Test apparatus and test methods for measuring the axial compression properties of composite pipes used in structural engineering
By designing a test device including end plate, semicircular steel bar and strain gauge, combined with a pressurization device controlled by a microcomputer, the edge effect and applicability of the axial compression performance measurement of composite tubes is solved, and the recombination is achieved High-precision measurement of axial compression performance of material pipes and accurate acquisition of nonlinear parameters.
Patent Information
- Application Number
- CN202110114293.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-01-27
AI Technical Summary
The existing axial compression test methods for composite pipes have edge effects, adverse effects on arc shape, and limited applicability, making it difficult to accurately measure the axial compression performance of composite pipes for structural engineering, especially in nonlinear situations, lack of direct measurement methods. and expression.
A test device including upper and lower end plates, semicircular steel bars, axial strain gauge, and circumferential strain gauge was designed. The end of the sample was fixed by adhesive and filled with high-strength gypsum, and the electro-hydraulic servo test was controlled by a microcomputer. The machine performs axial center pressurization, measures the test method of the axial and circumferential strain of the sample, and calculates the linear and nonlinear parameters of the axial compression.
It realizes high-precision measurement of the axial compression performance of composite pipes. It is suitable for composite pipes of different production processes and geometric sizes. It has wide applicability and repeatability, and can accurately obtain axial compression strength, elastic modulus, and loose ratio and nonlinear parameters.
Smart Images

Figure CN112858025B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a structural material performance detection technology in civil engineering, and in particular to a test device and a test method for measuring the axial compression performance of a composite material pipe used in structural engineering. Background Art
[0002] As a new type of material, fiber reinforced polymer (FRP) has excellent properties such as high strength and good corrosion resistance. In recent years, it has been widely used in the field of civil engineering. The most typical application is fiber reinforced composite pipe (hereinafter referred to as: composite pipe) to constrain concrete. Composite pipes can be made by hand using the fiber cloth wet laying method, or they can be directly made by pultrusion or fiber winding. Under the action of axial pressure, the lateral expansion of concrete can be effectively constrained by the fibers arranged close to the annular direction, thereby greatly improving the strength and ductility of the composite component. In addition, the outer composite pipe in the composite component can also be used as a template for pouring concrete. When pouring concrete, it needs to bear a certain construction load. Therefore, composite pipes for structural engineering often need to have a certain axial stiffness. However, since its fibers are mainly arranged close to the annular direction, the composite pipe shows obvious nonlinearity under axial compression. Therefore, for the application research and practice of composite pipes in civil engineering, it is of great significance to accurately measure the axial compression performance of composite pipes, including axial compression linear parameters (axial compression strength, axial compression elastic modulus and Poisson's ratio) and nonlinear parameters. In the test methods for measuring the compression performance of composite materials, in addition to the traditional straight strip sheet compression test, scholars from all over the world have also proposed various test methods, but these existing methods have certain limitations in practical engineering applications.
[0003] The compression test method for straight sheet materials to measure the compression properties of fiber-reinforced composite materials is clearly described in the test specifications of many countries and regions, such as "Standard Test Method for Unsupported Measurement of Compression Properties of Polymer-based Composite Materials Under Shear Load" [ASTM D3410 / D3410M-16(2014)], "Standard Test Method for Compression Properties of Polymer-based Composite Materials Using Combined Load Pressure Test Apparatus" [ASTM D6641 / D6641-16(2016)], "Test Method for In-plane Compression Properties of Fiber-reinforced Plastics" [GB / T5258(2008)], etc. However, the compression test method for straight sheet materials is mainly applicable to continuous unidirectional fiber-reinforced composite flat plates. For composite pipes used in structural engineering, in order to ensure that they have a certain axial stiffness, the winding or laying direction of the fiber often has a certain angle with the horizontal direction. For non-continuous eccentric materials, especially when the eccentricity is relatively large, the fiber material will be cut off at the edge of the sample to form an edge effect, which will make the material performance measured by the test have a large error; on the other hand, for composite pultruded or wound pipes, the sample cut along its axial direction has a certain curvature, and the straight sheet compression test method cannot be applied; for composite pipes made by manual wet laying, although straight sheet samples with the same material and the same layup as the pipe can be made and compression tests can be carried out, due to the difference in curvature between the two and the different production methods, the results of the straight sheet compression test method are difficult to accurately calibrate the actual performance of the composite pipe.
[0004] In order to eliminate the adverse effects of boundary effects and sample arc, the best solution is to directly use a complete pipe section as a sample when measuring the axial compression performance of composite pipes. For example, the Standard Test Method for Transverse Compression Performance of Hoop Wound Polymer Matrix Composite Circular Tubes [ASTM D5449 / D5449M-16 (2016)] and the Test Method for Axial Compression Performance of Fiber Reinforced Thermosetting Plastic Pipes [GB / T 5350-2005] adopt this method. The former is to embed the end of the circular tube into the groove of the end plate, and then axially pressurize the sample through the end plate. However, due to the very narrow groove of the end plate, it is difficult to adapt to the fluctuation of the diameter and wall thickness of the industrially produced fiber-wound pipe, and the test device is difficult to reuse; while the latter is to directly pressurize the sample after reinforcing the end of the tubular sample, but this method is only applicable to composite pipes with a nominal diameter of 50 to 100 mm and a ratio of diameter to reinforcement thickness not greater than 50.
[0005] In addition, there is no directly usable measurement method or expression method at home or abroad for the obvious nonlinearity of the axial direction of composite pipes used in structural engineering under bidirectional stress.
[0006] Therefore, in order to solve the limitations of the existing axial compression test methods for composite tubes, based on the existing technical conditions, a test device and test method for measuring the axial compression performance of composite tubes (including axial compression linear parameters and nonlinear parameters) is proposed, which is simple, feasible, structurally reliable and widely applicable. Summary of the invention
[0007] In view of the technical problems existing in the prior art, the purpose of the present invention is to provide a test device and a test method for measuring the axial compression performance of composite material pipes for structural engineering, which are specially used for high-precision measurement of tubular composite pipes.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] A test device for measuring the axial compression performance of a composite material pipe for structural engineering is characterized in that it includes an upper end plate, a lower end plate, a semicircular steel bar, an axial strain gauge, and annular strain gauge; the upper end plate and the lower end plate have the same structure, both including a circular end plate and a cylindrical protrusion located at the center of the end plate, two semicircular steel bars are fixed to the end plate by adhesive, an annular groove is formed between the two semicircular steel bars and the cylindrical protrusion, the groove is used to accommodate the end of the tubular pressure specimen, and the groove is filled with high-strength gypsum to fix the end of the specimen to the end plate; the axial strain gauge and the annular strain gauge are evenly distributed on the outer surface of the specimen around the circumference of the specimen, and are located in the middle of the specimen.
[0010] As a preferred embodiment, the test device for measuring the axial compression performance of composite material pipes for structural engineering further includes a plurality of steel sheets, which are placed between the ends of the sample and the end plate to ensure that the pipe wall of the sample is perpendicular to the end plate. With this arrangement, the axial center of the sample is guaranteed to be compressed in the later stage.
[0011] As a preference, the outer diameter of the cylindrical protrusion is 10 mm smaller than the nominal diameter of the test specimen.
[0012] As a preferred embodiment, the inner diameter of the semicircular steel bar is 40 mm larger than the nominal diameter of the sample. With this arrangement, the position of the semicircular steel bar is positioned according to the diameter and wall thickness of the tubular sample to adapt to the fluctuation of the sample diameter and the change of the wall thickness.
[0013] As a preferred embodiment, an axial strain gauge arranged along the axial direction and a circumferential strain gauge arranged along the circumferential direction constitute a group of strain gauges; the number of strain gauges is multiple groups, and they are evenly pasted on the outer wall of the sample along the circumference at a position half the height of the sample.
[0014] As a preferred embodiment, the test device for measuring the axial compression performance of the composite material pipe for structural engineering further includes a pressurizing device for axially pressurizing the sample.
[0015] The test method for measuring the axial compression performance of composite material pipes for structural engineering uses a test device for measuring the axial compression performance of composite material pipes for structural engineering, and comprises the following steps:
[0016] a. Sample preparation: Cut the sample from the composite material tube.
[0017] b. Installation of the specimen: Insert the upper end of the specimen into the cylindrical protrusion in the center of the upper end plate and perform preliminary centering; adjust the end face of the specimen along the two vertical radial directions of the specimen using a square ruler, and ensure that the specimen tube wall is perpendicular to the end plate by adding a steel sheet to the end face of the specimen; fix the two semicircular steel bars on the end plate using glue, and temporarily seal the gap between the two semicircular steel bars with tape; prepare high-strength gypsum colloid and fill it into the groove; after the high-strength gypsum in the groove hardens, invert the specimen and install the lower end plate in the same way as the upper end plate.
[0018] c. Loading: The test pressurizing equipment adopts a microcomputer-controlled electro-hydraulic servo testing machine. The tonnage is selected so that the load applied to the specimen falls within the range of 10% to 90% of the full load (try to fall on the full load side), and should not be less than 4% of the maximum tonnage of the testing machine; the specimen is pressurized uniformly, and the pressurization speed is an increase of 0.06% per minute in the axial strain of the specimen, and the loading process ensures that the upper and lower end plates are parallel.
[0019] d. Data selection and calculation: Select the test data of the axial strain range specified in the test process, and calculate the axial compression linear parameters and nonlinear parameters of the composite material tube.
[0020] As a preferred embodiment, in step a, the samples are taken from the same batch of composite material pipes used in the test or actual engineering, and the total number of samples is not less than 5; the ends of the samples are polished to smooth out the tumors or protrusions on the pipe wall.
[0021] Preferably, in step d, the axial compression linear parameters include axial compression strength, axial compression elastic modulus and Poisson's ratio, and the nonlinear parameters include axial compression secant modulus and axis compression secant Poisson's ratio.
[0022] As a preferred embodiment, the calculation process is:
[0023] The axial compressive strength of the specimen is calculated according to formula (1):
[0024]
[0025] Where:
[0026] P c ——Axial compressive strength of the specimen (MPa);
[0027] F c,max——maximum axial compressive load of the specimen (N);
[0028] d——average inner diameter of the sample (mm);
[0029] t——average thickness of the specimen (mm);
[0030] The axial stress of the specimen is calculated according to formula (2):
[0031]
[0032] Where:
[0033] σ x ——Axial stress of the specimen (MPa);
[0034] F c ——axial compressive load of the specimen (N);
[0035] The axial compressive elastic modulus is calculated according to formula (3):
[0036]
[0037] Where:
[0038] E x ——Axial compressive elastic modulus of the specimen (MPa);
[0039] Δε x - The average axial strain increment within the elastic range of the specimen should be at least 0.2%, preferably in the range of 0.1% to 0.3% of the average axial strain;
[0040] Δσ x ——with the average axial strain increment Δε x The corresponding average axial stress increment (MPa);
[0041] The Poisson's ratio of the sample is calculated according to formula (4):
[0042]
[0043] Where:
[0044] ν xθ ——Poisson’s ratio of axial compression of the specimen;
[0045] Δε θ ——with the average axial strain increment Δε x The corresponding average hoop strain increment;
[0046] The strain energy density of the sample under axial compression is calculated according to formula (5):
[0047]
[0048] Where:
[0049] ε x,i ——The i-th average axial strain of the specimen, starting from a value greater than or equal to 0.01% and ending at the point of maximum axial compressive load;
[0050] σ x,i ——with ε x,i The corresponding i-th axial stress (MPa);
[0051] U i ——with ε x,i The corresponding i-th axial compressive strain energy density (MPa);
[0052] The axial compression secant modulus of the specimen is calculated according to formula (6):
[0053]
[0054] Where:
[0055] E x,sec,i ——with ε x,i The corresponding i-th axial compression secant modulus;
[0056] The axial compression secant Poisson's ratio of the specimen is calculated according to formula (7):
[0057]
[0058] Where:
[0059] ν xθ,sec,i ——with ε x,i The corresponding Poisson's ratio of the i-th axial compression secant;
[0060] ε θ,i ——with ε x,i The corresponding i-th average hoop strain;
[0061] According to the calculation results, the axial compressive strain energy density and the axial secant modulus U are plotted respectively. i ~E x,sec,i and axial compressive strain energy density ~ axial secant Poisson's ratio U i ~v xθ,sec,i Data points;
[0062] The data points obtained by fitting the least square method are expressed by the axial secant modulus of the composite material tube under the composite stress state, that is, under the biaxial stress state or triaxial stress state, expressed by the strain energy density of the composite material tube using formula (8):
[0063]
[0064] Where:
[0065] E x,sec ——Axial secant modulus of the composite material pipe under bidirectional stress (MPa);
[0066] A, B, C - nonlinear coefficients of axial secant modulus obtained by fitting the experimental axial compression strain energy density ~ secant modulus data;
[0067] U * ——Axial compressive strain energy density of the axial compression specimen at maximum load (MPa);
[0068] ——Axial tangent modulus of the axial compression specimen at maximum load (MPa);
[0069] D, F——U>U * The nonlinear parameters of the rear axial secant modulus are calculated using equations (9) and (10) respectively:
[0070]
[0071] Under the composite material tube composite stress state, the axial Poisson's ratio expressed by the strain energy density is expressed by formula (11):
[0072]
[0073] Where:
[0074] ν xθ,sec ——Axial Poisson’s ratio of the composite material pipe under bidirectional stress;
[0075] a, b, c——axial secant Poisson's ratio nonlinear coefficients obtained by fitting the experimental axial compression strain energy density ~ secant Poisson's ratio data;
[0076] ——Axial tangent Poisson’s ratio of the axial compression specimen at maximum load;
[0077] k, f——for U>U * The nonlinear parameters of the rear axial secant Poisson's ratio are calculated using equations (12) and (13) respectively:
[0078]
[0079] For composite pipes used in structural engineering, the shear deformation of the composite pipe is usually ignored. The composite pipe is in axial compression and circumferential tension, and is considered to be in a biaxial stress state. Therefore, the strain energy density of the composite pipe in the biaxial stress state is calculated using formula (14):
[0080]
[0081] Where:
[0082] σ x , ε x ——Axial stress (MPa) and strain of the composite material pipe under biaxial stress state; σ θ , ε θ ——respectively are the hoop stress (MPa) and strain of the composite material pipe under biaxial stress state;
[0083] Therefore, the strain energy density of the biaxially stressed composite pipe at any time is obtained, formula (14), that is, the axial secant modulus E considering the nonlinearity of the composite pipe under the current stress state is obtained through formulas (8) to (13): x,sec and the axial secant Poisson's ratio ν xθ,sec .
[0084] The present invention has the following advantages:
[0085] 1. The present invention adopts a simple test device, which can accurately measure the axial compressive performance of the composite pipe, including axial compression linear parameters (axial compression strength, axial elastic modulus, axial Poisson's ratio) and nonlinear parameters (axial compression secant modulus, axis compression secant Poisson's ratio).
[0086] 2. The axial pressure device designed by the present invention embeds the end of the tubular sample into the groove of the end plate and fills it with high-strength gypsum to reinforce the end of the sample. The groove of the end plate has a certain degree of adjustment to adapt to the fluctuation of the diameter and wall thickness of the composite pipe.
[0087] 3. The wide applicability of the present invention is mainly reflected in the following three aspects: (1) In addition to typical composite pultrusion and winding tubes, all composite tubes handmade by wet laying can be applied to this method; (2) There is a high degree of acceptance for the discrete level of the measured composite tube geometric dimensions (diameter and thickness); (3) It is applicable to composite tubes with any fiber winding or laying angle.
[0088] 4. Axial pressurization of composite pipes can be achieved.
[0089] 5. The test device is easy to operate, simple in structure and can be reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0090] Figure 1 is a side view of the specimen.
[0091] Figure 2 It is a schematic diagram of the arrangement of strain gauges on the specimen.
[0092] Figure 3a is a side view of the upper and lower end plates.
[0093] Figure 3b is a top view of the upper and lower end plates.
[0094] Figure 3c It is a three-dimensional diagram of the upper end plate and the lower end plate.
[0095] Figure 4a It is a side view of two semicircular steel bars.
[0096] Figure 4b It is a top view of two semicircular steel bars.
[0097] Figure 4c It is a three-dimensional image of two semicircular steel bars.
[0098] Figure 5 This is a three-dimensional picture of the semicircular steel bars after installation.
[0099] Figure 6a-6d It is the installation diagram of the test device.
[0100] Figure 7 It is a three-dimensional diagram of the test device.
[0101] Figure 8 is the axial stress-strain curve of the test;
[0102] Fig. 9 is the experimental strain energy density-axial modulus and Poisson's ratio diagram.
[0103] Among them, 1 is the upper end plate, 2 is the lower end plate, 3 is the cylindrical protrusion, 4 is the semicircular steel bar, 5 is the test specimen, 6 is the axial strain gauge, and 7 is the annular strain gauge. DETAILED DESCRIPTION
[0104] The present invention will be further described in detail below in conjunction with specific implementation methods.
[0105] The test device for measuring the axial compression performance of composite material pipes for structural engineering includes an upper end plate, a lower end plate, a semicircular steel bar, an axial strain gauge, and a circumferential strain gauge. The upper end plate and the lower end plate have the same structure, both including a circular end plate and a cylindrical protrusion located in the center of the end plate, two semicircular steel bars are fixed on the end plate by adhesive, and form an annular groove with the cylindrical protrusion in the center of the end plate, wherein the position of the semicircular steel bar is positioned according to the diameter and wall thickness of the tubular sample to adapt to the fluctuation of the diameter and the change of the wall thickness of the sample; the compression sample is tubular, and its polished ends are respectively placed in the grooves of the upper and lower end plates, and the sample is fixed on the upper and lower end plates by filling a high-strength gypsum colloid material in the grooves; the upper and lower end plates that are finally fixed must be perpendicular to the axis of the sample to ensure that the axial center of the sample is compressed in the later stage; multiple groups of strain gauges are evenly attached to the middle of the outer wall of the sample, and each group of strain gauges includes an axially arranged strain gauge and a circumferentially arranged strain gauge to measure the axial strain and circumferential strain of the sample during compression.
[0106] The following is a detailed description:
[0107] 1 sample
[0108] 1.1 Sample type
[0109] The specimens shall be taken from the same batch of composite pipes used in the test or in the actual project, and the total number of specimens shall not be less than 5. The ends of the specimens shall be polished to smooth out the lumps or protrusions on the pipe wall. For specimen types, see Figure 1 D is the outer diameter of the sample; d is the inner diameter of the sample; H is the height of the sample; and t is the thickness of the sample.
[0110] 1.2 Sample size
[0111] The sample height H = 2 × fixed end height l + sample effective height L, where the sample effective height L is equal to 100mm, and the fixed end height l of the sample: when the diameter d is less than or equal to 200mm, l ≥ 20mm; when the diameter d is greater than 200mm and less than or equal to 400, l ≥ 30mm; when the diameter d is greater than 400mm and less than or equal to 600, l ≥ 40mm; when the diameter d is greater than 600mm, l ≥ 50mm.
[0112] 1.3 Requirements for the end face of the specimen
[0113] The end faces of the specimen should be flat, without delamination, tearing, etc., and the rest of the surface should be free of damage. The two end faces of the specimen should be as parallel as possible and perpendicular to the axis of the specimen, and the parallelism should not exceed 0.1mm.
[0114] 1.4 Pasting of sample strain gauge
[0115] like Figure 2 As shown, 4-8 groups of strain gauges are evenly pasted along the outer surface of the cross section at half the height of the specimen. If the diameter of the specimen is large, the number of strain gauges can be appropriately increased. Each group of strain gauges includes two unidirectional strain gauges, one arranged along the axial direction of the specimen and the other arranged along the circumferential direction. Strain gauges with a gauge length of 5mm to 20mm are preferably used.
[0116] 1.5 Number of samples
[0117] Each group of mechanical properties specimens shall not be less than 5, and there shall be 5 valid specimens in the same batch. The physical properties specimens shall comply with the requirements of the relevant standards.
[0118] 2 Test conditions
[0119] 2.1 Test environment conditions
[0120] 2.2.1 Laboratory standard environmental conditions
[0121] Temperature: (23±2)℃; Relative humidity: (50±10)%.
[0122] 2.2.2 Non-standard laboratory environmental conditions
[0123] If the laboratory standard environmental conditions are not available, select laboratory environmental conditions that are close to the laboratory standard environmental conditions.
[0124] 2.2 Test status adjustment
[0125] If conditions permit, place the device in an environment with a temperature of (23±2)℃ for at least 4 hours and conduct the test in the same environment. If conditions do not permit, conduct the test at the laboratory ambient temperature.
[0126] 3. Devices and equipment
[0127] 3.1 Test apparatus
[0128] The test device of the composite tube axial compression test method consists of upper and lower steel end plates and four semicircular steel bars, such as Figure 3a-3c , 4a-4c, 5 as shown.
[0129] 3.1.1 Upper and lower end plates
[0130] 3.1.1.1 The end plate of the test device is circular, with a cylindrical protrusion at the center. Figure 3a-3c The surface of the end plate should be flat and smooth.
[0131] 3.1.1.2 The diameter D1 of the end plate is (the outer diameter of the composite tube D+20) mm, and the diameter D2 of the cylindrical protrusion in the center of the end plate is (the inner diameter of the composite tube d-5) mm; the height h1 of the end plate (excluding the thickness of the cylindrical protrusion) is 10-20 mm, and the height h2 of the cylindrical protrusion is equal to the fixed end length l of the specimen.
[0132] 3.1.2 Semicircular steel bars
[0133] 3.1.2.1 Every two semicircular steel bars form a set, which can form a circle with two gaps, such as Figure 4a-4c shown.
[0134] 3.1.2.2 The diameter D3 of the circle formed by the two semicircular steel bars is (composite tube outer diameter D+5) mm, and the notch width b is 2-5 mm. The thickness t1 of the steel bar is 10 mm, and the height h3 is the same as the fixed end height l of the specimen.
[0135] 3.1.3 After the end plate and the two semicircular steel bars are assembled, the width B of the groove formed by the cylindrical protrusion in the center of the end plate and the semicircular steel bar is (composite tube thickness t+5) mm, which allows the end of the specimen to be stuck in the groove. Figure 5 As shown. The groove is filled with high-strength gypsum material to serve as the anchoring end when the specimen is axially loaded.
[0136] 3.2 Installation of test equipment
[0137] 3.2.1 Insert the upper end of the specimen into the cylindrical protrusion in the center of the upper end plate and align it initially. Figure 6a The end face of the specimen is adjusted along two perpendicular radial directions of the specimen by using a square ruler, and a small steel sheet is added to the end face of the specimen to ensure that the specimen tube wall and the end plate remain perpendicular, as shown in the figure. Figure 6b and 6c shown.
[0138] 3.2.2 Fix the two semicircular steel bars to the end plate by gluing, such as Figure 6d As shown, the gap between the two steel bars can be temporarily sealed with tape.
[0139] 3.2.3 Prepare high-strength gypsum colloid and fill it into the groove.
[0140] 3.2.4 After the plaster in the groove of the upper end plate has hardened, turn the specimen over and install the lower end plate in the same way as in 3.2.1 to 3.2.3 of the upper end plate. Figure 7 shown.
[0141] 3.3 Test equipment
[0142] The pressurizing equipment for the test should be a microcomputer-controlled electro-hydraulic servo testing machine. The tonnage should be selected so that the load applied to the specimen falls within the range of 10% to 90% of the full load (try to fall on the full load side) and should not be less than 4% of the maximum tonnage of the testing machine.
[0143] 3.4 Loading Speed
[0144] The axial loading rate was such that the axial strain of the specimen increased by 0.06% per minute.
[0145] 3.5 Alignment of the specimen
[0146] To ensure the axial pressure of the specimen, the specimen needs to be aligned and debugged before the formal loading begins. The specimen is initially loaded until the axial strain reaches about 0.02%, and the error value in the axial strain of the symmetrical arrangement is judged to be no more than 10% of the average value of the two, which means that the specimen alignment requirements are met. Otherwise, the position of the specimen needs to be adjusted until the alignment requirements are met.
[0147] 4 Test steps
[0148] 4.1 The specimens shall be prepared in accordance with the provisions of 1.1, 1.2, 1.3 and 1.4.
[0149] 4.2 The specimens shall be inspected visually. Any specimens with defects or not meeting the size and preparation requirements shall be discarded.
[0150] 4.3 Number the qualified samples and measure the sample dimensions. Measure the inner diameter, outer diameter and thickness of the sample respectively, with an accuracy of 0.01mm. On the two end faces of the sample, measure the outer diameter in two directions perpendicular to each other, and take the average value as the average outer diameter. Measure the wall thickness at eight equally spaced points on any end face of the sample, discard the maximum and minimum values, and take the average value of the remaining points as the average wall thickness. The wall thickness of the sample is the average of the average wall thickness of the two end faces.
[0151] 4.4 The specimen state shall be adjusted in accordance with the provisions of 2.2.
[0152] 4.5 The installation of the specimen shall be in accordance with the provisions of 3.2.
[0153] 4.6 The loading speed shall be in accordance with the provisions of 3.4, and the pressure shall be applied uniformly and continuously until the specimen fails.
[0154] 4.7 The specimen alignment requirements shall be in accordance with the provisions of 3.5.
[0155] 4.8 During the test, the data that needs to be collected and stored include: load, specimen strain and pressurization time.
[0156] 5 Calculation of linear axial performance parameters of composite tubes
[0157] 5.1 Figure 8 The figure shows the full-process axial stress-strain curve of the axial compression performance test of a typical composite pipe for structural engineering. The end point of the curve is when the axial load reaches the maximum value. Compression is defined as positive and tension is defined as negative.
[0158] 5.2 Calculate the axial compressive strength of the specimen according to formula (1):
[0159]
[0160] Where:
[0161] P c ——Axial compressive strength of the specimen (MPa);
[0162] F c,max ——maximum axial compressive load of the specimen (N);
[0163] d——average inner diameter of the sample (mm);
[0164] t——average thickness of the specimen (mm).
[0165] 5.3 Calculate the axial stress of the specimen according to formula (2):
[0166]
[0167] Where:
[0168] σx ——Axial stress of the specimen (MPa);
[0169] F c ——axial compressive load of the specimen (N);
[0170] 5.4 Calculate the axial compressive elastic modulus according to formula (3):
[0171]
[0172] Where:
[0173] E x ——Axial compressive elastic modulus of the specimen (MPa);
[0174] Δε x ——The average axial strain increment within the elastic range of the specimen, such as Figure 8 As shown, it should be at least 0.2%, and it is recommended to select the average axial strain range of 0.1% to 0.3%;
[0175] Δσ x ——with the average axial strain increment Δε x The corresponding average axial stress increment (MPa).
[0176] 5.5 Calculate the Poisson's ratio of the sample according to formula (4):
[0177]
[0178] Where:
[0179] ν xθ ——Poisson’s ratio of axial compression of the specimen;
[0180] Δε θ ——with the average axial strain increment Δε x The corresponding average hoop strain increment.
[0181] 6 Nonlinear axial properties of composite tubes under biaxial loading
[0182] The nonlinear axial performance parameters of the composite tube are expressed by the strain energy density based on Jones and Nelson's model.
[0183] 6.1 Calculate the strain energy density of the specimen under axial compression according to formula (5):
[0184]
[0185] Where:
[0186] ε x,i ——The i-th average axial strain of the specimen, starting from a value greater than or equal to 0.01% and ending at the maximum load point;
[0187] σ x,i ——with ε x,i The corresponding i-th axial stress (MPa);
[0188] U i ——with ε x,i Corresponding ith axial compressive strain energy density (MPa).
[0189] 6.2 Calculate the axial compression secant modulus of the specimen according to formula (6):
[0190]
[0191] Where:
[0192] E x,sec,i ——with ε x,i The corresponding i-th axial compression secant modulus.
[0193] 6.3 Calculate the axial compression secant Poisson's ratio of the specimen according to formula (7):
[0194]
[0195] Where:
[0196] ν xθ,sec,i ——with ε x,i The corresponding Poisson's ratio of the i-th axial compression secant;
[0197] ε θ,i ——with ε x,i The corresponding i-th average hoop strain.
[0198] 6.4 Based on the calculation results of 6.1, 6.2 and 6.3, the axial compressive strain energy density and axial secant modulus (U i ~E x,sec,i ) and axial compressive strain energy density ~ axial secant Poisson's ratio (U i ~v xθ,sec,i ) data points, such as Fig. 9 as shown in .
[0199] 6.5 As Fig. 9 As shown, by fitting the data points obtained in 6.4 by the least square method, the axial secant modulus expressed by the strain energy density of the composite tube under the composite stress state (biaxial stress or triaxial stress) is expressed by formula (8):
[0200]
[0201] Where:
[0202] E x,sec——Axial secant modulus of the composite pipe under bidirectional stress (MPa);
[0203] A, B, C - nonlinear coefficients of axial secant modulus obtained by fitting the experimental axial compression strain energy density ~ secant modulus data;
[0204] U * ——Axial compressive strain energy density of the axial compression specimen at maximum load (MPa);
[0205] ——Axial tangent modulus of the axial compression specimen at maximum load (MPa);
[0206] D, F——U>U * The nonlinear parameters of the rear axial secant modulus are calculated using equations (9) and (10) respectively:
[0207]
[0208] Under the composite stress state of the composite tube, the axial Poisson's ratio expressed by the strain energy density is expressed by formula (11):
[0209]
[0210] Where:
[0211] ν xθ,sec ——Axial Poisson's ratio of composite pipes for structural engineering under bidirectional load conditions;
[0212] a, b, c——axial secant Poisson's ratio nonlinear coefficients obtained by fitting the experimental axial compression strain energy density ~ secant Poisson's ratio data;
[0213] ——Axial tangent Poisson’s ratio of the axial compression specimen at maximum load;
[0214] k, f——for U>U * The nonlinear coefficient of the rear axial secant Poisson's ratio is calculated using equations (12) and (13) respectively:
[0215]
[0216] For composite pipes used in structural engineering, their shear deformation is usually ignored. They are in axial compression and circumferential tension, and can be considered to be in a biaxial stress state. Therefore, the strain energy density of the composite pipe in the biaxial stress state is calculated using formula (14):
[0217]
[0218] Where:
[0219] σ x , εx ——Axial stress (MPa) and strain of the composite pipe under biaxial stress state;
[0220] σ θ , ε θ ——respectively are the hoop stress (MPa) and strain of the composite pipe under bidirectional stress state.
[0221] Therefore, we have the strain energy density of the biaxially stressed composite pipe at any time, formula (14), and can obtain the axial secant modulus E of the composite pipe considering the nonlinearity of the composite pipe under the current stress state through formulas (8) to (13): x,sec and the axial secant Poisson's ratio ν xθ,sec .
[0222] 7 Test results
[0223] The arithmetic mean, standard deviation, coefficient of dispersion, etc. of the test results such as the axial initial elastic modulus and the axial initial Poisson's ratio should be calculated. For large coefficients of dispersion, the specific reasons should be analyzed. If it is due to sample quality problems, a new batch of samples should be made and tested again.
[0224] 7.1 Performance value of each specimen: X1, X2, X3, ..., Xn. If necessary, the damage of each specimen should be stated.
[0225] 7.2 Calculate the arithmetic mean according to formula (15) to three significant figures:
[0226]
[0227] Where:
[0228] ——arithmetic mean;
[0229] X i ——Performance value of each sample;
[0230] n——number of samples.
[0231] 7.3 Calculate the standard deviation S according to formula (16) to two significant figures:
[0232]
[0233] Where:
[0234] S——standard deviation.
[0235] 7.4 Calculate the dispersion coefficient C according to formula (17) v , calculated to two significant figures:
[0236]
[0237] Where:
[0238] C v ——Dispersion coefficient.
[0239] 7.5 Confidence interval for the mean.
[0240] Calculated according to ISO 2602:1980.
[0241] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A test device for measuring the axial compression properties of composite material pipes for structural engineering, characterized by: It includes an upper end plate, a lower end plate, a semicircular steel bar, an axial strain gauge, and an annular strain gauge; the upper end plate and the lower end plate have the same structure, both including a circular end plate and a cylindrical protrusion located at the center of the end plate, two semicircular steel bars are fixed on the end plate by adhesive, and an annular groove is formed between the two semicircular steel bars and the cylindrical protrusion, the groove is used to accommodate the end of the tubular pressure specimen, and the groove is filled with high-strength gypsum to fix the end of the specimen to the end plate; the axial strain gauge and the annular strain gauge are evenly distributed on the outer surface of the specimen around the circumference of the specimen, and are located in the middle of the specimen; The test device also includes a number of steel sheets, which are placed between the ends of the specimen and the end plates to ensure that the tube wall of the specimen is perpendicular to the end plates; A set of strain gauges is composed of an axial strain gauge arranged along the axial direction and a circumferential strain gauge arranged along the circumferential direction; the number of strain gauges is multiple groups, and they are evenly pasted on the outer wall of the specimen along the circumference at a position half the height of the specimen; The test apparatus also includes a pressurizing device for axially pressurizing the sample.
2. The test device for measuring the axial compression performance of composite material pipes for structural engineering according to claim 1, characterized in that: The outer diameter of the cylindrical protrusion is 10 mm smaller than the nominal diameter of the specimen.
3. The test device for measuring the axial compression performance of composite material pipes for structural engineering according to claim 1, characterized in that: The inner diameter of the semicircular steel bar is 40 mm larger than the nominal diameter of the test specimen.
4. A test method for measuring the axial compression performance of a composite material pipe for structural engineering, using the test device for measuring the axial compression performance of a composite material pipe for structural engineering as claimed in any one of claims 1 to 3, characterized in that: The steps include: a. Sample preparation: Cut the sample from the composite material tube; b. Sample installation: insert the upper end of the sample into the cylindrical protrusion in the center of the upper end plate and align it initially; adjust the end face of the sample along the two vertical radial directions of the sample by using a square ruler, and ensure that the sample tube wall is perpendicular to the end plate by adding a steel sheet to the end face of the sample; fix two semicircular steel bars on the end plate by gluing, and temporarily seal the gap between the two semicircular steel bars with adhesive tape; prepare high-strength gypsum colloid and fill it into the groove; after the high-strength gypsum in the groove hardens, turn the sample upside down and install the lower end plate in the same way as the upper end plate; c. Loading: The test pressurizing equipment adopts a microcomputer-controlled electro-hydraulic servo testing machine. The tonnage is selected so that the load applied to the specimen falls within the range of 10% to 90% of the full load, and should not be less than 4% of the maximum tonnage of the testing machine. The specimen is pressurized evenly, and the pressurization speed is 0.06% increase in the axial strain of the specimen per minute, and the upper and lower end plates are kept parallel during the loading process; d. Data selection and calculation: Select the test data of the axial strain range specified in the test process, and calculate the axial compression linear parameters and nonlinear parameters of the composite material tube.
5. The test method for measuring the axial compression performance of a composite material pipe for structural engineering according to claim 4, characterized in that: In step a, the samples are taken from the same batch of composite material pipes used in the test or in actual engineering, and the total number of samples is not less than 5; the ends of the samples are polished to smooth out the tumors or protrusions on the pipe wall.
6. The test method for measuring the axial compression performance of composite material pipes for structural engineering according to claim 4, characterized in that: In step d, the axial compression linear parameters include axial compression strength, axial compression elastic modulus and Poisson's ratio, and the nonlinear parameters include axial compression secant modulus and axis compression secant Poisson's ratio.
7. The test method for measuring the axial compression performance of a composite material pipe for structural engineering according to claim 6, characterized in that: The calculation process is, The axial compressive strength of the specimen is calculated according to formula (1): Where: P c ——Axial compressive strength of the specimen, in MPa; F c,max ——The maximum axial compressive load of the specimen, in N; d——average inner diameter of the sample, in mm; t——average thickness of the sample, in mm; The axial stress of the specimen is calculated according to formula (2): Where: σ x ——Axial stress of the specimen, in MPa; F c ——axial compressive load of the specimen, in N; The axial compressive elastic modulus is calculated according to formula (3): Where: E x ——Axial compressive elastic modulus of the specimen, in MPa; Δε x - the average axial strain increment within the elastic range of the specimen is at least 0.2%; Δσ x ——with the average axial strain increment Δε x The corresponding average axial stress increment is in MPa; The Poisson's ratio of the sample is calculated according to formula (4): Where: ν xθ ——Poisson’s ratio of axial compression of the specimen; Δε θ ——with the average axial strain increment Δε x The corresponding average hoop strain increment; The strain energy density of the sample under axial compression is calculated according to formula (5): Where: ε x,i ——The i-th average axial strain of the specimen, starting from a value greater than or equal to 0.01% and ending at the point of maximum axial compressive load; σ x,i ——with ε x,i The corresponding i-th axial stress is in MPa; U i ——with ε x,i The corresponding i-th axial compressive strain energy density, in MPa; The axial compression secant modulus of the specimen is calculated according to formula (6): Where: E x,sec,i ——with ε x,i The corresponding i-th axial compression secant modulus; The axial compression secant Poisson's ratio of the specimen is calculated according to formula (7): Where: ν xθ,sec,i ——with ε x,i The corresponding Poisson's ratio of the i-th axial compression secant; ε θ,i ——with ε x,i The corresponding i-th average hoop strain; According to the calculation results, the axial compressive strain energy density and the axial secant modulus U are plotted respectively. i ~E x,sec,i and axial compressive strain energy density ~ axial secant Poisson's ratio U i ~v xθ,sec,i Data points; The data points obtained by fitting the least square method are expressed by the axial secant modulus of the composite material tube under the composite stress state, that is, under the biaxial stress state or triaxial stress state, expressed by the strain energy density of the composite material tube using formula (8): Where: E x,sec ——Axial secant modulus of the composite material pipe under bidirectional stress, in MPa; A, B, C - nonlinear coefficients of axial secant modulus obtained by fitting the experimental axial compression strain energy density ~ secant modulus data; U * ——Axial compressive strain energy density of the axial compression specimen at maximum load, in MPa; ——Axial tangent modulus of the axial compression specimen at maximum load, in MPa; D, F——U>U * The nonlinear parameters of the rear axial secant modulus are calculated using equations (9) and (10) respectively: Under the composite material tube composite stress state, the axial Poisson's ratio expressed by the strain energy density is expressed by formula (11): Where: ν xθ,sec ——Axial Poisson’s ratio of the composite material pipe under bidirectional stress; a, b, c——axial secant Poisson's ratio nonlinear coefficients obtained by fitting the experimental axial compression strain energy density ~ secant Poisson's ratio data; ——Axial tangent Poisson’s ratio of the axial compression specimen at maximum load; k, f——for U>U * The nonlinear parameters of the rear axial secant Poisson's ratio are calculated using equations (12) and (13) respectively: For composite pipes used in structural engineering, the shear deformation of the composite pipe is ignored. The composite pipe is in axial compression and circumferential tension, and is considered to be in a biaxial stress state. Therefore, the strain energy density of the composite pipe in the biaxial stress state is calculated using formula (14): Where: σ x , ε x ——respectively, they are the axial stress and strain of the composite material pipe under bidirectional stress state, where the unit of axial stress is MPa; σ θ , ε θ ——respectively are the hoop stress and strain of the composite material pipe under bidirectional stress state, where the unit of hoop stress is MPa; Therefore, the strain energy density of the biaxially stressed composite pipe at any time is obtained, formula (14), that is, the axial secant modulus E considering the nonlinearity of the composite pipe under the current stress state is obtained through formulas (8) to (13): x,sec and the axial secant Poisson's ratio ν xθ,sec .
Citation Information
Patent Citations
Laterally constrained rock uniaxial compression test device
CN103900902A
Geotextile axial-compression clogging test device and method thereof
CN107703038A
Testing device for measuring axial compression performance of composite material pipe for structural engineering
CN214668249U
Method of determining mechanical characteristics of hollow tubular articles from polymer composite materials