Halftone Attenuated Phase Shift Blanks and Photomasks for Extreme Ultraviolet Lithography
By designing a halftone attenuated phase shift blank mask with high reflectivity, the problem of poor imaging performance of extreme ultraviolet lithography masks in the prior art is solved, and the log-slope of normalized image and mask error enhancement are improved Factors to achieve better imaging effects.
Patent Information
- Application Number
- CN202011136791.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-02
- Filing Date
- 2020-10-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-10-22
AI Technical Summary
Existing binary masks for extreme ultraviolet lithography are difficult to ensure good normalized image log-slope and mask error enhancement factors when manufacturing semiconductor devices of 10 nanometers or less, resulting in poor imaging performance.
A halftone attenuated phase shift blank mask is designed, including a reflective film, a cover film, a first etching termination film, a phase shifting film, a second etching termination film, an absorbing film and a hard mask arranged in sequence on a transparent substrate. The mold film, the phase shift film has a reflectivity of 20% or greater than 20%, for improving the normalized image log slope and mask error enhancement factors.
By increasing the reflectivity of the phase shift film, the characteristics of normalized image log-slope and mask error enhancement factors during wafer printing are significantly improved, ensuring better imaging performance and process tolerance.
Smart Images

Figure CN112698545B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a phase-shift blank mask and a photomask for extreme ultraviolet (EUV) lithography, and more particularly, to a half-tone attenuated phase-shift blank mask and a photomask for EUV lithography having a high reflectivity of 20% or more relative to an exposure wavelength so as to improve the characteristics of a normalized image log slope (NILS) and a mask error enhancement factor (MEEF) during wafer printing. Background Art
[0002] Recently, lithography technology for manufacturing semiconductors has evolved from ArF, ArFi, and multiple (MP) lithography to EUV lithography technology. EUV lithography is a technology that has attracted attention for manufacturing semiconductor devices of 10 nanometers or less because EUV lithography achieves solution and process simplification by using an exposure wavelength of 13.5 nanometers.
[0003] On the other hand, EUV lithography may not use existing refractive optical systems, such as lithography using KrF or ArF light, because EUV light is well absorbed by all materials and the refractive index of materials at the wavelength is close to 1. For this reason, in EUV lithography, a photomask using a reflective optical system is used.
[0004] The blank mask is a raw material of a photomask, and is constructed to include two thin films on a substrate to form a reflective structure: a reflective film that reflects EUV light and an absorption film that absorbs EUV light. In addition, the blank mask may include a cover film to protect the reflective film, a back-side conductive film for electrostatic clamping (e-chucking), and the like. More specifically, the blank mask for EUV is constructed to include a reflective film made of Mo / Si on a SiO2-TiO2-type low thermal expansion material (LTEM) substrate having a low thermal expansion coefficient, a ruthenium (Ru)-type cover film on the reflective film, and a tantalum (Ta)-type absorption film on the cover film. The photomask formed in this way has a form in which the absorption film is patterned, and uses the principle of forming a pattern on a wafer by using the opposite difference between the reflectivity of the reflective film and the reflectivity of the absorption film.
[0005] On the other hand, in recent years, it has been required to develop a blank mask for EUV for manufacturing a device of 10 nm or less (to be exact, 7 nm or 5 nm or less, and 3 nm or less in the future). Therefore, it is required to develop a blank mask having excellent normalized image logarithmic slope (NILS) and mask error enhancement factor (MEEF) due to the characteristics of the blank mask to EUV. Existing binary masks for extreme ultraviolet lithography have poor imaging performance because it is difficult to ensure a NILS of 2.0 or more when exposing a logic or DRAM device having a pattern with a pitch of 32 nm or less. Summary of the invention
[0006] [Technical issues]
[0007] Therefore, an object of the present disclosure is to provide a halftone attenuated phase-shift blank mask and a photomask for EUV lithography having excellent characteristics of Normalized Image Log Slope (NILS) and Mask Error Enhancement Factor (MEEF).
[0008] Another object of the present disclosure is to provide a halftone attenuated phase-shift blank mask and a photomask for EUV lithography having a high reflectivity of 20% or more and preferably 20% to 60% in a dark area (an area where an absorption film exists).
[0009] [Technical solution]
[0010] According to one aspect of the present disclosure, a halftone attenuated phase-shift blank mask for extreme ultraviolet lithography includes a reflective film, a cover film, a first etch stop film, a phase-shift film, a second etch stop film, and an absorption film sequentially disposed on a transparent substrate.
[0011] The blank mask may further include a hard mask film disposed on the absorption film.
[0012] The first etch stopper film may be made of silicon (Si) alone or a compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), boron (B), and metal is contained in silicon (Si).
[0013] The first etch stopper film may have a thickness of 1 nm to 5 nm.
[0014] The phase shift film may have a reflectivity of 20% or more with respect to the extreme ultraviolet exposure wavelength.
[0015] The phase shift film can be made of ruthenium (Ru) alone, of a compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H) and boron (B) is contained in ruthenium (Ru), or of a compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H) and boron (B) is contained in ruthenium (Ru) and molybdenum (Mo).
[0016] The phase shift film may have a thickness of 10 nanometers to 50 nanometers.
[0017] The second etch stopper film may be made of chromium (Cr), or a chromium (Cr) compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), and boron (B) is contained in chromium (Cr).
[0018] The second etch stopper film may have a thickness of 1 nm to 10 nm.
[0019] The absorption film may be made of tantalum (Ta) or a tantalum (Ta) compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), and boron (B) is contained in tantalum (Ta).
[0020] The absorber film may have a thickness of 10 nanometers to 50 nanometers.
[0021] The hard mask film may be made of chromium (Cr) or a chromium (Cr) compound in which at least one selected from oxygen (O), nitrogen (N), carbon (C), hydrogen (H), and boron (B) is contained in chromium (Cr).
[0022] According to another aspect of the present disclosure, a photomask having the above structure manufactured using a halftone attenuated phase-shift blank mask for extreme ultraviolet lithography is provided.
[0023] [Beneficial effects]
[0024] According to the present disclosure, the blank mask includes a phase shift film having a high reflectivity of 20% or more and preferably 20% to 60%. Therefore, the characteristics of NILS and MEEF are improved during wafer printing. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a cross-sectional view illustrating a half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to the present disclosure.
[0026] Description of Figure Numbers
[0027] 101: LTEM transparent substrate;
[0028] 102: reflective film;
[0029] 104: covering film;
[0030] 106: a first etching stop film;
[0031] 108: Phase shift film;
[0032] 110: second etching stop film;
[0033] 112: Absorption film;
[0034] 114: hard mask film;
[0035] 116: Resist film. DETAILED DESCRIPTION
[0036] Figure 1 is a cross-sectional view illustrating a half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to an embodiment of the present disclosure.
[0037] According to the present disclosure, a half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography has a structure in which a reflective film 102, a cover film 104 containing Ru, a first etch stop film 106, a phase-shift film 108, a second etch stop film 110, an absorption film 112, a hard mask film 114 and a resist film 116 are sequentially stacked on an LTEM transparent substrate 101, and 40 to 60 layers of Mo / Si are stacked in the reflective film 102.
[0038] The first etching stopper film 106 has an etching selectivity of 10 or more with respect to the capping film 104 containing Ru disposed thereunder. The first etching stopper film 106 may be made of silicon (Si) alone or made of a compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), boron (B), and metal is contained in silicon (Si), and is preferably made of a silicon (Si) compound containing at least silicon (Si) and nitrogen (N). The first etching stopper film 106 is etched by a chlorine (Cl)-based etching gas, and when oxygen (O) is contained, since Ru is etched together, it is preferred that the first etching stopper film 106 does not contain oxygen (O). The first etching stopper film 106 has a thickness of 1 nm to 5 nm, and preferably 2 nm to 4 nm. When the first etching stopper film 106 has a thickness of 5 nm or more, the reflectivity of the phase shift pattern in which the final pattern is formed is reduced, and when the first etching stopper film 106 has a thickness of 1 nm or less, it is difficult for the first etching stopper film 106 to function as an etching stopper.
[0039] The phase shift film 108 is made of a material having high transmittance and simple phase shift control with respect to the extreme ultraviolet exposure wavelength. For this purpose, the phase shift film 108 contains ruthenium (Ru) alone or a compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), and boron (B) is contained in ruthenium (Ru), and specifically, preferably contains nitrogen (N) and oxygen (O).
[0040] In addition, the phase shift film 108 contains at least one selected from tantalum (Ta), titanium (Ti), cobalt (Co), indium (In), niobium (Nb), molybdenum (Mo), nickel (Ni), and chromium (Co) contained in ruthenium (Ru) to reduce the shielding effect caused by the thickness, and may be made of a compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), and boron (B) is additionally contained in the material. Specifically, the phase shift film 108 contains molybdenum (Mo) among the materials, and is preferably made of a compound containing at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), and boron (B).
[0041] The phase shift film 108 may be formed in a single layer or in a multi-layer structure of two or more layers, and may be formed in a single layer or in continuous layers.
[0042] The phase shift film 108 has a phase shift amount of 120° to 240°, and preferably has a phase shift amount of 190° to 240° with respect to the extreme ultraviolet exposure wavelength.
[0043] After patterning, the phase shift film 108 has a reflectivity of 20% or more with respect to an exposure wavelength, and preferably has a reflectivity within a range of 20% to 60%.
[0044] The phase shift film 108 has a thickness of 10 to 50 nanometers, and preferably 20 to 40 nanometers.
[0045] The phase shift film 108 is etched by a fluorine (F)-based etching gas.
[0046] The second etch stopper film 110 is disposed on the phase shift film 108 and has an etching selectivity of 10 or more with respect to the formed absorption film 112 containing tantalum (Ta).
[0047] The second etching stopper film 110 may be made of a material etched by a chlorine (Cl)-based gas, and specifically, may be made of chromium (Cr) or a chromium (Cr) compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), and boron (B) is contained in chromium (Cr). The second etching stopper film 110 is preferably formed by including oxygen (O) in chromium (Cr). The second etching stopper film 110 has a thickness of 1 nm to 10 nm, preferably 5 nm or less, and more preferably 4 nm or less.
[0048] The absorption film 112 may be made of tantalum (Ta) or a tantalum (Ta) compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H) and boron (B) is contained in tantalum (Ta), and specifically, preferably made of one of TaN, TaBN, TaON and TaBON. The absorption film 112 has a thickness of 10 to 50 nanometers, preferably 10 to 40 nanometers.
[0049] The hard mask film 114 may be made of chromium (Cr) or a chromium (Cr) compound in which at least one of oxygen (O), nitrogen (N), carbon (C), hydrogen (H), and boron (B) is contained in chromium (Ca), and specifically, preferably made of a compound in which oxygen (O) is contained in at least chromium (Cr).
[0050] The hard mask film 114 has a thickness of 1 nm to 10 nm, and preferably 2 nm to 5 nm.
[0051] The resist film 116 has a thickness of 40 nm to 150 nm.
[0052] The blank mask according to the present disclosure having the above structure is provided with a phase shift film having a high reflectivity of 20% or more and preferably 20% to 60%, so that it is possible to ensure characteristics and process tolerances of NILS, mask error enhancement factor (MEEF), and the like during wafer printing.
[0053] (Example)
[0054] Fabrication of high-transmittance phase-shift blank masks for EUV
[0055] To manufacture a blank mask, a low thermal expansion material (LTEM) substrate 101 having a total indicated reading (TIR) controlled to be 30 nm or less and made of a SiO2-TiO2 assembly having a size of 6 inches×6 inches×0.25 inches is prepared.
[0056] Next, although Figure 1It is not described in the present invention, but a conductive film containing chromium (Cr) as a main component is formed on the rear surface of the LTEM substrate 101 using a DC magnetron reactive sputtering facility. The conductive film has a three-layer structure, each of which is made of CrCON, CrN and CrCON. Specifically, the conductive film uses a chromium (Cr) target, and the first layer made of CrCON adjacent to the rear surface of the substrate is formed with a thickness of 30 nanometers by injecting a gas of Ar:N2:CO2=7sccm:7sccm:7sccm and using a process power of 1.0 kilowatts. Thereafter, a second layer of a CrN film having a thickness of 20 nanometers is formed by injecting a gas of Ar:N2=5sccm:5sccm onto the CrCON film of the first layer and using a process power of 1.0 kilowatts. Subsequently, a third layer of a CrCON film having a thickness of 10 nanometers is formed by injecting a gas of Ar:N2:CO2=7sccm:7sccm:7sccm onto the CrN film of the second layer again and using a process power of 1.4 kilowatts. At this time, since the sheet resistance of the conductive film was measured using a 4-point probe, it was confirmed that there was no problem in the electrostatic clamping using the electrostatic chuck by indicating a sheet resistance value of 55Ω / Y, and the roughness measured in an area of 1 micrometer×1 micrometer using an AFM device was 0.4 nanometers RMS.
[0057] Thereafter, a molybdenum (Mo) layer and a silicon (Si) layer are each alternately formed on the front surface of the LTEM substrate 101 to have a thickness of 4.8 nanometers and a thickness of 2.2 nanometers by using an ion beam deposition low defect density (hereinafter referred to as 'IBD-LDD') device, and thus, a reflective film 102 in which 40 layers of Mo / Si are stacked is formed. Since the reflectivity of the reflective film 102 is measured using an EUV reflectometer, the indicated reflectivity is 67.8% at a wavelength of 13.5 nanometers. Since the surface roughness of the reflective film 102 is measured using an atomic force microscopy (AFM) device, the indicated surface roughness is 0.12 nanometers RMS, and when EUV exposure light is reflected from the reflective film 102, it can be confirmed that less diffuse reflection occurs due to the surface roughness. In addition, since the total indication reading of the reflective film 102 having an area of 142 square millimeters was measured using an ultra-flat device, the indicated TIR value was 54 nanometers, and when the TIR value of the LTEM substrate 101 was considered to be 45 nanometers, it was confirmed that there was minimal distortion of the pattern position due to the reflective film.
[0058] The cover film 104 is formed by stacking a ruthenium (Ru) layer having a thickness of 2.5 nanometers on the reflective film 102 using an IBD LDD device. Since the reflectivity was measured in the same manner as in the reflective film 102 after the cover film 104 was formed, the reflectivity was 65.8% at a wavelength of 13.5 nanometers, thus confirming that there was an extremely small change in the reflectivity compared to the reflectivity value of 67.8% of the reflective film 102. In addition, since the surface roughness and the total indication reading were measured in the same manner, the indicated surface roughness value was 0.13 nanometers RMS, which showed an extremely small change compared to the surface roughness value of the reflective film 102. The TIR value was also 54 nanometers, and therefore, it was confirmed that there was no change.
[0059] The first etch stopper film 106 made of SiN is formed on the capping film 104 to have a thickness of 3.5 nm by using a silicon (Si) target doped with boron (B), injecting a gas of Ar:N2=5 sccm:3 sccm, and using a process power of 0.6 kW.
[0060] The phase shift film 108 was formed on the first etch stopper film 106 to have a thickness of 39 nm by using a Ru target and using 10 sccm of Ar gas and 0.4 kW of process power. Since the reflectivity was measured after the phase shift film 108 was formed, it indicated that the reflectivity was 33.2% at a wavelength of 13.5 nm.
[0061] The second etch stopper film 110 is formed on the phase shift film 108 to have a thickness of 4 nm by using a Cr target, injecting gases of Ar:N2:NO=5 sccm:5 sccm:5 sccm, and using a process power of 0.6 kW.
[0062] The absorption film 112 made of TaN was formed on the second etch stopper film 110 to have a thickness of 30 nm by using a Ta target, injecting a gas of Ar:N2=9 sccm:1 sccm, and a process power of 0.6 kW. Since the reflectivity at 13.5 nm on the absorption film 112 was measured, the reflectivity was indicated to be 1.1%, and it was confirmed that there was no problem in the function of the absorption film.
[0063] The hard mask film 114 is formed on the absorption film 112 to have a thickness of 4 nm by using a Cr target, injecting gases of Ar:N2:NO=5 sccm:3 sccm:5 sccm, and using a process power of 0.6 kW.
[0064] A resist film 116 for electron beam is spin-coated to a thickness of 80 nm on the hard mask film 114 , and thus, a blank mask 100 for EUV is manufactured.
[0065] Above, the present disclosure has been particularly described by the embodiments of the present disclosure, but this is only for the purpose of illustrating and explaining the present disclosure, and is not intended to limit the meaning or scope of the present disclosure described in the claims. Therefore, a person of ordinary skill in the technical field of the present disclosure may understand that various modifications and other equivalent embodiments are possible according to the embodiments. Therefore, the actual technical scope of the present disclosure will be defined by the spirit of the appended claims.
Claims
1. A half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography, comprising: A reflective film, a cover film, a first etching stop film, a phase shift film, a second etching stop film and an absorption film are sequentially disposed on a transparent substrate; wherein the phase shift film has a reflectivity greater than 20% and 20% to 60% relative to an extreme ultraviolet exposure wavelength; wherein the phase shift film is made of ruthenium alone, a compound in which at least one of oxygen, nitrogen, carbon, hydrogen and boron is contained in ruthenium, or a compound in which at least one of oxygen, nitrogen, carbon, hydrogen and boron is contained in ruthenium and molybdenum; and The phase shift film has a thickness of 10 nanometers to 50 nanometers.
2. The half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to claim 1, further comprising: The hard mask film is disposed on the absorption film.
3. The half-tone attenuation type phase-shift blank mask for extreme ultraviolet lithography according to claim 1, wherein the first etch stop film is made of silicon alone or a compound in which at least one of oxygen, nitrogen, carbon, hydrogen, boron and metal is contained in silicon. 4 . The half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to claim 1 , wherein the first etch stop film has a thickness of 1 nm to 5 nm.
5. The half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to claim 1, wherein the second etch stop film is made of chromium or a chromium compound in which at least one of oxygen, nitrogen, carbon, hydrogen and boron is contained in chromium. 6 . The half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to claim 1 , wherein the second etch stop film has a thickness of 1 nm to 10 nm.
7. The half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to claim 1, wherein the absorption film is made of tantalum or a tantalum compound in which at least one of oxygen, nitrogen, carbon, hydrogen and boron is contained in tantalum. 8 . The half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to claim 1 , wherein the absorption film has a thickness of 10 nm to 50 nm.
9. The half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to claim 2, wherein the hard mask film is made of chromium or a chromium compound in which at least one selected from oxygen, nitrogen, carbon, hydrogen, and boron is contained in chromium.
10. A photomask manufactured using the half-tone attenuated phase-shift blank mask for extreme ultraviolet lithography according to any one of claims 1 to 9.