Mask Blanks and Photomasks

By adjusting the composition ratio and film thickness of the anti-reflection layer and the light-shielding layer in the mask blank, the problem of uneven cross-sectional shape caused by the difference in etching rate of the mask blank in the existing technology is solved, and a photomask with low reflectivity and high optical density is realized. Mold manufacturing ensures the verticality and high precision of the pattern.

CN112578629BActive Publication Date: 2024-10-22ULVAC COATING CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011031340.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-27
Publication Date
2024-10-22
Estimated Expiration
2040-09-27

AI Technical Summary

Technical Problem

When manufacturing photomasks, it is difficult to achieve low reflectivity and high optical density mask blanks with the existing technology, resulting in a large etching rate difference between the light shielding layer and the anti-reflective layer, forming uneven cross-sectional shapes, such as upper eaves and hems, affecting patterns. verticality and contrast.

Method used

An oxygen-nitrogen carbonized film containing chromium, oxygen, nitrogen and carbon is used as the lower and upper anti-reflective layers. The light-shielding layer is a nitride film of chromium and nitrogen. By adjusting the composition ratio and film thickness of each layer, the light-shielding layer and the anti-reflective layer are ensured The etching rate of the layer is close to that of the upper eaves and hems, thereby reducing the cross-sectional shape of the upper eaves and hems.

Benefits of technology

It realizes the control of the pattern cross-section shape under low reflectivity and high optical density, ensures the verticality and high precision of the cross-section shape during the patterning process of the mask blank, reduces the depression of the light-shielding layer, and improves the efficiency of the photomask. quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112578629B_ABST
    Figure CN112578629B_ABST
Patent Text Reader

Abstract

The present invention relates to a mask blank and a photomask, wherein the mask blank has a mask layer that becomes a photomask. The mask blank has a low reflectivity and a predetermined optical density, can make the etching rate of the light-shielding layer close to the etching rate of the anti-reflection layer, and can realize an appropriate cross-sectional shape with reduced upper and lower edges. The mask layer comprises: a lower anti-reflection layer laminated on a transparent substrate; a light-shielding layer disposed at a position farther from the transparent substrate than the lower anti-reflection layer; and an upper anti-reflection layer disposed at a position farther from the transparent substrate than the light-shielding layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a mask blank and a photomask, and in particular to a technology suitable for use in the manufacture of a double-sided low-reflection binary mask blank or a binary mask blank. Background Art

[0002] When manufacturing a photomask for a large panel such as an FPD (flat panel display), a mask blank having a light shielding layer is used as a binary mask. In addition, as the FPD becomes more precise, the need to form a fine pattern is increasing.

[0003] In such a mask blank, a structure in which a film made of a chromium material is laminated on a transparent substrate such as glass is generally used as a mask layer including a patterned light shielding layer or the like (Patent Document 1).

[0004] In order to produce a fine pattern, it is necessary to reduce the reflectivity of the front and back surfaces of the mask blank (for example, to 5% or less under exposure light having a wavelength of 436 nm) as a countermeasure against stray light during pattern formation.

[0005] As a film structure of a mask blank for achieving low reflectivity on the front and back surfaces, for example, a mask layer having at least a three-layer structure is known, wherein an antireflection layer (back surface), a light shielding layer, and an antireflection layer (front surface) are stacked on a glass substrate.

[0006] When such an antireflection layer is provided, in order to obtain a film with a low refractive index, an oxidized chromium oxide film or the like can be used as the antireflection layer.

[0007] Patent Document 1: Japanese Patent Publication No. 2001-305716

[0008] However, the etching rate of the chromium oxide film with a high oxygen concentration is reduced. As a result, when the chromium oxide film with a high oxygen concentration is used as the antireflection layer, the etching rate of the antireflection layer is lower than the etching rate of the light shielding layer, so the etching of the antireflection layer does not progress.

[0009] Therefore, when a mask pattern is produced, the etching of the light shielding layer progresses more than the anti-reflection layer, and the lateral etching amount, that is, the side etching amount in the mask blank becomes uneven in the thickness direction. Specifically, the following problem is found: that is, the central portion in the thickness direction of the mask layer is etched unnecessarily in large quantities, resulting in a cross-sectional shape with an upper eave (shroud) and a lower hem (hem), etc.

[0010] In order to make the cross-sectional shape of the pattern perpendicular to the glass substrate surface, the etching rate of each layer needs to be consistent, but in order to maintain the optical properties of each layer, the composition ratio is greatly different, so it is inevitable that the etching rate is greatly different. Therefore, a mask blank capable of forming a vertical pattern cross-sectional shape has not been realized.

[0011] Furthermore, when forming a pattern on a mask blank, there is a demand to cope with an optical density (for example, OD5) higher than the conventional optical density (OD3) in order to improve contrast.

[0012] In order to meet this requirement, the difference between the oxygen concentration of the light shielding layer and the oxygen concentration of the anti-reflection layer needs to be further increased, which results in a greater difference in etching rate between the light shielding layer and the anti-reflection layer.

[0013] Therefore, the deviation of the cross-sectional shape from the vertical direction, which is permissible at the conventional optical density (OD3), is not permissible at a high optical density (for example, OD5). Summary of the invention

[0014] The present invention is completed in view of the above situation, and achieves the purpose of providing a mask blank, which has a low reflectivity and a specified optical density, can make the etching rate of the light-shielding layer close to the etching rate of the anti-reflection layer, and can achieve an appropriate cross-sectional shape with reduced upper eaves and lower hems.

[0015] A mask blank according to one embodiment of the present invention has a mask layer that becomes a photomask, wherein the mask layer has: a lower antireflection layer laminated on a transparent substrate; a light shielding layer disposed at a position farther from the transparent substrate than the lower antireflection layer; and an upper antireflection layer disposed at a position farther from the transparent substrate than the light shielding layer. The lower antireflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen, and carbon, wherein the content of chromium contained in the lower antireflection layer is 25 atomic % to 50 atomic %, the content of oxygen contained in the lower antireflection layer is 30 atomic % to 50 atomic %, the content of nitrogen contained in the lower antireflection layer is 10 atomic % to 30 atomic %, and the content of carbon contained in the lower antireflection layer is 2 atomic % to 5 atomic %. The light shielding layer is a nitride film containing chromium and nitrogen, wherein the content of chromium contained in the light shielding layer is 70 atomic % to 95 atomic %, and the content of nitrogen contained in the light shielding layer is 5 atomic % to 20 atomic %. The upper anti-reflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen and carbon, the content of chromium contained in the upper anti-reflection layer is 25 atomic % to 50 atomic %, the content of oxygen contained in the upper anti-reflection layer is 55 atomic % to 70 atomic %, the content of nitrogen contained in the upper anti-reflection layer is 5 atomic % to 20 atomic %, and the content of carbon contained in the upper anti-reflection layer is 2 atomic % to 5 atomic %. Thus, the above-mentioned problem is solved.

[0016] A mask blank according to one embodiment of the present invention has a mask layer that becomes a photomask, wherein the mask layer has: a lower anti-reflection layer laminated on a transparent substrate; a light shielding layer disposed at a position farther from the transparent substrate than the lower anti-reflection layer; and an upper anti-reflection layer disposed at a position farther from the transparent substrate than the light shielding layer. The lower anti-reflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen, and carbon, wherein the content of chromium contained in the lower anti-reflection layer is 25 atomic % to 50 atomic %, the content of oxygen contained in the lower anti-reflection layer is 30 atomic % to 50 atomic %, the content of nitrogen contained in the lower anti-reflection layer is 10 atomic % to 30 atomic %, and the content of carbon contained in the lower anti-reflection layer is 2 atomic % to 5 atomic %. The light shielding layer is a nitride carbon film containing chromium, nitrogen and carbon, wherein the content of chromium in the light shielding layer is 70 atomic % to 95 atomic %, the content of nitrogen in the light shielding layer is 5 atomic % to 20 atomic %, and the content of carbon in the light shielding layer is 0 atomic % to 15 atomic %. The upper anti-reflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen and carbon, wherein the content of chromium in the upper anti-reflection layer is 25 atomic % to 50 atomic %, the content of oxygen in the upper anti-reflection layer is 55 atomic % to 70 atomic %, the content of nitrogen in the upper anti-reflection layer is 5 atomic % to 20 atomic %, and the content of carbon in the upper anti-reflection layer is 2 atomic % to 5 atomic %. Thus, the above-mentioned problem is solved.

[0017] In the mask blank according to one aspect of the present invention, the reflectance of exposure light having a wavelength of 365 nm to 436 nm may be 10% or less on both surfaces of the mask layer.

[0018] In the mask blank according to one aspect of the present invention, the reflectance of exposure light having a wavelength of 436 nm may be 5% or less on both surfaces of the mask layer.

[0019] In the mask blank according to one aspect of the present invention, in the mask layer, the thickness of the lower antireflection layer, the thickness of the light shielding layer, and the thickness of the upper antireflection layer may be set so that the optical density is 3.0 or more.

[0020] In the mask blank according to one embodiment of the present invention, the lower antireflection layer may have a thickness of 25.0 nm to 35.0 nm, the light shielding layer may have a thickness of 125.0 nm to 135.0 nm, and the upper antireflection layer may have a thickness of 25.0 nm to 35.0 nm.

[0021] In the mask blank according to one aspect of the present invention, the mask layer may have a thickness of 175.0 nm to 205.0 nm.

[0022] The mask blank according to one aspect of the present invention may include a photoresist layer provided at a position farther from the transparent substrate than the mask layer.

[0023] A photomask according to one aspect of the present invention is produced from the mask blank according to the above aspect.

[0024] A mask blank according to one embodiment of the present invention has a mask layer that becomes a photomask, wherein the mask layer has: a lower antireflection layer laminated on a transparent substrate; a light shielding layer disposed at a position farther from the transparent substrate than the lower antireflection layer; and an upper antireflection layer disposed at a position farther from the transparent substrate than the light shielding layer. The lower antireflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen, and carbon, wherein the content of chromium contained in the lower antireflection layer is 25 atomic % to 50 atomic %, the content of oxygen contained in the lower antireflection layer is 30 atomic % to 50 atomic %, the content of nitrogen contained in the lower antireflection layer is 10 atomic % to 30 atomic %, and the content of carbon contained in the lower antireflection layer is 2 atomic % to 5 atomic %. The light shielding layer is a nitride film containing chromium and nitrogen, wherein the content of chromium contained in the light shielding layer is 70 atomic % to 95 atomic %, and the content of nitrogen contained in the light shielding layer is 5 atomic % to 20 atomic %. The upper anti-reflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen and carbon, the content of chromium contained in the upper anti-reflection layer is 25 atomic % to 50 atomic %, more preferably 30 atomic % to 50 atomic %, the content of oxygen contained in the upper anti-reflection layer is 55 atomic % to 70 atomic %, the content of nitrogen contained in the upper anti-reflection layer is 5 atomic % to 20 atomic %, and the content of carbon contained in the upper anti-reflection layer is 2 atomic % to 5 atomic %. Thus, the above-mentioned problem is solved.

[0025] Thus, the patterned cross-sectional shape can be controlled within an appropriate range while maintaining the low reflectivity and required optical density of both surfaces of the mask layer. Specifically, for the upper and lower anti-reflection layers, the side of the light shielding layer is etched within a specified range to prevent the light shielding layer from being partially recessed.

[0026] Therefore, when manufacturing a photomask, the cross-sectional shape of the mask blank during patterning (resist coating, exposure, development, etching) can be made as vertical as possible. By making the pattern size affected by the cross-sectional shape of the pattern within a predetermined range, a high-definition photomask can be realized.

[0027] A mask blank according to one embodiment of the present invention has a mask layer that becomes a photomask, wherein the mask layer has: a lower antireflection layer laminated on a transparent substrate; a light shielding layer disposed at a position farther from the transparent substrate than the lower antireflection layer; and an upper antireflection layer disposed at a position farther from the transparent substrate than the light shielding layer. The lower antireflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen, and carbon, wherein the content of chromium contained in the lower antireflection layer is 25 atomic % to 50 atomic %, the content of oxygen contained in the lower antireflection layer is 30 atomic % to 50 atomic %, the content of nitrogen contained in the lower antireflection layer is 10 atomic % to 30 atomic %, and the content of carbon contained in the lower antireflection layer is 2 atomic % to 5 atomic %. The light shielding layer is a nitride carbon film containing chromium, nitrogen and carbon, the content of chromium contained in the light shielding layer is 70 atomic % to 95 atomic %, the content of nitrogen contained in the light shielding layer is 5 atomic % to 20 atomic %, and the content of carbon contained in the light shielding layer is 0 atomic % to 15 atomic %. The upper anti-reflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen and carbon, the content of chromium contained in the upper anti-reflection layer is 25 atomic % to 50 atomic %, more preferably 30 atomic % to 50 atomic %, the content of oxygen contained in the upper anti-reflection layer is 55 atomic % to 70 atomic %, the content of nitrogen contained in the upper anti-reflection layer is 5 atomic % to 20 atomic %, and the content of carbon contained in the upper anti-reflection layer is 2 atomic % to 5 atomic %. Thus, the above-mentioned problem is solved.

[0028] Thus, the patterned cross-sectional shape can be controlled within an appropriate range while maintaining the low reflectivity and required optical density of both surfaces of the mask layer. Specifically, for the upper and lower anti-reflection layers, the side of the light shielding layer is etched within a specified range to prevent the light shielding layer from being partially recessed.

[0029] Therefore, when manufacturing a photomask, the cross-sectional shape of the mask blank during patterning (resist coating, exposure, development, etching) can be made as vertical as possible. By making the size of the pattern affected by the cross-sectional shape of the pattern within a predetermined range, a high-definition photomask can be realized.

[0030] In the mask blank involved in one embodiment of the present invention, the reflectivity of exposure light with a wavelength of 365nm to 436nm can be less than 10% on both sides of the mask layer, and in particular, the reflectivity of exposure light with a wavelength of 436nm can be less than 5% on both sides of the mask layer.

[0031] Thus, by setting the composition ratio of each layer to be within the above range, a preferred cross-sectional shape can be achieved, and a low reflectance range required for patterning can be achieved.

[0032] In addition, the above-mentioned reflectivity on the transparent substrate side is the reflectivity including the transparent substrate.

[0033] In the mask blank according to one aspect of the present invention, in the mask layer, the thickness of the lower antireflection layer, the thickness of the light shielding layer, and the thickness of the upper antireflection layer may be set so that the optical density is 3.0 or more.

[0034] Therefore, by setting the composition ratio of each layer to be within the above range, a preferred cross-sectional shape can be achieved, and the range of optical density required for patterning can be achieved.

[0035] In the mask blank according to one embodiment of the present invention, the lower antireflection layer may have a thickness of 25.0 nm to 35.0 nm, the light shielding layer may have a thickness of 125.0 nm to 135.0 nm, and the upper antireflection layer may have a thickness of 25.0 nm to 35.0 nm.

[0036] Therefore, by setting the composition ratio of each layer to be within the above range, a preferred cross-sectional shape can be achieved, and the range of optical density required for patterning can be achieved.

[0037] In the mask blank according to one aspect of the present invention, the mask layer may have a thickness of 175.0 nm to 205.0 nm.

[0038] Thus, by setting the composition ratio of each layer within the above range, a preferred cross-sectional shape can be realized, and the range of optical density required for patterning and the range of low reflectance required for patterning can be realized.

[0039] The mask blank according to one aspect of the present invention may include a photoresist layer provided at a position farther from the transparent substrate than the mask layer.

[0040] The photomask according to one aspect of the present invention can be produced using any of the mask blanks described above.

[0041] According to the present invention, it is possible to provide a mask blank having a low reflectivity and a predetermined optical density, making the etching rate of the light shielding layer close to the etching rate of the anti-reflection layer, and realizing an appropriate cross-sectional shape with reduced upper and lower edges. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 It is a cross-sectional view showing a mask blank according to the first embodiment of the present invention.

[0043] Figure 2 It is a cross-sectional view showing a mask blank according to the first embodiment of the present invention.

[0044] Figure 3 It is a cross-sectional view showing a photomask according to the first embodiment of the present invention.

[0045] Figure 4 It is a schematic diagram showing a film forming apparatus in a method for manufacturing a mask blank and a photomask according to the first embodiment of the present invention.

[0046] Figure 5 This is a graph showing the front spectral reflectance in Examples and Comparative Examples of the mask blanks according to the present invention.

[0047] Figure 6 This is a graph showing the back surface spectral reflectance in Examples and Comparative Examples of the mask blanks according to the present invention.

[0048] Figure 7 This is a SEM photograph showing the cross-sectional shape of the mask blank after patterning in Example 1 according to the present invention.

[0049] Figure 8 This is a SEM photograph showing the cross-sectional shape of the mask blank after patterning in Example 2 according to the present invention.

[0050] Fig. 9 This is a SEM photograph showing the cross-sectional shape after patterning in Comparative Example 1 of the mask blank according to the present invention.

[0051] Fig.10 This is a SEM photograph showing the cross-sectional shape after patterning in Comparative Example 2 of the mask blank according to the present invention.

[0052] Fig.11 This is a SEM photograph showing the cross-sectional shape after patterning in Comparative Example 3 of the mask blank according to the present invention.

[0053] Fig.12 This is a bird's-eye SEM photograph showing the shape of the mask blank after patterning in Experimental Example 1 according to the present invention.

[0054] Fig.13 This is a bird's-eye SEM photograph showing the shape of the mask blank after patterning in Experimental Example 2 according to the present invention.

[0055] Fig.14 This is a bird's-eye SEM photograph showing the shape after patterning in Comparative Example 1 of the mask blank according to the present invention.

[0056] Fig.15 This is a bird's-eye SEM photograph showing the shape after patterning in Comparative Example 2 of the mask blank according to the present invention.

[0057] Fig.16This is a bird's-eye SEM photograph showing the shape after patterning in Comparative Example 3 of the mask blank according to the present invention. DETAILED DESCRIPTION

[0058] Hereinafter, a mask blank, a photomask, a method for manufacturing a mask blank, and a method for manufacturing a photomask according to a first embodiment of the present invention will be described with reference to the drawings.

[0059] Figure 1 is a cross-sectional view showing a mask blank in this embodiment, Figure 2 1 is a cross-sectional view showing a mask blank in the present embodiment. In the drawing, reference numeral 10B denotes a mask blank.

[0060] The mask blank 10B according to the present embodiment is provided for a binary mask (photomask) used when the wavelength of exposure light falls within a range of about 365 nm to 436 nm.

[0061] like Figure 1 As shown, the mask blank 10B involved in this embodiment includes: a glass substrate (transparent substrate) 11; a lower anti-reflection layer 12 formed on the glass substrate 11; a light-shielding layer 13 formed on the lower anti-reflection layer 12; and an upper anti-reflection layer 14 formed on the light-shielding layer 13.

[0062] That is, the light shielding layer 13 is provided at a position farther from the glass substrate 11 than the lower anti-reflection layer 12. In addition, the upper anti-reflection layer 14 is provided at a position farther from the glass substrate 11 than the light shielding layer 13.

[0063] These lower antireflection layer 12 , light shielding layer 13 , and upper antireflection layer 14 configure a mask layer which is a low-reflection laminate film having optical characteristics required for a photomask.

[0064] In addition, if Figure 1 As shown, the mask blank 10B involved in this embodiment can also be as follows Figure 2 As shown in the figure, a photoresist layer 15 is formed in advance on a mask layer on which a lower antireflection layer 12, a light shielding layer 13, and an upper antireflection layer 14 are laminated.

[0065] In addition, the mask blank 10B according to the present embodiment may have a structure in which a chemical-resistant layer, a protective layer, a laminating layer, an etching stop layer, etc. are laminated in addition to the lower anti-reflection layer 12, the light-shielding layer 13, and the upper anti-reflection layer 14. Figure 2 As shown, a photoresist layer 15 may be formed on these laminated films.

[0066] As the glass substrate (transparent substrate) 11, a material having excellent transparency and optical isotropy, such as a quartz glass substrate, can be used. The size of the glass substrate 11 is not particularly limited, and can be appropriately selected according to the substrate (such as LCD (liquid crystal display), plasma display, organic EL (electroluminescence) display and other FPD substrates) to be exposed using the mask.

[0067] In this embodiment, as the glass substrate (transparent substrate) 11, a rectangular substrate with a side length of about 100 mm to a side length of more than 2000 mm can be used. In addition, a substrate with a thickness of less than 1 mm, a substrate with a thickness of several mm, or a substrate with a thickness of more than 10 mm can also be used.

[0068] In addition, the flatness of the glass substrate 11 can be reduced by grinding the surface of the glass substrate 11. The flatness of the transparent substrate 11 can be, for example, 20 μm or less. As a result, the depth of focus of the mask becomes deeper, which can make a great contribution to the formation of a fine and high-precision pattern. In addition, the flatness is preferably 10 μm or less, which is a small value.

[0069] The lower antireflection layer 12 has Cr (chromium) as a main component. The lower antireflection layer 12 contains C (carbon), O (oxygen), and N (nitrogen).

[0070] In addition, the lower anti-reflection layer 12 may also have different compositions in the thickness direction. In addition, in this case, as the lower anti-reflection layer 12, it is also possible to laminate one material or two or more materials selected from Cr monomer and Cr oxide, nitride, carbide, oxynitride, carbonitride and oxycarbonitride.

[0071] As described later, the thickness of the lower antireflection layer 12 and the composition ratio (atomic %) of Cr, N, C, O, etc. are set so as to obtain predetermined optical characteristics and etching rate.

[0072] For example, the lower anti-reflection layer 12 is an oxynitride carbonization film containing chromium, oxygen, nitrogen and carbon, and the composition ratio in the lower anti-reflection layer 12 can be set to a chromium content (chromium concentration) of 25 atomic% to 50 atomic%, an oxygen content (oxygen concentration) of 30 atomic% to 50 atomic%, a nitrogen content (nitrogen concentration) of 10 atomic% to 30 atomic%, and a carbon content (carbon concentration) of 2 atomic% to 5 atomic%.

[0073] The thickness of the lower antireflection layer 12 is set according to the optical properties required for the lower antireflection layer 12 and varies according to the composition ratio of Cr, N, C, O, etc. The thickness of the lower antireflection layer 12 may be 25.0 nm to 35.0 nm.

[0074] Thus, the lower antireflection layer 12 can be set to have a reflectivity including the glass substrate 11 of 5% or less in the wavelength range of about 365 nm to 436 nm, especially in the exposure light with a wavelength of 436 nm.

[0075] The light shielding layer 13 has Cr (chromium) as a main component. The light shielding layer 13 contains N (nitrogen).

[0076] In addition, the light shielding layer 13 may also have different compositions in the thickness direction. In addition, in this case, the light shielding layer 13 may also be constructed by laminating one or more materials selected from Cr monomer and Cr oxide, nitride, carbide, oxynitride, carbonitride and oxycarbonitride.

[0077] As described later, the thickness of the light shielding layer 13 and the composition ratio (atomic %) of Cr, N, C, O, etc. are set so as to obtain predetermined optical characteristics and etching rate.

[0078] For example, the light shielding layer 13 is a nitride film containing chromium and nitrogen, and the chromium content can be set to 70 atomic % to 95 atomic % and the nitrogen content can be set to 5 atomic % to 20 atomic %.

[0079] Alternatively, the light shielding layer 13 is a nitride carbon film containing chromium, nitrogen and carbon, and may be set to have a chromium content of 70 to 95 atomic %, a nitrogen content of 5 to 20 atomic %, and a carbon content of 0 to 15 atomic %.

[0080] The thickness of the light shielding layer 13 is set according to the optical characteristics required for the light shielding layer 13 and varies according to the composition ratio of Cr, N, C, O, etc. The thickness of the light shielding layer 13 may be 125.0 nm to 135.0 nm.

[0081] The upper antireflection layer 14 has Cr (chromium) as a main component. The upper antireflection layer 14 contains C (carbon), O (oxygen), and N (nitrogen).

[0082] In addition, the upper anti-reflection layer 14 may also have different compositions in the thickness direction. In addition, in this case, the upper anti-reflection layer 14 may also be constructed by laminating one material or two or more materials selected from Cr monomer and Cr oxide, nitride, carbide, oxynitride, carbonitride and oxycarbonitride.

[0083] As described later, the thickness of the upper antireflection layer 14 and the composition ratio (atomic %) of Cr, N, C, O, etc. are set so as to obtain predetermined optical characteristics and etching rate.

[0084] For example, the upper anti-reflection layer 14 is an oxynitride carbon film containing chromium, oxygen, nitrogen and carbon, and the composition ratio in the upper anti-reflection layer 14 can be set to a chromium content of 25 atomic% to 50 atomic%, more preferably a chromium content of 30 atomic% to 50 atomic%, an oxygen content of 55 atomic% to 70 atomic%, a nitrogen content of 5 atomic% to 20 atomic%, and a carbon content of 2 atomic% to 5 atomic%.

[0085] The thickness of the upper antireflection layer 14 is set according to the optical properties required for the upper antireflection layer 14 and varies according to the composition ratio of Cr, N, C, O, etc. The thickness of the upper antireflection layer 14 may be 25.0 nm to 35.0 nm.

[0086] Thus, the upper antireflection layer 14 can be set so that the reflectivity of the upper antireflection layer 14 is 5% or less in the wavelength range of about 365 nm to 436 nm, especially in the exposure light with a wavelength of 436 nm.

[0087] Regarding the mask layer formed by laminating the lower antireflection layer 12 , the light shielding layer 13 , and the upper antireflection layer 14 , the film thickness of the mask layer may be 175.0 nm to 205.0 nm.

[0088] The mask blank 10B in this embodiment can be set so that the reflectivity under the exposure light with a wavelength of 436nm is 5% or less on both sides of the mask layer formed by laminating the lower anti-reflection layer 12, the light shielding layer 13 and the upper anti-reflection layer 14. In addition, the mask layer formed by laminating the lower anti-reflection layer 12, the light shielding layer 13 and the upper anti-reflection layer 14 can be set so that the optical density is 3.0 or more.

[0089] In addition, the mask blank 10B in the present embodiment can make the etching rates of the lower anti-reflection layer 12, the light-shielding layer 13 and the upper anti-reflection layer 14 close by setting the composition ratio of the lower anti-reflection layer 12, the light-shielding layer 13 and the upper anti-reflection layer 14 within the above-mentioned range, and as described later, it is possible to achieve a cross-sectional shape in which the generation of upper eaves and lower hems is reduced.

[0090] In the method for manufacturing a mask blank in the present embodiment, the lower antireflection layer 12 is formed on the glass substrate (transparent substrate) 11 , the light shielding layer 13 is formed, and then the upper antireflection layer 14 is formed.

[0091] When a protective layer, a laminating layer, a chemical resistant layer, an etching stop layer, etc. other than the lower antireflection layer 12, the light shielding layer 13, and the upper antireflection layer 14 are laminated, the method for manufacturing the mask blank may include a laminating step of laminating these layers.

[0092] As an example, an etching stop layer including metal silicide can be cited.

[0093] Figure 3 It is a cross-sectional view showing a photomask in this embodiment.

[0094] like Figure 3 As shown, the binary mask (photomask) 10 in this embodiment has a structure in which a lower antireflection layer 12, a light shielding layer 13, and an upper antireflection layer 14 are laminated as a mask blank 10B and formed by patterning.

[0095] Next, a method for manufacturing the photomask 10 from the mask blank 10B of the present embodiment will be described.

[0096] As a resist pattern forming process, Figure 2 As shown, a photoresist layer 15 is formed on the outermost surface of the mask blank 10B. Alternatively, a mask blank 10B having a photoresist layer 15 formed on the outermost surface may be prepared in advance. The photoresist layer 15 may be a positive type or a negative type. As a material for the photoresist layer 15, a material that can cope with etching of a chromium-based material may be used. As the photoresist layer 15, a liquid resist may be used.

[0097] Next, the photoresist layer 15 is exposed and developed to form a resist pattern outside the upper antireflection layer 14. The resist pattern functions as a mask used for etching the lower antireflection layer 12, the light shielding layer 13, and the upper antireflection layer 14.

[0098] The appropriate shape of the resist pattern is determined according to the etching patterns of the lower antireflection layer 12, the light shielding layer 13, and the upper antireflection layer 14. As an example, the resist pattern is set so that the light-transmitting region has an opening width corresponding to the opening width size of the light shielding pattern to be formed.

[0099] Next, as an upper anti-reflection pattern forming step, the upper anti-reflection layer 14 is wet-etched using an etching solution over the resist pattern to form an upper anti-reflection pattern 14 p .

[0100] As the etching solution used in the upper anti-reflection pattern forming step, an etching solution containing ammonium cerium nitrate can be used. For example, ammonium cerium nitrate containing an acid such as nitric acid or perchloric acid is preferably used.

[0101] Next, as a light shielding pattern forming step, the light shielding layer 13 is wet-etched using an etching solution, passing over the upper anti-reflection pattern 14 p , to form a light shielding pattern 13 p .

[0102] As the etching liquid used in the light shielding pattern forming step, similarly to the upper anti-reflection pattern forming step, an etching liquid containing ammonium cerium nitrate can be used. For example, ammonium cerium nitrate containing an acid such as nitric acid or perchloric acid is preferably used.

[0103] Next, as a lower anti-reflection pattern forming step, the lower anti-reflection layer 12 is wet-etched across the patterned light shielding pattern 13 p , the upper anti-reflection pattern 14 p , and the resist pattern to form a lower anti-reflection pattern 12 p .

[0104] As the etching liquid used in the lower anti-reflection pattern forming step, similarly to the upper anti-reflection pattern forming step and the light shielding pattern forming step, an etching liquid containing ammonium cerium nitrate can be used. For example, ammonium cerium nitrate containing an acid such as nitric acid or perchloric acid is preferably used.

[0105] In addition, the mask blank 10B in the present embodiment can make the etching rates of the lower anti-reflection layer 12, the light shielding layer 13, and the upper anti-reflection layer 14 close to each other by setting the composition ratio of the lower anti-reflection layer 12, the light shielding layer 13, and the upper anti-reflection layer 14 within the above range. Therefore, after the upper anti-reflection pattern 14p, the light shielding pattern 13p, and the lower anti-reflection pattern 12p are formed by etching, as the cross-sectional shape of the photomask 10, an excellent cross-sectional shape close to vertical can be obtained.

[0106] In addition, in the light shielding pattern forming step, the composition ratio of the light shielding layer 13 is set to be different from the above-mentioned range of the upper and lower anti-reflection layers 12 and 14, so the etching rate is reduced compared to the case where no special setting is made. Therefore, compared with the etching in this case, the etching of the light shielding pattern 13p progresses slowly. As a result, the etching rates of the light shielding layer 13, the lower anti-reflection layer 12, and the upper anti-reflection layer 14 can be made close.

[0107] That is, the angle (taper angle) θ formed by the upper anti-reflection pattern 14p, the shading pattern 13p, and the lower anti-reflection pattern 12p and the front surface of the glass substrate 11 is close to a right angle. For example, the angle θ can be set to about 90°. In addition, the upper anti-reflection pattern 14p, the shading pattern 13p, and the lower anti-reflection pattern 12p can be etched in a manner that all have the same pattern shape when the glass substrate 11 is observed from the normal direction.

[0108] In addition, in the case of the mask blank 10B on which other films such as a laminating layer are formed in advance, patterning is performed into a predetermined shape corresponding to the upper anti-reflection pattern 14p, the light shielding pattern 13p, and the lower anti-reflection pattern 12p by wet etching using an etching solution for the film. Patterning of other films such as a laminating layer can be performed by a predetermined process before or after patterning of the lower anti-reflection layer 12, the light shielding layer 13, and the upper anti-reflection layer 14 according to the lamination order.

[0109] Furthermore, the lower antireflection layer 12 , the light shielding layer 13 , and the upper antireflection layer 14 can have their cross-sectional shapes after patterning improved by changing their oxygen concentrations in the film thickness direction.

[0110] Specifically, for the lower anti-reflection layer 12, the light shielding layer 13, and the upper anti-reflection layer 14, that is, the Cr film, the higher the oxygen concentration in the film, the lower the etching rate. Therefore, for the lower anti-reflection layer 12, the light shielding layer 13, and the upper anti-reflection layer 14, by making the oxygen concentration on the upper layer side higher than the oxygen concentration on the lower layer side, the etching rate on the upper layer side can be made lower than the etching rate on the lower layer side.

[0111] At the same time, by changing the composition ratio of carbon, nitrogen, and other elements other than oxygen in the film thickness direction, the etching rate and optical characteristics can be set to a predetermined state.

[0112] In summary, if Figure 3 As shown, the photomask 10 having the upper anti-reflection pattern 14p, the light shielding pattern 13p, and the lower anti-reflection pattern 12p can be obtained.

[0113] Next, a method for manufacturing a mask blank in the present embodiment will be described with reference to the drawings.

[0114] Figure 4 It is a schematic diagram which shows the manufacturing apparatus of the mask blank in this embodiment.

[0115] The mask blank 10B in this embodiment is formed by Figure 4 The manufacturing device shown is used to manufacture.

[0116] Figure 4 The manufacturing device S10 shown is a reciprocating sputtering device. The manufacturing device S10 has a loading chamber S11, an unloading chamber S16, and a film forming chamber (vacuum processing chamber) S12. The film forming chamber S12 is connected to the loading chamber S11 through a sealing mechanism S17, and is connected to the unloading chamber S16 through a sealing mechanism S18.

[0117] The loading chamber S11 is provided with a transport mechanism S11 a for transporting the glass substrate 11 brought in from the outside to the film forming chamber S12 , and an exhaust mechanism S11 f such as a rotary pump for roughly evacuating the inside of the loading chamber S11 .

[0118] The unloading chamber S16 is provided with a transport mechanism S16a for transporting the glass substrate 11 after film formation from the film formation chamber S12 to the outside and an exhaust mechanism S16f such as a rotary pump for roughly evacuating the inside of the unloading chamber S16.

[0119] The film forming chamber S12 is provided with a substrate holding mechanism S12 a and three-stage film forming mechanisms S13 , S14 , and S15 as mechanisms for three film forming processes.

[0120] The substrate holding mechanism S12a holds the glass substrate 11 conveyed by the conveying mechanism S11a so that the glass substrate 11 faces the targets S13b, S14b, and S15b during film formation. The substrate holding mechanism S12a can convey the glass substrate 11 from the loading chamber S11 and convey the glass substrate 11 to the unloading chamber S16.

[0121] In the structure of the film forming chamber S12, a film forming mechanism S13 is provided at a position close to the loading chamber S11. The film forming mechanism S13 supplies a film forming material to the first film forming mechanism among three film forming mechanisms S13, S14, and S15.

[0122] The film forming mechanism S13 includes: a cathode electrode (back plate) S13c having a target S13b; and a power supply S13d for applying a sputtering voltage of a negative potential to the back plate S13c.

[0123] The film forming mechanism S13 comprises: a gas introduction mechanism S13e, which is used to introduce gas into the area near the cathode electrode (back plate) S13c in the film forming chamber S12; and a high vacuum exhaust mechanism S13f such as a turbomolecular pump, which is used to perform high vacuum on the area near the cathode electrode (back plate) S13c in the film forming chamber S12.

[0124] Furthermore, a film forming mechanism S14 is provided at an intermediate position between the loading chamber S11 and the unloading chamber S16 of the film forming chamber S12 . The film forming mechanism S14 supplies film forming materials to the second film forming mechanism among the three film forming mechanisms S13 , S14 , and S15 .

[0125] The film forming mechanism S14 includes: a cathode electrode (back plate) S14c having a target S14b; and a power supply S14d for applying a sputtering voltage of a negative potential to the back plate S14c.

[0126] The film forming mechanism S14 comprises: a gas introduction mechanism S14e, which is used to focus on introducing gas into the area near the cathode electrode (back plate) S14c in the film forming chamber S12; and a high vacuum exhaust mechanism S14f such as a turbomolecular pump, which is used to focus on high vacuuming the area near the cathode electrode (back plate) S14c in the film forming chamber S12.

[0127] In addition, in the structure of the film forming chamber S12, a film forming mechanism S15 is provided at a position close to the unloading chamber S16. The film forming mechanism S15 supplies a film forming material to the third film forming mechanism among the three film forming mechanisms S13, S14, and S15.

[0128] The film forming mechanism S15 includes: a cathode electrode (back plate) S15c having a target S15b; and a power supply S15d for applying a sputtering voltage of a negative potential to the back plate S15c.

[0129] The film forming mechanism S15 comprises: a gas introduction mechanism S15e, which is used to focus on introducing gas into the area near the cathode electrode (back plate) S15c in the film forming chamber S12; and a high vacuum exhaust mechanism S15f such as a turbomolecular pump, which is used to focus on high vacuuming the area near the cathode electrode (back plate) S15c in the film forming chamber S12.

[0130] Gas barriers S12g for suppressing gas flow are respectively provided in the areas near the cathode electrodes (back plates) S13c, S14c, and S15c of the film forming chamber S12, so that the gas supplied by the gas introduction mechanisms S13e, S14e, and S15e will not be mixed into the adjacent film forming mechanisms S13, S14, and S15. These gas barriers S12g are constructed so that the substrate holding mechanism S12a can move between the adjacent film forming mechanisms S13, S14, and S15.

[0131] In the film forming chamber S12 , each of the three-stage film forming mechanisms S13 , S14 , and S15 has a composition and conditions required for sequentially forming a film on the glass substrate 11 .

[0132] In the present embodiment, the film forming unit S13 forms the lower anti-reflection layer 12 , the film forming unit S14 forms the light shielding layer 13 , and the film forming unit S15 forms the upper anti-reflection layer 14 .

[0133] Specifically, in the film forming mechanism S13 , the target S13 b is made of a material containing chromium, which is a composition necessary for forming the lower antireflection layer 12 on the glass substrate 11 .

[0134] At the same time, in the film forming mechanism S13, corresponding to the film formation of the lower anti-reflection layer 12, the process gas supplied by the gas introduction mechanism S13e contains carbon, nitrogen, oxygen, etc., and together with the sputtering gas such as argon and nitrogen, the conditions are set to a specified gas partial pressure.

[0135] In addition, according to the film forming conditions, the high vacuum exhaust mechanism S13f is exhausted.

[0136] In addition, in the film forming mechanism S13 , the sputtering voltage applied from the power supply S13 d to the back plate S13 c is set in accordance with the film forming of the lower antireflection layer 12 .

[0137] In the film forming mechanism S14 , the target S14 b is made of a material containing chromium, which is a composition necessary for forming the light shielding layer 13 on the lower antireflection layer 12 .

[0138] At the same time, in the film forming mechanism S14 , corresponding to the film formation of the light shielding layer 13 , the process gas supplied from the gas introduction mechanism S14 e contains carbon, nitrogen, oxygen, etc., and is set to a predetermined gas partial pressure together with a sputtering gas such as argon and nitrogen.

[0139] In addition, according to the film forming conditions, exhaust is performed by the high vacuum exhaust mechanism S14f.

[0140] In addition, in the film forming mechanism S14 , a sputtering voltage applied from the power supply S14 d to the back plate S14 c is set in accordance with the film forming of the light shielding layer 13 .

[0141] In the film forming mechanism S15 , the target S15 b is made of a material containing chromium, which is a component necessary for forming the upper antireflection layer 14 on the light shielding layer 13 .

[0142] At the same time, in the film forming mechanism S15, corresponding to the film formation of the upper anti-reflection layer 14, the process gas supplied from the gas introduction mechanism S15e contains carbon, nitrogen, oxygen, etc., and is conditioned to a specified gas partial pressure together with a sputtering gas such as argon and nitrogen.

[0143] In addition, according to the film forming conditions, the high vacuum exhaust mechanism S15f is exhausted.

[0144] In addition, in the film forming mechanism S15 , a sputtering voltage applied from the power supply S15 d to the back plate S15 c is set in accordance with the film forming of the upper antireflection layer 14 .

[0145] exist Figure 4 In the manufacturing device S10 shown, a glass substrate 11 transported from a loading chamber S11 by a transport mechanism S11a is subjected to three-stage sputtering film formation while being transported by a substrate holding mechanism S12a in a film forming chamber (vacuum processing chamber) S12. Then, the glass substrate 11 on which film formation has been completed is transported out of an unloading chamber S16 by a transport mechanism S16a.

[0146] In the lower anti-reflection layer forming step, in the film forming mechanism S13, the sputtering gas and the reaction gas are supplied from the gas introduction mechanism S13e to the area near the back plate S13c of the film forming chamber S12. In this state, a sputtering voltage is applied to the back plate (cathode electrode) S13c from an external power supply. In addition, a predetermined magnetic field can be formed on the target S13b by a magnetron magnetic circuit.

[0147] In the area near the back plate S13c in the film forming chamber S12, ions of the sputtering gas excited by the plasma collide with the target S13b of the cathode electrode S13c, causing particles of the film forming material to fly out. And, since the flying particles are combined with the reaction gas and then attached to the glass substrate 11, a lower anti-reflection layer 12 with a predetermined composition is formed on the front surface of the glass substrate 11.

[0148] Similarly, in the light shielding layer forming step, in the film forming mechanism S14, the sputtering gas and the reaction gas are supplied from the gas introduction mechanism S14e to the area near the back plate S14c of the film forming chamber S12. In this state, a sputtering voltage is applied to the back plate (cathode electrode) S14c from an external power supply. In addition, a predetermined magnetic field can also be formed on the target S14b by a magnetron magnetic circuit.

[0149] In the area near the back plate S14c in the film forming chamber S12, ions of the sputtering gas excited by the plasma collide with the target S14b of the cathode electrode S14c, causing particles of the film forming material to fly out. Furthermore, since the flying particles are combined with the reaction gas and then adhere to the lower anti-reflection layer 12, a light shielding layer 13 with a predetermined composition is formed on the front surface of the lower anti-reflection layer 12.

[0150] Similarly, in the upper anti-reflection layer forming step, in the film forming mechanism S15, the sputtering gas and the reaction gas are supplied from the gas introduction mechanism S15e to the area near the back plate S15c of the film forming chamber S12. In this state, a sputtering voltage is applied to the back plate (cathode electrode) S15c from an external power supply. In addition, a predetermined magnetic field can also be formed on the target S15b by a magnetron magnetic circuit.

[0151] In the area near the back plate S15c in the film forming chamber S12, ions of the sputtering gas excited by plasma collide with the target S15b of the cathode electrode S15c, causing particles of the film forming material to fly out. And, after the flying particles combine with the reaction gas, they adhere to the light shielding layer 13, thereby forming an upper anti-reflection layer 14 with a predetermined composition on the front surface of the light shielding layer 13.

[0152] At this time, during the film formation of the lower anti-reflection layer 12, nitrogen-containing gas, oxygen-containing gas, carbon-containing gas, sputtering gas, etc. at a specified partial pressure are supplied from the gas introduction mechanism S13e and switched in a manner that controls the partial pressure, thereby setting the composition of the lower anti-reflection layer 12 within a set range.

[0153] In addition, during the film formation of the light-shielding layer 13, nitrogen-containing gas, oxygen-containing gas, carbon-containing gas, sputtering gas, etc. are supplied at a specified partial pressure from the gas introduction mechanism S14e and switched in a manner that controls the partial pressure, thereby setting the composition of the light-shielding layer 13 within a set range.

[0154] At this time, during the film formation of the upper anti-reflection layer 14, nitrogen-containing gas, oxygen-containing gas, carbon-containing gas, sputtering gas, etc. at a specified partial pressure are supplied from the gas introduction mechanism S15e and switched in a manner that controls the partial pressure, thereby setting the composition of the upper anti-reflection layer 14 within a set range.

[0155] Here, examples of the oxygen-containing gas include CO 2 (carbon dioxide), O 2 (oxygen), N 2 O (nitrous oxide), NO (nitrogen monoxide), and CO (carbon monoxide).

[0156] In addition, examples of the carbon-containing gas include CO 2 (carbon dioxide), CH 4 (methane), C 2 H 6 (ethane), and CO (carbon monoxide).

[0157] In the film formation of the lower antireflection layer 12 , the light shielding layer 13 , and the upper antireflection layer 14 , the targets S13 b , S14 b , and S15 b may be replaced as necessary.

[0158] In addition to the formation of the lower anti-reflection layer 12, the light shielding layer 13, and the upper anti-reflection layer 14, other films may be laminated. In this case, the mask blank 10B of the present embodiment is manufactured by sputtering under sputtering conditions of a target, gas, etc. corresponding to the material of the other film, or by laminating the film by other film forming methods.

[0159] Next, the film properties of the lower antireflection layer 12 , the light shielding layer 13 , and the upper antireflection layer 14 in this embodiment will be described.

[0160] First, a chromium compound film as a main component film of the lower anti-reflection layer 12 is formed on the glass substrate 11 for forming a mask by sputtering or the like. The chromium compound film formed at this time is preferably a film containing chromium, oxygen, nitrogen, carbon, etc. By controlling the composition and film thickness of chromium, oxygen, nitrogen, and carbon contained in the film of the lower anti-reflection layer 12, it is possible to form the lower anti-reflection layer 12 having desired optical properties and etching rate. Since the chromium compound has a strong chemical resistance to acid or alkaline solutions and a hydrophobic property, it is suitable to use the chromium compound in the interface in contact with the photoresist.

[0161] Next, a chromium compound film is formed as the light shielding layer 13 by sputtering or the like.

[0162] Here, when the light shielding layer 13 is formed only of a chromium compound film and no other film is present, the reflectivity is high at about 25%. Therefore, it is preferable to form upper and lower antireflection layers 12 and 14 as low reflection layers on the front and back surfaces of the light shielding layer 13 to reduce the reflectivity.

[0163] In this way, by laminating the lower anti-reflection layer 12, the light shielding layer 13 and the upper anti-reflection layer 14, a mask layer having the high optical density (OD5) and the required etching rate required for the photomask 10 can be formed from a material of chromium compound with strong chemical resistance.

[0164] Specifically, Ar, NO, and CO2 can be selected as the gas used in forming the lower anti-reflection layer 12 and the upper anti-reflection layer 14. Here, by setting the ratio of NO:CO2 gas to 1:10 to 10:1, an excellent cross-sectional shape with less upper and lower edges can be obtained. In addition, it can be seen that the reflectivity can be 10% or less for exposure light with a wavelength of 365nm to 436nm, and in particular, the reflectivity can be 5% or less for exposure light with a wavelength of 436nm.

[0165] It is also found that the photomask 10 has a high optical density (OD5) required by setting the film thicknesses of the lower antireflection layer 12, the light shielding layer 13, and the upper antireflection layer 14 to 25.0 nm to 35.0 nm, 125.0 nm to 135.0 nm, and 25.0 nm to 35.0 nm, respectively.

[0166] [Example]

[0167] Next, the composition ratios of the lower antireflection layer 12 , the light shielding layer 13 , and the upper reflection antireflection layer 14 during film formation were verified.

[0168] <Example 1>

[0169] A chromium compound film was formed as a three-layer mask layer on a glass substrate by sputtering.

[0170] When forming the chromium compound film as the light shielding layer, sputtering is performed using nitrogen gas.

[0171] When forming the chromium compound film as the upper and lower antireflection layers, sputtering was performed using nitrogen gas. In addition, CO2 gas and NO gas were selected as oxidizing gases, and the partial pressure of each gas was changed. The gas ratio is shown in Figure 1 .

[0172] [Table 1]

[0173]

[0174] Table 2 shows the film thickness of the lower antireflection layer 12 , the film thickness of the light shielding layer 13 , the film thickness of the upper antireflection layer 14 , and the total film thickness of the mask layer.

[0175] [Table 2]

[0176]

[0177] The changes in the composition ratios of N, O, Cr, and C in the layers of Example 1 were determined by Auger electron spectroscopy. Table 3 shows the results.

[0178] [Table 3]

[0179]

[0180] In addition, the spectral reflectance of the front side (upper antireflection layer side) corresponding to the wavelength in Example 1 is shown in FIG. Figure 5 And Table 4.

[0181] [Table 4]

[0182] Front reflection R%(365nm) R%(405nm) R%(436nm) Example 1 6.5% 4.2% 4.6% Example 2 8.2% 4.5% 3.8% Comparative Example 1 4.6% 2.8% 3.9% Comparative Example 2 5.6% 2.9% 3.3% Comparative Example 3 4.1% 4.5% 7.1%

[0183] Similarly, the spectral reflectance of the back side (glass substrate side) corresponding to the wavelength in Example 1 is Figure 6 And Table 5.

[0184] [Table 5]

[0185] Back reflection R%(365nm) R%(405nm) R%(436nm) Example 1 6.7% 4.7% 4.4% Example 2 8.2% 5.6% 4.6% Comparative Example 1 6.4% 10.7% 15.3% Comparative Example 2 7.9% 5.6% 4.4% Comparative Example 3 5.3% 8.7% 12.6%

[0186] These results show that in Example 1, the reflectance of the front and back surfaces under exposure light with a wavelength of 365 nm to 436 nm is 10% or less, and particularly under exposure light with a wavelength of 436 nm, the reflectance is 5% or less.

[0187] <Example 2>

[0188] A chromium compound film was formed as a three-layer mask layer on a glass substrate by sputtering.

[0189] When forming the chromium compound film as the light shielding layer, sputtering is performed using nitrogen gas.

[0190] When forming the chromium compound films as the upper and lower antireflection layers, sputtering was performed using nitrogen gas. In addition, CO2 gas and NO gas were selected as oxidizing gases, and the partial pressure of each gas was changed. The gas ratio is shown in Table 1.

[0191] Table 2 shows the film thickness of the lower antireflection layer 12 , the film thickness of the light shielding layer 13 , the film thickness of the upper antireflection layer 14 , and the total film thickness of the mask layer.

[0192] The changes in the composition ratios of N, O, Cr, and C in the layers of Example 2 were determined by Auger electron spectroscopy. The results are shown in Table 6.

[0193] [Table 6]

[0194]

[0195] In addition, the spectral reflectance of the front side (upper antireflection layer side) corresponding to the wavelength in Example 2 is shown in FIG. Figure 5 And Table 4.

[0196] Similarly, the spectral reflectance of the back side (glass substrate side) corresponding to the wavelength in Example 2 is shown in Figure 6 And Table 5.

[0197] From these results, it can be seen that in Example 2, the reflectance of the front and back surfaces under exposure light with a wavelength of 365nm to 436nm is less than 10%, and in particular, the reflectance under exposure light with a wavelength of 436nm is less than 5%.

[0198] <Comparative Examples 1 to 3>

[0199] As in the first embodiment described above, a chromium compound film was formed as a three-layer mask layer by sputtering.

[0200] In Comparative Examples 1 and 3, argon and nitrogen were used for sputtering when forming the chromium compound film as the light shielding layer. In Comparative Example 2, nitrogen, argon, and methane were used for sputtering when forming the chromium compound film as the light shielding layer.

[0201] When forming the chromium compound films as the upper and lower antireflection layers, sputtering was performed using nitrogen gas. In addition, CO2 gas and NO gas were selected as oxidizing gases, and the partial pressure of each gas was changed. The gas ratio is shown in Table 1.

[0202] Table 2 shows the film thicknesses of the lower antireflection layer 12 , the light shielding layer 13 , and the upper antireflection layer 14 , and the total film thickness of the mask layer.

[0203] The changes in the composition ratios of N, O, Cr, and C in the layers of Comparative Examples 1 to 3 were determined by Auger electron spectroscopy. The results are shown in Tables 7 to 9.

[0204] [Table 7]

[0205]

[0206] [Table 8]

[0207]

[0208] [Table 9]

[0209]

[0210] In addition, the spectral reflectance of the front side (upper antireflection layer side) corresponding to the wavelength in Comparative Examples 1 to 3 is shown in FIG. Figure 5 And Table 4.

[0211] Similarly, the spectral reflectance of the back side (glass substrate side) corresponding to the wavelength in Comparative Examples 1 to 3 is shown in FIG. Figure 6 And Table 5.

[0212] From these results, it can be seen that the reflectance of the front surface under the exposure light with a wavelength of 365nm to 436nm is 10% or less in Comparative Examples 1 to 3, and the reflectance of the back surface under the exposure light with a wavelength of 365nm to 436nm is 10% or less in Comparative Example 2. However, it can be seen that the reflectance on the back surface is not 10% or less in Comparative Examples 1 and 3.

[0213] According to the purpose of the light shielding layer and the anti-reflection layer, it is necessary to significantly change the gas composition ratio in each layer of the film. Since the light shielding layer has a high optical density (e.g., OD5), it is necessary to reduce the oxidizing gas. In addition, due to the low reflectivity of the anti-reflection layer, it is necessary to absorb a large amount of oxidizing gas into the film. Therefore, the gas composition ratio in the film is increased in the light shielding layer and the anti-reflection layer, resulting in a difference in etching rate.

[0214] Next, the etching shapes during the film formation of the lower antireflection layer 12 , the light shielding layer 13 , and the upper antireflection layer 14 were verified.

[0215] <Example 1>

[0216] The mask blank prepared in Example 1 was patterned (resist coating, exposure, development, etching), and its cross-sectional shape was observed by SEM. The results are shown in Figure 7 In addition, the bird's-eye view of the patterned boundary is shown in Fig.12 .

[0217] also, Figure 7 The magnification is 80,000 times. Fig.12 The magnification is 30,000 times.

[0218] As a result, in Experimental Example 1, the upper eave (the length of the upper anti-reflection layer flying out from the light-shielding layer) is 50nm, and the lower hem (the length of the lower anti-reflection layer flying out from the light-shielding layer) is 59nm.

[0219] <Example 2>

[0220] The mask blank prepared in Example 2 was patterned (resist coating, exposure, development, etching), and its cross-sectional shape was observed by SEM. The results are shown in FIG. Figure 8 In addition, the bird's-eye view of the patterned boundary is shown in Fig.13 .

[0221] also, Figure 8 The magnification is 80,000 times. Fig.13 The magnification is 30,000 times.

[0222] As a result, in Experimental Example 2, the upper eaves (the length of the upper anti-reflection layer flying out from the light-shielding layer) are 57nm, and the lower hem (the length of the lower anti-reflection layer flying out from the light-shielding layer) are 40nm.

[0223] <Comparative Example 1>

[0224] The mask blank was patterned (resist coating, exposure, development, etching) in the same manner as in Example 1, and its cross-sectional shape was observed by SEM. The results are shown in Fig. 9 In addition, the bird's-eye view of the patterned boundary is shown in Fig.14 .

[0225] also, Fig. 9 The magnification is 80,000 times. Fig.14 The magnification is 30,000 times.

[0226] As a result, in Comparative Example 1, the upper eave (the length of the upper anti-reflection layer flying out from the light-shielding layer) is 79nm, and the lower hem (the length of the lower anti-reflection layer flying out from the light-shielding layer) is 145nm.

[0227] <Comparative Example 2>

[0228] The produced mask blank was patterned (resist coating, exposure, development, etching) in the same manner as in Example 1, and its cross-sectional shape was observed by SEM. The results are shown in Fig.10 In addition, the bird's-eye view of the patterned boundary is shown in Fig.15 .

[0229] also, Fig.10 The magnification is 80,000 times. Fig.15 The magnification is 30,000 times.

[0230] As a result, in Comparative Example 2, the upper eaves (the length of the upper anti-reflection layer flying out from the light-shielding layer) are 140nm, and the lower hem (the length of the lower anti-reflection layer flying out from the light-shielding layer) are 52nm.

[0231] <Comparative Example 3>

[0232] The produced mask blank was patterned (resist coating, exposure, development, etching) in the same manner as in Example 1, and its cross-sectional shape was observed by SEM. The results are shown in Fig.11 In addition, the bird's-eye view of the patterned boundary is shown in Fig.16 .

[0233] also, Fig.11 The magnification is 80,000 times. Fig.16 The magnification is 30,000 times.

[0234] As a result, in Comparative Example 3, the upper eaves (the length of the upper anti-reflection layer flying out from the light-shielding layer) are 128nm, and the lower hem (the length of the lower anti-reflection layer flying out from the light-shielding layer) are 154nm.

[0235] Based on these results, it can be confirmed that in Comparative Examples 1 to 3, the anti-reflection layer on the glass layer side (back side) and the anti-reflection layer on the upper side (front side) are both in a protruding shape compared to the light shielding layer (the upper layer is in an eaves shape, and the lower layer is in a hem shape). This is because the etching rate of the anti-reflection layer and the light shielding layer is different.

[0236] It is found that the mask blank of the present invention can form an excellent cross-sectional shape and can manufacture a high-definition photomask.

[0237] Description of Reference Numerals

[0238] 10…Photomask

[0239] 10B...Mask Blank

[0240] 11…Glass substrate (transparent substrate)

[0241] 12…Lower anti-reflection layer

[0242] 12p…Lower anti-reflection pattern

[0243] 13…Light-shielding layer

[0244] 13p…Shading pattern

[0245] 14…Upper anti-reflection layer

[0246] 14p…Upper anti-reflection pattern

Claims

1. A mask blank having a mask layer to be a photomask, wherein: The mask layer has: a lower anti-reflection layer laminated on the transparent substrate; a light shielding layer disposed at a position farther from the transparent substrate than the lower anti-reflection layer; and The upper anti-reflection layer is arranged at a position farther from the transparent substrate than the light shielding layer. The composition ratio of nitrogen, oxygen, chromium and carbon in each of the lower anti-reflection layer, the light shielding layer and the upper anti-reflection layer is determined by Auger electron spectroscopy. The lower anti-reflection layer is an oxynitride carbonization film containing chromium, oxygen, nitrogen and carbon, the content of chromium contained in the lower anti-reflection layer is 34 atomic % to 38 atomic %, the content of oxygen contained in the lower anti-reflection layer is 38 atomic % to 44 atomic %, the content of nitrogen contained in the lower anti-reflection layer is 15 atomic % to 19 atomic %, the content of carbon contained in the lower anti-reflection layer is 4 atomic % to 5 atomic %, The light shielding layer is a nitride film containing chromium and nitrogen. The content of chromium in the light shielding layer is 82 atomic % to 90 atomic %, and the content of nitrogen in the light shielding layer is 5 atomic % to 8 atomic %. The upper anti-reflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen and carbon, the chromium content contained in the upper anti-reflection layer is 25 atomic % to 32 atomic %, the oxygen content contained in the upper anti-reflection layer is 56 atomic % to 67 atomic %, the nitrogen content contained in the upper anti-reflection layer is 5 atomic % to 13 atomic %, the carbon content contained in the upper anti-reflection layer is 2 atomic % to 4 atomic %, The reflectivity of the exposure light with a wavelength of 365nm to 436nm is less than 10% on both sides of the mask layer. The reflectivity of the exposure light with a wavelength of 436 nm is less than 5% on both sides of the mask layer.

2. A mask blank having a mask layer to be a photomask, wherein: The mask layer has: a lower anti-reflection layer laminated on the transparent substrate; a light shielding layer disposed at a position farther from the transparent substrate than the lower anti-reflection layer; and The upper anti-reflection layer is arranged at a position farther from the transparent substrate than the light shielding layer. The composition ratio of nitrogen, oxygen, chromium and carbon in each of the lower anti-reflection layer, the light shielding layer and the upper anti-reflection layer is determined by Auger electron spectroscopy. The lower anti-reflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen and carbon, the content of chromium contained in the lower anti-reflection layer is 32 atomic % to 37 atomic %, the content of oxygen contained in the lower anti-reflection layer is 39 atomic % to 44 atomic %, the content of nitrogen contained in the lower anti-reflection layer is 15 atomic % to 20 atomic %, the content of carbon contained in the lower anti-reflection layer is 3 atomic % to 5 atomic %, The light shielding layer is a nitride carbon film containing chromium, nitrogen and carbon, wherein the content of chromium in the light shielding layer is 78 atomic % to 85 atomic %, the content of nitrogen in the light shielding layer is 5 atomic % to 8 atomic %, and the content of carbon in the light shielding layer is 7 atomic % to 11 atomic %. The upper anti-reflection layer is an oxynitride carbon film containing chromium, oxygen, nitrogen and carbon, the content of chromium contained in the upper anti-reflection layer is 25 atomic % to 30 atomic %, the content of oxygen contained in the upper anti-reflection layer is 55 atomic % to 68 atomic %, the content of nitrogen contained in the upper anti-reflection layer is 5 atomic % to 12 atomic %, the content of carbon contained in the upper anti-reflection layer is 2 atomic % to 4 atomic %, The reflectivity of the exposure light with a wavelength of 365nm to 436nm is less than 10% on both sides of the mask layer. The reflectivity of the exposure light with a wavelength of 436 nm is less than 5% on both sides of the mask layer.

3. The mask blank according to claim 1 or 2, wherein: In the mask layer, the film thickness of the lower antireflection layer, the film thickness of the light shielding layer, and the film thickness of the upper antireflection layer are set so that the optical density is 3.0 or more.

4. The mask blank according to claim 3, wherein: The thickness of the lower anti-reflection layer is 25.0 nm to 35.0 nm. The film thickness of the light shielding layer is 125.0nm to 135.0nm, The upper antireflection layer has a thickness of 25.0 nm to 35.0 nm.

5. The mask blank according to claim 4, wherein: The mask layer has a thickness of 175.0 nm to 205.0 nm.

6. The mask blank according to claim 1, wherein: A photoresist layer is provided, and the photoresist layer is disposed at a position farther from the transparent substrate than the mask layer.

7. A photomask manufactured from the mask blank according to any one of claims 1 to 6.