Method for forming thin layer and method for manufacturing nonvolatile memory device using the same

By forming stacked structures with different lattice sizes on the semiconductor substrate and using a buffer layer with a higher hardness than the upper material, the problem of gaps and vacancies at the interface is solved, improving the stability of the stacked structure and the performance of the non-volatile memory device. .

CN112802851BActive Publication Date: 2024-10-18SK HYNIX INC
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202010517797.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-09
Publication Date
2024-10-18
Estimated Expiration
2040-06-09

AI Technical Summary

Technical Problem

In existing semiconductor manufacturing technology, gaps and vacancies are easily generated at the interface in the stacked structure, leading to mechanical instability and potential defects, affecting the uniformity and performance of the thin layer.

Method used

A stacked structure with different lattice sizes is formed on the semiconductor substrate, and a buffer layer with a higher hardness than the upper material is inserted at the interface to reduce tensile stress, improve interface characteristics through buffering, and reduce the generation of voids and vacancies.

Benefits of technology

Through the use of the buffer layer, the deformation and micro-cracks of the laminated structure are reduced, the interface stability and the uniformity of the thin layer are improved, and the performance of the non-volatile memory device is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112802851B_ABST
    Figure CN112802851B_ABST
Patent Text Reader

Abstract

Method for forming a thin layer and method for manufacturing a non-volatile memory device using the same. A method for manufacturing a non-volatile memory device includes forming a gate insulating layer on a semiconductor substrate having a source layer. The method also includes forming a silicon nitride layer having a buffered upper surface on the gate insulating layer, wherein the buffered upper surface of the silicon nitride layer has a higher hardness than the hardness of the silicon nitride layer. The method also includes forming a silicon oxide layer on the buffered upper surface of the silicon nitride layer. The method additionally includes alternately forming additional silicon nitride layers and additional silicon oxide layers on the silicon oxide layer to form a stacked structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Various embodiments may generally relate generally to semiconductor manufacturing technology, and more particularly, to methods of forming thin layers and methods of using the same to manufacture nonvolatile memory devices. Background Art

[0002] The semiconductor device may include a plurality of stacked thin layers. A specific layer of the thin layers may have a bonding characteristic with respect to an upper layer and a lower layer of the specific layer. In addition, the thin layer may have a uniform thickness.

[0003] The thin layer may be used for wiring, electrodes, insulating layers in a specific element, or sacrificial layers for defining a specific area. Summary of the invention

[0004] According to an embodiment of the present disclosure, a method for manufacturing a non-volatile memory device includes: forming a first sacrificial layer on a semiconductor substrate; and forming a second sacrificial layer on the first sacrificial layer to form a sacrificial structure. The method also includes forming an insulating interlayer on the sacrificial structure. The method also includes alternately forming additional sacrificial structures and additional insulating interlayers to form a stacked structure.

[0005] According to an embodiment of the present disclosure, a method for manufacturing a non-volatile memory device includes forming a gate insulating layer on a semiconductor substrate having a source layer. The method also includes forming a silicon nitride layer having a buffered upper surface on the gate insulating layer, wherein the buffered upper surface of the silicon nitride layer has a higher hardness than the hardness of the silicon nitride layer. The method also includes forming a silicon oxide layer on the buffered upper surface of the silicon nitride layer. The method additionally includes alternately forming additional silicon nitride layers and additional silicon oxide layers on the silicon oxide layer to form a stacked structure.

[0006] According to an embodiment of the present disclosure, a method for forming a thin layer includes: forming a first layer having a first lattice size and forming a second layer having a second lattice size on the first layer, the second lattice size being smaller than the first lattice size. The method also includes buffering an upper surface of the second layer to provide the upper surface of the second layer with a hardness higher than that of other parts of the second layer. The method also includes forming a third layer having the first lattice size and the same material as the first layer on the buffered upper surface of the second layer.

[0007] According to an embodiment of the present disclosure, a method for manufacturing a non-volatile memory device includes: forming a sacrificial structure including different layers on a semiconductor substrate; and forming an insulating interlayer on the sacrificial structure. The method also includes alternately forming additional sacrificial structures and additional insulating interlayers to form a stacked structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] The above and other aspects, features, and advantages of the subject matter of the present disclosure will be more clearly understood from the following detailed description taken in conjunction with the accompanying drawings, in which:

[0009] Figure 1 is a cross-sectional view illustrating a thin layer structure according to an example embodiment;

[0010] Figure 2 and Figure 3 is a diagram illustrating a lattice size between thin layers according to an example embodiment;

[0011] Figures 4 to 8 is a cross-sectional view illustrating a method of forming a thin layer according to an example embodiment;

[0012] Fig. 9 is a circuit diagram illustrating a nonvolatile memory device according to an example embodiment;

[0013] Fig.10 is an example Fig. 9 A perspective view of a non-volatile memory device in; and

[0014] Figures 11 to 16 is a cross-sectional view illustrating a method of manufacturing a nonvolatile memory device according to example embodiments. DETAILED DESCRIPTION

[0015] Various embodiments of the present teachings are described in more detail with reference to the accompanying drawings. The accompanying drawings are schematic illustrations of various embodiments (and intermediate structures). As such, variations in the configuration and shape of the examples due to, for example, manufacturing techniques and / or tolerances are contemplated. Therefore, the described embodiments should not be construed as limited to the specific configurations and shapes illustrated herein, but may include deviations in configuration and shape without departing from the spirit and scope of the present teachings as defined in the appended claims.

[0016] The present teaching is described herein with reference to the cross-sectional views and / or plan views of idealized embodiments. However, the embodiments presented should not be construed as limiting the present teaching. Although some embodiments of the present teaching are shown and described, it will be appreciated by those of ordinary skill in the art that these embodiments may be modified without departing from the principles and spirit of the present teaching.

[0017] Figure 1 is a cross-sectional view illustrating a thin layer structure according to example embodiments.

[0018] Reference Figure 1 , the thin layer structure 10 of the example embodiment may include a first layer 12 , a second layer 14 , and a third layer 16 that are sequentially stacked.

[0019] The first layer 12 and the third layer 16 may include substantially the same material. The second layer 14 may include a material different from the material of the first layer 12 and the third layer 16. In addition, the second layer 14 may have a second lattice size different from the first lattice size of the first layer 12 and the third layer 16. For example, the second lattice size of the second layer 14 may be smaller than the first lattice size of the first layer 12 and the third layer 16. The first layer 12 and the third layer 16 may include silicon oxide (SiO 2 The second layer 14 may include silicon nitride (Si 3 N 4 ).

[0020] Figure 2 and Figure 3 is a diagram illustrating a lattice size between thin layers according to example embodiments.

[0021] Reference Figure 2 The first layer 12 including silicon oxide may have a first lattice size. The second layer 14a including silicon nitride may have a second lattice size smaller than the first lattice size.

[0022] For example, when the second layer 14 a may be stacked on the first layer 12 , an upper surface of the first layer 12 and a lower surface of the second layer 14 a may form a bonding interface. Figure 2 B1 in may represent a bonding interface.

[0023] When the second layer 14a having a relatively large lattice size can be formed on the first layer 12 having a relatively small lattice size, the bonder of the first layer 12 can be arranged in a compressive manner to be connected to the bonder of the second layer 14a, so that the bonder of the bonding interface can be arranged mechanically stably. Therefore, no gaps and vacancies are generated at the interface between the first layer 12 and the second layer 14a.

[0024] On the contrary, Figure 3 As shown, when the third layer 16 having the first lattice size may be formed on the second layer 14a having the second lattice size, the bond of the second layer 14a may be expanded to be combined with the bond of the third layer, thereby possibly generating an unstable interface bond between the second layer 14a and the third layer 16. In addition, a tensile stress may be applied to the bonding interface of the second layer 14a to generate a potential defect at the interface B2 between the second layer 14a and the third layer 16. The potential defect may cause a void and a vacancy V. The void and the vacancy V may cause microcracks and cuts to be generated between the second layer 14a and the third layer 16.

[0025] Microcracks and cuts may act as an impediment in providing the second layer 14a with a uniform thickness.

[0026] According to an exemplary embodiment, in order to improve the interface characteristics between the second layer 14a and the third layer 16, as shown in FIG. Figure 1 As shown, the buffer layer 14 b may be interposed between the second layer 14 a and the third layer 16 .

[0027] The buffer layer 14b may include a material having the same etching selectivity relative to the etchant used to etch the second layer 14a and having a hardness greater than the hardness of the second layer 14a. For example, the buffer layer 14b may include a silicon-rich silicon nitride layer. The silicon-rich silicon nitride layer may correspond to a silicon nitride layer having a silicon content higher than the silicon content of the silicon nitride layer in the second layer 14a. In addition, the silicon-rich silicon nitride layer may correspond to a silicon nitride layer containing silicon having a stoichiometric ratio not less than the stoichiometric ratio of an ordinary silicon nitride layer. Alternatively, the buffer layer 14b may include a silicon nitride layer containing impurities such as carbides, boron, etc. For example, the buffer layer 14b may include SiCN, SiBN, SiCBN, etc.

[0028] As described above, when a buffer layer 14b having a hardness greater than that of the second layer 14a can be inserted between the second layer 14a constructed to withstand tensile stress and the third layer 16 configured to withstand compressive stress, although tensile stress can be applied to the buffer layer 14b, the generation of voids or vacancies V can be reduced by the shape maintenance properties of the buffer layer 14b.

[0029] In example embodiments, the buffer layer 14b may include a single layer interposed between the second layer 14a and the third layer 16. However, the buffer layer 14b may be interpreted as an upper surface portion having a different property from that of the second layer 14a. The different property may mean that the hardness of the buffer layer 14b is greater than the hardness of the second layer 14a. Hereinafter, a process of treating the upper surface portion of the second layer 14a to provide a hardness greater than that of the second layer 14a may be referred to as a buffer process.

[0030] Figure 4 and Figure 5 is a cross-sectional view illustrating a method of forming a thin layer according to example embodiments.

[0031] Reference Figure 4, the second layer 14a may be formed on the first layer 12. The second layer 14a may have a second lattice size that is smaller than the first lattice size of the first layer 12. For example, the first layer 12 may include a silicon oxide layer, and the second layer 14a may include a silicon nitride layer. The first layer 12 and the second layer 14a may be formed in the same deposition equipment by an in-situ process. For example, the first layer 12 and the second layer 14a may be formed by a chemical vapor deposition (CVD) process, a plasma enhanced chemical vapor deposition (PECVD) process, an atomic layer deposition (ALD) process, etc. The first layer 12 may be formed by a reaction between a silicon source and an oxygen source. The second layer 14a may be formed by a reaction between a silicon source and a nitrogen source.

[0032] For example, a silicon source and an oxygen source may be supplied to form the first layer 12 having a first target thickness. After forming the first layer 12, the supply of the oxygen source may be stopped. Then, a silicon source and a nitrogen source may be supplied to form the second layer 14a on the first layer 12.

[0033] Reference Figure 5 , after forming the second layer 14a, the supply of the silicon source (Si+) can be increased while maintaining the supply of the nitrogen source to form the buffer layer 14b. When the buffer layer 14b can be interpreted as a separation layer, the second layer 14a can be interpreted as a preliminary second layer 14a. In addition, the sum of the thickness of the preliminary second layer 14a and the thickness of the buffer layer 14b can correspond to the set thickness. Alternatively, the buffer layer 14b can be interpreted as the buffered surface of the second layer 14a.

[0034] Although not shown in the drawings, the third layer 16 may be formed on the buffer layer 14 b or the buffer-treated surface 14 b .

[0035] According to example embodiments, although the etchant may penetrate into the interface, the buffer layer 14b or the buffer-treated surface 14b may have a shape-retaining property through relatively high hardness to reduce interface separation. As a result, generation of defects such as notches and microcracks may be reduced.

[0036] Figures 6 to 8 is a cross-sectional view illustrating a method of forming a thin layer according to example embodiments.

[0037] Reference Figure 6 The silicon source and the nitrogen source may be supplied to the upper surface of the first layer 12 to form a preliminary second layer 14c. The thickness of the preliminary second layer 14c may be about 50% to about 80% of the target thickness of the second layer 14.

[0038] A silicon nitride layer including impurities may be formed on the upper surface of the preliminary second layer 14c to form a buffer layer 14b. The buffer layer 14b may be formed by additionally supplying a silicon source, nitrogen, and an impurity source. The impurity source may include at least one of a carbide source and a boron source. The buffer layer 14b may be formed with the preliminary second layer 14c by an in-situ process. Therefore, the buffer layer 14b may include at least one of SiBN, SiCN, and SiBCN. For example, the sum of the thickness of the preliminary second layer 14c and the thickness of the buffer layer 14b may correspond to the target thickness of the second layer 14. Then, the third layer 16 may be formed on the buffer layer 14b.

[0039] Reference Figure 7 , a second layer 14a may be formed on the first layer 12. Impurities may be implanted into the second layer 14a. The impurities may be activated to form a buffered surface 14b. For example, the impurities may include carbides, boron, etc.

[0040] Reference Figure 8 Instead of implanting impurities to form the buffered surface 14b, the upper surface of the second layer 14a may be treated with a gas containing impurities. The gas may include CF 4 Gas, C 4 F 8 Gas and C 4 F 6 at least one of the gases.

[0041] According to example embodiments, the buffer layer 14b or the buffered surface 14b may play a role in increasing the hardness of the silicon nitride layer. In addition, impurities in the buffer layer 14b or the buffered surface 14b may replace voids or vacancies of the bonding interface to reduce defects such as notches and microcracks caused by voids and vacancies V.

[0042] The method of forming a thin layer may be applied to various semiconductor devices. In example embodiments, the method of forming a thin layer may be applied to a nonvolatile memory device.

[0043] Fig. 9 is a circuit diagram illustrating a nonvolatile memory device according to an example embodiment, and Fig.10 is an example Fig. 9 A three-dimensional diagram of a non-volatile memory device in FIG.

[0044] Reference Fig. 9 , a nonvolatile memory device may include a plurality of strings ST, a plurality of bit lines BL, a plurality of word lines WL, a plurality of drain select lines DSL, a plurality of source select lines SSL, and a common source line CSL. The number of strings ST, bit lines BL, word lines WL, drain select lines DSL, and source select lines SSL may vary according to different types of semiconductor devices.

[0045] The string ST may be connected between the bit line BL and the common source line CSL. In an example embodiment, three strings ST may be connected to the bit line BL. However, the number of strings ST connected to the bit line BL may be changed. Each string ST may include a source select transistor SST, a plurality of memory cells MC, and a drain select transistor DST connected in series to each other. In an example embodiment, eight memory cells MC may be connected in series between a source select transistor SST and a drain select transistor DST. However, the number of source select transistors SST, drain select transistors DST, and memory cells MC connected between the source select transistors SST and the drain select transistors DST may be changed. In an example embodiment, the memory cells MC and the string ST may correspond to a NAND flash memory cell and a NAND string, respectively.

[0046] The source select transistor SST may selectively connect the common source line CSL and the memory cells MC adjacent to the common source line CSL according to a voltage level of the source select line SSL.

[0047] The drain select transistor DST may selectively connect the bit line BL and the memory cells MC adjacent to the bit line BL according to a voltage level of the drain select line DSL.

[0048] The memory cells MC in the string ST may be connected in series between a source selection transistor SST and a drain selection transistor DST. Each of the memory cells MC may be selected in response to a word line WL. The selected memory cell MC may perform a read operation, a program operation, and an erase operation according to the voltages of the word line WL, the source selection line SSL, the drain selection line DSL, the bit line BL, and the common source line CSL.

[0049] Each memory cell MC may be configured to store one or more bits. For example, each memory cell MC may be used as a single-level cell (SLC), a multi-level cell (MCL), or a triple-level cell (TLC).

[0050] Nonvolatile memory devices may be integrated on a semiconductor substrate in a three-dimensional structure.

[0051] Reference Fig.10 , the substrate SUB may include a semiconductor material such as silicon containing p-type impurities. The common source line CSL may be disposed in the substrate SUB. The common source line CSL may be doped with n-type impurities. The common source line CSL may extend in the X direction. The common source lines CSL may be arranged to be spaced apart from each other in the Y direction.

[0052] A plurality of stacked structures STS may be arranged on the substrate SUB. Each stacked structure STS may include conductive layers GE and insulating interlayers ILD that are alternately stacked. The stacked structure STS may be divided by slits. Each stacked structure STS divided by the slits may correspond to one block.

[0053] The conductive layer GE in the stacked structure STS may be used as a source selection line SSL, a word line WL, or a drain selection line DSL. For example, in an example embodiment, the lowermost conductive layer GE may correspond to the source selection line SSL, and the uppermost conductive layer GE may correspond to the drain selection line DSL. The remaining conductive layers GE between the source selection line SSL and the drain selection line DSL may correspond to the word line WL of the memory cell MC.

[0054] A channel column CP may be formed through the stacked structure STS. The channel column CP may be connected to the substrate SUB. The channel column CP may be arranged between adjacent common source lines CSL. The channel column CP may be arranged in a matrix shape along the XY direction. Each channel column CP may have a cylindrical shape extending in the Z direction.

[0055] The channel layer CH and the memory layer ML may be interposed between the channel pillar CP and the stacked structure STS. The channel layer CH may be connected to the channel pillar CP. The memory layer ML may include a tunnel insulating layer Tox, a blocking insulating layer Box, and a data storage layer CTN. The tunnel insulating layer Tox may be in contact with the channel layer CH. The blocking insulating layer Box may be in contact with the stacked structure STS. The data storage layer CTN may be interposed between the tunnel insulating layer Tox and the blocking insulating layer Box.

[0056] A gate insulating layer different from the memory layer ML may be formed between the gate electrode layer GE and the channel pillar CP as the drain select line DSL and / or between the gate electrode layer GE and the channel pillar CP as the source select line SSL.

[0057] A memory cell MC may include a word line WL, a memory layer ML, and a channel layer CH. The word line WL may be configured to surround a channel pillar CP. The memory layer ML and the channel layer CH may correspond to the corresponding word line WL. The source selection transistor SST may include a source selection line SSL, a memory layer ML, and a channel layer CH. The source selection line SSL may be configured to surround a channel pillar CP. The memory layer ML and the channel layer CH may correspond to the corresponding source selection line SSL. The drain selection transistor DST may include a drain selection line DSL, a memory layer ML or a gate insulating layer, and a channel layer CH. The drain selection line DSL may be configured to surround a channel pillar CP. The memory layer ML and the channel layer CH may correspond to the corresponding drain selection line DSL.

[0058] A drain contact DC may be formed on the channel pillar CP. The drain contact DC may include a semiconductor material such as silicon doped with n-type impurities. In example embodiments, the drain contact DC may be located on the channel pillar CP. Alternatively, the drain contact DC may be located on the channel pillar CP and also in the stacked structure STS. A bit line BL extending in the Y direction may be formed on the drain contact DC.

[0059] Figures 11 to 16 is a cross-sectional view illustrating a method of manufacturing a nonvolatile memory device according to example embodiments.

[0060] Reference Fig.11 , the source layer 110 may be formed on the semiconductor substrate 100. The semiconductor substrate 100 may include a silicon substrate doped with p-type impurities. The source layer 110 may include an impurity region in the semiconductor substrate 100. The source layer 110 may be formed by activating n-type impurities. The source layer 110 may include a plurality of linear shapes along the Y direction. The source layer 110 may correspond to Fig. 9 and 10 Then, a gate insulating layer 115 may be formed on the semiconductor substrate 110 having the source layer 110. The gate insulating layer 115 may include a silicon oxide layer.

[0061] Reference Fig.12 , the sacrificial structure 120 may be formed on the gate insulating layer 115. The sacrificial structure 120 may include a main sacrificial layer 120a and a buffer sacrificial layer 120b. Alternatively, the sacrificial structure 120 may include a sacrificial layer 120a having a buffered surface 120b. For example, the main sacrificial layer 120a may be formed on the gate insulating layer 115. The main sacrificial layer 120a may include a silicon nitride layer. The main sacrificial layer 120a may be formed by a CVD process, a PECVD process, an ALD process, a PEALD process, etc.

[0062] The buffer sacrificial layer 120b may be formed on the main sacrificial layer 120a. The buffer sacrificial layer 120b may have the same etching selectivity with respect to an etchant used to etch the main sacrificial layer 120a.

[0063] In addition, the hardness of the buffer sacrificial layer 120b may be higher than that of the main sacrificial layer 120a having the same etching selectivity. For example, the buffer sacrificial layer 120b may include a silicon nitride layer having a silicon concentration richer than that of the main sacrificial layer 120a (hereinafter, a silicon-rich silicon nitride layer). The buffer sacrificial layer 120b including the silicon-rich silicon nitride layer may be formed with the main sacrificial layer 120a through an in-situ process (see Figure 4 ).

[0064] Alternatively, the buffer sacrificial layer 120b may include a silicon nitride layer including impurities, which has a higher hardness than the main sacrificial layer 120a having the same etching selectivity. For example, the impurities may include silicon, carbide, boron, etc. The buffer sacrificial layer 120b including impurities may be formed by additionally supplying an impurity gas when forming the silicon nitride layer (see Figure 6 The buffer sacrificial layer 120b including impurities may be formed by implanting impurities into the silicon nitride layer and then activating the impurities (see Figure 7 The buffer sacrificial layer 120b may be formed by treating the surface of the main sacrificial layer 120a with a fluorine carbide gas (see Figure 8 ).

[0065] Reference Fig.13 The insulating interlayer 125 may be formed on the sacrificial structure 120, specifically, on the buffer sacrificial layer 120b. In example embodiments, the insulating interlayer 125 may include an insulating material having an etch selectivity different from that of the sacrificial structure 120. The insulating interlayer 125 may include a silicon oxide layer.

[0066] Here, the lattice size of the silicon oxide layer may be greater than the lattice size of the silicon nitride layer of the sacrificial structure 120. Therefore, when the sacrificial layer includes the silicon nitride layer and the insulating interlayer 125 including silicon oxide may be formed on the silicon nitride layer, potential defects caused by stress difference may be generated at the interface between the silicon nitride layer and the silicon oxide layer. As a result, voids and vacancies may be generated at the upper surface of the silicon nitride layer and the lower surface of the silicon oxide layer.

[0067] However, according to example embodiments, the sacrificial structure 120 may include a buffer sacrificial layer 120b or a buffer-treated surface 120b on the main sacrificial layer 120a. Therefore, generation of voids and vacancies between the sacrificial layer 120 and the insulating interlayer 125 may be mitigated or suppressed.

[0068] When the hardness of the buffer sacrificial layer 120b may be higher than that of the main sacrificial layer 120a, although lattice distortion may be generated at the bonding interface, the deformation amount of the stacked structure 120 may be reduced due to the shape-maintaining property of the buffer sacrificial layer 120b. In addition, although the etchant may penetrate into the interface between the buffer sacrificial layer 120b and the main sacrificial layer 120a, the buffer sacrificial layer 120b and the main sacrificial layer 120a are not easily separated. As a result, the generation of microcracks and cuts may be reduced.

[0069] Furthermore, when the buffer sacrificial layer 120 b may include an impurity density greater than that of the main sacrificial layer 120 a , the lattice may be narrowed by the impurities, that is, the impurities may replace vacancies to reduce micro cracks and undercuts.

[0070] Reference Fig.14The sacrificial structures 120 and the insulating interlayers 125 may be alternately stacked on the insulating interlayers 125 to form a stacked structure STS. The thickness of the uppermost insulating interlayer 125 a among the insulating interlayers 125 may be greater than the thickness of the other insulating interlayers 125 .

[0071] Reference Fig.15 , a channel pillar CP may be formed in the stack structure STS. The channel pillar CP may be formed in a hole H formed through the stack structure STS. The hole H may be configured to expose the semiconductor substrate 100 between the source layers 110 .

[0072] The hole H may be formed by a plasma dry etching process. In some embodiments, due to the buffer sacrificial layer 120b, the bonding characteristics between the sacrificial structure 120 and the insulating interlayer 125 may be improved. Therefore, the etching gas used to form the hole H may not penetrate into the interface between the sacrificial structure 120 and the insulating interlayer 125 to prevent the notch. As a result, the hole H may have a flat inner surface perpendicular to the surface of the semiconductor substrate 110 without a notch of the interface.

[0073] In addition, forming the channel pillar CP may include forming the memory layer ML and forming the channel layer CH.

[0074] The memory layer ML may be formed on the inner surface of the hole H. As indicated above, since the bonding characteristics between the sacrificial structure 120 and the insulating interlayer 125 may be improved, the hole H may have a uniform inner surface without a cutout or a concave portion. Therefore, the memory layer ML may also be formed on the inner surface of the hole H without an uneven portion.

[0075] Here, forming the memory layer ML may include forming a blocking insulating layer Box. The blocking insulating layer Box may include a silicon oxide layer. The data storage layer CTN may be formed on the blocking insulating layer Box. The data storage layer CTN may include a charge trapping layer, for example, a variable resistance layer including a silicon nitride layer, a silicon layer, a phase change layer, a metal oxide layer, etc. A tunnel insulating layer Tox may be formed on the data storage layer CTN. The thickness of the tunnel insulating layer Tox may be less than the thickness of the blocking insulating layer Box. The tunnel insulating layer Tox may include a silicon oxide layer. The memory layer ML may be planarized until the insulating interlayer 125 may be exposed. The planarized memory layer ML may remain in the hole H.

[0076] The channel layer CH may be formed on the memory layer ML. The channel layer CH may include a polysilicon layer doped with conductive impurities. The channel layer CH may be planarized to be located in the hole H. Since the channel layer CH may be formed on the memory layer ML, the channel layer CH may also not have an uneven portion.

[0077] Forming the channel pillar CP may include forming a core insulation layer 130 and a capping pattern 135 in the hole H.

[0078] The core insulating layer 130 may be formed in the hole H in which the memory layer ML and the channel layer CH may be formed. The core insulating layer 130 may include a perhydropolysilazane inorganic spin-on dielectric (PSZ-SOD) having good gap filling characteristics. The core insulating layer 130 may be planarized to be located in the hole H.

[0079] The core insulation layer 130 may be etched until the height of the core insulation layer 130 is lower than the height of the hole H to form a recessed portion in the hole H. For example, a conductive layer may be formed in the recessed portion to form a capping pattern 135. In example embodiments, the capping pattern 135 may be formed in the recessed portion located in the hole H. Alternatively, the capping pattern 135 may be formed on the core insulation layer 130 without forming the recessed portion.

[0080] Reference Fig.16 , a slit S may be formed through the stack structure STS. The slit S may divide the memory cell array of the nonvolatile memory device into blocks. For example, the width of the slit S may be greater than the width of the hole H. The slit S may be configured to expose the source layer 110 .

[0081] The sidewalls of the insulating interlayers 125 and 125 a and the sacrificial structure 120 may be exposed through the slits S. As shown in FIG.

[0082] An etchant (eg, PH 3 Because the main sacrificial layer 120a and the buffer sacrificial layer 120b in the sacrificial structure 120 may have the same etching selectivity for the etchant, the PH 3 The solution removes the main sacrificial layer 120a and the buffer sacrificial layer 120b at the same etching speed. Therefore, a space may be generated between the insulating interlayers 125 and 125a.

[0083] Since the bonding characteristics between the sacrificial structure 120 and the insulating interlayers 125 and 125 a may be improved, the memory layer ML and the channel layer CH may not penetrate into the sacrificial structure 120 to provide a space having a uniform shape.

[0084] Then, the space may be filled with a conductive material to rearrange the gate lines SSL, WL, and DSL of the memory strings.

[0085] According to example embodiments, a buffer sacrificial layer or a buffered surface may be formed between a main sacrificial layer including a silicon nitride layer and an insulating interlayer including a silicon oxide layer. The buffer sacrificial layer may be interposed between a main sacrificial layer having a relatively large lattice size and an insulating interlayer having a relatively small lattice size to reduce stress applied to the main sacrificial layer. Therefore, no gaps or vacancies are generated between the sacrificial structure and the insulating interlayer.

[0086] Therefore, since there will be no gaps and vacancies between the sacrificial structure and the insulating interlayer, the etchant used to form a hole through the stacked structure will not penetrate into the stacked structure to prevent the generation of the cut. As a result, the sacrificial structure can have a uniform thickness and a uniform shape to provide a word line with a uniform width and thickness.

[0087] The above embodiments are intended to illustrate rather than limit the present teachings. Various alternatives and equivalents are possible. The present teachings are not limited to the embodiments described herein. The present teachings are also not limited to any particular type of semiconductor device. In view of the present disclosure, other additions, reductions or modifications are obvious and are intended to fall within the scope of the appended claims.

[0088] CROSS-REFERENCE TO RELATED APPLICATIONS

[0089] This application claims the benefit of Korean Application No. 10-2019-0145651 filed on November 14, 2019, in the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference.

Claims

1. A method for manufacturing a non-volatile memory device, the method comprising the steps of: forming a first sacrificial layer on a semiconductor substrate; forming a second sacrificial layer on the first sacrificial layer to form a sacrificial structure; forming an insulating interlayer on the sacrificial structure; as well as alternately forming additional sacrificial structures and additional insulating interlayers to form a stacked structure, Wherein, the hardness of the second sacrificial layer is higher than that of the first sacrificial layer.

2. The method according to claim 1, wherein: The first sacrificial layer and the second sacrificial layer have the same etching selectivity with respect to an etchant.

3. The method according to claim 1, wherein: The step of forming the first sacrificial layer and the second sacrificial layer comprises the following steps: supplying a silicon source and a nitrogen source to the chamber for a first time interval to form the first sacrificial layer; and The supply amount of the silicon source is increased while the supply amount of the nitrogen source is maintained for a second time interval to form the second sacrificial layer.

4. The method according to claim 1, wherein: The step of forming the first sacrificial layer includes forming a silicon nitride layer on the semiconductor substrate, and the step of forming the second sacrificial layer includes forming a silicon nitride layer including impurities on the first sacrificial layer.

5. The method according to claim 4, wherein: The impurities include at least one of carbides and boron.

6. The method according to claim 5, wherein: The step of forming the second sacrificial layer comprises: forming a silicon nitride layer on the first sacrificial layer; implanting the impurities into the silicon nitride layer; and The impurities in the silicon nitride layer are activated.

7. The method according to claim 5, wherein: The step of forming the second sacrificial layer comprises: forming a silicon nitride layer on the first sacrificial layer; and The surface of the silicon nitride layer is treated using a gas containing the impurities.

8. The method according to claim 1, further comprising the steps of: etching the stacked structure until the first region of the semiconductor substrate is exposed to form a hole; forming a channel post in the hole; etching the stacked structure until the second region of the semiconductor substrate is exposed to form a slit; as well as The sacrificial structure is selectively removed.

9. A method of manufacturing a non-volatile memory device, the method comprising the steps of: Providing a semiconductor substrate having a source layer; forming a gate insulating layer on the semiconductor substrate; forming a silicon nitride layer having a buffered upper surface on the gate insulating layer; forming a silicon oxide layer on the buffered upper surface of the silicon nitride layer; as well as forming an additional silicon nitride layer and an additional silicon oxide layer alternately on the silicon oxide layer to form a stacked structure, Wherein, the hardness of the buffered upper surface of the silicon nitride layer is higher than the hardness of the silicon nitride layer.

10. The method according to claim 9, wherein: The step of forming the silicon nitride layer having the buffered upper surface comprises the following steps: supplying a silicon source and a nitrogen source to form a preliminary silicon nitride layer; and The content of the silicon source is increased while maintaining the supply amount of the nitrogen source to form the buffered upper surface.

11. The method according to claim 9, wherein: The step of forming the silicon nitride layer having the buffered upper surface comprises the following steps: forming a preliminary silicon nitride layer by a reaction between a silicon source and a nitrogen source; implanting impurities into the upper surface of the preliminary silicon nitride layer; and The impurities in the periphery of the upper surface of the preliminary silicon nitride layer are activated.

12. The method according to claim 11, wherein: The impurities include at least one of carbides and boron.

13. The method according to claim 9, wherein: The step of forming the silicon nitride layer having the buffered upper surface comprises the following steps: reacting a silicon source with a nitrogen source to form a preliminary silicon nitride layer; and The surface of the preliminary silicon nitride layer is treated using a gas containing impurities.

14. The method according to claim 13, wherein: The gas containing impurities includes at least one of CF4 gas, C4F8 gas and C4F6 gas.

15. A method for forming a thin layer, the method comprising the steps of: forming a first layer having a first lattice size; forming a second layer having a second lattice size on the first layer, the second lattice size being smaller than the first lattice size; performing a buffer treatment on the upper surface of the second layer to provide the upper surface of the second layer with a hardness higher than that of other portions of the second layer; as well as A third layer having the first lattice size and made of the same material as that of the first layer is formed on the buffered upper surface of the second layer.

16. The method according to claim 15, wherein: The step of forming the first layer and the third layer includes forming a silicon oxide layer, and wherein the step of forming the second layer includes forming a silicon nitride layer.

17. The method according to claim 15, wherein: The step of buffering the upper surface of the second layer includes implanting at least one of silicon, boron and carbide into the upper surface of the second layer.

18. A method of manufacturing a non-volatile memory device, the method comprising the steps of: forming a sacrificial structure including different layers on a semiconductor substrate; forming an insulating interlayer on the sacrificial structure; as well as alternately forming additional sacrificial structures and additional insulating interlayers to form a stacked structure, The step of forming the sacrificial structure comprises the following steps: forming a sacrificial layer; and A buffer treatment is performed on the surface of the sacrificial layer to change a first material of an upper region of the sacrificial layer into a second material having a higher hardness than the first material.

Citation Information

Patent Citations

  • Method of forming thin films and Method of Manufacturing Non-Volatile Memory Device Using the Same

    KR1020210058330A

  • Fabrication method of splitgate type flash memory

    CN106206596A

  • Semiconductor device and manufacture method for the same

    CN107403729A

  • Three-dimensional memory and forming method thereof

    CN110299366A

  • 3D flash memory device including cell gate patterns having blocking barrier patterns and methods of fabricating the same

    CN112103294A