Curable resin composition, use thereof, and method for producing the same
By using specific combinations of polyamide resins, polyisocyanates and epoxy compounds, a resin layer with high adhesion and heat resistance is formed, and the problems of degradation of durability and voids in hot water in the prior art are solved, and the high temperature is achieved durability and corrosion resistance.
Patent Information
- Application Number
- CN202110040244.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-01-13
AI Technical Summary
Prior Art When forming an adhesion resin layer on a metal surface, durability in hot water is reduced and voids between the metal and the adhesive layer may appear, affecting corrosion resistance and durability.
A combination of a polyamide resin having a melting point of 170°C or higher and a polyamide resin having a melting point of 150°C or lower is used to form a curable resin composition for forming a high Adhesive and heat-resistant adhesive layer, and through the combination of specific ratios and reactive groups, the uniformity and adhesion of the resin layer are ensured.
A composite member that maintains high adhesion and heat resistance at high temperatures is realized, avoiding gaps between the adhesive layer and the metal, and improving the durability and corrosion resistance of the composite member.
Smart Images

Figure BDA0002895540960000241
Abstract
Description
Technical Field
[0001] The present disclosure relates to a curable resin composition that can be used to impart high durability and adhesion to a substrate such as a metal, a composite member in which the surface of a substrate is covered with a cured film of the curable resin composition, a composite molded member in which a resin layer is formed on the cured film, and a method for producing the same. Background Art
[0002] For the purpose of improving the corrosion resistance and durability of metals, coatings have been formed using flow dipping methods, electrostatic coating methods, and the like. In particular, in applications where high durability is required, such as structural members of transportation vehicles such as vehicles (automobiles, etc.) and aircraft, hybrid members have been manufactured by priming metal, molding a resin on the primer layer (adhesive (sticker) layer), and causing hybridization to occur.
[0003] JP 2007-190917 A (Patent Document 1) and its corresponding US 2011 / 0143142 A1 describe a method for manufacturing a hybrid component formed of a metal and a polymer, wherein the metal is bonded to the polymer using a hot melt adhesive based on a copolyamide further comprising an isocyanate and an epoxide, wherein the hot melt adhesive comprises a copolyamide based on laurin lactam, 2.5%-15% of a blocked isocyanate, and 2.5%-10% of an epoxide. According to the document, the hot melt adhesive includes Degussa's VESTAMELT X1038-P1 [60% laurolactam, 25% caprolactam, and 15% AH salt (a mixture of 50% adipic acid and 50% hexamethylenediamine)] (95%), VESTAGON BF1540-P1 (5%), and Araldite GT7004 (5%), and in the final step, the polymer structure is formed by injection molding.
[0004] Citation List
[0005] Patent Literature
[0006] Patent Document 1: JP 2007-190917 A Summary of the invention
[0007] Technical issues
[0008] When the adhesive according to Patent Document 1 is electrostatically coated and heated, an adhesive layer having high adhesion to metal can be formed, and by molding a thermoplastic resin on the adhesive layer via injection molding, a hybrid component having high durability can be manufactured. However, due to unknown reasons, when the hybrid component formed in this way is immersed in hot water, adhesion may be reduced. In addition, when a thermoplastic resin is molded on the adhesive layer by injection molding, voids may be generated at the interface between the metal and the adhesive layer. As a result, high corrosion resistance and durability cannot be maintained for a long time.
[0009] Therefore, an object of the present invention is to provide a curable resin composition that can be used to impart high durability and adhesion to a substrate such as a metal, a composite member in which the surface of the substrate is coated with a coating layer (adhesive layer or cured film) of the curable resin composition, a composite molded member in which a resin is molded on the adhesive layer, and a method for producing the same.
[0010] Another object of the present invention is to provide a curable resin composition that can be used to form an adhesive layer (or cured film) having high adhesion to a substrate such as a metal and excellent heat resistance, a composite component using the resin composition (a composite component primed with the curable resin composition), a composite molded component, and a method for manufacturing the same.
[0011] Still another object of the present invention is to provide a curable resin composition suitable for obtaining a composite molded member having high adhesion and heat resistance even when a polyamide resin is molded on an adhesive layer (or a cured film) at a temperature of 260° C. or lower.
[0012] Solution to the problem
[0013] As a result of diligent studies to achieve the above-mentioned purpose, the present inventors have discovered that by combining a polyamide resin (A) having an amino group, a blocked polyisocyanate (B), and an epoxy compound (C), wherein the polyamide resin (A) is a combination of a polyamide resin (A1) having a melting point of 170°C or higher and a polyamide resin (A2) having a melting point of 150°C or lower in a specific ratio, high durability and adhesion to substrates such as metals can be imparted, and the present invention has been completed thereby.
[0014] That is, the curable resin composition of the present disclosure is a resin composition comprising: a polyamide resin (A) having an amino group, a blocked polyisocyanate (B), and an epoxy compound (C), wherein the polyamide resin (A) comprises a polyamide resin (A1) having a melting point of 170° C. or higher and a polyamide resin (A2) having a melting point of 150° C. or lower, and the mass ratio of the polyamide resin (A1) to the polyamide resin (A2) is 65 / 35-35 / 65 in the form of the former / the latter. The polyamide resin (A) may be granular. The curable resin composition may be a granular mixture. The mass ratio of the polyamide resin (A1) to the polyamide resin (A2) may be 60 / 40-40 / 60 in the form of the former / the latter. The amino group concentration of the polyamide resin (A1) or the polyamide resin (A2) may be 80 mmol / kg or greater. The blocked polyisocyanate (B) may have a glass transition temperature of 60-110° C., a melting point of 70-130° C., and a dissociation temperature of 120-200° C. The epoxy compound (C) may include a bisphenol epoxy resin having a softening temperature of 75° C. or higher. The ratio of the isocyanate group of the blocked polyisocyanate (B) may be 1.5-5 mol relative to 1 mol of the amino group of the polyamide resin (A), and the ratio of the epoxy group of the epoxy compound (C) may be 0.1-0.8 mol relative to 1 mol of the amino group of the polyamide resin (A). The isocyanate group of the blocked polyisocyanate (B) may be in excess of 15-450 mmol / kg relative to the amino group of the polyamide resin (A). The concentration of the epoxy group may be 3-35 mol% relative to the total molar number of the amino group, the isocyanate group, and the epoxy group. The total molar number of isocyanate groups of the blocked polyisocyanate (B) may be 1.3-50 times the total molar number of amino groups of the polyamide resin (A). The blocked polyisocyanate (B) may be contained in a ratio of 5-30 parts by mass relative to 100 parts by mass of the polyamide resin (A), and the epoxy compound (C) may be contained in a ratio of 5-30 parts by mass relative to 100 parts by mass of the polyamide resin (A).
[0015] The present disclosure also includes a composite member in which an adhesive layer of the curable resin composition is formed on the surface of a substrate. In addition, the present disclosure also includes a method for manufacturing a composite member, which includes coating the surface of a substrate with the curable resin composition to form an adhesive layer.
[0016] The present disclosure also includes a composite molded component in which a composition comprising at least a thermoplastic resin is molded or laminated on an adhesive layer of the composite component. The substrate may be a metal substrate. The thermoplastic resin may include a polyamide resin having a melting point higher than that of the polyamide resin (A). In addition, the present disclosure also includes a method for manufacturing a composite molded component, which includes molding or laminating a composition comprising at least a thermoplastic resin on an adhesive layer of the composite component.
[0017] Note that in this specification and claims, epoxy compounds, including epoxy resins, may be referred to simply as "epoxy compounds", and the protected isocyanate groups of blocked polyisocyanates may be referred to simply as "isocyanate groups". In addition, epoxy groups, including glycidyl groups, may be referred to simply as "epoxy groups".
[0018] Furthermore, various aspects disclosed in this specification may be combined with any other features disclosed herein.
[0019] Advantageous Effects of the Invention
[0020] In the present disclosure, a polyamide resin (A) having an amino group, a blocked polyisocyanate (B), and an epoxy compound (C) are combined, wherein the polyamide resin (A) is a combination of a polyamide resin (A1) having a melting point of 170°C or higher and a polyamide resin (A2) having a melting point of 150°C or lower in a specific ratio. Therefore, a composite member coated with an adhesive layer (or cured film) having high durability and adhesion to a substrate such as a metal can be manufactured, and a composite molded member can be manufactured by molding or laminating a thermoplastic resin on the adhesive layer. In addition, the composite member that has been primed with a curable resin composition to form an adhesive layer (or reactive adhesive layer) is highly adhesive (tackiness) to a substrate such as a metal, and the heat resistance of the composite member can also be improved. Therefore, even if the polyamide resin is molded or laminated on the adhesive layer (or cured film) at a temperature of 280° C. or lower, a uniform and highly durable composite molded component can be obtained without generating voids at the interface between the substrate such as metal and the adhesive layer. DETAILED DESCRIPTION
[0021] Polyamide resin having amino group (A)
[0022] The polyamide-based resin (A) has an amino group, and by having the amino group, the adhesive property of the adhesive layer formed from the curable resin composition can be improved.
[0023] The polyamide-based resin (A) comprises a polyamide resin (including a homo- or co-polyamide resin) and a polyamide elastomer (polyamide block copolymer), and may be formed from any of the following amide-forming components (a) to (c).
[0024] (a) a first amide-forming component which is a combination of an alkylenediamine component and an alkane dicarboxylic acid component;
[0025] (b) a second amide-forming component consisting of at least one of a lactam component and an aminocarboxylic acid component;
[0026] (c) a first amide-forming component and a second amide-forming component.
[0027] That is, the polyamide resin may be formed from any one of the amide-forming components (a)-(c) (a first amide-forming component; a second amide-forming component; a combination of a first amide-forming component and a second amide-forming component), and the polyamide elastomer may be prepared using a polyamide formed from any one of the amide-forming components (a)-(c). Note that the lactam component and the aminocarboxylic acid component having the same carbon number and branched structure may be considered as components equivalent to each other.
[0028] The polyamide resin may be an alicyclic polyamide, but is generally an aliphatic polyamide in many cases. In addition, the polyamide resin may be a homopolyamide resin or a copolyamide resin (copolymerized polyamide resin). Note that the copolyamide resin may be, for example: a copolyamide resin formed by a first amide-forming component having a different carbon number; a copolyamide resin of a first amide-forming component and a second amide-forming component; or a copolyamide resin formed by a second amide-forming component having a different carbon number. Note that a copolyamide resin formed by a first amide-forming component and / or a second amide-forming component having a different carbon number may be referred to as a first copolyamide resin, and a copolyamide resin of a first amide-forming component and / or a second amide-forming component and a copolymerization component (alicyclic or aromatic component) may be referred to as a second copolyamide resin.
[0029] Examples of the alkylenediamine component include C 4-18 Alkylene diamines such as tetramethylene diamine, hexamethylene diamine, octamethylene diamine, decanediamine, dodecane diamine, tetradecane diamine, and octadecane diamine. These diamine components can be used alone or in combination of two or more. Preferred diamine components include at least C 8-18 Alkylene diamine, preferably C 10-16 Alkylene diamine, more preferably C 11-16 Alkylene diamines, and especially C 11-14 Alkylenediamines such as dodecanediamine.
[0030] Examples of the alkane dicarboxylic acid component include C 4-36Alkanedicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, and octadecanedioic acid. These dicarboxylic acid components can be used alone or in combination of two or more. Preferred dicarboxylic acid components include C 8-18 Alkanedicarboxylic acids such as C 10-16 Alkanedicarboxylic acids, preferably C 12-14 Alkanedicarboxylic acids.
[0031] In the first amide-forming component, the diamine component may be used in the range of about 0.8-1.2 mol, preferably about 0.9-1.1 mol, relative to 1 mol of the dicarboxylic acid component.
[0032] Examples of the lactam component include C 4-20 Lactams such as ε-caprolactam, ω-capryllactam, ω-nonanolactam, ω-decanolactam, ω-undecanolactam, ω-laurolactam (or ω-lauryllactam or dodecanolactam), and ω-tridecanolactam. Examples of the aminocarboxylic acid component include C 4-20 Aminocarboxylic acids include ω-aminodecanoic acid, ω-aminoundecanoic acid, ω-aminododecanoic acid, and ω-aminotridecanoic acid. These lactam components and aminocarboxylic acid components may be used alone or in combination of two or more.
[0033] Preferred lactam components are, for example, C 8-18 Lactam, preferably C 10-16 Lactams such as C 10-15 lactam, more preferably C 10-14 Lactams such as C 11-13 Lactam. Preferred aminocarboxylic acids have the same carbon number as the preferred lactam component above. In particular, the lactam component and / or the aminocarboxylic acid often contain at least C 11-12 Lactam components and / or aminocarboxylic acids (eg, undecanoic acid, laurolactam or laurin lactam, aminoundecanoic acid, and aminododecanoic acid), for example, lactam components and / or aminocarboxylic acids having 12 carbons.
[0034] The ratio (molar ratio) of the first amide forming component to the second amide forming component can be selected from the following range: in the form of former / latter, about 100 / 0-0 / 100, for example, about 90 / 10-0 / 100 such as 80 / 20-5 / 95, preferably about 75 / 25-10 / 90 such as 70 / 30-15 / 85, more preferably about 60 / 40-20 / 80.
[0035] Preferred polyamide resins include at least C 8-18 Alkylene chain (or linear alkylene chain), such as C 8-16 Alkylene chains such as C 9-15Alkylene chain, preferably C 10-14 Alkylene chains such as C 11-14 Alkylene chain, and more preferably C 11-13 Alkylene chains such as C 11-12 The alkylene chain components serve as the first and / or second amide forming components.
[0036] The polyamide resin formed of such a component has high heat resistance and excellent adhesion to a substrate such as metal, and can be used to form a uniform and strong adhesive layer (primer layer or reactive adhesive layer) on the surface of the substrate.
[0037] Note that using the C 8-18 The polyamide resin as the first and / or second amide-forming component may be a homopolyamide resin (a homopolyamide resin comprising a component of an alkylene chain having a specific carbon number) or a first copolyamide resin (a homopolyamide resin comprising a component of an alkylene chain having a different carbon number). 8-18 A copolymer of various components of an alkylene chain; or having C 8-18 A first copolyamide resin having an alkylene chain (or a linear alkylene chain) component and a first and / or second amide-forming component having a short chain).
[0038] Note that examples of the first amide-forming component having a short chain include: 4-7 Alkylenediamines such as tetramethylenediamine, hexamethylenediamine, and trimethylhexamethylenediamine; C 6-7 Alkanedicarboxylic acids such as adipic acid and pimelic acid. Meanwhile, examples of the second amide-forming component having a short chain include: C 4-7 Lactams such as δ-valerolactam, ε-caprolactam, and ω-enantholactam, and C 4-7 Aminocarboxylic acid. The first and second amide-forming components having a short chain may be used in a small amount, for example, about 0-50 mol%, preferably 0-40 mol%, and more preferably 0-30 mol% relative to the total amount of the first and second amide-forming components.
[0039] In addition, if necessary, the copolyamide resin may be a copolymer (second copolyamide resin) of a copolymer component copolymerizable with the first and / or second amide forming component. The diamine component used as the copolymer component may be an alicyclic diamine component or an aromatic diamine component such as meta-xylylene diamine. Examples of the alicyclic diamine component include: diamino C 5-10 Cycloalkanes such as diaminocyclohexane; bis(amino 5-8 Cycloalkyl)C 1-3Alkanes such as bis(4-aminocyclohexyl)methane, bis(4-amino-3-methylcyclohexyl)methane, and 2,2-bis(4-aminocyclohexyl)propane; and hydrogenated xylylenediamine. In addition, the dicarboxylic acid component as the copolymerization component may be an alicyclic dicarboxylic acid component, for example, C 5-10 Cycloalkane-dicarboxylic acids such as cyclohexane-1,4-dicarboxylic acid and cyclohexane-1,3-dicarboxylic acid may be used, or aromatic dicarboxylic acids such as terephthalic acid and isophthalic acid may be used. Note that alicyclic diamine components and / or alicyclic dicarboxylic acid components may be used as copolymerization components to be copolymerized with the first and / or second amide forming components to form alicyclic polyamide resins such as transparent polyamides.
[0040] In the polyamide resin, the ratio of the first and second amide forming components to the entire components may be about 60-100 mol %, such as 70-100 mol %, preferably about 80-100 mol %, such as 85-97 mol %, and more preferably about 90-100 mol %.
[0041] Note that the polyamide resin may be a modified polyamide such as a polyamide having a branched structure introduced by using a small amount of a polycarboxylic acid component and / or a polyamine component.
[0042] Examples of such polyamide resins include: homopolyamide resins such as polyamide 8, polyamide 9, polyamide 10, polyamide 11, polyamide 12, polyamide 13, polyamide 610, polyamide 611, polyamide 612, polyamide 911, polyamide 912, polyamide 1010, and polyamide 1012; and copolyamides such as polyamide 6 / 10, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 12, polyamide 6 / 12 / 612, polyamide 10 / 12, polyamide 11 / 12, polyamide 12 / 13, polyamide 12 / 18, and polyamide 14 / 18. These polyamide resins can be used alone or in combination of two or more. Note that in the polyamide resin, the components separated by the symbol " / " refer to the first amide forming component or the second amide forming component, rather than the alkylenediamine component or the alkane dicarboxylic acid component in the first amide forming component.
[0043] Examples of the polyamide elastomer (polyamide block copolymer) include polyamide block copolymers formed of a polyamide segment as a hard segment (or hard block) (corresponding to the polyamide segment of the polyamide resin mentioned above, such as polyamide 11 or polyamide 12) and a soft segment (or soft block). The soft segment can be formed, for example, of polyether, polyester, or polycarbonate. Typical polyamide elastomers are polyamide-polyether block copolymers such as polyetheramide, for example, a polyamide block with a dicarboxyl group as the end and a polyC block with a diol as the end. 2-6A block copolymer of an alkylene glycol block (or a polyoxyalkylene block). Note that the polyamide elastomer may have an ester bond.
[0044] In the polyamide elastomer, when measured by gel permeation chromatography (GPC), the number average molecular weight (in terms of polystyrene) of the soft segment can be selected from the range of about 100-10000, and can be about 300-5000, such as 500-5000, preferably about 1000-2000. The ratio (mass ratio) of the polyamide block (polyamide segment) to the soft segment (or block) can be, for example, about 75 / 25-10 / 90, preferably about 70 / 30-15 / 85 in the form of the former / the latter.
[0045] Among these polyamide-based resins, the above-mentioned polyamide resins are preferred.
[0046] The polyamide-based resin (A) is selected from the above-mentioned polyamide resins, and comprises a combination of a polyamide-based resin (A1) having a melting point of 170° C. or higher and a polyamide-based resin (A2) having a melting point of 150° C. or lower.
[0047] The melting point of the polyamide-based resin (A1) may be any as long as it is 170°C or higher, and may be, for example, about 170-220°C, or may be about 175-210°C, preferably 175-200°C, more preferably about 175-190°C, and particularly preferably about 175-185°C.
[0048] Note that in this specification and claims, the melting point can be measured by differential scanning calorimetry (DSC), and when a plurality of peaks are shown by DSC, the melting point refers to a temperature corresponding to the highest peak on the high temperature side of the plurality of peaks.
[0049] The polyamide resin (A1) having such a melting point may be a homopolyamide resin or a copolyamide resin of the above-mentioned polyamide resins, wherein 8-16 Alkylene chain (preferably C 10-14 Alkylene chain, more preferably C 11-13 The ratio of the component containing an alkylene chain (alkylene chain) to the total amount of the components (monomers) (or the first and second amide-forming components) forming the polyamide-based resin is about 65-100 mol%, such as 65-98 mol%, preferably about 70-100 mol%, such as 75-98 mol%, more preferably about 80-100 mol%, such as 85-100 mol%, and particularly about 90-100 mol%, such as 95-100 mol%. Particularly preferred polyamide-based resin (A1) is a homo- or co-polyamide resin, particularly a homopolyamide resin, containing at least one amide-forming component selected from the following: C 11-13Lactam and / or C 11-13 Aminocarboxylic acid, for example, laurolactam, aminoundecanoic acid, or aminododecanoic acid. Specific examples of the polyamide-based resin (A1) include polyamide 610, polyamide 612, polyamide 1010, polyamide 1012, polyamide 10, polyamide 11, and polyamide 12, among which homopolymers of polyamide 11 and polyamide 12 such as laurolactam are widely used.
[0050] The polyamide resin (A1) preferably has low water absorption or hygroscopicity. That is, the water absorption of the polyamide resin (A1) may be about 1% by mass or less, such as 0.01-0.8% by mass, preferably about 0.75% by mass or less, such as 0.05-0.65% by mass, more preferably about 0.65% by mass or less, such as 0.1-0.55% by mass, and particularly about 0.5% by mass or less, such as 0.1-0.4% by mass, or may be about 0.1-0.65% by mass, preferably about 0.12-0.55% by mass, more preferably about 0.15-0.45% by mass, and particularly about 0.3% by mass or less, such as 0.15-0.25% by mass.
[0051] Note that in this specification and claims, the measurement of water absorption is based on the water absorption test specified in ASTM D570. The water absorption can be obtained by cooling the dried sample in a desiccator, measuring the mass of the sample, immersing the sample in water at 23° C. for 24 hours, patting the sample dry with a piece of cloth and wiping off excess water, measuring the mass of the sample, and calculating the mass change (increase rate) of the sample piece. A sample having a thickness of 0.125 inches (about 0.32 cm) can be used.
[0052] When measured according to ISO 62 at a relative humidity of 50% RH and a room temperature of 23° C., the equilibrium moisture content of the polyamide-based resin (A1) may be, for example, about 2% by mass or less, such as 0.1-1.8% by mass, preferably about 1.5% by mass or less, such as 0.3-1.5% by mass, more preferably about 1.3% by mass or less, such as 0.4-1.3% by mass, and particularly about 1% by mass or less, such as 0.5-0.9% by mass, or may be about 0.5-0.85% by mass, such as 0.6-0.8% by mass.
[0053] The saturated moisture content of the polyamide-based resin (A1) may be about 5% by mass or less, such as 0.5-4.5% by mass, preferably about 0.5-4% by mass, such as 0.6-3.8% by mass, more preferably about 0.8-3.5% by mass, such as 1-3% by mass, and particularly about 1.1-2.8% by mass, such as 1.2-2.7% by mass, when measured according to ISO 62 Method A after immersion in water at 23°C for 1 week.
[0054] The average concentration of amide bonds per repeating unit of the polyamide resin (A1) is preferably low. The average concentration of amide bonds may be, for example, about 1-10 mol / kg, such as 2-9 mol / kg, preferably about 3-8 mol / kg, such as 4-7 mol / kg, and more preferably about 5-7 mol / kg.
[0055] The polyamide resin (A1) has an amino group (particularly, a terminal amino group) to improve the adhesion of the adhesive layer to a substrate such as metal. The amino group concentration C of the polyamide resin (A1) is NH2 (Unit: mmol / kg) may be selected from the range of about 5-300, but is preferably 80 or more, and may be, for example, about 80-250, preferably about 90-200, more preferably about 100-170, even more preferably about 100-160, and particularly about 125-150. When the amino group concentration of the polyamide-based resin (A1) is high, the adhesion of the adhesive layer formed of the curable resin composition can be greatly improved.
[0056] The carboxyl group (terminal carboxyl group) concentration (unit: mmol / kg) of the polyamide resin (A1) is not particularly limited, and may be, for example, about 50 or less, such as 0-25, typically about 20 or less, such as 1-15, preferably about 10 or less, such as 1.5-7, and more preferably about 2-5.
[0057] In the polyamide resin (A1), the ratio of amino groups to carboxyl groups is not particularly limited, but the amino group concentration is preferably higher than the carboxyl group concentration. The ratio (molar ratio) of amino groups to carboxyl groups in the polyamide resin (A1) may be, for example, about 60 / 40-100 / 0, such as 70 / 30-99.9 / 0.1, preferably about 80 / 20-100 / 0, such as 85 / 15-99.5 / 0.5, and more preferably about 90 / 10-99 / 1, such as 95 / 5-98 / 2.
[0058] Note that in the present specification and claims, the amino group concentration and the carboxyl group concentration can be measured by a common method such as a titration method. For example, the amino group concentration can be measured by dissolving a sample of the polyamide resin in a mixed solvent of phenol and ethanol at a volume ratio of 10:1 to prepare a 1 wt % solution, and then performing neutralization titration with a 1 / 100N HCl aqueous solution. Meanwhile, the carboxyl group concentration can be measured by dissolving a sample of the polyamide resin in benzyl alcohol to prepare a 1 wt % benzyl alcohol solution, and then performing neutralization titration with a 1 / 100N KOH aqueous solution.
[0059] The number average molecular weight of the polyamide resin (A1) (unit: ×10 4) can be selected from, for example, the following range: about 0.5-20, such as 0.7-15, preferably about 0.8-10, such as 0.9-8, and more preferably about 1-7, such as 1-5.
[0060] Note that, in the present specification and claims, the molecular weight can be measured in terms of polymethyl methacrylate by gel permeation chromatography using HFIP (hexafluoroisopropanol) as a solvent.
[0061] The polyamide resin (A1) may have a melt flow rate (MFR, unit: g / 10 min) of about 1-100, such as 2-80, preferably about 5-75, such as 7-60, and more preferably about 10-50, such as 12-35, at a temperature of 230° C. and a load of 2.16 kg.
[0062] Note that, in this specification and claims, MFR can be measured according to ISO 1133 using a melt flow rate meter.
[0063] The polyamide resin (A1) is solid at room temperature and is preferably granular. The average particle size D50 of the granular polyamide resin (A1) may be about 3 μm or more, for example, about 3-100 μm, preferably 5-80 μm, more preferably about 10-70 μm, and particularly about 30-60 μm.
[0064] Note that, in the present specification and claims, the average particle size D50 is represented by a number average primary particle size, and can be measured by a common method, for example, a method using a particle size distribution measuring apparatus employing a laser diffraction / scattering method.
[0065] The melting point of the polyamide-based resin (A2) may be any as long as it is 150°C or lower, for example, about 90-150°C, or about 100-150°C, preferably about 110-145°C, more preferably about 110-140°C, and particularly about 110-130°C.
[0066] The polyamide resin (A2) having such a melting point may be a copolyamide resin of the following combinations among the above-mentioned polyamide resins: 4-7 Alkylene chain, preferably C 4-6 Alkylene chain, more preferably C 5-6 alkylene chain component; and having C 8-16 Alkylene chain, preferably C 10-14 Alkylene chain, more preferably C 11-13 With respect to the total amount of the components (monomers) forming the polyamide resin (or the first and second amide forming components), the amount of C 4-7The ratio of the alkylene chain component may be, for example, 30-75 mol%, preferably 30-70 mol%, more preferably 35-65 mol%, and particularly 40-60 mol%. Specific examples of the polyamide-based resin (A2) include polyamide 6 / 10, polyamide 6 / 11, polyamide 6 / 12, polyamide 6 / 66 / 12, and polyamide 6 / 12 / 612.
[0067] The water absorption of the polyamide resin (A2) may be, for example, about 5% by mass or less, such as 0.01-5% by mass, preferably about 3% by mass or less, such as 0.1-2.5% by mass, more preferably about 2.5% by mass or less, such as 0.5-2% by mass, and particularly about 2% by mass or less, such as 1-2% by mass.
[0068] When a flat plate having a size of 100 mm×100 mm×2 mm molded by injection molding is immersed in water at 23° C. for 5 days, the equilibrium moisture content of the polyamide-based resin (A2) may be, for example, about 3.5 mass % or less, such as 0.5-3.5 mass %, preferably about 3.0 mass % or less, such as 0.5-3.0 mass %, more preferably about 2.5 mass % or less, such as 0.5-2.5 mass %, and particularly about 2.0 mass % or less, such as 0.5-2.0 mass %.
[0069] The average concentration of the amide bonds of each repeating unit of the polyamide resin (A2) is preferably low. The average concentration of the amide bonds may be, for example, about 3-7 mol / kg, such as 3.5-7.0 mol / kg, preferably about 4-7 mol / kg, such as 4.5-6.5 mol / kg, and more preferably about 5.0-6.5 mol / kg.
[0070] The polyamide resin (A2) has an amino group (particularly, a terminal amino group) to improve the adhesion of the adhesive layer to a substrate such as metal. The amino group concentration C of the polyamide resin (A2) is NH2 (Unit: mmol / kg) can be selected from the range of about 5 to 300, but is preferably 80 or more, and may be, for example, about 80 to 260, preferably about 90 to 250, more preferably about 100 to 230, even more preferably about 120 to 220, and particularly about 150 to 200. When the amino group concentration of the polyamide-based resin (A2) is high, the adhesion of the adhesive layer formed of the curable resin composition can be greatly improved.
[0071] The carboxyl group (terminal carboxyl group) concentration (unit: mmol / kg) of the polyamide resin (A2) is not particularly limited, and may be, for example, about 50 or less, such as 0-20, typically about 10 or less, such as 0.5-10, preferably about 5 or less, such as 0.8-3, and more preferably about 1-2.
[0072] In the polyamide resin (A2), the ratio of amino to carboxyl is not particularly limited, but the amino concentration is preferably higher than the carboxyl concentration. The ratio (molar ratio) of amino to carboxyl in the polyamide resin (A2) may be, for example, about 60 / 40-100 / 0, such as 70 / 30-99.95 / 0.05, preferably about 80 / 20-100 / 0, such as 90 / 10-99.9 / 0.1, and more preferably about 95 / 5-99.7 / 0.3, such as 99 / 1-99.5 / 0.5.
[0073] The number average molecular weight of the polyamide resin (A2) (unit: ×10 4 ) can be calculated based on the amount of the terminal group measured using a titration method, and can be selected from, for example, the following ranges: about 0.5-3.0 such as 0.5-2.8, preferably about 0.5-2.5 such as 0.6-2.3, and more preferably about 0.6-1.5 such as 0.6-1.1.
[0074] The polyamide resin (A2) is solid at room temperature and is preferably granular. The average particle size D50 of the granular polyamide resin (A2) may be about 3 μm or more, for example, about 3-100 μm, preferably 5-80 μm, more preferably about 10-70 μm, and particularly about 30-60 μm.
[0075] The mass ratio of the polyamide-based resin (A1) to the polyamide-based resin (A2) in the form of the former / the latter may be about 65 / 35-35 / 65, preferably about 60 / 40-40 / 60, more preferably about 55 / 45-40 / 60, even more preferably about 50 / 50-40 / 60, and particularly about 50 / 50-45 / 55. In the present disclosure, by combining the polyamide-based resin (A1) and the polyamide-based resin (A2) in such a ratio, both the adhesion and the heat resistance of the curable resin composition can be achieved in a compatible manner.
[0076] The total ratio of the polyamide resin (A1) and the polyamide resin (A2) in the polyamide resin (A) may be 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. The total ratio may be entirely occupied by the polyamide resin (A1) and the polyamide resin (A2) (100% by mass). If the total ratio of the polyamide resin (A1) and the polyamide resin (A2) is too small, there is a risk that the adhesion of the curable resin composition may not be improved.
[0077] The polyamide resin (A) may optionally contain various additives, for example: a stabilizer, for example, a heat stabilizer, a weather stabilizer, an antioxidant, or a UV absorber; a colorant; a filler; a plasticizer; a lubricant; a flame retardant; an antistatic agent; or a silane coupling agent. The additives may be used alone or in combination of two or more. In the polyamide resin (A), the ratio of the additives may be 10% by mass or less, for example, about 0.01-10% by mass.
[0078] Blocked polyisocyanate (B)
[0079] The polyisocyanate of the blocked polyisocyanate (B) may be any of the following: an aromatic polyisocyanate, an alicyclic polyisocyanate, an aliphatic polyisocyanate, or a heterocyclic polyisocyanate. Examples of the aromatic polyisocyanate include diisocyanates such as toluene diisocyanate (TDI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), naphthalene diisocyanate (NDI), bis(isocyanatophenyl)methane (MDI), 1,3-bis(isocyanatophenyl)propane, bis(isocyanatophenyl)ether, bis(isocyanatophenyl)sulfone, and toluidine diisocyanate (TODI). Examples of the alicyclic polyisocyanate include: diisocyanates such as cyclohexane-1,4-diisocyanate, isophorone diisocyanate (IPDI), hydrogenated xylylene diisocyanate, and hydrogenated bis(isocyanatophenyl)methane; and triisocyanates such as dicycloheptane triisocyanate. Examples of the aliphatic polyisocyanate include: C 2-12 Alkane diisocyanates such as propylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), trimethylhexamethylene diisocyanate (TMDI), and lysine diisocyanate (LDI); alkane triisocyanates such as 1,3,6-hexamethylene triisocyanate and 1,6,11-undecane triisocyanate methyloctane.
[0080] These polyisocyanates can be derivatives thereof, for example: polymers such as dimers, trimers (polyisocyanates with isocyanurate rings), and tetramers; adducts; modified products such as biuret modified products, allophanate modified products, and urea modified products; and urethane oligomers. In particular, the derivatives of the polyisocyanates include: adducts of polyisocyanates (alkane polyisocyanates such as hexamethylene diisocyanate) and polyols (such as trimethylolpropane and pentaerythritol), biuret of the above polyisocyanates, isocyanurates with isocyanurate rings (isocyanurate skeletons) (for example, polyisocyanates with isocyanurate rings as trimers of hexamethylene diisocyanate), and polyisocyanates with isocyanate dimer skeletons.
[0081] Among these polyisocyanates, aliphatic polyisocyanates, aromatic polyisocyanates (such as TDI and MDI) or derivatives thereof (such as HDI or a trimer thereof) are often used.
[0082] Examples of the blocking agent (protective agent) of the blocked polyisocyanate (B) include: alcohols such as isopropanol and 2-ethylhexanol; phenols such as phenol, cresol, xylenol, and resorcinol; oximes such as acetone oxime, methyl ethyl ketone oxime, and cyclohexane oxime; lactams such as ε-caprolactam; and active methylene compounds such as ethyl acetoacetate. These blocking agents can be used alone or in combination of two or more. These blocking agents can be selected according to the type of the polyisocyanate, the dissociation temperature, etc., and phenols, oximes, ε-caprolactams, or active methylene compounds are often used.
[0083] The content of the isocyanate group (blocked isocyanate group) of the blocked polyisocyanate (B) may be, for example, about 5-30% by mass, such as 7.5-25% by mass, and preferably about 10-20% by mass, such as 12.5-17.5% by mass, or may be about 13-20% by mass, such as 14-18% by mass, preferably 15-17% by mass.
[0084] The isocyanate equivalent weight (unit: g / eq. (gram / equivalent)) of the blocked polyisocyanate (B) may be, for example, about 150-350, preferably about 175-300, and more preferably about 200-280, such as 230-275.
[0085] In the blocked polyisocyanate (B), the concentration C of the isocyanate group (blocked isocyanate group) is NCO (Unit: mmol / kg) may be, for example, about 500-5500 such as 750-5250, preferably about 1000-5000 such as 1500-4500, more preferably about 2000-4500 such as 2500-4000, or may be about 3000-4000.
[0086] The blocked polyisocyanate (B) is generally solid at room temperature, and the glass transition temperature of the blocked polyisocyanate (B) may be, for example, about 50-120°C, preferably about 60-110°C, such as 65-95°C, and more preferably about 70-100°C, such as 75-85°C, and typically may be about 65-100°C, such as 70-90°C.
[0087] The melting point of the blocked polyisocyanate (B) may be, for example, about 70-130°C, preferably about 80-120°C, and even more preferably about 90-115°C, or may be about 80-125°C, such as 95-115°C.
[0088] The dissociation temperature of the blocked polyisocyanate (B) (the temperature at which the blocking agent is desorbed (released) and the isocyanate group is regenerated) may be, for example, about 100-220° C., such as 120-200° C., preferably about 130-190° C., such as 140-180° C., and more preferably about 150-170° C., such as 155-165° C. If the dissociation temperature is too low, the storage stability of the curable resin composition tends to decrease. Meanwhile, if the dissociation temperature is too high, the coating film forming temperature or the baking temperature will increase, resulting in reduced processability and the risk of reduced adhesion of the adhesive layer.
[0089] Note that a dissociation catalyst, for example, a tin compound such as dibutyltin laurate, a tertiary amine such as N-methylmorpholine, or a metal organic acid salt such as an alkali metal acetate and an alkaline earth metal acetate may be added to adjust the dissociation temperature.
[0090] The blocked polyisocyanate is generally in the form of a powder in many cases.
[0091] Epoxide (C)
[0092] Examples of epoxy compounds (or epoxy resins) (C) include glycidyl ether compounds, glycidyl ester compounds, glycidyl amine compounds, heterocyclic epoxy compounds, and alicyclic epoxy compounds, and the epoxy compounds (or epoxy resins) (C) have multiple glycidyl groups or oxirane rings. Examples of the glycidyl ether compounds (glycidyl ether epoxy resins) include: bisphenol type epoxy resins, which are epoxy resins based on bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, and bisphenol fluorene; naphthol epoxy resins; biphenyl epoxy resins; trisphenol methane epoxy resins; novolac epoxy resins such as phenol novolac epoxy resins and cresol novolac epoxy resins; and modified novolac epoxy resins.
[0093] Examples of the glycidyl ester compound (glycidyl ester epoxy resin) include polyvalent carboxylic acid glycidyl esters such as diglycidyl phthalate, tetrahydrophthalic acid, and hexahydrophthalic acid.
[0094] Examples of the glycidylamine compound (glycidylamine epoxy resin) include tetraglycidylaminodiphenylmethane and triglycidylaminophenol.
[0095] Examples of the heterocyclic epoxy compound (heterocyclic epoxy resin) include triglycidyl isocyanurate (triazine epoxy resin) and hydantoin epoxy resin.Examples of the alicyclic epoxy compound (alicyclic epoxy resin) include epoxy resins in which a cyclohexene ring is epoxidized.
[0096] These epoxy compounds can be used alone or in combination of two or more. Preferred epoxy compounds are epoxy resins with high softening points or melting points, for example, glycidyl ether epoxy resins, glycidyl amine epoxy resins, and alicyclic epoxy resins, and in particular glycidyl ether epoxy resins (bisphenol-type epoxy resins) based on bisphenols such as bisphenol A. In addition, the epoxy compound may be a monomer, but preferably comprises a polymer (e.g., a polymer that is at least a trimer) such as a dimer, trimer, tetramer, pentamer, and decamer. Such a polymer often has a hydroxyl group as it polymerizes. The ratio of the polymer in gel permeation chromatography may be about 45-99.9%, preferably about 50-99%, and more preferably about 55-98%.
[0097] The epoxy equivalent weight (unit: g / eq.) of the epoxy compound (C) can be selected from the following range: about 250-5000, for example, about 300-3000, such as 400-2500, preferably 500-2000, such as 600-1700, more preferably about 650-1000, such as 700-800, or can be about 450-1500, such as 500-1200, preferably about 550-1000, such as 600-900, and more preferably about 650-800, such as 700-770.
[0098] Epoxy group concentration C of epoxy compound (C) EP (Unit: mmol / kg) may be, for example, about 100-1000, such as 150-900, preferably about 200-800, such as 250-750, more preferably about 300-700, such as 350-650, or may be about 400-600, such as 450-570.
[0099] In addition, the hydroxyl group concentration (unit: mmol / kg) of the epoxy compound (or epoxy resin) (C) may be, for example, about 500-5500, such as 750-5250, preferably about 1000-5000, such as 1500-4500, more preferably about 2000-4500, such as 2500-4000, or may be about 3000-4000, such as 3300-3800.
[0100] The softening point or melting point of the epoxy compound (C) may be, for example, about 75°C or higher, such as 75-125°C, preferably about 80°C or higher, such as 80-115°C, and more preferably about 85°C or higher, such as 90-110°C, or may be about 95-105°C.
[0101] The epoxy compound (C) is generally solid at room temperature and is often in the form of a powder.
[0102] Since the epoxy compound (C) is reactive with the amino group of the polyamide resin (A) and improves the adhesion to the substrate such as metal, the adhesion to the substrate such as metal is greatly improved. In addition, the epoxy compound of the polymer (including dimer, trimer, etc.) may have a hydroxyl group (secondary hydroxyl group). The hydroxyl group is reactive with the blocked polyisocyanate (B) and participates in the adhesion to the substrate such as metal, thereby further improving the adhesion to the substrate.
[0103] The ratio of each component
[0104] In the present disclosure, the amino group (and carboxyl group) of the polyamide resin (A), the isocyanate group of the blocked polyisocyanate (B), and the epoxy group (and hydroxyl group) of the epoxy compound (C) react in a complex manner and appear to adhere to a substrate such as a metal with high adhesion. For example, typically, it appears that the isocyanate group of the blocked polyisocyanate (B) reacts with the amino group (and hydroxyl group of the epoxy compound (C)) of the polyamide resin (A), while the epoxy group of the epoxy compound (C) reacts with the amino group (and carboxyl group) of the polyamide resin (A), thereby forming an adhesive layer (cured film or primer layer) on the substrate. Therefore, the ratio of each component and the ratio of the reactive groups of each component also become complex.
[0105] The quantitative ratio of the polyamide resin (A) can be selected based on the concentration of the reactive group of each component, and can be, for example, about 50-95% by mass, such as 60-90% by mass, but is usually about 65-90% by mass, such as 65-85% by mass, preferably about 67-83% by mass, such as 70-80% by mass, or can be about 70-90% by mass, such as 75-85% by mass, relative to 100% by mass of the total amount of the polyamide resin (A), the blocked polyisocyanate (B), and the epoxy compound (C). When the ratio of the polyamide resin (A) is too small or too large, the adhesion to the substrate tends to decrease.
[0106] It seems that the blocked polyisocyanate (B) reacts with the amino group of the polyamide resin (A) to greatly improve the mechanical strength and thermal properties of the adhesive layer, thereby improving the adhesion to the substrate. Therefore, the quantitative ratio of the polyamide resin (A) and the blocked polyisocyanate (B) can be selected based on the concentration, reactivity, etc. of the functional groups (reactive groups) of each component. The ratio of the isocyanate group (blocked isocyanate group) of the blocked polyisocyanate (B) relative to the amino group of 1 mol concentration of the polyamide resin (A) can be, for example, about 0.5-7 mol, such as 0.7-6 mol, preferably about 1-5 mol, but can be typically selected from the range of excess moles, such as about 1.1-5.5 mol, and can be, for example, about 1.5-5 mol, such as 1.75-4.5 mol, preferably about 2-4 mol, such as 2.25-3.75 mol, and more preferably about 2.5-3.5 mol, such as 2.75-3.4 mol. When the ratio of the blocked polyisocyanate is too small, there is a risk that the adhesion and heat resistance to substrates such as metals will be reduced. At the same time, when the ratio is too large, free polyisocyanates remain, which appear to deteriorate the properties of the adhesive layer. In addition, when an excess amount of blocked polyisocyanate (B) is used, the reactivity with the molding resin of the composite molding component (for example, a thermoplastic resin with reactive groups such as hydroxyl or amino groups, and examples are polyester resins and polyamide resins) can also be improved, and the adhesion to the molding resin can also be improved. This may be because even when the adhesive layer is cured, the adhesive layer also acts as an active primer layer (active intermediate layer).
[0107] In particular, the isocyanate group (NCO) concentration C of the blocked polyisocyanate (B) is NCO (mmol / kg) to the amino concentration C of polyamide resin (A) NH2 The ratio of (mmol / kg) to (mmol / kg) is not particularly limited, and the amino group concentration may be excessive, but generally the isocyanate group concentration is high. For example, the isocyanate group (NCO) concentration (mmol / kg) is often excessive relative to the amino group (NH2) concentration (mmol / kg). The isocyanate group concentration (C NCO ) and the amino concentration (C NH2 ) between (Δ(C NCO -C NH2)) may be, for example, about 15-450mmol / kg, for example, 20-400mmol / kg, preferably about 30-300mmol / kg, for example, 35-250mmol / kg, and more preferably about 40-200mmol / kg, for example, 45-185mmol / kg, or may be 20mmol / kg or more, preferably 30mmol / kg or more, and more preferably 40mmol / kg or more. Relative to the total molar number of amino groups of polyamide resin (A), the total molar number of isocyanate groups of blocked polyisocyanate (B) may be, for example, about 1.3-50 times, for example, 1.5-40 times, preferably about 2-35 times, for example, 2.5-25 times, more preferably about 2.7-15 times, for example, 3-10 times, or may be about 2.7-10 times, for example, 3-8.5 times.
[0108] The ratio of the blocked polyisocyanate (B) may be about 2.5-35 parts by mass, preferably about 5-30 parts by mass, such as 7.5-25 parts by mass, and more preferably about 10-20 parts by mass, such as 10-15 parts by mass, relative to 100 parts by mass of the polyamide resin (A).
[0109] The ratio of the epoxy group of the epoxy compound (C) relative to the amino group of 1 mol concentration of the polyamide resin (A) may be, for example, about 0.1-1 mol, for example, 0.2-0.9 mol, preferably about 0.2-0.8 mol, for example, 0.25-0.7 mol, more preferably about 0.3-0.6 mol, for example, 0.35-0.55 mol, or may be about 0.35-0.6 mol, for example, 0.4-0.5 mol. Note that the ratio (mmol / kg) of the carboxyl group of the polyamide resin (A) to the epoxy group of the epoxy compound (C) may be, for example, about 0.01 / 1-0.5 / 1, for example, 0.02 / 1-0.4 / 1, preferably about 0.03 / 1-0.3 / 1, for example, 0.04 / 1-0.2 / 1, and more preferably about 0.05 / 1-0.2 / 1, for example, 0.06 / 1-0.15 / 1 in the form of the former / the latter.
[0110] The ratio (mmol / kg) of the isocyanate group of the blocked polyisocyanate (B) to the hydroxyl group (secondary hydroxyl group) of the epoxy compound (C) can be, for example, about 0.5 / 1-1.5 / 1, such as 0.7 / 1-1.3 / 1, and preferably about 0.8 / 1-1.2 / 1, such as 0.9 / 1-1.1 / 1, in the form of the former / the latter.
[0111] Note that the mass ratio of the blocked polyisocyanate (B) to the epoxy compound (C) may be about 20 / 80-80 / 20, preferably about 30 / 70-70 / 30, and more preferably about 40 / 60-60 / 40 in the form of the former / the latter.
[0112] Epoxy group concentration C relative to the total amount (total moles) of amino groups, isocyanate groups, and epoxy groups (mmol / kg) EP It may be, for example, about 2-40 mol%, such as 3-35 mol%, but may generally be about 5-30 mol%, such as 5-25 mol%, preferably about 7-25 mol%, such as 8-20 mol%, and more preferably about 10-20 mol%, such as 10-18 mol%, or may be 6 mol% or more, and more preferably 8 mol% or more. In particular, when the isocyanate group concentration C NCO As mentioned above, relative to the amino concentration C NH2 Excess, and the epoxy group concentration C EP At the ratio described above, heat resistance can be further improved.
[0113] Relative to 100 parts by mass of the polyamide resin (A), the ratio of the epoxy compound (C) may be, for example, about 2.5-35 parts by mass, preferably about 5-30 parts by mass, such as 7.5-25 parts by mass, and more preferably about 10-20 parts by mass, such as 10-15 parts by mass, or may be about 10-22 parts by mass. When the ratio of the epoxy compound (C) is too small, the adhesion to the substrate such as metal tends to decrease. At the same time, when the ratio of the epoxy compound (C) is too large, the epoxy compound (C) remains, which appears to deteriorate the properties of the adhesive layer. Note that when an excess amount of the epoxy compound (C) is used, the reactivity with the molding resin of the composite molding component (for example, a thermoplastic resin having a reactive group such as a carboxyl group or an amino group, and examples are polyester resins and polyamide resins) may also be improved, and the adhesion to the molding resin may also be improved. This may be because even when the adhesive layer is cured, the adhesive layer also acts as an active primer layer (active intermediate layer).
[0114] Form of curable resin composition
[0115] The curable resin composition of the present disclosure may be a liquid composition (solution composition or dispersion) containing a solvent, or may have a powdery or granular form. The curable resin composition may generally be a mixture (powdered mixture or granular mixture) of a granular (powdered) polyamide resin (A), a granular blocked polyisocyanate (B), and a granular epoxy compound (C). The curable resin composition may also be in the form of a powdery or granular material (a composition solidified into a block) of the composition in which the above components (polyamide resin (A), blocked polyisocyanate (B), and epoxy compound (C)) are mixed.
[0116] The average particle size D50 of each of the components in the form of powder or granular material (polyamide-based resin (A), blocked polyisocyanate (B), and epoxy compound (C)) can be selected from, for example, the range of about 1-300 μm, and typically can be about 2-200 μm, such as 5-150 μm, preferably about 10-100 μm, such as 15-80 μm, and more preferably about 20-70 μm, as long as the uniformity of the coating film is not impaired.
[0117] Although the curable resin composition of the present disclosure may be a solution, when the curable resin composition is in a solid state (in the form of a powder or granular material), even when the amino group of the polyamide resin (A), the isocyanate group of the blocked polyisocyanate (B), and the epoxy group of the epoxy compound (C) are reactive to each other, the reaction between the components can be suppressed, resulting in high storage stability. In addition, as described above, the curable resin composition of the present disclosure exhibits high adhesiveness or adhesion to a substrate (e.g., a metal substrate). Therefore, the curable resin composition of the present disclosure is effective in improving corrosion resistance, durability, etc. by covering or coating a substrate (or member) with a coating film to protect the substrate.
[0118] The curable resin composition of the present disclosure may further include common additives. In addition to the additives exemplified in the section about polyamide resin (A), examples of common additives include, for example, curing agents and curing accelerators. These additives may be used alone or in combination of two or more. In the composition, the ratio of the additive may be 10% by mass or less, for example, about 0.01-10% by mass.
[0119] Composite component and method for manufacturing the same
[0120] The composite member can be produced by coating the surface of a substrate (or member) with the curable resin composition (adhesive resin composition) to form an adhesive layer (cured film or primer layer).
[0121] The type of the substrate is not particularly limited, and examples include: metals, for example, iron or iron alloys such as stainless steel, aluminum or aluminum alloys, copper, and zinc; ceramics, for example, pottery, porcelain, oxide-based ceramics, nitride-based ceramics, and boride-based ceramics; plastics, for example, thermosetting or photocurable resins such as epoxy-based resins, phenol-based resins, and polyimide-based resins, or heat-resistant thermoplastic resins (for example, engineering plastics) such as polyalkylene glycol arylate resins, polyarylate resins, aromatic polyamide resins, polycarbonate resins, polyurethane resins, thermoplastic polyimide resins, polyphenylene ether resins, polyether ketone resins, polyether ether ketone resins, polyphenylene sulfide resins, polysulfone resins, polyether sulfone resins, and liquid crystal plastic molded products; and wood. The substrate may be a composite substrate, for example: a substrate provided with a vapor deposition film or the like; and a laminate substrate, for example, a laminate of a metal and a heat-resistant thermoplastic resin.
[0122] Preferred substrates are metals such as iron (eg, steel plate), aluminum, or alloys thereof (eg, stainless steel). Depending on the type, these substrates may be subjected to surface treatments such as degreasing, polishing, electrochemical machining, and rough surface machining.
[0123] Can use common application or coating method to base material with described curable resin composition coating.Meanwhile, in the case of described curable resin composition in powder form, powder coating method such as fluidized bed coating (it is the method that forms coating film by immersing base material such as heated metal in powder or granular material in fluid phase), electrostatic powder coating and electrodeposition coating such as cationic electrodeposition coating can be used.Note, in the hot spray method etc. that is coated after melting step, before forming coating film, along with melting and heating, each reactive group in component can react with each other.Described electrostatic powder coating method can be, for example, electrostatic spray method or electrostatic fluidized bed coating method (wherein powder is electrostatically attracted and adhered to base material to form coating film fluidized bed coating method).In order to form uniform coating film (adhesive layer) on the surface of base material, can adopt the electrostatic powder coating method with little thermal history that can suppress the consumption of reactive group in each component.
[0124] In order to react the polyamide resin (A), the blocked polyisocyanate (B), and the epoxy compound (C) with each other, the coating film may be formed by heating (or baking) to form a cured film. The heating temperature (or baking temperature) may be, for example, about 150-250° C., preferably about 170-230° C., more preferably about 175-200° C., and even more preferably about 180-190° C. In addition, the heating time (or baking time) may be, for example, about 1-10 minutes, preferably about 2-8 minutes, and more preferably about 3-6 minutes.
[0125] The thickness of the coating film (adhesive layer or cured film) formed in this manner may be, for example, about 1-500 μm, and may typically be about 5-250 μm, preferably about 10-200 μm, and more preferably about 25-175 μm such as 50-150 μm.
[0126] Such an adhesive layer not only exhibits high adhesion to a substrate or a member but also has high heat resistance, etc. Therefore, even when the thermoplastic resin is molded, no void is generated at the interface between the substrate and the adhesive layer (or cured film) regardless of the molding conditions, which is useful for forming a uniform molded part with high adhesion and durability.
[0127] Composite molded component and method for manufacturing the same
[0128] The composite molded member can be produced by molding or laminating a composition containing at least a thermoplastic resin on an adhesive layer of the above-mentioned composite member (a composite member having a substrate such as a metal substrate and an adhesive layer formed on a surface of the substrate).
[0129] The type of the thermoplastic resin is not particularly limited, and examples include: olefin-based resins, such as polyethylene-based resins, polypropylene-based resins, modified or copolymerized olefin-based resins, and cyclic olefin-based resins; styrene-based resins, such as styrene-based copolymers such as acrylonitrile-styrene-based resins (AS resins), high-impact polystyrene resins, and rubber-reinforced styrene-based resins such as acrylonitrile-styrene-butadiene resins (ABS resins); (meth)acrylic resins; vinyl acetate resins, or derivatives thereof, such as polyvinyl alcohol resins and polyvinyl acetal resins; vinyl chloride resins; polyester-based resins, such as, Polyalkylene glycol arylate resin or polyarylate resin such as polyethylene terephthalate resin, polybutylene terephthalate resin, and polyethylene naphthalate resin; polyamide resin; polycarbonate resin; polyurethane resin; thermoplastic polyimide resin; polyacetal resin; polyether resin such as polyphenylene ether resin, polyether ketone resin, and polyether ether ketone resin; polyphenylene sulfide resin; polysulfone resin such as polysulfone resin and polyether sulfone resin; liquid crystal plastic such as liquid crystal aromatic polyester resin; and thermoplastic elastomer such as olefin-based elastomer, styrene-based elastomer, polyester-based elastomer, polyamide-based elastomer, polyurethane-based elastomer, and fluorine-based elastomer. Depending on the application, rubber (or unvulcanized rubber composition) such as ethylene-propylene-diene rubber may also be used. These thermoplastic resins may be used alone or in combination of two or more.
[0130] The thermoplastic resin may have functional groups (reactive groups) such as hydroxyl, carboxyl, amino and blocked isocyanate groups. Note that it is expected that the adhesion improved due to the reaction with the molding resin or the laminated sheet (this may be because the adhesive layer is active). In particular, when reactive groups such as amino, isocyanate groups, and / or epoxy groups (especially, at least isocyanate groups) remain in the adhesive layer, the adhesive layer is also active even after curing. Therefore, the reactive groups remaining in the adhesive layer can react with the functional groups (reactive groups) of the thermoplastic resin to improve the adhesion to the molding resin or the laminated sheet.
[0131] In an embodiment of the present invention, a thermoplastic resin having a melting point or a glass transition temperature less than or equal to the melting point of the polyamide resin of the curable resin composition may also be molded. At the same time, when a thermoplastic resin having a melting point higher than the melting point of the polyamide resin is molded, a resin molded portion or a laminated portion having high adhesion and durability and not generating a gap at the interface between a substrate such as a metal and the adhesive layer may still be formed. Therefore, in order to form a resin molded portion or a laminated portion having high heat resistance and durability, the thermoplastic resin may have a melting point or a glass transition temperature greater than or equal to the melting point of the polyamide resin. Depending on the type of the thermoplastic resin, the melting point or glass transition temperature of such a thermoplastic resin may be, for example, about 100-350° C., such as 160-330° C., preferably about 170-300° C., such as 200-280° C., and may typically be about 180-270° C., such as 190-260° C., preferably about 200-250° C., such as 200-240° C. In particular, the melting point of the thermoplastic resin (especially in the case of a polyamide-based resin) may be, for example, about 200-250° C., preferably about 210-240° C., more preferably about 215-230° C., and particularly about 220-230° C.
[0132] Preferred thermoplastic resins may be, for example, aromatic polyester resins, such as polyalkylene glycol aromatic ester resins or polyarylate resins, which may have hydroxyl groups and / or carboxyl groups at the terminals, or may be polyamide-based resins which may have amino groups and / or carboxyl groups, and in particular, may be polyamide-based resins having amino groups. Examples of the polyamide-based resins include: polyamide 46; polyamide 6; polyamide 66; alicyclic polyamides containing alicyclic diamine components and / or alicyclic dicarboxylic acid components as polymerization components; polyamide MXD-6, which is a polyamide resin containing at least xylene diamine and adipic acid as reaction components; and non-crystalline polyamides, such as polyamide resins containing at least terephthalic acid and trimethylhexamethylene diamine as reaction components. Note that the amino group concentration and carboxyl group concentration of the polyamide-based resin are the same as those described above. Among these, aliphatic polyamides are preferred, and polyamide 6 is particularly preferred.
[0133] The thermoplastic resin may optionally contain a variety of additives, such as: stabilizers, such as heat-resistant stabilizers, weather-resistant stabilizers, antioxidants, and UV absorbers; colorants; magnetic materials, such as paramagnetic materials such as ferrites and ferromagnetic materials such as magnets; fillers; reinforcing agents; plasticizers; lubricants; flame retardants; antistatic agents; and silane coupling agents. Additives can be used alone or in combination of two or more. The reinforcing agent may be a granular reinforcing agent, such as calcium carbonate, barium sulfate, titanium oxide, silicon dioxide, aluminum oxide, mica, clay, talc, and carbon black, or may be a fibrous reinforcing agent, such as organic fibers such as rayon, nylon, vinylon, and aramid, and inorganic fibers such as glass fibers, carbon fibers, metal fibers, and whiskers. Preferred reinforcing agents are fibrous reinforcing agents such as glass fibers. Relative to 100 parts by mass of the thermoplastic resin, the content of the reinforcing agent may be, for example, about 5-50 parts by mass, and preferably about 10-40 parts by mass.
[0134] The composition containing the thermoplastic resin can be molded (overmolded (over-injection molding) or molded), or laminated on the adhesive layer in the form of a sheet. The molding of the thermoplastic resin composition can be carried out according to a commonly used insert molding method. A composite molded component in which a molded portion of the thermoplastic resin composition is formed in a laminated form on the adhesive layer of the composite component can be obtained by melting the thermoplastic resin composition and molding using injection molding or the like. For example, a thermoplastic resin composition, a thermoplastic resin composition containing the magnetic material, or a thermoplastic resin composition containing a reinforcing agent such as glass fiber can be melted, kneaded, and injection molded on the adhesive layer to prepare a composite molded product in which a resin layer, a magnetic layer, or a reinforcing layer is formed on a substrate such as a metal.
[0135] In addition, the thermoplastic resin composition may be directly laminated on the adhesive layer in the form of a molten sheet after undergoing melt extrusion molding in the form of a sheet. Alternatively, a thermoplastic resin composition containing a reinforcing agent such as glass fiber may be molded into the form of a sheet or tape (e.g., an oriented sheet or tape (unidirectional material) in which a fibrous reinforcing agent is oriented in a predetermined direction), and the molded sheet or tape may be directly laminated (laminated after heating) on the adhesive layer. Note that by laminating an oriented sheet or tape, a composite molded product having excellent mechanical properties can be manufactured even if the thickness of a substrate such as a metal is small.
[0136] In an embodiment of the present invention, even if the heating temperature for molding or laminating the thermoplastic resin is relatively low, the composition comprising the thermoplastic resin can be firmly and stably adhered to the substrate. The heating temperature (e.g., the barrel temperature of injection molding) may be 280° C. or lower, for example, about 230-280° C., preferably about 240-275° C., more preferably about 250-270° C., and even more preferably about 260-270° C.
[0137] Example
[0138] Hereinafter, the present invention is described in more detail based on Examples, but the present invention is not limited to these Examples. The following materials were used in the following Examples and Comparative Examples.
[0139] Substrate
[0140] The steel plate (stainless steel plate SUS430, available from Nippon Testpanel Co., Ltd) was used after degreasing.
[0141] Polyamide resin
[0142] PA12: Polyamide 12 (available from Daicel-Evonik Ltd., having a water absorption of 0.25%, an amino group concentration of 145 mmol / kg, a carboxyl group concentration of 4 mmol / kg, a number average molecular weight of 13423, and an average particle size of 47 μm when in powder form)
[0143] coPA: copolyamide 6 / 66 / 12 (available from Daicel-Evonik Ltd., having a water absorption of 1.5%, an amino group concentration of 187 mmol / kg, a carboxyl group concentration of 1.5 mmol / kg, a number average molecular weight of 10610, and an average particle size of 42 μm when in powder form)
[0144] Note that the water absorption is measured using the water absorption test specified in ASTM D570. In addition, the amino group concentration and the carboxyl group concentration are measured by the above-mentioned neutralization titration method. In addition, the average particle size is measured using a particle size distribution measuring device using a laser diffraction / scattering method, in which the polyamide resin is frozen and pulverized.
[0145] Blocked isocyanate
[0146] b-NCO: blocked isocyanate ("VESTAGON BF 1540", isocyanate dimer polyisocyanate adduct, available from Evonik, having an isocyanate group concentration of 3600 mmol / kg, a glass transition temperature of 84° C. or less, and in a powder form)
[0147] Note that the isocyanate group concentration is calculated from the isocyanate content.
[0148] Epoxides
[0149] Epoxy: Bisphenol A epoxy resin (available from Mitsubishi Chemical Corporation, having an epoxy group concentration of 500 mmol / kg, a hydroxyl group concentration of 3600 mmol / kg, and in powder form)
[0150] The epoxy group concentration is calculated from the epoxy equivalent weight, and the hydroxyl group concentration is calculated based on the number of repeating units obtained from the molecular weight of the epoxy resin.
[0151] Molding resin
[0152] PA6: "CM1011GF30", available from Toray Industries, Inc., has an equilibrium water absorption of 2.5% at 23°C and 50% Rh (The Toray Method / Japan Engineering Plastics Technical Committee, 12th Edition, April 2015).
[0153] Examples and Reference Examples Composite members were prepared by mixing polyamide resin powder, blocked polyisocyanate powder, and epoxy resin powder in the ratios shown in Table 1 to prepare a powder mixture, electrostatically coating the powder mixture on a degreased substrate to a thickness of about 100 μm, and placing the resulting article in an oven and heating at 185° C. for 5 minutes to form a coating film.
[0154] A composite molded article was prepared by injection molding (insert molding) molding resin PA6 on the coating film of the composite member at a cylinder temperature of 280° C. or 270° C. using an injection molding machine (“ET40V”, available from Toyo Machinery & Metal Co., Ltd.) to form a resin layer having a thickness of 3 mm.
[0155] Adhesive strength
[0156] The adhesive strength of the resin layer of the obtained composite molded article to the substrate was measured according to ISO 19095-2 Type B at an adhesion test temperature of from 23 to 80°C.
[0157] The results are shown in Table 1.
[0158] [Table 1]
[0159] Table 1
[0160]
[0161] As revealed by the results shown in Table 1, at a cylinder temperature of 270° C. or 280° C., the resin composition of the Examples exhibited high adhesive strength even when the adhesion test temperature was increased.
[0162] Industrial Applicability
[0163] The curable resin composition of the present disclosure is suitable for use as an adhesive resin composition for manufacturing a composite molded product (hybridized component) in which a substrate such as metal and resin are compounded (hybridized). The composite molded product obtained according to an embodiment of the present invention can be used for applications where high durability is required, such as the following: vehicles such as automobiles, trains, airplanes or aircraft, and ships, or structural members or underbody members (suspension, wheels, brakes, etc.) of vehicles (transportation equipment or transportation vehicles); and parts or components (structural members, etc.) of track structures, such as rail structures. In particular, the composite molded component can be applied to vehicle structural members (automobile parts or components, etc.) such as front ends (bumpers).
Claims
1. A curable resin composition, which is an adhesive resin composition for producing a composite molded product requiring high durability, wherein the resin composition include: A polyamide resin (A) having an amino group; Blocked polyisocyanate (B); and Epoxy compound (C), wherein The polyamide-based resin (A) comprises a polyamide-based resin (A1) having a melting point of 170° C. or higher and a water absorption of 1% by mass or less and a polyamide-based resin (A2) having a melting point of 150° C. or lower and a water absorption of 5% by mass or less; and The mass ratio of the polyamide-based resin (A1) to the polyamide-based resin (A2) is 60 / 40 to 40 / 60 in the form of the former / the latter. 2 . The curable resin composition according to claim 1 , wherein the polyamide-based resin (A) is in a granular form. 3 . The curable resin composition according to claim 1 , wherein the curable resin composition is a granular mixture. 4 . The curable resin composition according to claim 1 , wherein the amino group concentration of the polyamide-based resin (A1) and the amino group concentration of the polyamide-based resin (A2) are each 80 mmol / kg or more.
5. The curable resin composition according to claim 1 or 2, wherein The blocked polyisocyanate (B) has a glass transition temperature of 60-110° C., a melting point of 70-130° C., and a dissociation temperature of 120-200° C.; and The epoxy compound (C) includes a bisphenol type epoxy resin having a softening temperature of 75° C. or higher.
6. The curable resin composition according to claim 1 or 2, wherein The ratio of the isocyanate group of the blocked polyisocyanate (B) is 1.5-5 mol relative to 1 mol of the amino group of the polyamide resin (A); and The ratio of the epoxy group of the epoxy compound (C) is 0.1-0.8 mol relative to 1 mol of the amino group of the polyamide resin (A).
7. The curable resin composition according to claim 1 or 2, wherein The isocyanate group of the blocked polyisocyanate (B) is in excess of 15-450 mmol / kg relative to the amino group of the polyamide resin (A); and The concentration of the epoxy group is 3 to 35 mol % relative to the total molar number of the amino group, the isocyanate group, and the epoxy group.
8. The curable resin composition according to claim 1 or 2, wherein The total molar number of the isocyanate groups of the blocked polyisocyanate (B) is 1.3-50 times the total molar number of the amino groups of the polyamide resin (A); and The blocked polyisocyanate (B) is contained in an amount of 5 to 30 parts by mass based on 100 parts by mass of the polyamide resin (A), and the epoxy compound (C) is contained in an amount of 5 to 30 parts by mass based on 100 parts by mass of the polyamide resin (A). 9 . A composite member, wherein an adhesive layer of the curable resin composition according to claim 1 is formed on a surface of a substrate.
10. A method for producing a composite component, wherein include: The surface of a substrate is coated with the curable resin composition according to any one of claims 1 to 8 to form an adhesive layer. 11 . A composite molded member, wherein a composition containing at least a thermoplastic resin is molded or laminated on the adhesive layer of the composite member according to claim 9 .
12. The composite molded member according to claim 11, wherein The substrate is a metal substrate; and the thermoplastic resin includes a polyamide-based resin having a melting point higher than that of the polyamide-based resin (A).
13. A method for producing a composite molded component, wherein include: A composition containing at least a thermoplastic resin is molded or laminated on the adhesive layer of the composite structural member according to claim 9 .
Citation Information
Patent Citations
Hybrid member containing reactive hot melt adhesive
JP2007190917A
Hybrid components containing reactive hotmelt adhesives
US20110143142A1
Curable resin composition, composite member, and production method therefor
CN112638979A
Bonding coating material for voice coil, winding cylinder and voice coil
JP1997227827A