Preparation method of Al-MOFs@C loaded polyurethane foam porous composite material for treating fluorine-containing wastewater

Through Al-MOFs@C loaded polyurethane foam porous composite material, the problem of low-concentration fluorine-containing wastewater treatment is solved, and high-efficiency fluorine ion adsorption and material regenerative properties are achieved, which is suitable for water quality optimization.

CN113058573BActive Publication Date: 2024-11-22TIANJIN TONGYU ENVIRONMENTAL PROTECTION & ENERGY SAVING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110349385.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-11-22
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively treat low-concentration fluorine-containing wastewater. The traditional chemical precipitation method is costly, has high energy consumption and cannot meet strict emission standards. The application of adsorption method in low-concentration fields is limited, and it is difficult to recover adsorption particles.

Method used

Al-MOFs@C loaded polyurethane foam porous composite material is used to load Al-MOFs nanoparticles and carbon materials into PUF through hydrothermal synthesis to form a new adsorbent with high specific surface area and multiple adsorption sites for water bodies Removal of fluoride ions.

Benefits of technology

It realizes efficient treatment of low-concentration fluorine-containing wastewater, significantly improves adsorption rate and capacity, and has stable renewability of the material, which is suitable for water quality optimization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113058573B_ABST
    Figure CN113058573B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an Al-MOFs@C loaded polyurethane foam porous composite material for treating low-concentration fluorine-containing wastewater, comprising the steps of: 1. dissolving aluminum salt and organic acid in a certain volume of deionized water, stirring and fully dissolving at room temperature, and transferring to a reactor for hydrothermal synthesis reaction, the reaction conditions are 100°C, 24h, and obtaining Al-MOFs nanoparticles by centrifugation technology; 2. placing Al-MOFs nanoparticles, carbon materials and polyurethane foam (PUF) in a reactor at the same time by a hydrothermal synthesis method, using water as a solvent, the reaction temperature is 100°C, the reaction time is 24h, and Al-MOFs and carbon materials are loaded in PUF materials to obtain Al-MOFs@C-PUF porous polymer composite materials. The invention has the beneficial effects of having a good removal effect for fluorine ions that are difficult to remove at low concentrations, and optimizing water quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of porous polymer adsorption, and in particular relates to a method for preparing an Al-MOFs@C loaded polyurethane foam porous composite material for treating fluorine-containing wastewater, which is used for removing pollutants in water bodies. Background Art

[0002] Fluorine is a trace element required by the human body, but excessive intake of fluoride ions can be toxic to animals and plants. The World Health Organization (WHO) stipulates that the fluoride content in drinking water should be less than 1.5 mg / L. In recent years, with the rapid development of the processing and use of fluoride, especially in the electronics industry and the fluoride industry, the discharge of fluoride-containing wastewater has continued to rise, and reasonable collection and effective purification have become the key to achieving clean production. Therefore, controlling the fluoride ion concentration in water can effectively meet water quality standards.

[0003] Industrial production, such as the production of electronic components and circuit boards in the electronics industry and the production of stainless steel plates in steel mills, requires the use of fluorine-containing acid mixtures for cleaning, corrosion, and etching, which will produce a large amount of high-concentration fluorine-containing wastewater. Calcium salts and lime are usually used to precipitate high-concentration fluorine-containing wastewater. Fluoride ions react with calcium ions to form CaF 2 Sedimentation is a technology that is simple, inexpensive, and easy to handle, and is widely used. However, the fluoride concentration in the effluent is about 20 mg / L. It is difficult to form effective precipitates and reduce the fluoride ion content in the water by further deep treatment, and the effluent quality standard cannot be met. After the fluoride-containing wastewater in the electronics industry is treated with traditional chemical coagulation and sedimentation technology, the fluoride ion content is usually >12ppm, which also cannot meet the increasingly stringent emission standards (<3ppm). In addition, the addition of reagents increases the difficulty of secondary treatment and increases the cost of residual sludge treatment. Therefore, it is important to study the deep treatment technology of fluoride-containing wastewater.

[0004] At present, the main methods for treating fluoride-containing wastewater at home and abroad include chemical precipitation and coagulation sedimentation, reverse osmosis, ion exchange, electrocoagulation, membrane treatment, etc., but these treatment methods are prone to unstable effluent quality, high energy consumption, high cost, and serious secondary pollution. Adsorption is a method for removing pollutants from water bodies efficiently and quickly. It has high adsorption efficiency and is easy to operate. It is a commonly used method for removing pollutants in industrial applications. However, how to increase the specific surface area of ​​the adsorbent, improve the mass transfer efficiency of the adsorbent pores, and increase the adsorption sites is the key to increasing the adsorption capacity of the adsorbent material and increasing the adsorption rate. In addition, adsorption is usually used to treat low-concentration fluoride-containing wastewater. Although the adsorption effect is excellent, the difficulty in recovering the adsorbed particles hinders its application in the field of low-concentration fluoride-containing wastewater.

[0005] Metal-organic frameworks (MOFs) are organic-inorganic hybrid crystalline porous network structure materials constructed by connecting organic units and inorganic units. MOFs have a stable pore cage structure, ordered network structure variability, designability, and ultra-high specific surface area, showing great application prospects, especially in the field of environmental applications, which has attracted widespread attention from researchers. Polyurethane foam (PUF) porous polymer is a high molecular polymer containing repeated carbamate groups in the main chain of the molecule. At the same time, it also contains lipid, ether, urea and other groups according to different needs. PUF porous polymer has excellent mechanical strength and large freedom of structural design. It can be used as an adsorption porous material in the field of water treatment.

[0006] In summary, a 3D porous foam polymer adsorbent material with high specific surface area and multiple adsorption sites is developed for the removal of fluoride ions in water bodies, especially for fluoride ions that are difficult to remove at low concentrations, and has a good removal effect, thereby optimizing water quality. Summary of the invention

[0007] In order to solve the above problems, the purpose of the present invention is to provide a novel PUF porous polymer composite material with adsorption function by loading Al-MOFs@C material on PUF porous polymer. The advantage of the present invention is that it combines the ultra-high specific surface area, variable structure, and modifiable design of both MOFs and PUF, as well as the improvement of the structure and performance of the main body after carbon material coating, and is applied to the removal of pollutants in water bodies, especially the efficient treatment of low-concentration fluoride-containing wastewater in water bodies.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing an Al-MOFs@C-loaded polyurethane foam porous composite material for treating fluorine-containing wastewater, comprising the following steps:

[0010] (1) Preparation of Al-MOFs materials: Aluminum salt and organic acid were dissolved in a certain volume of deionized water, stirred at room temperature until fully dissolved, and then transferred to a reactor for hydrothermal synthesis reaction at 100°C for 24 h. Al-MOFs nanoparticles were obtained by centrifugation.

[0011] (2) Al-MOFs nanoparticles, carbon materials and PUF were placed in a reactor at the same time through a hydrothermal synthesis method, with water as the solvent, the reaction temperature being 100 °C and the reaction time being 24 h, so that Al-MOFs and carbon materials were loaded in the PUF material to obtain an Al-MOFs@C-PUF porous polymer composite material.

[0012] The aluminum salt described in step (1) includes aluminum chloride, aluminum sulfate, and aluminum nitrate, and the organic acid includes pyromellitic acid, terephthalic acid, and 1,3,5-pyromellitic acid.

[0013] The PUF described in step (2) is a polyether polyurethane foam porous polymer.

[0014] The carbon material additives described in step (2) include biochar, graphene, carbon nanotubes, and carbon fibers.

[0015] The beneficial effects of the present invention are as follows: the method described in the present invention combines the characteristics of Al-MOFs controllable structure and excellent performance with the characteristics of PUF porous polymer such as large specific surface area, high stability and low cost, and combines the improvement of the structure and performance of the main body after carbon material coating to prepare Al-MOFs@C-PUF porous polymer material, which is applied to the field of water defluorination, especially has good application prospects for the treatment of low-concentration fluoride-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is an electron microscope comparison diagram of the Al-MOFs loaded PUF porous composite material, the Al-MOFs@C loaded PUF porous composite material and the PUF porous material prepared in Example 1 of the present invention;

[0017] Figure 2 is the adsorption isotherm curve of the Al-MOFs@C loaded PUF porous composite material in Example 2 of the present invention;

[0018] Figure 3 is the adsorption kinetics curve of the Al-MOFs@C loaded PUF porous composite material in Example 3 of the present invention;

[0019] Figure 4 This is the regeneration performance curve of the Al-MOFs@C loaded PUF porous composite material in Example 3 of the present invention. DETAILED DESCRIPTION

[0020] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments:

[0021] The present invention discloses a method for preparing an Al-MOFs@C-loaded polyurethane foam porous composite material for treating low-concentration fluorine-containing wastewater. The method comprises the following steps:

[0022] (1) Preparation of Al-MOFs materials: Aluminum salt and organic acid were dissolved in a certain volume of deionized water, stirred at room temperature until fully dissolved, and then transferred to a reactor for hydrothermal synthesis reaction at 100°C for 24 h. Al-MOFs nanoparticles were obtained by centrifugation.

[0023] (2) Al-MOFs nanoparticles, carbon materials and PUF were placed in a reactor at the same time through a hydrothermal synthesis method, with water as the solvent, the reaction temperature being 100 °C and the reaction time being 24 h, so that Al-MOFs and carbon materials were loaded in the PUF material to obtain an Al-MOFs@C-PUF porous polymer composite material.

[0024] in:

[0025] The method described in step (1) is a conventional method, and similar preparation methods can be obtained from public literature. The raw material aluminum salt includes aluminum chloride, aluminum sulfate, aluminum nitrate, etc.; the organic acid includes pyromellitic acid, terephthalic acid, 1,3,5-pyromellitic acid, etc.

[0026] References:

[0027] JJZhao,LQXu,YZSu,HWYu,H.Liu,SPQian,WGZheng,YQZhao,Zr-MOFs loaded on polyurethane foam by polydopamine for enhanced dye adsorption,J.Environ.Sci.,101(2021)177-188.

[0028] J.Li,JLGong,GMZeng,P.Zhang,B.Song,WCCao,HYLiu,SYHuan,Zirconium-based metal organic frameworks loaded on polyurethane foam membrane for simultaneous removal of dyes with different charges,J.ColloidInterf.Sci.,527(2018)267-279.

[0029] The PUF described in step (2) is a common polyether polyurethane foam porous polymer, which has the advantage of having excellent hydrolysis resistance. The preparation method thereof can be obtained from public literature.

[0030] The carbon material additives described in step (2) include biochar, graphene, carbon nanotubes, carbon fibers, etc.

[0031] The present invention uses a Japanese Hitachi S-4800 scanning electron microscope to observe the microstructure of the coating surface.

[0032] The specific steps of some adsorption performance and regeneration performance test instructions are as follows:

[0033] 1. Adsorption isotherm experiment

[0034] Accurately weigh the mass of the dried Al-MOFs@C-PUF porous polymer material prepared in the embodiment and place it in a polyethylene bottle, add a certain volume of sodium fluoride solution of different concentrations (5 mg / L, 10 mg / L, 20 mg / L, 50 mg / L, 80 mg / L, 100 mg / L, 300 mg / L), adjust the pH of the solution to 5-6 with 0.1 mol / L hydrochloric acid aqueous solution, place the polyethylene bottle in a constant temperature oscillator at a speed of 100 r / min and a temperature of 25°C. After 5-10 hours, take out the polyethylene bottle, extract a certain volume of solution to determine the concentration after fluoride ion adsorption, and use an ion chromatograph to determine the fluoride ion.

[0035] 2. Kinetic adsorption experiments

[0036] A certain mass of the Al-MOFs@C-PUF porous polymer material prepared in the example is placed in a polyethylene bottle and a sodium fluoride solution of a certain concentration and volume is added. The adsorption reaction is carried out by constant temperature oscillation. A small amount of the adsorbed fluorine-containing solution is taken out at regular intervals and its concentration is measured until the concentration measurement values ​​of the taken out fluorine-containing solution are continuously equal, i.e., adsorption saturation is reached, and the equilibrium time required for adsorption kinetic saturation is obtained.

[0037] 3. Regeneration performance experiment

[0038] After the first adsorption experiment reached equilibrium, 10% aluminum sulfate aqueous solution was used for desorption for one hour, and then rinsed with a large amount of deionized water and dried before repeating the experiment for the second time. The above method was repeated 10 times, and the regeneration rate was calculated for 10 times. This defluorination regeneration technology is a conventional analytical method.

[0039] Example 1

[0040] (1) Preparation of Al-MOFs materials: Aluminum sulfate and pyromellitic acid were dissolved in a certain volume of deionized water, stirred at room temperature until fully dissolved, and then transferred to a reactor for hydrothermal synthesis reaction at 100°C for 24 hours. Al-MOFs nanoparticles were obtained by centrifugation.

[0041] (2) Al-MOFs nanoparticles, biochar and PUF were placed in a reactor at the same time through a hydrothermal synthesis method, with water as the solvent, the reaction temperature being 100 °C and the reaction time being 24 h, so that Al-MOFs and biochar were loaded in the PUF material to obtain an Al-MOFs@C-PUF porous polymer composite material.

[0042] The Al-MOFs@C loaded polyurethane foam porous composite material prepared in this example for treating low-concentration fluorine-containing wastewater was tested, and the results are as follows:

[0043] 1. The surface morphology of the composite material changed significantly after being loaded with MOFs and MOFs@C, indicating that MOFs and MOFs@C were successfully loaded on the PUF porous material. Figure 1 shown.

[0044] 2. The composite material Al-MOFs@C-PUF porous polymer has a maximum fluorine adsorption capacity of 3.5 mg / g in a 100 mg / L sodium fluoride solution.

[0045] 3. The adsorption kinetics of the composite Al-MOFs@C-PUF porous polymer showed that its adsorption equilibrium time was 18 minutes. Compared with traditional adsorption materials, the adsorption rate was significantly improved.

[0046] 4. The composite material Al-MOFs@C-PUF porous polymer has stable regeneration performance, and after 10 cycles, its adsorption capacity remains above 80%.

[0047] Example 2

[0048] (1) Preparation of Al-MOFs materials: Aluminum chloride and terephthalic acid were dissolved in a certain volume of deionized water, stirred at room temperature until fully dissolved, and then transferred to a reactor for hydrothermal synthesis reaction at 100°C for 24 hours. Al-MOFs nanoparticles were obtained by centrifugation.

[0049] (2) Al-MOFs nanoparticles, carbon nanotubes and PUF were placed in a reactor at the same time through a hydrothermal synthesis method, with water as the solvent, the reaction temperature being 100 °C and the reaction time being 24 h, so that Al-MOFs and carbon nanotubes were loaded in the PUF material to obtain an Al-MOFs@C-PUF porous polymer composite material.

[0050] The Al-MOFs@C loaded polyurethane foam porous composite material prepared in this example for treating low-concentration fluorine-containing wastewater was tested, and the results are as follows:

[0051] 1. The surface morphology of the composite material changed significantly after being loaded with Al-MOFs and Al-MOFs@C, indicating that Al-MOFs and Al-MOFs@C were successfully loaded on the PUF porous material.

[0052] 2. The composite Al-MOFs@C-PUF porous polymer has a maximum fluoride adsorption capacity of 3.0 mg / g in a 100 mg / L sodium fluoride solution. Figure 2 shown.

[0053] 3. The adsorption kinetics of the composite Al-MOFs@C-PUF porous polymer showed that its adsorption equilibrium time was 15 minutes. Compared with traditional adsorption materials, the adsorption rate was significantly improved.

[0054] 4. The composite material Al-MOFs@C-PUF porous polymer has stable regeneration performance, and after 10 cycles, its adsorption capacity remains above 82%.

[0055] Example 3

[0056] (1) Preparation of Al-MOFs materials: Aluminum nitrate and 1,3,5-trimethylbenzene carboxylic acid were dissolved in a certain volume of deionized water, stirred at room temperature until fully dissolved, and then transferred to a reactor for hydrothermal synthesis reaction at 100°C for 24 h. Al-MOFs nanoparticles were obtained by centrifugation.

[0057] (2) Al-MOFs nanoparticles, carbon black and PUF were placed in a reactor at the same time through a hydrothermal synthesis method, with water as the solvent, the reaction temperature being 100 °C and the reaction time being 24 h, so that Al-MOFs and carbon black were loaded in the PUF material to obtain an Al-MOFs@C-PUF porous polymer composite material.

[0058] The Al-MOFs@C loaded polyurethane foam porous composite material prepared in this example for treating low-concentration fluorine-containing wastewater was tested, and the results are as follows:

[0059] 1. The surface morphology of the composite material changed significantly after being loaded with Al-MOFs and Al-MOFs@C, indicating that Al-MOFs and Al-MOFs@C were successfully loaded on the PUF porous material.

[0060] 2. The maximum fluorine adsorption capacity of the composite material Al-MOFs@C-PUF porous polymer in 100 mg / L sodium fluoride solution is 3.3 mg / g.

[0061] 3. The adsorption kinetics of the composite Al-MOFs@C-PUF porous polymer showed that its adsorption equilibrium time was 15 min. Compared with traditional adsorption materials, the adsorption rate was significantly improved, such as Figure 3 shown.

[0062] 4. The composite Al-MOFs@C-PUF porous polymer has stable regeneration performance. After 10 cycles, its adsorption capacity remains above 85%. Figure 4 shown.

[0063] In summary, the above are only representative embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an Al-MOFs@C-loaded polyurethane foam porous composite material for treating fluoride-containing wastewater, comprising the following steps: (1) Preparation of Al-MOFs material: dissolving aluminum salt and organic acid in deionized water, stirring at room temperature until fully dissolved, and then transferring to a reactor at a temperature of 100°C for hydrothermal synthesis reaction for 24 hours, and obtaining Al-MOFs nanoparticles by centrifugation technology; the organic acid includes pyromellitic acid, terephthalic acid, and 1,3,5-pyromellitic acid; (2) Al-MOFs nanoparticles, carbon materials, and polyurethane foam (PUF) were placed in a reactor at the same time through a hydrothermal synthesis method. Water was used as the solvent. The reaction temperature was 100 °C and the reaction time was 24 h. Al-MOFs and carbon materials were loaded into the PUF material to obtain an Al-MOFs@C-PUF porous polymer composite material.

2. The method for preparing an Al-MOFs@C-loaded polyurethane foam porous composite material for treating fluorine-containing wastewater according to claim 1, characterized in that: The aluminum salt described in step (1) includes aluminum chloride, aluminum sulfate, and aluminum nitrate.

3. The method for preparing an Al-MOFs@C-loaded polyurethane foam porous composite material for treating fluorine-containing wastewater according to claim 1, characterized in that: The PUF described in step (2) is a polyether polyurethane foam porous polymer.

4. The method for preparing an Al-MOFs@C-loaded polyurethane foam porous composite material for treating fluorine-containing wastewater according to claim 1, characterized in that: The carbon material additives described in step (2) include biochar, graphene, carbon nanotubes, and carbon fibers.