All-solid-state battery and method for manufacturing the same

By increasing the interface roughness of the conductive material layer in an all-solid battery, the reliability and film peeling problems caused by thinning the solid electrolyte layer are solved, and the stability and performance of the battery are improved.

CN113054199BActive Publication Date: 2024-11-05TAIYO YUDEN KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011562864.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-25
Publication Date
2024-11-05
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

In an all-solid battery, in order to ensure the battery capacity, it is necessary to thin the solid electrolyte layer, but this may lead to a problem of reducing reliability and film peeling, making it difficult to take into account reliability and suppress film peeling.

Method used

By forming a conductive material layer with a high interface roughness on both sides of the solid electrolyte layer, the interface roughness on at least one side is ensured to be greater than the interface roughness between the solid electrolyte layer and the electrode layer, and the density between the electrode layer and the solid electrolyte layer is improved. , thereby inhibiting short circuit and film peeling.

Benefits of technology

In the case of thinning the solid electrolyte layer, the reliability and cycling characteristics of the battery are improved, the occurrence of short circuits and film peeling is reduced, and the stability and performance of the battery are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113054199B_ABST
    Figure CN113054199B_ABST
Patent Text Reader

Abstract

The present invention provides an all-solid-state battery and a method for manufacturing the same that can suppress the occurrence of short circuits and membrane peeling. The all-solid-state battery is characterized in that it includes: a solid electrolyte layer with an oxide-based solid electrolyte as the main component; a first electrode structure formed on the first main surface of the solid electrolyte layer, wherein two first electrode layers containing active materials sandwich a first collector layer with a conductive material as the main component; and a second electrode structure formed on the second main surface of the solid electrolyte layer, wherein two second electrode layers containing active materials sandwich a second collector layer with a conductive material as the main component, and at least one of the roughness of the interface between the first collector layer and the two first electrode layers and the roughness of the interface between the second collector layer and the two second electrode layers is greater than the roughness of the interface between the solid electrolyte layer and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an all-solid-state battery and a method for manufacturing the same. Background Art

[0002] All-solid batteries using oxide solid electrolytes are highly anticipated as a technology that can provide safe secondary batteries that do not catch fire or produce toxic gases, which may occur with organic electrolytes, sulfide solid electrolytes, etc. In order to ensure battery capacity, it is desirable to make the solid electrolyte layer thin. However, if the solid electrolyte layer is made thin, short circuits and cycle characteristics are prone to deterioration, making it difficult to ensure reliability.

[0003] Therefore, the following technology is disclosed: by making the standard deviation of the thickness of the solid electrolyte film less than 5μm, the solid electrolyte layer is flattened, thereby improving the battery characteristics (cycle characteristics) of an all-solid-state battery with a solid electrolyte thickness of more than 10μm (for example, refer to Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-157362 Summary of the invention

[0007] Technical problem to be solved by the invention

[0008] In order to further secure the battery capacity, it is desired to further reduce the thickness of the solid electrolyte layer. However, as the thickness is reduced, there is a possibility that the reliability cannot be fully secured.

[0009] In addition, in the stacked all-solid battery, the first electrode layer, the collector layer, the second electrode layer and the solid electrolyte layer are stacked. In order to make the solid electrolyte layer after thinning flat, it is considered that each layer other than the solid electrolyte layer is also flattened. However, as the main component of the collector layer, metals, carbon, etc. as conductive materials are mostly used, and as the main component of the electrode layer, ceramics are mostly used, therefore, film peeling is easily occurred at the interface of different materials, resulting in a deterioration in the yield rate. Due to the above reasons, only each layer is flattened, and it is difficult to ensure reliability and suppress film peeling.

[0010] The present invention has been made in view of the above-mentioned technical problems, and an object of the present invention is to provide an all-solid-state battery and a method for manufacturing the same that can ensure reliability and suppress film peeling.

[0011] Means for solving technical problems

[0012] The all-solid-state battery of the present invention is characterized in that it includes: a solid electrolyte layer whose main component is an oxide-type solid electrolyte; a first electrode structure formed on the first main surface of the solid electrolyte layer, wherein two first electrode layers containing active materials sandwich a first collector layer whose main component is a conductive material; and a second electrode structure formed on the second main surface of the solid electrolyte layer, wherein two second electrode layers containing active materials sandwich a second collector layer whose main component is a conductive material, and at least either the roughness of the interface between the first collector layer and the two first electrode layers and the roughness of the interface between the second collector layer and the two second electrode layers is greater than the roughness of the interface between the solid electrolyte layer and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer.

[0013] In the above-mentioned all-solid-state battery, the thickness of the solid electrolyte layer may be 8 μm or less.

[0014] In the above-mentioned all-solid-state battery, it may be that: when the coefficient of variation of the thickness of multiple different parts is taken as the interface roughness value, at least any one of the roughness value of the interface between the first collector layer and the two first electrode layers and the roughness value of the interface between the second collector layer and the two second electrode layers is greater than 20%, and the roughness value of the interface between the solid electrolyte layer and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer is less than 40%.

[0015] In the above-mentioned all-solid-state battery, it may be that: when the coefficient of variation of the thickness of multiple different parts is taken as the interface roughness value, at least either one of the roughness value of the interface between the first current collector layer and the two first electrode layers and the roughness value of the interface between the second current collector layer and the two second electrode layers is less than 50%.

[0016] The method for manufacturing a fully solid-state battery of the present invention is characterized in that it includes: a step of preparing a stacked body; and a step of firing the stacked body, wherein the stacked body includes: a solid electrolyte green sheet containing particles of an oxide-type solid electrolyte; a first stacked body stacked on a first main surface of the solid electrolyte green sheet, wherein two layers of first electrode layers containing an active material are sandwiched by a paste for a first current collector containing a conductive material; and a second stacked body stacked on a second main surface of the solid electrolyte green sheet, wherein two layers of second electrode layers containing an active material are sandwiched by a paste for a second current collector containing a conductive material. The present invention relates to a body paste, and the particle size of at least any one of the first collector paste and the second collector paste is adjusted so that at least any one of the roughness of the interface between the first collector layer obtained by the first collector paste and the two first electrode layers obtained by the first electrode layer paste and the roughness of the interface between the second collector layer obtained by the second collector paste and the two second electrode layers obtained by the second electrode layer paste is greater than the roughness of the interface between the solid electrolyte layer obtained by the solid electrolyte raw sheet and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer.

[0017] Effects of the Invention

[0018] According to the present invention, it is possible to provide an all-solid-state battery and a method for manufacturing the battery that can suppress the occurrence of a short circuit and suppress film peeling. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a schematic cross-sectional view showing the basic structure of an all-solid-state battery.

[0020] Figure 2 is a schematic cross-sectional view of an all-solid-state battery according to an embodiment.

[0021] Figure 3 yes Figure 2 A partial enlarged view of .

[0022] Figure 4 This is a diagram illustrating a method for measuring interface roughness.

[0023] Figure 5 This is a diagram illustrating the flow of a method for manufacturing an all-solid-state battery.

[0024] Figure 6 It is a diagram illustrating a lamination process.

[0025] Description of Reference Numerals

[0026] 10 first electrode, 11 first electrode layer, 12 first current collector layer, 20 second electrode, 21 second electrode layer, 22 second current collector layer, 30 solid electrolyte layer, 40a first external electrode, 40b second external electrode, 100 all-solid-state battery. DETAILED DESCRIPTION

[0027] Hereinafter, embodiments will be described with reference to the drawings.

[0028] (Implementation Method)

[0029] Figure 1 is a schematic cross-sectional view showing the basic structure of the all-solid-state battery 100. Figure 1 As illustrated in the figure, the all-solid-state battery 100 has a structure in which a solid electrolyte layer 30 of an oxide type is sandwiched between a first electrode 10 and a second electrode 20. The first electrode 10 is formed on the first main surface of the solid electrolyte layer 30, and has a structure in which a first electrode layer 11 and a first collector layer 12 are stacked, and the first electrode layer 11 is arranged on the solid electrolyte layer 30 side. The second electrode 20 is formed on the second main surface of the solid electrolyte layer 30, and has a structure in which a second electrode layer 21 and a second collector layer 22 are stacked, and the second electrode layer 21 is arranged on the solid electrolyte layer 30 side.

[0030] When the all-solid battery 100 is used as a secondary battery, one of the first electrode 10 and the second electrode 20 is used as a positive electrode and the other is used as a negative electrode. In this embodiment, as an example, the first electrode 10 is used as a positive electrode and the second electrode 20 is used as a negative electrode.

[0031] The solid electrolyte layer 30 is not particularly limited as long as it is an oxide-based solid electrolyte. For example, a phosphate-based solid electrolyte with a NASICON structure can be used. The phosphate-based solid electrolyte with a NASICON structure has high conductivity and is stable in the atmosphere. The phosphate-based solid electrolyte is, for example, a phosphate containing lithium. The phosphate is not particularly limited, and examples thereof include composite lithium phosphate salts with Ti (for example, LiTi2(PO4)3) and the like. Alternatively, part or all of Ti may be replaced with a tetravalent transition metal such as Ge, Sn, Hf, or Zr. In addition, in order to increase the Li content, part of Ti may be replaced with a trivalent transition metal such as Al, Ga, In, Y, or La. More specifically, for example, Li 1+x Al x Ge 2-x (PO4)3、Li 1+x Al x Zr 2-x (PO4)3、Li 1+x Al x Ti 2-x(PO4)3, etc. For example, it is preferred that a Li-Al-Ge-PO4 type material to which a transition metal is pre-added is the same as the transition metal contained in the phosphate having an olivine-type crystal structure contained in the first electrode layer 11 and the second electrode layer 21. For example, in the case where the first electrode layer 11 and the second electrode layer 21 contain a phosphate containing Co and Li, it is preferred that the solid electrolyte layer 30 contain a Li-Al-Ge-PO4 type material to which Co is pre-added. In this case, the effect of suppressing the dissolution of the transition metal contained in the electrode active material into the electrolyte can be obtained. In the case where the first electrode layer 11 and the second electrode layer 21 contain a phosphate containing a transition element other than Co and Li, it is preferred that the solid electrolyte layer 30 contain a Li-Al-Ge-PO4 type material to which the transition metal is pre-added.

[0032] At least the first electrode layer 11 used as the positive electrode of the first electrode layer 11 and the second electrode layer 21 contains a substance having an olivine-type crystal structure as an electrode active material. It is preferred that the second electrode layer 21 also contains the electrode active material. As such an electrode active material, phosphates containing transition metals and lithium can be cited. The olivine-type crystal structure is a crystal of natural olivine (olivine), which can be identified by X-ray diffraction.

[0033] As a typical example of an electrode active material having an olivine-type crystal structure, LiCoPO4 containing Co can be used. Phosphates in which Co of a transition metal is replaced in the chemical formula can also be used. Here, the ratio of Li and PO4 can be changed accordingly with the valence. As transition metals, Co, Mn, Fe, Ni, etc. are preferably used.

[0034] The electrode active material having an olivine-type crystal structure functions as a positive electrode active material in the first electrode layer 11 that functions as a positive electrode. For example, when only the first electrode layer 11 contains an electrode active material having an olivine-type crystal structure, the electrode active material functions as a positive electrode active material. When the second electrode layer 21 also contains an electrode active material having an olivine-type crystal structure, in the second electrode layer 21 that functions as a negative electrode, although its mechanism of action is not completely clear, it is possible to exert the effects of increased discharge capacity and increased operating potential accompanying discharge, and it is presumed that these effects are caused by forming a partial solid solution state with the negative electrode active material.

[0035] In the case where both the first electrode layer 11 and the second electrode layer 21 contain an electrode active material having an olivine crystal structure, the respective electrode active materials preferably contain transition metals that may be the same or different from each other. "May be the same or different from each other" means that the electrode active materials contained in the first electrode layer 11 and the second electrode layer 21 may contain the same transition metal or may contain transition metals of different types. The first electrode layer 11 and the second electrode layer 21 may contain only one transition metal or may contain more than two transition metals. Preferably, the first electrode layer 11 and the second electrode layer 21 contain the same transition metal. More preferably, the chemical composition of the electrode active materials contained in the two electrode layers is the same. By containing the same transition metal or the same composition of electrode active materials in the first electrode layer 11 and the second electrode layer 21, the similarity of the composition of the two electrode layers is improved, and therefore, the following effect is achieved: even if the positive and negative terminals of the all-solid-state battery 100 are reversed, it can be actually used without malfunctioning according to the purpose.

[0036] The second electrode layer 21 of the first electrode layer 11 and the second electrode layer 21 may also contain a substance known as a negative electrode active material. By making only one electrode layer contain a negative electrode active material, it becomes clear that the one electrode layer acts as a negative electrode and the other electrode layer acts as a positive electrode. In the case where only one electrode layer contains a negative electrode active material, it is preferred that the one electrode layer is the second electrode layer 21. In addition, it is also possible to make the two electrode layers contain a substance known as a negative electrode active material. Regarding the negative electrode active material of the electrode, appropriate reference can be made to the prior art of secondary batteries, for example, compounds such as titanium oxide, lithium titanium composite oxide, lithium titanium composite phosphate, carbon, and lithium vanadium phosphate can be listed.

[0037] In the preparation of the first electrode layer 11 and the second electrode layer 21, in addition to these active materials, conductive materials such as oxide solid electrolyte materials, carbon or metals (conductive aids) and the like may be added. By uniformly dispersing these materials in water or an organic solvent together with a binder and a plasticizer, an electrode layer paste may be obtained. Metals as conductive aids include Pd, Ni, Cu, Fe, and alloys containing these.

[0038] The first current collector layer 12 and the second current collector layer 22 contain a conductive material as a main component. For example, metal, carbon, etc. can be used as the conductive material of the first current collector layer 12 and the second current collector layer 22.

[0039] Figure 21 is a schematic cross-sectional view of a fully solid battery 100a having a plurality of stacked battery cells. The fully solid battery 100a includes: a stacking sheet 60 having a substantially rectangular parallelepiped shape; a first external electrode 40a provided on a first end face of the stacking sheet 60; and a second external electrode 40b provided on a second end face opposite to the first end face.

[0040] The two surfaces other than the upper surface and the lower surface in the stacking direction of the laminated sheet 60 among the four surfaces other than the two end surfaces are called side surfaces. The first external electrode 40a and the second external electrode 40b extend to the upper surface, the lower surface and the two side surfaces in the stacking direction of the laminated sheet 60. However, the first external electrode 40a and the second external electrode 40b are spaced apart from each other.

[0041] In the following description, components having the same composition range, the same thickness range, and the same particle size distribution range as those of the all-solid-state battery 100 are denoted by the same reference numerals, and detailed description thereof is omitted.

[0042] In the all-solid battery 100a, a plurality of first collector layers 12 and a plurality of second collector layers 22 are alternately stacked. The end edges of the plurality of first collector layers 12 are exposed at the first end surface of the laminate sheet 60, but not at the second end surface. The end edges of the plurality of second collector layers 22 are exposed at the second end surface of the laminate sheet 60, but not at the first end surface. Thus, the first collector layers 12 and the second collector layers 22 are alternately connected to the first external electrode 40a and the second external electrode 40b.

[0043] The first electrode layer 11 is stacked on the first collector layer 12. The solid electrolyte layer 30 is stacked on the first electrode layer 11. The solid electrolyte layer 30 extends from the first external electrode 40a to the second external electrode 40b. The second electrode layer 21 is stacked on the solid electrolyte layer 30. The second collector layer 22 is stacked on the second electrode layer 21. Another second electrode layer 21 is stacked on the second collector layer 22. Another solid electrolyte layer 30 is stacked on the second electrode layer 21. The solid electrolyte layer 30 extends from the first external electrode 40a to the second external electrode 40b. The first electrode layer 11 is stacked on the solid electrolyte layer 30. In the all-solid battery 100a, these stacked units are repeatedly formed. Thus, the all-solid battery 100a has a structure in which a plurality of battery cells are stacked.

[0044] In order to ensure the battery capacity, it is desirable to make the solid electrolyte layer 30 thin. For example, the thickness of the solid electrolyte layer 30 is 10 μm or less, preferably 8 μm or less, more preferably 7 μm or less, and further preferably 6 μm or less. However, when the solid electrolyte layer 30 is made thin, short circuits and cycle characteristics are easily deteriorated, making it difficult to ensure reliability.

[0045] Therefore, it is possible to planarize the solid electrolyte layer 30. In order to ensure the planarization of the solid electrolyte layer 30, it is possible to planarize the other layers. However, since the main component materials of the first collector layer 12 and the second collector layer 22 are different from the main component materials of the first electrode layer 11 and the second electrode layer 21, film peeling is likely to occur at the interface of each layer, resulting in a poor yield. Therefore, it is difficult to achieve both reliability and film peeling by only planarizing each layer.

[0046] Therefore, the all-solid-state battery 100 , 100 a of the present embodiment has a structure capable of ensuring reliability and suppressing film peeling.

[0047] Figure 3 yes Figure 2 A partial enlarged view of the Figure 3 In the figure, hatching is omitted. Figure 3 As illustrated in , a first electrode layer 11 is stacked under the solid electrolyte layer 30 (first main surface), a first collector layer 12 is stacked under the first electrode layer 11, and another first electrode layer 11 is stacked under the first collector layer 12. That is, the first collector layer 12 is sandwiched by two first electrode layers 11. The first collector layer 12 and the two first electrode layers 11 are referred to as the first electrode structure. A second electrode layer 21 is stacked on the solid electrolyte layer 30 (second main surface), a second collector layer 22 is stacked on the second electrode layer 21, and another second electrode layer 21 is stacked on the second collector layer 22. That is, the second collector layer 22 is sandwiched by two second electrode layers 21. The second collector layer 22 and the two second electrode layers 21 are referred to as the second electrode structure.

[0048] In the present embodiment, the roughness of the interface between the first current collector layer 12 and the two first electrode layers 11 sandwiching the first current collector layer 12 is greater than the roughness of the interface between the solid electrolyte layer 30 and the first electrode layer 11 and the second electrode layer 21 sandwiching the solid electrolyte layer 30. The roughness of the interface between the second current collector layer 22 and the two second electrode layers 21 sandwiching the second current collector layer 22 is greater than the roughness of the interface between the solid electrolyte layer 30 and the first electrode layer 11 and the second electrode layer 21 sandwiching the solid electrolyte layer 30.

[0049] In this structure, first, the roughness of the interface between the solid electrolyte layer 30 and the first electrode layer 11 and the second electrode layer 21 sandwiching the solid electrolyte layer 30 is small. Thus, the solid electrolyte layer 30 becomes flat. Therefore, it is possible to suppress the penetration of the solid electrolyte layer 30 caused by the electrode layer, thereby suppressing the short circuit. In addition, the cycle characteristics and self-discharge characteristics are also improved. That is, the reliability is improved. The first electrode layer 11, the second electrode layer 21 and the solid electrolyte layer 30 are all mainly composed of ceramics. Therefore, the adhesion between the first electrode layer 11 and the solid electrolyte layer 30 and the adhesion between the second electrode layer 21 and the solid electrolyte layer 30 are good.

[0050] Secondly, the roughness of the interface between the first collector layer 12 and the two first electrode layers 11 sandwiching the first collector layer 12 is large. In this case, an anchoring effect can be obtained, and the adhesion between the first collector layer 12 and the two first electrode layers 11 sandwiching the first collector layer 12 is improved, thereby suppressing film peeling. In addition, the roughness of the interface between the second collector layer 22 and the two second electrode layers 21 sandwiching the second collector layer 22 is large. In this case, an anchoring effect can be obtained, and the adhesion between the second collector layer 22 and the two second electrode layers 21 sandwiching the second collector layer 22 is improved, thereby suppressing film peeling. In addition, even if the first electrode layer 11 penetrates the first collector layer 12 as the roughness increases, only the two first electrode layers 11 are connected. In addition, even if the second electrode layer 21 penetrates the second collector layer 22 as the roughness increases, only the two second electrode layers 21 are connected. Therefore, the occurrence of short circuit can be suppressed.

[0051] As can be seen from the above, the all-solid-state batteries 100 and 100a of the present embodiment can ensure reliability and suppress film peeling.

[0052] Here, an example of a method for obtaining the roughness value of the interface is described. The cross section of the all-solid-state battery 100a is observed using a SEM (scanning electron microscope). Ten SEM photographs of any portion are taken at a magnification such that the length of the solid electrolyte layer 30 is 7 to 9 times the thickness of the solid electrolyte layer 30. Figure 4 As shown in the example, for each photo, 30 equally spaced vertical lines are drawn in the longitudinal direction. The vertical lines are parallel to the stacking direction. Along the vertical lines, the thickness of the solid electrolyte layer 30 is measured (30 locations are measured for each photo, a total of 30 locations × 10 photos = 300 locations). The average value and standard deviation are calculated, and the coefficient of variation is calculated: CV value = standard deviation / average value (%). This value can be used as the roughness value of the interface between the solid electrolyte layer 30 and the first electrode layer 11 and the second electrode layer 21 that sandwich the solid electrolyte layer 30.

[0053] Similarly, 10 SEM photographs of an arbitrary portion are taken at a magnification such that the length of the first current collector layer 12 is 7 to 9 times the thickness of the first current collector layer 12. Figure 4 As shown in the example, for each photo, 30 equally spaced vertical lines are drawn in the longitudinal direction. Along the vertical lines, the thickness of the first collector layer 12 is measured (30 locations are measured for each photo, a total of 30 locations × 10 photos = 300 locations). The average value and standard deviation are calculated, and the coefficient of variation is calculated: CV value = standard deviation / average value (%). This value can be used as the roughness value of the interface between the first collector layer 12 and the two first electrode layers 11 sandwiching the first collector layer 12.

[0054] Similarly, 10 SEM photographs of an arbitrary portion are taken at a magnification such that the length of the second current collector layer 22 is 7 to 9 times the thickness of the second current collector layer 22. Figure 4 As shown in the example, for each photo, 30 equally spaced vertical lines are drawn in the longitudinal direction. Along the vertical lines, the thickness of the second collector layer 22 is measured (30 locations are measured for each photo, a total of 30 locations × 10 photos = 300 locations). The average value and standard deviation are calculated, and the coefficient of variation is calculated: CV value = standard deviation / average value (%). This value can be used as the roughness value of the interface between the second collector layer 22 and the two second electrode layers 21 sandwiching the second collector layer 22.

[0055] When the roughness value (first CV value) of the interface between the solid electrolyte layer 30 and the first electrode layer 11 and the second electrode layer 21 sandwiching the solid electrolyte layer 30 is too large, there is a possibility that the solid electrolyte layer 30 cannot be sufficiently flattened. Therefore, it is preferable to set an upper limit for the first CV value. For example, the first CV value is preferably 40% or less, more preferably 35% or less, and further preferably 30% or less.

[0056] When the roughness value (second CV value) of the interface between the first collector layer 12 and the two first electrode layers 11 sandwiching the first collector layer 12, and the roughness value (second CV value) of the interface between the second collector layer 22 and the two second electrode layers 21 sandwiching the second collector layer 22 are too small, it may not be possible to fully suppress film peeling. Therefore, it is preferred to set a lower limit for the second CV value. For example, the second CV value is preferably 20% or more, more preferably 22% or more, and further preferably 30% or more.

[0057] On the other hand, when the second CV value is too large, the resistance may increase. Therefore, it is preferable to set an upper limit for the second CV value. For example, the second CV value is preferably 50% or less, more preferably 45% or less, and further preferably 40% or less.

[0058] In the present embodiment, the roughness of the interface between the first current collector layer 12 and the two first electrode layers 11 sandwiching the first current collector layer 12, and the roughness of the interface between the second current collector layer 22 and the two second electrode layers 21 sandwiching the second current collector layer 22 are both greater than the roughness of the interface between the solid electrolyte layer 30 and the first electrode layer 11 and the second electrode layer 21 sandwiching the solid electrolyte layer 30, but the present invention is not limited thereto. As long as the roughness of any one of them is greater than the roughness of the interface between the solid electrolyte layer 30 and the first electrode layer 11 and the second electrode layer 21 sandwiching the solid electrolyte layer 30, it is sufficient.

[0059] The thickness of the first electrode layer 11 and the second electrode layer 21 is, for example, 10 μm or less, 9 μm or less, or 8 μm or less. The thickness of the first current collector layer 12 and the second current collector layer 22 is, for example, 10 μm or less, 9 μm or less, or 8 μm or less.

[0060] Next, a method for manufacturing the all-solid-state battery 100 a will be described. Figure 5 It is a diagram illustrating the flow of a method for manufacturing the all-solid-state battery 100 a.

[0061] (Ceramic Raw Material Powder Production Process)

[0062] First, a powder of an oxide solid electrolyte constituting the above-mentioned solid electrolyte layer 30 is prepared. For example, raw materials, additives, etc. may be mixed, and a solid phase synthesis method or the like may be used to prepare a powder of an oxide solid electrolyte constituting the solid electrolyte layer 30. The obtained powder may be dry-milled to adjust it to a desired average particle size. For example, the desired average particle size may be adjusted by a planetary ball mill using a 5 mm φ ZrO2 ball.

[0063] The additive includes a sintering aid, which may be any one or more glass components such as a Li-BO compound, a Li-Si-O compound, a Li-CO compound, a Li-SO compound, or a Li-PO compound.

[0064] (Green Sheet Production Process)

[0065] Next, the obtained powder is uniformly dispersed in an aqueous solvent or an organic solvent together with a binding material, a dispersant, a plasticizer, etc., and wet-pulverized to obtain a solid electrolyte slurry with a desired average particle size. At this time, a bead mill, a wet jet mill, various mixers, a high-pressure homogenizer, etc. can be used. From the viewpoint of being able to simultaneously adjust and disperse the particle size distribution, a bead mill is preferably used. A binder is added to the obtained solid electrolyte slurry to obtain a solid electrolyte paste. By applying the obtained solid electrolyte paste, a green sheet can be made. The coating method is not particularly limited, and a slit coating method, a reverse coating method, a gravure coating method, a strip coating method, a blade coating method, etc. can be used. The particle size distribution after wet pulverization can be measured, for example, using a laser diffraction measuring device using a laser diffraction scattering method.

[0066] (Electrode layer paste preparation process)

[0067] Next, an electrode layer paste for making the above-mentioned first electrode layer 11 and second electrode layer 21 is prepared. For example, the electrode layer paste can be obtained by uniformly dispersing a conductive auxiliary agent, an active material, a solid electrolyte material, an adhesive, a plasticizer, etc. in water or an organic solvent. As a solid electrolyte material, the above-mentioned solid electrolyte paste can be used. As a conductive auxiliary agent, Pd, Ni, Cu, Fe, alloys containing them, or various carbon materials can be further used. In the case where the composition of the first electrode layer 11 and the second electrode layer 21 is different, it is sufficient to prepare each electrode layer paste separately.

[0068] (Current Collector Paste Preparation Process)

[0069] Next, a collector paste for making the above-mentioned first collector layer 12 and second collector layer 22 is prepared. For example, the collector paste can be obtained by uniformly dispersing Pd powder, carbon black, plate-like graphite carbon, adhesive, dispersant, plasticizer, etc. in water or an organic solvent. In this case, the dispersion is performed so that the particle size of the powder component is not less than 1 μm. In addition, in order to make the second CV value greater than the first CV value, the particle size of each powder is adjusted so that the relationship of (average particle size of collector paste)>(average particle size of electrode layer paste)>(average particle size of solid electrolyte green sheet) can be obtained.

[0070] (Lamination process)

[0071] like Figure 6As shown in the example, the electrode layer paste 52 is printed on one side of the raw sheet 51, and then the collector paste 53 is printed, and then the electrode layer paste 52 is printed. In the area where the electrode layer paste 52 and the collector paste 53 are not printed on the raw sheet 51, the reverse pattern 54 is printed. As the reverse pattern 54, the same material as the raw sheet 51 can be used. The printed multiple raw sheets 51 are alternately stacked to obtain a laminate. In this case, the laminate is obtained in such a way that the electrode layer paste 52 and the collector paste 53 are alternately exposed on the two end faces in the laminate.

[0072] (Firing process)

[0073] Next, the obtained laminate is fired. The firing conditions are not particularly limited, and may be exemplified by an oxidizing atmosphere or a non-oxidizing atmosphere, with the maximum temperature preferably being 400°C to 1000°C, and more preferably 500°C to 900°C. In order to fully remove the binder before reaching the maximum temperature, a process may be provided in which the temperature is maintained at a temperature lower than the maximum temperature in an oxidizing atmosphere. In order to reduce process costs, it is preferred to fire at the lowest possible temperature. Reoxidation treatment may be performed after firing. Through the above process, a laminate sheet 60 is generated.

[0074] (External Electrode Forming Step)

[0075] Then, a metal paste is applied to the two end surfaces of the laminated sheet 60 and sintered. Thus, the first external electrode 40a and the second external electrode 40b can be formed. Alternatively, the laminated sheet 60 can be placed on a special jig and the electrodes can be formed by sputtering, wherein the special jig allows the first external electrode 40a and the second external electrode 40b to be exposed at intervals on the upper surface, the lower surface, and the two side surfaces of the laminated sheet 60 that are in contact with the two end surfaces. Alternatively, the first external electrode 40a and the second external electrode 40b can be formed by plating the formed electrodes.

[0076] [Example]

[0077] Next, an all-solid-state battery was produced according to the embodiment and its characteristics were investigated.

[0078] (Example 1)

[0079] Co3O4, Li2CO3, ammonium dihydrogen phosphate, Al2O3 and GeO2 were mixed and Li containing a specified amount of Co was produced by solid phase synthesis. 1.3 Al 0.3 Ge 1.7(PO4)3 is used as solid electrolyte material powder. The obtained powder is dry-pulverized using ZrO2 balls. Then, a solid electrolyte slurry is prepared by wet pulverization (dispersion medium: ion exchange water or ethanol). A binder is added to the obtained slurry to obtain a solid electrolyte paste, thereby preparing a green sheet. LiCoPO4 and Co containing a specified amount of LiCoPO4 and Co are synthesized by solid phase synthesis in the same manner as above. 1.3 Al 0.3 Ti 1.7 (PO4)3.

[0080] The electrode active material and the solid electrolyte material are highly dispersed using a wet bead mill, etc., to prepare a ceramic paste consisting only of ceramic particles. Next, the ceramic paste and the conductive material are thoroughly mixed to prepare an electrode layer paste.

[0081] On the raw sheet, a screen with a prescribed pattern is used to print the paste for the electrode layer, and then the Pd paste as the collector layer paste is printed, and then the electrode layer paste is printed. The printed sheets are staggered and overlapped 10 sheets in a manner that the electrodes are led to the left and right, and the components obtained by overlapping the raw sheets are pasted on the top and bottom as a covering layer, and are pressed by hot pressing, and the stacked body is cut into a prescribed size by a cutter. The 200 sheets obtained by cutting are heat-treated at 300°C to 500°C for degreasing, and heat-treated at 900°C or less to sinter them to produce a sintered body.

[0082] Observe the cross section of each sample using SEM. Take 10 SEM photos of any part at a magnification where the length of the solid electrolyte layer 30 is 7 to 9 times the thickness of the solid electrolyte layer 30, and for each photo, draw 30 equally spaced vertical lines in the longitudinal direction. Measure the thickness of the solid electrolyte layer 30 along the vertical lines (measure 30 parts for each photo, a total of 30 parts × 10 photos = 300 parts). Calculate the average value and standard deviation, and calculate the coefficient of variation: CV value = standard deviation / average value (%). This value is used as the roughness value (first CV value) of the interface between the solid electrolyte layer 30 and the first electrode layer 11 and the second electrode layer 21 sandwiching the solid electrolyte layer 30.

[0083] Similarly, 10 SEM photos of any part are taken at a magnification such that the length of the first collector layer 12 is 7 to 9 times the thickness of the first collector layer 12, and for each photo, 30 equally spaced vertical lines are drawn in the longitudinal direction. Along the vertical lines, the thickness of the collector is measured (30 parts are measured for each photo, a total of 30 parts × 10 photos = 300 parts). The average value and standard deviation are calculated, and the coefficient of variation is calculated: CV value = standard deviation / average value (%). This value is used as the roughness value (second CV value) of the interface between the first collector layer 12 and the two first electrode layers 11 sandwiching the first collector layer 12.

[0084] Similarly, 10 SEM photos of any part are taken at a magnification such that the length of the second collector layer 22 is 7 to 9 times the thickness of the second collector layer 22, and 30 equally spaced vertical lines are drawn in the longitudinal direction for each photo. The thickness of the collector is measured along the vertical lines (30 parts are measured for each photo, and a total of 30 parts × 10 photos = 300 parts are measured). The average value and standard deviation are calculated, and the coefficient of variation is calculated: CV value = standard deviation / average value (%). This value is used as the roughness value (second CV value) of the interface between the second collector layer 22 and the two layers of the second electrode layer 21 sandwiching the second collector layer 22.

[0085] The average thickness of the solid electrolyte layer 30 was 8 μm. The first CV value was 30%. The second CV value was 34%.

[0086] (Example 2)

[0087] In Example 2, the average thickness of the solid electrolyte layer 30 is 7 μm. The first CV value is 30%. The second CV value is 34%. Other conditions are the same as those in Example 1.

[0088] (Example 3)

[0089] In Example 3, the average thickness of the solid electrolyte layer 30 is 6 μm. The first CV value is 30%. The second CV value is 34%. Other conditions are the same as those in Example 1.

[0090] (Example 4)

[0091] In Example 4, the average thickness of the solid electrolyte layer 30 is 7 μm. The first CV value is 30%. The second CV value is 50%. Other conditions are the same as those in Example 1.

[0092] (Example 5)

[0093] In Example 5, the average thickness of the solid electrolyte layer 30 is 7 μm. The first CV value is 40%. The second CV value is 50%. Other conditions are the same as those in Example 1.

[0094] (Example 6)

[0095] In Example 6, the average thickness of the solid electrolyte layer 30 is 5 μm. The first CV value is 18%. The second CV value is 22%. Other conditions are the same as those in Example 1.

[0096] (Comparative Example)

[0097] In the comparative example, the average thickness of the solid electrolyte layer 30 is 7 μm. The first CV value is 35%. The second CV value is 34%. Other conditions are the same as those in Example 1.

[0098] (Short circuit rate)

[0099] For Examples 1 to 6 and the comparative example, the presence or absence of short circuit was determined for each sample. -3 S / cm or more, it is judged that a short circuit has occurred. The number of samples to be measured is 100, and the ratio of the number of samples that have short circuits is calculated as the short circuit rate. If the short circuit rate is ≤5%, it is judged as very good "◎", if 5%<short circuit rate≤10%, it is judged as good "○", if 10%<short circuit rate<15%, it is judged as slightly good "△", if 15%≤short circuit rate, it is judged as unqualified "×".

[0100] (Cycle Characteristics)

[0101] For Examples 1 to 6 and Comparative Examples, each sample was charged and discharged repeatedly at 10C at 25°C in a voltage range of 2.5V-0V, and (200th discharge capacity / first discharge capacity) was used as the cycle characteristics relative to the first discharge capacity. If 90% < cycle characteristics, it is judged to be very good "◎", if 85% ≤ cycle characteristics ≤ 90%, it is judged to be good "○", if 80% ≤ cycle characteristics < 85%, it is judged to be slightly good "△", and if cycle characteristics < 80%, it is judged to be unqualified "×".

[0102] (Self-discharge characteristics)

[0103] For Examples 1 to 6 and Comparative Examples, the voltage of each sample was monitored in an open circuit at 25°C after full charge. The (voltage value after 50 hours / voltage value immediately after the measurement) was calculated as the self-discharge characteristic. If 95% ≤ self-discharge characteristic, it is judged as very good "◎", if 90% ≤ self-discharge characteristic <95%, it is judged as good "○", if 80% ≤ self-discharge characteristic <90%, it is judged as slightly good "△", and if self-discharge characteristic <80%, it is judged as unqualified "×".

[0104] Table 1 shows the results of Examples 1 to 6 and Comparative Example.

[0105] [Table 1]

[0106]

[0107] In Example 1, the short circuit occurrence rate was 3%, which was judged to be very good. The cycle characteristics were 92%, which was judged to be very good. The self-discharge characteristics were 96%, which was judged to be very good.

[0108] In Example 2, the short circuit occurrence rate was 5%, which was judged to be very good. The cycle characteristics were 91%, which was judged to be very good. The self-discharge characteristics were 95%, which was judged to be very good.

[0109] In Example 3, the short circuit occurrence rate was 9%, which was judged to be good. The cycle characteristics were 87%, which was judged to be good. The self-discharge characteristics were 90%, which was judged to be good.

[0110] In Example 4, the short circuit occurrence rate was 7%, which was judged to be good. The cycle characteristics were 90%, which was judged to be very good. The self-discharge characteristics were 92%, which was judged to be good.

[0111] In Example 5, the short circuit occurrence rate was 13%, which was judged to be slightly good. The cycle characteristics were 82%, which was judged to be slightly good. The self-discharge characteristics were 83%, which was judged to be slightly good.

[0112] In Example 6, the short circuit occurrence rate was 11%, which was judged to be slightly good. The cycle characteristics were 85%, which was judged to be good. The self-discharge characteristics were 88%, which was judged to be slightly good.

[0113] In the comparative example, the short circuit occurrence rate was 15%, which was judged as unacceptable. The cycle characteristic was 79%, which was judged as unacceptable. The self-discharge characteristic was 80%, which was judged as slightly good.

[0114] If any of the short circuit occurrence rate, cycle characteristics and self-discharge characteristics is not unqualified, the comprehensive judgment is judged as qualified "0". If any of the short circuit occurrence rate, cycle characteristics and self-discharge characteristics is unqualified, the comprehensive judgment is judged as unqualified "×".

[0115] In Examples 1 to 6, the comprehensive judgment was judged as qualified "0". It can be considered that this is because the solid electrolyte layer 30 is sufficiently flattened due to the first CV value < the second CV value. On the other hand, in the comparative example, the comprehensive judgment was judged as unqualified "×". It can be considered that this is because the solid electrolyte layer 30 is not sufficiently flattened due to the first CV value ≥ the second CV value.

[0116] (Film peeling)

[0117] The presence or absence of film peeling was confirmed for each sample of Examples 1 to 6 and the Comparative Example. In Examples 1 to 6, no film peeling occurred in any sample. It is considered that this is because, since the first CV value is less than the second CV value, an anchoring effect can be obtained, and the adhesion between the collector layer and the two electrode layers sandwiching the collector layer is improved. On the other hand, in the Comparative Example, there are samples in which film peeling occurred. It is considered that this is because, since the first CV value is greater than the second CV value, the adhesion between the collector layer and the two electrode layers sandwiching the collector layer cannot be fully obtained.

[0118] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-mentioned specific embodiments, and various modifications and changes can be made within the scope of the gist of the present invention described in the claims.

Claims

1. An all-solid-state battery, It is characterized in that include: A solid electrolyte layer mainly composed of an oxide-based solid electrolyte; a first electrode structure formed on the first main surface of the solid electrolyte layer, wherein two first electrode layers containing an active material sandwich a first current collector layer containing a conductive material as a main component; and a second electrode structure formed on the second main surface of the solid electrolyte layer, wherein two second electrode layers containing active materials sandwich a second current collector layer containing a conductive material as a main component; At least one of the roughness values ​​of the interface between the first current collector layer and the two first electrode layers and the roughness values ​​of the interface between the second current collector layer and the two second electrode layers is greater than the roughness value of the interface between the solid electrolyte layer and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer. The roughness value of the interface is the coefficient of variation calculated based on the standard deviation and average value of the thickness of multiple different parts: CV value = standard deviation / average value, the unit is %, The roughness value of the interface between the solid electrolyte layer and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer is the CV value of the thickness of the solid electrolyte layer. The roughness value of the interface between the first current collector layer and the two first electrode layers sandwiching the first current collector layer is the CV value of the thickness of the first current collector layer. The roughness value of the interface between the second current collector layer and the two second electrode layers sandwiching the second current collector layer is the CV value of the thickness of the second current collector layer. At least one of the roughness value of the interface between the first current collector layer and the two first electrode layers and the roughness value of the interface between the second current collector layer and the two second electrode layers is 20% or more, The roughness value of the interface between the solid electrolyte layer and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer is 40% or less.

2. The all-solid-state battery according to claim 1, Features: The solid electrolyte layer has a thickness of 8 μm or less.

3. The all-solid-state battery according to claim 1 or 2, Features: At least one of a roughness value of an interface between the first current collector layer and the two first electrode layers and a roughness value of an interface between the second current collector layer and the two second electrode layers is 50% or less.

4. A method for manufacturing an all-solid-state battery, It is characterized in that include: A step of preparing a laminate; and a step of firing the laminate, The laminate comprises: a solid electrolyte green sheet containing particles of an oxide-based solid electrolyte; a first laminate laminated on a first main surface of the solid electrolyte green sheet, wherein two layers of a first electrode layer paste containing an active material sandwich a first collector paste containing a conductive material; and a second laminate laminated on a second main surface of the solid electrolyte green sheet, wherein two layers of a second electrode layer paste containing an active material sandwich a second collector paste containing a conductive material. The particle size of at least one of the first collector paste and the second collector paste is adjusted so that at least one of the roughness values ​​of the interface between the first collector layer obtained from the first collector paste and the two first electrode layers obtained from the first electrode layer paste and the roughness values ​​of the interface between the second collector layer obtained from the second collector paste and the two second electrode layers obtained from the second electrode layer paste is greater than the roughness value of the interface between the solid electrolyte layer obtained from the solid electrolyte green sheet and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer, The roughness value of the interface is the coefficient of variation calculated based on the standard deviation and average value of the thickness of multiple different parts: CV value = standard deviation / average value, the unit is %, The roughness value of the interface between the solid electrolyte layer and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer is the CV value of the thickness of the solid electrolyte layer. The roughness value of the interface between the first current collector layer and the two first electrode layers sandwiching the first current collector layer is the CV value of the thickness of the first current collector layer. The roughness value of the interface between the second current collector layer and the two second electrode layers sandwiching the second current collector layer is the CV value of the thickness of the second current collector layer. At least one of the roughness value of the interface between the first current collector layer and the two first electrode layers and the roughness value of the interface between the second current collector layer and the two second electrode layers is 20% or more, The roughness value of the interface between the solid electrolyte layer and the first electrode layer and the second electrode layer sandwiching the solid electrolyte layer is 40% or less.