that the mass ratio of the sea component to the island component is sea component / island component=25 / 75 while supplying. Then, the molten fiber is ejected through the spinneret set to a nozzle temperature of 260°C.

[0088] Then, the molten fibers ejected from the spinneret were sucked and stretched by a jet nozzle-type suction device to spin sea-island type composite long fibers with a fineness of 2.1 dtex. The jet nozzle-type suction device adjusted the airflow pressure so that the average spinning speed was 3700 m / min. The spun sea-island type composite long fibers were continuously deposited on a movable net while being sucked from the back of the net. The deposited amount can be adjusted by adjusting the moving speed of the net. Then, in order to suppress the fuzzing on the surface, the sea-island type composite long fibers deposited on the net were lightly pressed with a 42°C metal roller. Then, the sea-island type composite long fibers were peeled off from the net and passed between a checkered metal roller with a surface temperature of 75°C and a back roller, thereby being hot pressed with a linear pressure of 200 N / mm. In this way, the surface fibers were pre-melted into a grid-like shape with a unit area weight of 34 g / m 2 Long fiber web.

[0089] Next, an oil solution mixed with an antistatic agent was sprayed on the surface of the obtained long fiber web, and then 10 long fiber webs were stacked using a stacking device to produce a total unit area weight of 340 g / m 2 The laminated web was sprayed with a needle-breaking prevention oil. The laminated web was then needle-punched to achieve a three-dimensional entanglement treatment. Specifically, a needle with six hooks and a distance of 3.2 mm from the needle tip to the first hook was used, and the needle depth was 8.3 mm, and the needles were punched alternately from both sides of the laminate at 3300 punctures / cm 2 The area shrinkage caused by the needle punching treatment was 18%, and the unit area weight of the entangled web after the needle punching was 415g / m 2 .

[0090] The obtained entangled web was densified by performing a wet heat shrinkage treatment as described below. Specifically, 10% by mass of water at 18°C ​​was uniformly sprayed on the entangled web, and the web was placed in a gas atmosphere at a temperature of 70°C and a relative humidity of 95% without applying tension for 3 minutes and heat-treated, thereby causing wet heat shrinkage to increase the apparent fiber density. The area shrinkage rate caused by the wet heat shrinkage treatment was 45%, and the unit area weight of the densified entangled web was 750 g / m 2 , the apparent density is 0.52g / cm 3 Then, in order to further densify the entangled web, dry heat roll pressing was performed to adjust the apparent density to 0.60 g / cm 3 .

[0091] Next, an emulsion of a water-based polyurethane that forms a cross-linked structure after solidification (an emulsion of polyurethane with a solid content concentration of 30% mainly composed of polycarbonate / ether-based polyurethane) was impregnated into the densified entangled web as a polyurethane elastomer, and then dried in a drying oven at 150°C.

[0092] Next, the entangled web to which the water-based polyurethane was applied was immersed in hot water at 95°C for 20 minutes to extract and remove the sea component contained in the island-in-sea composite long fibers, and dried in a drying furnace at 120°C to obtain an artificial leather substrate of a nonwoven fabric impregnated with water-based polyurethane and containing ultrafine long fibers with a fineness of 0.1 dtex. The mass ratio of the nonwoven fabric / water-based polyurethane of the obtained artificial leather substrate was 90 / 10. Then, the obtained artificial leather substrate was sliced ​​in the thickness direction and cut into two pieces, and the surface was polished with 600-grit sandpaper to perform a napping treatment.

[0093] Then, the napped artificial leather was immersed in a dye bath at 90°C containing 8% owf of a cationic dye Nichilon Red-GL (manufactured by Niksei Chemicals Co., Ltd.; containing 4% washable chlorine in the dye) and 1 g / L of 90% acetic acid as a dyeing auxiliary at a bath ratio of 1:30 for 40 minutes to dye it red. Then, the following process was repeated twice: in the same dye bath, washing was performed at 70°C for 20 minutes using a hot water bath containing 2 g / L of SORUJIN R as an anionic surfactant. Then, drying was performed after washing to obtain a dyed napped artificial leather.

[0094] As described above, a dyed napped artificial leather comprising a nonwoven fabric of ultrafine long fibers having a fineness of 0.1 dtex and having a napped surface on one side was obtained. The napped artificial leather obtained had a thickness of 0.6 mm and a weight per unit area of ​​350 g / m 2 In addition, the length of the raised fibers was about 80 μm.

[0095] Then, the spinning stability, color development, color transferability, and tear strength of the sea-island type composite long fibers were evaluated for the napped artificial leather as described below.

[0096] [Spinning stability]

[0097] As described above, the stability during stretching by suction using an air jet nozzle type suction device in which the air flow pressure was adjusted so that the average spinning speed was 3700 m / min was determined according to the following criteria.

[0098] A: No broken wire.

[0099] B: There are many defects caused by broken yarns, or spinning cannot be done due to broken yarns.

[0100] [Color rendering]

[0101] Using a spectrophotometer (CM-3700 manufactured by Minolta Co., Ltd.), the L* a * b*Color system coordinate value to calculate brightness L * The value is the average of three points measured at the average position selected from the entire test piece.

[0102] [Color transfer]

[0103] A 0.8 mm thick vinyl chloride film (white) was placed on the surface of the cut napped artificial leather, and pressure was applied evenly so that the load was 750 g / cm 2 Then, the film was placed in an atmosphere of 50°C and 15% relative humidity for 16 hours. Then, the color difference ΔE between the vinyl chloride film before and after the color transition was measured using a spectrophotometer. * , judged according to the following criteria.

[0104] Level 5: 0.0≤ΔE * ≤0.2

[0105] Level 4-5: 0.2<ΔE * ≤1.4

[0106] Level 4: 1.4<ΔE * ≤2.0

[0107] Level 3-4: 2.0<ΔE * ≤3.0

[0108] Level 3: 3.0<ΔE * ≤3.8

[0109] Level 2-3: 3.8<ΔE * ≤5.8

[0110] Level 2: 5.8<ΔE * ≤7.8

[0111] Level 1-2: 7.8<ΔE * ≤11.4

[0112] Level 1: 11.4<ΔE *

[0113] [Tear strength]

[0114] Cut a test piece of 10cm long x 4cm wide from the dyed napped artificial leather. Then, cut a 5cm slit in the center of the short side of the test piece parallel to the long side. Then, use a tensile tester to clamp each slice on the chuck of the clamp and measure the SS curve at a tensile speed of 10cm / min. Divide the maximum load by the unit area weight of the test piece obtained in advance, and use the obtained value as the tear strength per 1mm thickness. The value is the average of 3 test pieces.

[0115] [Peel strength]

[0116] Two test pieces of 15 cm in length and 2.5 cm in width were cut from the obtained dyed napped artificial leather. Then, a laminated body was obtained in which two test pieces were sandwiched with a 100 μm polyurethane film (NASA-600, 10 cm in length and 2.5 cm in width) and overlapped. It should be noted that the polyurethane film was not overlapped on the 2.5 cm portion at both ends of each test piece. Then, a flat-plate hot press was used at a temperature of 130°C and a surface pressure of 5 kg / cm 2 The laminate was pressed for 60 seconds under the conditions of , and the laminate was bonded to prepare an evaluation sample. For the obtained evaluation sample, a tensile tester was used at room temperature, and the unbonded 2.5 cm portion was clamped between the upper and lower clamps, respectively, and the SS curve was measured at a tensile speed of 10 cm / min. The central value of the portion where the SS curve was in a substantially constant state was taken as the average value, and the value obtained by dividing by the sample width of 2.5 cm was taken as the peel strength. The value is the average value of 3 test pieces.

[0117] [Martindale wear loss]

[0118] The Martindale abrasion loss was measured in accordance with JIS L 1096. Specifically, a circular test piece with a diameter of 38 mm was cut from the obtained dyed napped artificial leather. Then, the test piece was placed under standard conditions (20°C × 65% RH) for 24 hours, and the weight W was measured. 1 (mg). Then, the standard friction cloth and the test piece are installed in the Martindale wear tester, and a load of 12KPa is applied to rub the surfaces against each other until the counter reaches 35,000 times. Then, the weight W of the test piece after the test is completed is measured. 2 (mg), and the wear loss W (mg) (W 1 -W 2 ).

[0119] [Chlorine content]

[0120] According to the method of BS EN 14582:2007, the chlorine content in the dyed napped artificial leather was quantitatively determined.

[0121] [Glass transition temperature and melting point]

[0122] The glass transition temperature and melting point of the polyester were measured using a differential scanning calorimeter (DSC) manufactured by Mettler (TA-3000).

[0123] The results are shown in Table 1 below.

[0124]

[0125] [Example 2]

[0126] As the thermoplastic resin of the island component, tetrabutyl sulfoisophthalate was used. PET modified with salt (tetrabutyl sulfoisophthalate A dyed napped artificial leather was obtained in the same manner as in Example 1 except that 2.5 mol% of salt units, 5 mol% of 1,4-cyclohexanedicarboxylic acid units, and 5 mol% of adipic acid units were added. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0127] [Example 3]

[0128] As the thermoplastic resin of the island component, tetrabutyl sulfoisophthalate was used. PET modified with salt (tetrabutyl sulfoisophthalate A dyed napped artificial leather was obtained in the same manner as in Example 1 except that 3 mol% of salt units, 5 mol% of 1,4-cyclohexanedicarboxylic acid units, and 5 mol% of adipic acid units were added. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0129] [Example 4]

[0130] As the thermoplastic resin of the island component, tetrabutyl sulfoisophthalate was used. PET modified with salt (tetrabutyl sulfoisophthalate A dyed napped artificial leather was obtained in the same manner as in Example 1 except that the amount of the napped artificial leather was 1.7 mol % and the amount of the isophthalic acid unit was 3 mol %. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0131] [Example 5]

[0132] As the thermoplastic resin of the island component, tetrabutyl sulfoisophthalate was used. PET modified with salt (tetrabutyl sulfoisophthalate A dyed napped artificial leather was obtained in the same manner as in Example 1 except that the amount of the salt unit was 1.7 mol % and the isophthalic acid unit was 6 mol %. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0133] [Example 6]

[0134] A dyed napped artificial leather was obtained in the same manner as in Example 1 except that the mass ratio of the nonwoven fabric / aqueous polyurethane in the obtained artificial leather substrate was changed to 80 / 20. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0135] [Example 7]

[0136] A dyed napped artificial leather was obtained in the same manner as in Example 1 except that the mass ratio of the nonwoven fabric / aqueous polyurethane in the obtained artificial leather substrate was changed to 75 / 25. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0137] [Example 8]

[0138] A dyed napped artificial leather was obtained in the same manner as in Example 1 except that PET modified with tetrabutylammonium salt of sulfoisophthalic acid (containing 1.7 mol% of tetrabutylammonium salt of sulfoisophthalic acid unit, 5 mol% of 1,4-cyclohexanedicarboxylic acid, and 5 mol% of adipic acid) was used as the thermoplastic resin of the island component. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0139] [Example 9]

[0140] A dyed napped artificial leather was obtained in the same manner as in Example 1 except that the same thermoplastic resin as in Example 4 was used as the island component and a composite spinning nozzle was used, wherein the composite spinning nozzle could form a cross-section having 12 island components of uniform cross-sectional areas distributed in the sea component.

[0141] [Example 10]

[0142] Using the same thermoplastic resin as in Example 4 for the island component and a composite spinning nozzle which can form a cross section in which 12 island components with uniform cross-sectional areas are distributed in the sea component, high-speed spinning of sea-island type composite long fibers with a fineness of 3.3 dtex was performed. In addition, a dyed napped artificial leather was obtained in the same manner as in Example 1.

[0143] [Example 11]

[0144] As the thermoplastic resin of the island component, tetrabutyl sulfoisophthalate was used. PET modified with salt (tetrabutyl sulfoisophthalate A dyed napped artificial leather was obtained in the same manner as in Example 1 except that the amount of the salt unit was 1.7 mol %. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0145] [Example 12]

[0146] As the thermoplastic resin of the island component, tetrabutyl sulfoisophthalate was used. PET modified with salt (tetrabutyl sulfoisophthalate A dyed napped artificial leather was obtained in the same manner as in Example 1 except that the amount of the salt unit was 2.5 mol %. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0147] [Comparative Example 1]

[0148] As the thermoplastic resin of the island component, tetrabutyl sulfoisophthalate was used. PET modified with salt (tetrabutyl sulfoisophthalate A dyed napped artificial leather was obtained in the same manner as in Example 1 except that 4 mol% of salt units, 5 mol% of 1,4-cyclohexanedicarboxylic acid units, and 5 mol% of adipic acid units were added. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0149] [Comparative Example 2]

[0150] As the thermoplastic resin of the island component, PET modified with sodium salt of sulfoisophthalic acid (containing 1.7 mol% of sodium salt of sulfoisophthalic acid unit, 5 mol% of 1,4-cyclohexanedicarboxylic acid unit, and 5 mol% of adipic acid unit) was used. The spinning of the island-type composite long fiber was carried out in the same manner as in Example 1 except that the above-mentioned method was used. However, since the molten polymer ejected from the spinning nozzle was cooled and the tension when the average spinning speed was 3700 m / min was sucked by the jet nozzle with the air flow pressure adjusted, the melt spinning could not be carried out stably. Therefore, the pressure of the suction air was reduced and the melt spinning was carried out at a low speed. The subsequent steps were the same as in Example 1, and a dyed napped artificial leather was obtained. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0151] [Comparative Example 3]

[0152] The napped artificial leather obtained in the same manner as in Example 1 was immersed in a dye bath at 90°C containing 8% owf of a cationic dye Nichilon Red-GL (manufactured by Niksei Chemicals Co., Ltd.; containing 4% washable chlorine in the dye) and 1 g / L of 90% acetic acid as a dyeing auxiliary at a bath ratio of 1:30 for 40 minutes to dye it red. Then, the following process was repeated twice: in the same dye bath, washing was performed at 70°C for 20 minutes using a hot water bath containing no anionic surfactant. Then, after washing, drying was performed to obtain a dyed napped artificial leather.

[0153] [Comparative Example 4]

[0154] A napped artificial leather was obtained in the same manner as in Example 1 except that PET (containing 6 mol% of isophthalic acid units) modified with isophthalic acid was used as the thermoplastic resin of the island component. Then, the napped artificial leather was subjected to flow dyeing at 130° C. for 1 hour using D.Red-W, Kiwalon Rubin 2GW, and Kiwalon Yellow 6GF as disperse dyes, and reduction washing was performed in the same dyeing bath to obtain a dyed napped artificial leather. Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0155] [Reference Example 1]

[0156] A dyed napped artificial leather was obtained in the same manner as in Example 1 except that the long fiber web was entangled under the following conditions.

[0157] An oil solution mixed with an antistatic agent was sprayed on the surface of the obtained long fiber web, and then 10 long fiber webs were stacked using a stacking device to produce a total unit area weight of 340 g / m 2 The laminated web was sprayed with a needle-breaking prevention oil. The laminated web was then needle-punched to achieve a three-dimensional entanglement treatment. Specifically, a needle with 6 hooks and a distance of 3.2 mm from the needle tip to the first hook was used, and the needle depth was 8.3 mm, and the needles were punched alternately from both sides of the laminate at 2400 punctures / cm 2 The area shrinkage caused by the needle punching treatment was 18%, and the unit area weight of the entangled web after the needle punching was 415g / m 2 .

[0158] Then, the obtained napped artificial leather was evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0159] Referring to Table 1, it can be seen that for the napped artificial leathers of Examples 1 to 12 of the present invention, the tear strength per 1 mm thickness is 30 N or more, and the peel strength is 3 kg / cm or more. Therefore, the Martindale abrasion loss of any of the napped artificial leathers is 100 mg / 35,000 times or less. In addition, the chlorine content is 90 ppm or less, and the result of the color transfer evaluation is 4 or more. It should be noted that the high-speed spinning stability during the manufacture of Examples 1 to 10 is excellent, but the high-speed spinning stability of Examples 11 and 12 is poor.

[0160] On the other hand, for the napped artificial leather of Comparative Example 1 using ultrafine fibers of polyester containing 4 mol% of units represented by formula (II), the tear strength and peel strength are low. Therefore, the Martindale abrasion loss is large. In addition, for the napped artificial leather of Comparative Example 2 using ultrafine fibers of polyester containing 1.7 mol% of sodium salt of sulfoisophthalic acid, the tear strength and peel strength are low, so the Martindale abrasion loss is large. Moreover, the high-speed spinning stability during manufacturing is also poor. In addition, for the napped artificial leather of Comparative Example 3 that was washed in a hot water bath that does not contain anionic surfactants during washing after cationic dyeing, the chlorine content is high and the color transfer is extremely poor. In addition, the color transfer of the napped artificial leather of Comparative Example 4 that was dyed with disperse dyes is also extremely poor. In addition, for Reference Example 1, although the high-speed spinning stability during manufacturing is excellent, the cohesion state is low, so the tear strength and peel strength are low, so the Martindale abrasion loss is large.

[0161] Industrial Applicability

[0162] The napped artificial leather obtained in the present invention can be preferably used as a surface material for clothing, shoes, furniture, car seats, sundry goods, and the like.

Claims

1. An artificial leather substrate, comprising a nonwoven fabric of long-fiber cationic dye-dyeable polyester fibers having a fineness of 0.07 to 0.9 dtex, and a polymer elastic body imparted to the interior of the nonwoven fabric, wherein: The cationic dye-dyeable polyester fiber comprises a polyester containing a dicarboxylic acid unit mainly composed of a terephthalic acid unit and a diol unit mainly composed of an ethylene glycol unit. As the dicarboxylic acid unit, it contains (i) the following formula (I b ) and contains 1.5 to 1.7 mol % of sulfoisophthalate units represented by (ii) 1,4-cyclohexanedicarboxylic acid units and 1 to 6 mol % of adipic acid units, or (iii) 1 to 6 mol % of isophthalic acid units. Formula (I b ), X represents the season ions or quaternary ammonium ions.

2. The artificial leather substrate according to claim 1, wherein The cationic dye-dyeable polyester contains 0 to 0.2 mol % of an alkali metal salt unit of sulfoisophthalic acid as the dicarboxylic acid unit.

3. The artificial leather substrate according to claim 1, wherein The cationic dye-dyeable polyester fiber has a glass transition temperature Tg in the range of 60-70°C.

4. A napped artificial leather substrate, comprising: the artificial leather substrate according to claim 1 having a napped surface subjected to a napping treatment on at least one side thereof.

5. A napped artificial leather dyed with a cationic dye, which is obtained by dyeing the napped artificial leather substrate according to claim 4 with a cationic dye, The napped artificial leather dyed with a cationic dye * The value is ≤50 and the chlorine content is below 90ppm.

6. The napped artificial leather dyed with a cationic dye as claimed in claim 5, wherein the tear strength per 1 mm thickness is 30 N or more, and the peel strength is 3 kg / cm or more.

7. The napped artificial leather dyed with a cationic dye as claimed in claim 5, wherein the Martindale abrasion loss thereof is 100 mg / 35,000 times or less under a load of 12 KPa.

8. The napped artificial leather dyed with a cationic dye as claimed in claim 5, wherein: In the color transfer evaluation of PVC at a load of 0.75 kg / cm, 50° C., and 16 hours, the color difference level was judged to be 4 or more.

9. A method for producing a napped artificial leather dyed with a cationic dye, the method comprising: A step of preparing the artificial leather substrate according to claim 1, The artificial leather substrate is dyed with a cationic dye and then washed in a hot water bath at 50 to 100° C. containing an anionic surfactant to reduce the chlorine content to 90 ppm or less; and Before or after the dyeing and washing steps, at least one side of the artificial leather substrate is subjected to a raising treatment. in, The napped artificial leather dyed with a cationic dye * Value ≤50.