A macroscopic film with molecular separation properties
By preparing graphene oxide macroscopic films under low energy consumption conditions, we can use its unique properties to achieve efficient separation of miscible mixed solvents, solve the problem of low separation efficiency in the existing technology, and provide a cheap, easy-to-obtain, and stable separation method. solution.
Patent Information
- Application Number
- CN202011448675.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Existing membrane separation technology is not efficient in separating two components with similar molecular sizes, and it is difficult to achieve effective separation of miscible mixed solvents under low energy consumption conditions.
Using graphene oxide as the membrane material, a macro membrane with excellent separation performance was prepared by dispersing it in water and modifying it with inorganic salts, followed by filtration under reduced pressure. The concentration of graphene oxide is 0.05~5mg/mL, the modifier concentration is 0.01~5mol/L, the decompression pressure is 0.01~0.099MPa, and the film thickness is 1~1000μm.
It achieves efficient separation of miscible mixed solvents under low energy consumption conditions, with low cost, simple process, good physical and chemical stability, and shows different penetration behaviors for a variety of solvents, especially in the separation of ethanol-water and ethanol-toluene. It has obvious separation effect in mixed solvents.
Smart Images

Figure CN112657345B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a macro film constructed by nanostructured primitives and capable of separating mutually soluble mixed solvents. Background Art
[0002] Membrane is a functional material that can selectively separate multi-component substances. In recent years, inorganic thin film materials have attracted more and more attention. This is because, first of all, the process of using inorganic thin films to separate mixed components is a typical physical separation process. No chemical additives are required during the separation process, which can not only ensure that the product is not contaminated, but also protect the stability of the structure and properties of the film itself. Secondly, the process of thin film separation generally only needs to be carried out at room temperature, which can not only ensure that the loss of effective ingredients is small, but also the energy consumption required for the separation process is extremely low. Compared with traditional freeze concentration or evaporation concentration, the energy consumption required for membrane separation is only 1 / 3 to 1 / 8 of the former. Thirdly, the process of thin film separation is simple, easy to operate and automatically controlled.
[0003] Based on the many advantages of the above-mentioned membrane separation technology, the membrane separation process has been widely recognized and valued by countries around the world. Especially in today's situation of deteriorating ecological environment, severe shortage of resources and energy, membrane separation technology is even more important. Therefore, how to design and prepare separation membranes with high selectivity, high stability and high flux has become one of the hot topics of research in the 21st century. Some scientists have pointed out that whoever masters membrane technology will master the future of the chemical industry!
[0004] Generally speaking, the principle of membrane separation is based on the molecular size of the separated components and the pore size of the membrane. Molecules smaller than the pore size of the membrane can pass through the membrane, while molecules larger than the pore size of the membrane cannot pass through the membrane, which is the molecular sieve effect. However, it is precisely because of this principle that the membrane separation process also has certain limitations. For example, the separation efficiency is not high for two components with similar molecular sizes. To overcome this defect and further improve the separation performance of the membrane, it is necessary to redesign a new membrane based on different principles.
[0005] As a natural two-dimensional structure, graphene oxide is an ideal structural unit for preparing thin film materials. The various oxygen-containing groups (hydroxyl, carboxyl and epoxy) contained in its sheets and at the edges of the sheets make graphene oxide have relatively active chemical properties, so it is easy to be chemically modified. In addition, the large π system formed by its special six-membered ring structure gives it a high electron cloud density, which is easy to interact with external ions with opposite electrical properties. These unique properties make graphene oxide have excellent potential in the field of thin film separation. Summary of the invention
[0006] The purpose of the present invention is to provide a macro film which can separate mutually soluble mixed solvent molecules under the condition of low energy consumption.
[0007] In order to achieve the above-mentioned purpose, the macroscopic film with molecular separation performance provided by the present invention is prepared by the following method: graphene oxide is dispersed in water to form a graphene oxide dispersion, and then an inorganic salt is used as a modifier to perform cation modification on it, and the cation-modified suspension is filtered under reduced pressure to obtain the macroscopic film.
[0008] In the graphene oxide dispersion, the concentration of graphene oxide is 0.05 to 5 mg / mL, and preferably the concentration of graphene oxide is 0.5 to 1.5 mg / mL.
[0009] The above-mentioned modifier is any one of NaCl, KCl, CaCl2, Ca(NO3)2, MgCl2, MnCl2, and YCl3, and the concentration of the modifier in the dispersion is controlled to be 0.01 to 5 mol / L, preferably the concentration of the modifier in the dispersion is controlled to be 0.1 to 1 mol / L.
[0010] The pressure of the above-mentioned reduced pressure filtration is 0.01 to 0.099 MPa.
[0011] The thickness of the above-mentioned macro film is 1 to 1000 μm.
[0012] The beneficial effects of the present invention are as follows:
[0013] The raw materials used for the macro film of the present invention are cheap and easy to obtain, low in cost, simple in preparation process, low in energy consumption, and its thickness, size and shape can be adjusted by changing the amount of raw materials, the shape and size of the vacuum filtration device, etc., and the adjustment method is simple. The obtained film has good physical and chemical stability, exhibits different permeation behaviors to a variety of common solvents, and the film has excellent separation performance in the separation of mutually soluble mixed solvent molecules, such as having obvious separation effect in the separation of mutually soluble mixed solvents such as ethanol-water and ethanol-toluene, and has good application prospects in separation engineering, sewage treatment and other related fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is Na in Example 1 + Photograph of the modified graphene oxide macrofilm and scanning electron microscope image of its cross section.
[0015] Figure 2 It is a comparison chart of the flux size of the macroscopic films prepared in Examples 1, 4, 7, and 10 for different solvents.
[0016] Figure 3 is Na in Example 1 +Comparison of different permeation fluxes of modified graphene oxide macrofilms to solvents.
[0017] Figure 4 is Ca in Example 4 2+ Comparison of different permeation fluxes of modified graphene oxide macrofilms to solvents.
[0018] Figure 5 Mg in Example 7 2+ Comparison of different permeation fluxes of modified graphene oxide macrofilms to solvents.
[0019] Figure 6 is Y in Example 10 3+ Comparison of different permeation fluxes of modified graphene oxide macrofilms to solvents.
[0020] Figure 7 is Na in Example 1 + Analysis of ethanol content in the original solution and the filtrate before and after the modified graphene oxide macrofilm separated ethanol-water mixed solvent.
[0021] Figure 8 is Na in Example 1 + Analysis of ethanol content in the original solution and the filtrate before and after separation of ethanol-toluene mixed solvent by modified graphene oxide macrofilm. DETAILED DESCRIPTION
[0022] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0023] Example 1
[0024] Weigh 0.25g of solid graphene oxide, add it to a beaker containing 500mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 0.5mg / mL. Measure 80mL of the graphene oxide dispersion, and add NaCl to it under continuous stirring so that the concentration of NaCl in the dispersion is 0.250mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under a pressure of 0.09MPa to obtain Na + Modified graphene oxide macro film (denoted as Na + -GO film).
[0025] Example 2
[0026] Weigh 0.5 g of solid graphene oxide, add it to a beaker containing 500 mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 1.0 mg / mL. Measure 80 mL of the graphene oxide dispersion, and add NaCl to it under continuous stirring so that the concentration of NaCl in the dispersion is 0.250 mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under a pressure of 0.09 MPa to obtain Na + Modified graphene oxide macro film (denoted as Na + -GO film).
[0027] Example 3
[0028] Weigh 1.0 g of solid graphene oxide, add it to a beaker containing 500 mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 2.0 mg / mL. Measure 80 mL of the graphene oxide dispersion, and add NaCl to it under continuous stirring so that the concentration of NaCl in the dispersion is 0.50 mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under a pressure of 0.09 MPa to obtain Na + Modified graphene oxide macro film (denoted as Na + -GO film).
[0029] Example 4
[0030] Weigh 0.25g of solid graphene oxide, add it to a beaker containing 500mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 0.5mg / mL. Measure 80mL of the graphene oxide dispersion, and add CaCl2 thereto under continuous stirring so that the concentration of CaCl2 in the dispersion is 0.250mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under a pressure of 0.09MPa to obtain CaCl2. 2+ Modified graphene oxide macro film (denoted as Ca 2+ -GO).
[0031] Example 5
[0032] Weigh 0.5 g of solid graphene oxide, add it to a beaker containing 500 mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 1.0 mg / mL. Measure 80 mL of the graphene oxide dispersion, and add CaCl2 thereto under continuous stirring so that the concentration of CaCl2 in the dispersion is 0.250 mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under reduced pressure at a pressure of 0.09 MPa to obtain CaCl2. 2+ Modified graphene oxide macro film (denoted as Ca 2 + -GO).
[0033] Example 6
[0034] Weigh 1.0 g of solid graphene oxide, add it to a beaker containing 500 mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 2.0 mg / mL. Measure 80 mL of the graphene oxide dispersion, and add CaCl2 thereto under continuous stirring so that the concentration of CaCl2 in the dispersion is 0.50 mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under reduced pressure at a pressure of 0.09 MPa to obtain CaCl2. 2+ Modified graphene oxide macro film (denoted as Ca 2 + -GO).
[0035] Example 7
[0036] Weigh 0.25g of solid graphene oxide, add it to a beaker containing 500mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 0.5mg / mL. Measure 80mL of the graphene oxide dispersion, and add MgCl2 thereto under continuous stirring so that the concentration of MgCl2 in the dispersion is 0.250mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under a pressure of 0.09MPa to obtain Mg 2+ Modified graphene oxide macro film (denoted as Mg 2 + -GO).
[0037] Example 8
[0038] Weigh 0.5 g of solid graphene oxide, add it to a beaker containing 500 mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 1.0 mg / mL. Measure 80 mL of the graphene oxide dispersion, and add MgCl2 thereto under continuous stirring so that the concentration of MgCl2 in the dispersion is 0.250 mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under a pressure of 0.09 MPa to obtain Mg 2+ Modified graphene oxide macro film (denoted as Mg 2 + -GO).
[0039] Example 9
[0040] Weigh 1.0 g of solid graphene oxide, add it to a beaker containing 500 mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 2.0 mg / mL. Measure 80 mL of the graphene oxide dispersion, and add MgCl2 thereto under continuous stirring to make the concentration of MgCl2 in the dispersion 0.50 mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under reduced pressure at a pressure of 0.09 MPa to obtain Mg 2+Modified graphene oxide macro film (denoted as Mg 2 + -GO).
[0041] Example 10
[0042] Weigh 0.25g of solid graphene oxide, add it to a beaker containing 500mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to make the graphene oxide further uniformly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 0.5mg / mL. Measure 80mL of the graphene oxide dispersion, and add YCl3 thereto under continuous stirring so that the concentration of YCl3 in the dispersion is 0.250mol / L, and then use a KH5200E ultrasonic cleaner to ultrasonicate for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under reduced pressure at a pressure of 0.09MPa to obtain Y 3+ Modified graphene oxide macro film (denoted as Y 3+ -GO).
[0043] Embodiment 11
[0044] Weigh 0.5g of solid graphene oxide, add it to a beaker containing 500mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, ultrasonicate it with a KH5200E ultrasonic cleaner for 0.5 hours to make the graphene oxide further uniformly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 1.0mg / mL. Measure 80mL of the graphene oxide dispersion, and add YCl3 thereto under continuous stirring so that the concentration of YCl3 in the dispersion is 0.250mol / L, and then ultrasonicate it with a KH5200E ultrasonic cleaner for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under reduced pressure at a pressure of 0.09MPa to obtain Y 3+ Modified graphene oxide macro film (denoted as Y 3+ -GO).
[0045] Example 12
[0046] Weigh 1.0 g of solid graphene oxide, add it to a beaker containing 500 mL of deionized water, stir to make the added solid graphene oxide preliminarily dispersed in the water, and after stirring, ultrasonicate it with a KH5200E ultrasonic cleaner for 0.5 hours to make the graphene oxide further evenly dispersed in the water to obtain a graphene oxide dispersion with a concentration of 2.0 mg / mL. Measure 80 mL of the graphene oxide dispersion, and add YCl3 thereto under continuous stirring so that the concentration of YCl3 in the dispersion is 0.50 mol / L, and then ultrasonicate it with a KH5200E ultrasonic cleaner for 0.5 hours to obtain a uniformly dispersed suspension. The obtained suspension is filtered under reduced pressure at a pressure of 0.09 MPa to obtain Y 3+ Modified graphene oxide macro film (denoted as Y 3+ -GO).
[0047] In order to demonstrate the beneficial effects of the present invention, the inventors have conducted various characterizations and performance tests on the macroscopic films prepared in the above embodiments. The specific results are shown in Figures 1 to 6 .Depend on Figure 1 It can be seen that the obtained macroscopic film is a layered structure constructed by GO nanosheets. Figure 2 The results show that methanol, ethanol, propanol and butanol can hardly pass through the macroscopic film, aromatic solvents can pass through the macroscopic film with a certain flux (benzene, toluene, xylene, diphenyl ether, chlorobenzene, bromobenzene), and solvents with lone electron pairs such as acetone, acetonitrile, dichloromethane and ethyl acetate can pass through the macroscopic film unimpeded. Figures 3 to 6 The results also proved Figure 2 The law is that alcohol solvents (methanol, ethanol, propanol, butanol) can hardly penetrate the macroscopic membrane, while aromatic solvents can penetrate the macroscopic membrane with a large flux (benzene, toluene, xylene, diphenyl ether, chlorobenzene, bromobenzene).
[0048] The inventors further used the macroscopic films prepared in Examples 1, 4, 7, and 10 to perform filtration separation experiments on ethanol-water mixed solvents and ethanol-toluene mixed solvents (ethanol volume content is 50%), and analyzed the ethanol content in the original solution and the filtrate before and after separation. Among them, for the ethanol-water mixed solvent, during the separation process, a certain volume of the filtrate was weighed, its density was calculated, and the corresponding ethanol content was obtained by checking the standard curve; for the ethanol-toluene mixed solvent, the original solution before separation and the collected filtrate were subjected to nuclear magnetic resonance hydrogen spectroscopy ( 1 H-NMR) characterization, the results are shown in Figure 7 and Figure 8 .Depend on Figure 7 It can be seen that the ethanol content before separation is 50%, and the density of the filtrate after separation using the macroscopic membrane of Example 1 is 0.9888. The corresponding ethanol content in the filtrate is reduced to 4.5% by checking the standard curve; Figure 8 The results show that the residual ethanol content in the filtrate after separation using the macro film of Example 1 is reduced from 50% before separation to 3.5% in the filtrate. The separation performance of the macro films prepared in Examples 4, 7, and 10 is similar to that of the macro film of Example 1. This indicates that the macro film of the present invention can play a more obvious separation role for the above-mentioned mixed solvent.
Claims
1. Application of a macroscopic film in separating a mixture of an alcohol solvent and an aromatic solvent, characterized in that The macro film is prepared by the following method: dispersing graphene oxide in water to form a graphene oxide dispersion, then using an inorganic salt as a modifier to perform cation modification on the graphene oxide dispersion, and filtering the cation modified suspension under reduced pressure to obtain the macro film; In the graphene oxide dispersion, the concentration of graphene oxide is 0.5 to 1.5 mg / mL; The modifier is any one of NaCl, KCl, CaCl2, Ca(NO3)2, MgCl2, MnCl2, and YCl3, and the concentration of the modifier in the dispersion is controlled to be 0.01 to 5 mol / L; The pressure of the reduced pressure filtration is 0.01 to 0.099 MPa; The thickness of the macro film is 1 to 1000 μm; The alcohol solvent is methanol, ethanol, propanol or butanol; The aromatic solvent is benzene, toluene, xylene, diphenyl ether, chlorobenzene or bromobenzene.
2. The use of the macroscopic film according to claim 1 in separating a mixture of an alcohol solvent and an aromatic solvent, characterized in that: The concentration of the modifier in the dispersion is controlled to be 0.1-1 mol / L.