Active matrix substrate and method for manufacturing the same

By adopting a specific laminated film structure and etching process in the active matrix substrate, the problem of high contact resistance of the source contact part in the lower source structure substrate is solved, and the low resistance between the oxide semiconductor TFT and the source bus is achieved Contact simplifies the manufacturing process.

CN113257835BActive Publication Date: 2024-11-26SHARP KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110096761.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-02-07
Filing Date
2021-01-25
Publication Date
2024-11-26
Estimated Expiration
2041-01-25

AI Technical Summary

Technical Problem

In the lower source structure substrate, it is difficult to reduce the contact resistance of the source contact portion, and it is difficult to form a good contact between the oxide semiconductor layer of the oxide semiconductor TFT and the source bus, resulting in difficult to suppress the contact resistance.

Method used

An active matrix substrate structure is adopted, in which a source contact hole is formed between the oxide semiconductor layer of the oxide semiconductor TFT and the source bus through a specific laminated film structure and an etching process, and a connecting electrode is formed using the same conductive film material to Reduce contact resistance and optimize the etching process of the insulating layer through the thinned region to reduce the manufacturing process and use of photomasks.

Benefits of technology

The contact resistance between the oxide semiconductor layer and the source bus of the oxide semiconductor TFT is effectively reduced, the number of manufacturing processes and the use of photomasks is reduced, the effect of suppressing contact resistance is improved, and the process damage of the oxide semiconductor layer is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113257835B_ABST
    Figure CN113257835B_ABST
Patent Text Reader

Abstract

An active matrix substrate comprises a plurality of gate bus lines, a plurality of source bus lines, a lower insulating layer, an interlayer insulating layer, a plurality of oxide semiconductor TFTs, pixel electrodes and a plurality of source contacts, wherein each oxide semiconductor TFT comprises: an oxide semiconductor layer, which is arranged on the lower insulating layer; a gate electrode, which is arranged on a portion of the oxide semiconductor layer via the gate insulating layer; and a source electrode, which is formed between the substrate and the lower insulating layer and is formed of the same conductive film as the source bus lines, and each source contact comprises: a source contact hole, which is formed in the lower insulating layer and the interlayer insulating layer and exposes a portion of a first region of the oxide semiconductor layer and a portion of a source electrode in one oxide semiconductor TFT; and a connecting electrode, which is arranged on the interlayer insulating layer and in the source contact hole and is connected to a portion of the first region and a portion of the source electrode in the source contact hole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an active matrix substrate and a method for manufacturing the same. Background Art

[0002] Display devices having an active matrix substrate in which a switching element is provided for each pixel have been widely used. An active matrix substrate having a thin film transistor (Thin Film Transistor: hereinafter referred to as "TFT") as a switching element is called a TFT substrate. In addition, in this specification, the portion of the TFT substrate corresponding to the pixel of the display device is referred to as a pixel area or a pixel. In addition, the TFT provided as a switching element in each pixel of the active matrix substrate is referred to as a "pixel TFT". A plurality of source bus lines and a plurality of gate bus lines are provided in the TFT substrate, and a pixel TFT is arranged near their intersection. The source electrode of the pixel TFT is connected to one of the source bus lines, and the gate electrode is connected to one of the gate bus lines.

[0003] In recent years, it has been proposed to use oxide semiconductors instead of amorphous silicon and polycrystalline silicon as the material of the active layer of TFT. This type of TFT is called "oxide semiconductor TFT". Oxide semiconductors have a higher mobility than amorphous silicon. Therefore, oxide semiconductor TFTs can operate at a higher speed than amorphous silicon TFTs. In addition, oxide semiconductor films are formed by a simpler process than polycrystalline silicon films, so they can also be used in devices that require a large area.

[0004] Most oxide semiconductor TFTs are bottom-gate TFTs, but top-gate oxide semiconductor TFTs have also been proposed (for example, Patent Document 1 and Patent Document 2).

[0005] Patent Document 1 discloses a top-gate TFT in which a gate electrode is disposed on a portion of an oxide semiconductor layer via a gate insulating layer, and source and drain electrodes are disposed on an insulating layer covering the gate electrode.

[0006] On the other hand, Patent Document 2 of the applicant of the present application proposes a substrate structure in which a source electrode and a source bus are arranged on the substrate side closer to the gate bus (hereinafter referred to as the "lower source structure"). In this structure, the source bus is arranged on the substrate side closer to the oxide semiconductor layer of the oxide semiconductor TFT, and the gate bus is arranged above the oxide semiconductor layer. According to the TFT substrate with a lower source structure (hereinafter referred to as the "lower source structure substrate"), the insulating layer between the source bus and the gate bus can be thickened, thereby reducing the parasitic capacitance generated at the intersection of these buses.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2015-109315

[0010] Patent Document 2: International Publication No. 2015 / 186619 Summary of the invention

[0011] Problem that the invention aims to solve

[0012] In the lower source structure substrate, for example, the active layer of the pixel TFT is arranged on the insulating layer (lower insulating layer) covering the corresponding source bus, and is connected to the source bus in a contact hole (source contact hole) formed in the lower insulating layer. In this specification, the connection portion that electrically connects the active layer of the pixel TFT to the source bus is referred to as a "source contact portion".

[0013] According to research conducted by the inventors of the present application, it has been found that it is difficult to reduce the contact resistance of the source contact portion in the lower source structure substrate.

[0014] In conventional lower source structure substrates, for example, after forming a source contact hole in the lower insulating layer to expose a portion of the source bus line, the exposed surface of the source bus line may be damaged during processing, resulting in failure to form a good contact between the source bus line and the oxide semiconductor layer.

[0015] In addition, when an oxide semiconductor TFT is used as a pixel TFT, the oxide semiconductor layer of the oxide semiconductor TFT is connected to the upper surface of the source bus in the source contact portion. If the source bus is formed of a low-resistance metal film such as a Cu film in order to reduce the wiring resistance of the source bus, it is difficult to suppress the contact resistance of the source contact portion to be low because the low-resistance metal film such as the Cu film and the oxide semiconductor layer do not easily form an ohmic junction.

[0016] In addition, in order to reduce the contact resistance of the source contact portion, for example, a stacked film with a Cu film as the main layer and a Ti film as the upper layer can be considered as the source bus. The Ti film can form an ohmic junction with the oxide semiconductor layer, so compared with the case where the source bus is formed only by the Cu film, the contact resistance between the source bus and the oxide semiconductor layer can be reduced. However, when such a stacked film is patterned to form a source bus, after wet etching the Cu film, it is necessary to dry etch the Ti film separately, which increases the number of manufacturing steps.

[0017] One embodiment of the present invention provides an active matrix substrate including an oxide semiconductor TFT as a pixel TFT and capable of reducing the contact resistance between an oxide semiconductor layer of the oxide semiconductor TFT and a source bus line.

[0018] Solutions for solving problems

[0019] This specification discloses an active matrix substrate and a method for manufacturing the active matrix substrate described in the following items.

[0020] [Item 1] An active matrix substrate having a plurality of pixel regions and comprising:

[0021] substrate;

[0022] A plurality of gate bus lines and a plurality of source bus lines supported on the main surface of the substrate, wherein the plurality of source bus lines are located closer to the substrate than the plurality of gate bus lines;

[0023] a lower insulating layer, located between the plurality of source bus lines and the plurality of gate bus lines, and covering the plurality of source bus lines;

[0024] an interlayer insulating layer covering the plurality of gate bus lines;

[0025] a plurality of oxide semiconductor TFTs arranged corresponding to the plurality of pixel regions; and

[0026] A pixel electrode is disposed in each of the plurality of pixel regions.

[0027] Each of the plurality of oxide semiconductor TFTs has:

[0028] an oxide semiconductor layer, which is disposed on the lower insulating layer, and includes a channel region and a first region and a second region respectively located on both sides of the channel region, the first region being electrically connected to a corresponding one of the plurality of source bus lines, and the second region being electrically connected to the pixel electrode;

[0029] a gate electrode disposed on a portion of the oxide semiconductor layer via a gate insulating layer and electrically connected to a corresponding one of the plurality of gate bus lines, wherein the gate electrode and the plurality of gate bus lines are formed of the same conductive film; and

[0030] a source electrode formed between the substrate and the lower insulating layer and electrically connected to a corresponding one of the plurality of source bus lines, wherein the source electrode and the plurality of source bus lines are formed of the same conductive film,

[0031] The active matrix substrate further includes a plurality of source contacts each electrically connecting one of the plurality of oxide semiconductor TFTs to the corresponding one of the source bus lines, each of the source contacts having:

[0032] a source contact hole formed in the lower insulating layer and the interlayer insulating layer and exposing a portion of the first region of the oxide semiconductor layer and a portion of the source electrode in the one oxide semiconductor TFT, the source contact hole including a lower opening formed in the lower insulating layer and an upper opening formed in the interlayer insulating layer; and

[0033] A connecting electrode is arranged on the interlayer insulating layer and in the source contact hole, and is connected to the portion of the first region and the portion of the source electrode in the source contact hole.

[0034] [Item 2] The active matrix substrate according to Item 1,

[0035] In the source contact hole, a side surface of the oxide semiconductor layer is aligned with a side surface of the lower opening.

[0036] [Item 3] The active matrix substrate according to Item 1 or 2,

[0037] In each of the source contact portions, when viewed in the normal direction of the substrate, an edge portion of the oxide semiconductor layer extends across the upper opening portion of the source contact hole.

[0038] [Item 4] The active matrix substrate according to Item 1 or 2,

[0039] In each of the source contacts, the first region of the oxide semiconductor layer has a first opening.

[0040] When viewed in a normal direction to the substrate, the first opening of the oxide semiconductor layer is located inside the upper opening of the source contact hole.

[0041] [Item 5] The active matrix substrate according to any one of Items 1 to 4,

[0042] Each of the oxide semiconductor TFTs further includes a drain electrode formed on the interlayer insulating layer and electrically connected to a corresponding one of the plurality of pixel electrodes.

[0043] The connection electrode of each of the source contacts is formed of the same conductive film as the drain electrode of each of the oxide semiconductor TFTs.

[0044] [Item 6] The active matrix substrate according to any one of Items 1 to 4,

[0045] The connection electrode of each source contact portion is formed of the same transparent conductive film as the plurality of pixel electrodes.

[0046] [Item 7] The active matrix substrate according to any one of Items 1 to 6,

[0047] In each of the source contacts, the lower insulating layer has a thin film region, a thickness d1 of the thin film region is smaller than a thickness d2 of a region of the lower insulating layer overlapping the channel region when viewed from a normal direction of the substrate,

[0048] The lower opening of the source contact hole is formed in the thin-filmed region.

[0049] [Item 8] The active matrix substrate according to Item 7,

[0050] In each of the source contacts, the oxide semiconductor layer partially covers the thin-filmed region.

[0051] [Item 9] The active matrix substrate according to Item 7 or 8,

[0052] The thickness d1 of the thin-film region is less than or equal to 1 / 2 of the thickness d2 of a region of the lower insulating layer that overlaps with the channel region when viewed in the normal direction of the substrate.

[0053] [Item 10] The active matrix substrate according to any one of Items 1 to 6,

[0054] The active matrix substrate comprises a display region including the plurality of pixel regions and a non-display region located around the display region.

[0055] It also includes a plurality of wiring connection parts arranged in the non-display area.

[0056] Each of the plurality of wiring connection portions has:

[0057] a first wiring line formed of the same conductive film as the plurality of source bus lines;

[0058] The lower insulating layer is extended on the first wiring;

[0059] a second wiring line formed of the same conductive film as the plurality of gate bus lines;

[0060] an insulating layer disposed between the second wiring and the lower insulating layer;

[0061] The interlayer insulating layer is extended on the second wiring;

[0062] a wiring contact hole formed in the lower insulating layer and the interlayer insulating layer so as to expose a portion of the first wiring and a portion of the second wiring; and

[0063] The wiring connection electrode is arranged on the interlayer insulating layer and in the wiring contact hole, and is connected to the part of the first wiring and the part of the second wiring in the wiring contact hole.

[0064] [Item 11] The active matrix substrate according to any one of Items 7 to 9,

[0065] The active matrix substrate comprises a display region including the plurality of pixel regions and a non-display region located around the display region.

[0066] It also includes a plurality of wiring connection parts arranged in the non-display area.

[0067] Each of the plurality of wiring connection portions has:

[0068] a first wiring line formed of the same conductive film as the plurality of source bus lines;

[0069] The lower insulating layer is extended on the first wiring;

[0070] a second wiring line formed of the same conductive film as the plurality of gate bus lines;

[0071] an insulating layer disposed between the second wiring and the lower insulating layer;

[0072] The interlayer insulating layer is extended on the second wiring;

[0073] a wiring contact hole formed in the lower insulating layer and the interlayer insulating layer so as to expose a portion of the first wiring and a portion of the second wiring; and

[0074] a wiring connection electrode, which is arranged on the interlayer insulating layer and in the wiring contact hole, and is connected to the part of the first wiring and the part of the second wiring in the wiring contact hole,

[0075] The wiring contact hole of each wiring connection portion includes another lower opening formed in the lower insulating layer and another upper opening formed in the interlayer insulating layer.

[0076] In each of the wiring connection portions, the lower insulating layer has another thin-film region.

[0077] When viewed from the normal direction of the substrate, the other lower opening of the wiring contact hole is formed in the other thin-filmed region.

[0078] [Item 12] The active matrix substrate according to Item 5,

[0079] The active matrix substrate further comprises an upper insulating layer covering the connection electrode and the drain electrode in each pixel region.

[0080] The upper insulating layer has a pixel contact hole for exposing a portion of the drain electrode.

[0081] The pixel electrode is disposed on the upper insulating layer and in the pixel contact hole, and is connected to the portion of the drain electrode in the pixel contact hole.

[0082] [Item 13] The active matrix substrate according to Item 12,

[0083] Each of the pixel regions further includes a first electrode disposed on a portion of the pixel electrode so as to be in contact with an upper surface of the pixel electrode.

[0084] The first electrode is formed of a metal film, and when viewed from a normal direction of the substrate, the first electrode overlaps the entire pixel contact hole.

[0085] [Item 14] The active matrix substrate according to Item 13,

[0086] Also available:

[0087] a plurality of touch wirings arranged on the upper insulating layer; and

[0088] a plurality of touch sensor electrodes, each of which is electrically connected to any one of the plurality of touch wirings;

[0089] Each of the plurality of touch wires has a stacked structure including a lower layer formed of the same transparent conductive film as the plurality of pixel electrodes and an upper layer formed of the same metal film as the first electrode.

[0090] [Item 15] The active matrix substrate according to any one of Items 1 to 14,

[0091] The oxide semiconductor layer includes an In—Ga—Zn—O-based semiconductor.

[0092] [Item 16] The active matrix substrate according to Item 15,

[0093] The above-mentioned In-Ga-Zn-O-based semiconductor includes a crystalline portion.

[0094] [Item 17] A method for manufacturing an active matrix substrate,

[0095] The active matrix substrate has a plurality of pixel regions, a plurality of source bus lines and a plurality of gate bus lines, and a plurality of oxide semiconductor TFTs corresponding to the plurality of pixel regions. In the method for manufacturing the active matrix substrate, each TFT forming region in which each of the plurality of oxide semiconductor TFTs is formed includes:

[0096] Step (a), forming a first conductive film on a substrate, and patterning the first conductive film to form a first metal layer including a source electrode of the oxide semiconductor TFT, wherein the source electrode is formed integrally with a corresponding one of the plurality of source bus lines;

[0097] Step (b), forming a lower insulating layer on the first metal layer;

[0098] Step (c), forming an oxide semiconductor layer of the oxide semiconductor TFT on the lower insulating layer;

[0099] Step (d), forming a gate insulating film and a second conductive film in a manner covering the oxide semiconductor layer, patterning the gate insulating film and the second conductive film, thereby forming a gate insulating layer from the gate insulating film, and forming a second metal layer including a gate electrode of the oxide semiconductor TFT from the second conductive film, wherein the gate electrode is formed integrally with a corresponding one of the plurality of gate bus lines, and is disposed on a portion of the oxide semiconductor layer via the gate insulating layer;

[0100] Step (e), forming an interlayer insulating layer covering the second metal layer;

[0101] Step (f) of patterning the interlayer insulating layer and the lower insulating layer to form a source contact hole exposing a portion of the source electrode of the oxide semiconductor TFT and a portion of the oxide semiconductor layer; and

[0102] Step (g), forming a third conductive film on the interlayer insulating layer and in the source contact hole, and forming a connecting electrode in the source contact hole that contacts the portion of the source electrode and the portion of the oxide semiconductor layer by patterning the third conductive film.

[0103] [Item 18] The method for manufacturing an active matrix substrate according to Item 17,

[0104] The method further includes forming a thin-film region in the lower insulating layer between the steps (b) and (c).

[0105] In the step (f), the source contact hole is formed by patterning the interlayer insulating layer and the thin-filmed region of the lower insulating layer.

[0106] [Item 19] The method for manufacturing an active matrix substrate according to Item 17 or 18,

[0107] The step (f) includes forming a drain contact hole in the interlayer insulating layer to expose another portion of the oxide semiconductor layer.

[0108] The step (g) includes the step of forming a drain electrode in contact with the other portion of the oxide semiconductor layer in the drain contact hole by patterning the third conductive film.

[0109] [Item 20] The method for manufacturing an active matrix substrate according to Item 19,

[0110] Each of the plurality of pixel regions further includes:

[0111] Step (h), forming an upper insulating layer on the interlayer insulating layer, and forming a pixel contact hole in the upper insulating layer to expose a portion of the drain electrode of the oxide semiconductor TFT;

[0112] Step (i), forming a first transparent conductive film and a fourth conductive film on the upper insulating layer and in the pixel contact hole, and forming a stacked film including a pixel electrode formed of the first transparent conductive film and a conductive layer formed of the fourth conductive film by patterning the first transparent conductive film and the fourth conductive film; and

[0113] Step (j) of further patterning the conductive layer to form a first electrode disposed on a portion of the pixel electrode, wherein the first electrode overlaps the entire pixel contact hole when viewed from a normal direction of the substrate.

[0114] [Item 21] The method for manufacturing an active matrix substrate according to Item 20,

[0115] The step (i) further includes a step of forming a plurality of touch wirings by patterning the first transparent conductive film and the fourth conductive film.

[0116] [Item 22] The active matrix substrate according to Item 1 or 2,

[0117] In each of the source contacts, the first region of the oxide semiconductor layer has a cutout portion,

[0118] When viewed from a normal direction of the substrate, the cutout portion of the oxide semiconductor layer at least partially overlaps with the upper opening of the source contact hole.

[0119] Effects of the Invention

[0120] According to one embodiment of the present invention, an active matrix substrate including an oxide semiconductor TFT as a pixel TFT and capable of reducing the contact resistance between an oxide semiconductor layer of the oxide semiconductor TFT and a source bus line can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0121] Figure 1 1 is a schematic diagram showing an example of a planar structure of the active matrix substrate 101 .

[0122] Figure 2A It is a plan view illustrating a pixel region in the active matrix substrate 101 according to the first embodiment.

[0123] Figure 2B The active matrix substrate 101 is Figure 2A A cross-sectional view taken along line IIb-IIb' is shown.

[0124] Figure 3A The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0125] Figure 3B The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0126] Figure 3C The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0127] Figure 3D The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0128] Figure 3E The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0129] Figure 3F The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0130] Figure 3G The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0131] Figure 3H The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0132] Fig. 3I The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0133] Figure 3J The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0134] Figure 3K The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0135] Figure 3L The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 101 .

[0136] Figure 4A It is a cross-sectional view illustrating a wiring connection portion.

[0137] Figure 4B It is a cross-sectional view showing another example of the wiring connection portion.

[0138] Figure 5A FIG. 1 is a plan view showing a pixel region in an active matrix substrate 102 according to a modified example.

[0139] Figure 5B The active matrix substrate 102 is Figure 5A A cross-sectional view taken along the line Vb-Vb' is shown.

[0140] Figure 5C FIG. 1 is a plan view of a pixel region in another active matrix substrate illustrating a modified example.

[0141] Figure 5D It is along Figure 5C A cross-sectional view along the Vd-Vd' line is shown.

[0142] Figure 5E It is along Figure 5C A cross-sectional view along the Ve-Ve' line is shown.

[0143] Fig. 6A It is a plan view showing a pixel region in the active matrix substrate 103 according to the second embodiment.

[0144] Figure 6B The active matrix substrate 103 is Fig. 6A A cross-sectional view taken along line VIb-VIb' is shown.

[0145] Fig. 7A The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 103 .

[0146] Figure 7B The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 103 .

[0147] Figure 7C The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 103 .

[0148] Fig.7D The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 103 .

[0149] Fig. 7E The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 103 .

[0150] Fig. 8A It is a cross-sectional view illustrating a wiring connection portion.

[0151] Figure 8B It is a cross-sectional view showing another example of the wiring connection portion.

[0152] Fig.9A It is a plan view showing a pixel region in an active matrix substrate 104 according to the third embodiment.

[0153] Fig. 9B The active matrix substrate 104 is Fig.9A A cross-sectional view taken along line IXb-IXb' is shown.

[0154] Fig. 10A The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 104 .

[0155] Fig. 10B The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 104 .

[0156] Fig. 10C The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 104 .

[0157] Fig. 10D The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 104 .

[0158] Fig. 10E The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 104 .

[0159] Fig.10F The diagram is a cross-sectional view illustrating a process of manufacturing the active matrix substrate 104 .

[0160] Fig.11A It is a plan view showing a pixel region in an active matrix substrate 105 according to the fourth embodiment.

[0161] Fig. 11B The active matrix substrate 105 is Fig.11A A cross-sectional view taken along line XIb-XIb' is shown.

[0162] Fig. 12A The diagram is a cross-sectional view showing a process of forming a source contact according to a reference example.

[0163] Fig. 12BThe diagram is a cross-sectional view showing a process of forming a source contact according to a reference example.

[0164] Fig. 12C The diagram is a cross-sectional view showing a process of forming a source contact according to a reference example.

[0165] Fig.12D The diagram is a cross-sectional view showing a process of forming a source contact according to a reference example.

[0166] Fig.12E The diagram is a cross-sectional view showing a process of forming a source contact according to a reference example.

[0167] Fig.13 It is a top view of an oxide semiconductor TFT of a reference example. DETAILED DESCRIPTION

[0168] (First embodiment)

[0169] Hereinafter, an active matrix substrate according to a first embodiment will be described with reference to the drawings.

[0170] <Basic Structure of Active Matrix Substrate 101>

[0171] Figure 1 1 is a top view schematically showing an example of an active matrix substrate 101. The active matrix substrate 101 has a display region DR that contributes to display and a peripheral region (frame region) FR located outside the display region DR. The display region DR includes a plurality of pixel regions PIX arranged in a matrix. The pixel region PIX (sometimes also referred to as "pixel") is a region corresponding to a pixel of a display device. The non-display region FR is a region located around the display region DR and does not contribute to display.

[0172] The active matrix substrate 101 includes a substrate 1, a plurality of pixel TFTs (hereinafter referred to as "TFTs") 20 supported by the substrate 1, a plurality of pixel electrodes PE, a plurality of gate bus lines GL for supplying gate signals to the TFTs 20, and a plurality of source bus lines SL for supplying source signals to the TFTs 20 in the display region DR. The TFTs 20 are oxide semiconductor TFTs using an oxide semiconductor layer as an active layer.

[0173] Each pixel area PIX is defined by, for example, a gate bus line GL and a source bus line SL. The source bus line SL extends in a direction intersecting the gate bus line GL.

[0174] Each TFT 20 and each pixel electrode PE are provided corresponding to one pixel region PIX among the plurality of pixel regions PIX. The gate electrode of the TFT 20 is electrically connected to one gate bus line GL among the gate bus lines GL. A portion of the oxide semiconductor layer of the TFT 20 (referred to as the "first region") is electrically connected to one source bus line SL among the source bus lines SL. Another portion of the oxide semiconductor layer of the TFT 20 (referred to as the "second region") is electrically connected to the pixel electrode PE.

[0175] When the active matrix substrate 101 is applied to a display device of a transverse electric field mode such as an FFS (Fringe Field Switching) mode, an electrode (common electrode) CE common to a plurality of pixels PIX is provided on the active matrix substrate 101 .

[0176] Peripheral circuits such as drivers can be provided in the non-display region FR. In this example, a gate driver GD for driving the gate bus GL and an SSD (Source Shared Driving) circuit Sc for driving the source bus SL in a time-sharing manner are formed monolithically. The SSD circuit Sc is connected to a source driver SD mounted, for example, in a COG (Chip on Glass) manner.

[0177] <Structure of Pixel Region of Active Matrix Substrate 101>

[0178] Hereinafter, the structure of the pixel region of the active matrix substrate of the present embodiment will be described by taking the active matrix substrate of the display device of the FFS mode as an example with reference to the accompanying drawings. The FFS mode is a mode of a transverse electric field method in which a pair of electrodes are provided on one of the substrates and an electric field is applied to the liquid crystal molecules in a direction parallel to the substrate surface (lateral direction).

[0179] In the following description, the layer including electrodes / wirings, etc. formed by the same conductive film (first conductive film) as the source bus line SL is referred to as the "first metal layer M1" (or "source metal layer"), and the layer including electrodes / wirings, etc. formed by the same conductive film (second conductive film) as the gate bus line GL is referred to as the "second metal layer M2" (or "gate metal layer"). The first metal layer M1 is located closer to the substrate side than the second metal layer M2 (lower source structure). In addition, the active matrix substrate 101 of the present embodiment further has a layer including electrodes / wirings, etc. formed by a third conductive film above the second metal layer M2. The layer formed by the third conductive film is referred to as the "third metal layer M3". In the present embodiment, the third metal layer M3 includes a drain electrode of the oxide semiconductor TFT.

[0180] In the drawings, the layer where the electrode, wiring, etc. are formed may be indicated in parentheses after the reference numerals of the components. For example, "(M1)" may be added after the reference numerals of the electrodes or wiring formed in the first metal layer M1.

[0181] Figure 2A is a top view illustrating a pixel region in the active matrix substrate 101. Figure 2B 1 is a cross-sectional view of the pixel region along line IIb-IIb′ crossing the TFT 20 .

[0182] like Figure 2A and Figure 2B As shown, the active matrix substrate 101 includes: a substrate 1 having a main surface; a first metal layer M1 including a plurality of source bus lines SL extending in the column direction; a second metal layer M2 including a plurality of gate bus lines GL extending in the row direction; and a lower insulating layer 5. The first metal layer M1 is disposed on the substrate 1 side relative to the second metal layer M2 (lower source structure). The lower insulating layer 5 is disposed between the first metal layer M1 and the second metal layer M2, covering the first metal layer M1.

[0183] The active matrix substrate 101 further includes a plurality of top-gate TFTs 20, a plurality of pixel electrodes PE, and a plurality of source contacts SC. The TFTs 20, the pixel electrodes PE, and the source contacts SC are each provided corresponding to each of the plurality of pixel regions. The active matrix substrate 101 further includes an interlayer insulating layer 10 covering the second metal layer M2, an upper insulating layer 13, and a common electrode CE.

[0184] A plurality of source bus lines SL are provided on the main surface of the substrate 1. The lower insulating layer 5 is provided so as to cover the first metal layer M1 including the source bus lines SL.

[0185] Next, the configuration of the TFT 20 and the source contact portion SC in each pixel region will be described.

[0186] In each pixel region, the TFT 20 includes an oxide semiconductor layer 7 disposed on the lower insulating layer 5 , a gate electrode GE disposed on a portion of the oxide semiconductor layer 7 via a gate insulating layer 9 , and a source electrode SE.

[0187] The oxide semiconductor layer 7 includes a channel region 7c and a first region 7s and a second region 7d respectively arranged on both sides thereof. The first region 7s and the second region 7d are low-resistance regions having a resistivity lower than that of the channel region 7c. The gate electrode GE is arranged so as to overlap the channel region 7c when viewed in the normal direction of the main surface of the substrate 1 (hereinafter referred to as the "normal direction of the substrate 1"). The gate insulating layer 9 may cover the channel region 7c and not cover the first region 7s and the second region 7d.

[0188] The first region 7s of the oxide semiconductor layer 7 in the TFT 20 is electrically connected to a corresponding source bus line SL in a source contact portion SC described later, and the second region 7d is electrically connected to a corresponding pixel electrode PE in a pixel contact portion described later.

[0189] The source electrode SE is formed using the same conductive film as the source bus line SL (i.e., in the first metal layer M1). The source electrode SE is electrically connected to the corresponding source bus line SL. The source electrode SE may also be formed integrally with the corresponding source bus line SL. For example, the source electrode SE may also be a part of the corresponding source bus line SL. In this case, the part of the source bus line SL located at the source contact portion SC is referred to as the "source electrode SE".

[0190] The gate electrode GE of the TFT 20 is formed using the same conductive film as the gate bus GL (i.e., in the second metal layer M2). The gate electrode GE is electrically connected to the corresponding gate bus GL. The gate electrode GE may also be formed integrally with the corresponding gate bus GL. For example, the gate electrode GE may also be a part of the corresponding gate bus GL. In this case, the portion of the gate bus GL that overlaps with the oxide semiconductor layer 7 when viewed from the normal direction of the substrate 1 is referred to as the "gate electrode GE".

[0191] In the example shown in the figure, the gate insulating layer 9 is formed only in a region overlapping with the second metal layer M2 when viewed from the normal direction of the substrate 1. That is, the edge of the gate insulating layer 9 is aligned with the edge of the second metal layer M2.

[0192] The TFT 20 may also have a light shielding layer 3 on the substrate 1 side of the oxide semiconductor layer 7. The light shielding layer 3 is formed in the first metal layer M1. The light shielding layer 3 may be configured to overlap with at least the channel region 7c in the oxide semiconductor layer 7 when viewed from the normal direction of the substrate 1. Thus, it is possible to suppress the degradation of the characteristics of the oxide semiconductor layer 7 caused by light from the substrate 1 side (backlight).

[0193] The interlayer insulating layer 10 is formed so as to cover the oxide semiconductor layer 7 , the gate insulating layer 9 , and the second metal layer M2 . The interlayer insulating layer 10 may be in contact with the first region 7 s and the second region 7 d of the oxide semiconductor layer 7 .

[0194] The drain electrode DE of the TFT 20 is formed on the interlayer insulating layer 10. The drain electrode DE is disposed on the interlayer insulating layer 10 and in an opening (drain contact hole) CHd provided in the interlayer insulating layer 10, and is connected to the second region 7d of the oxide semiconductor layer 7 in the drain contact hole CHd.

[0195] The source contact portion SC connects the first region 7s of the oxide semiconductor layer 7 of the TFT 20 to the corresponding source bus line SL. The source contact portion SC includes: a source contact hole CHs formed in the interlayer insulating layer 10 and the lower insulating layer 5 to expose a portion of the source bus line SL and a portion of the first region 7s of the oxide semiconductor layer 7; and a connecting electrode 8 formed using the same conductive film as the drain electrode DE (i.e., in the third metal layer M3).

[0196] The source contact hole CHs includes a lower opening portion 5s formed in the lower insulating layer 5 and an upper opening portion 10s formed in the interlayer insulating layer 10. The source contact hole CHs can be formed, for example, by etching the interlayer insulating layer 10 and the lower insulating layer 5 using the oxide semiconductor layer 7 as an etching stopper. In this case, in the source contact hole CHs, the side surface of the oxide semiconductor layer 7 is aligned with the side surface of the lower opening portion 5s. In the present embodiment, when viewed from the normal direction of the substrate 1, the edge (periphery) of the oxide semiconductor layer 7 extends across the upper opening portion 10s. In addition, when viewed from the normal direction of the substrate 1, the lower opening portion 5s is arranged inside the upper opening portion 10s and does not overlap with the oxide semiconductor layer 7.

[0197] The connection electrode 8 is formed on the interlayer insulating layer 10 and in the source contact hole CHs, and is connected in the source contact hole CHs to the exposed portion of the source bus line SL and the exposed portion of the first region 7s of the oxide semiconductor layer 7 (here, the upper surface and side surface of the end of the first region 7s). The connection electrode 8 may be in direct contact with both the source bus line SL and the first region 7s.

[0198] The proportion of the area S1 of the portion where the upper opening 10s overlaps with the oxide semiconductor layer 7 when viewed from the normal direction of the substrate 1 (i.e., the contact area between the connecting electrode 8 and the upper surface of the oxide semiconductor layer 7) in the entire area of ​​the upper opening 10s can be, for example, greater than 1 / 3 and less than 2 / 3.

[0199] The upper insulating layer 13 is configured to cover the interlayer insulating layer 10 and the third metal layer M3. The upper insulating layer 13 includes, for example, an inorganic insulating layer (passivation film) 11. As shown in the figure, the upper insulating layer 13 may have a stacked structure including an inorganic insulating layer 11 and an organic insulating layer 12 formed on the inorganic insulating layer 11. The organic insulating layer 12 may not be formed. Alternatively, the organic insulating layer 12 may be formed only in the display area.

[0200] The pixel electrode PE and the common electrode CE are arranged with the dielectric layer 17 interposed therebetween. In this example, the pixel electrode PE is arranged on the common electrode CE with the dielectric layer 17 interposed therebetween. In addition, the common electrode CE may be formed on the pixel electrode PE with the dielectric layer 17 interposed therebetween. In this specification, the electrode located on the substrate 1 side of the common electrode CE and the pixel electrode PE is referred to as the "lower transparent electrode", and the electrode arranged on the lower transparent electrode with the dielectric layer 17 interposed therebetween is referred to as the "upper transparent electrode". In addition, the layer including the lower transparent electrode is referred to as the "lower transparent conductive layer T1", and the layer including the upper transparent electrode is referred to as the "upper transparent conductive layer T2". In the upper transparent electrode (the pixel electrode PE in this example), one or more slits (openings) s or cutouts are provided in each pixel region.

[0201] The pixel electrode PE is separated for each pixel region. The pixel electrode PE is electrically connected to the drain electrode DE of the corresponding TFT 10 in the pixel contact portion. In the present embodiment, the pixel electrode PE is arranged on the dielectric layer 17, and is connected to the drain electrode DE in the pixel contact hole CHp formed in the upper insulating layer 13 and the dielectric layer 17. The pixel contact hole CHp includes an opening 11p of the inorganic insulating layer 11, an opening 12p of the organic insulating layer 12, and an opening 17p of the dielectric layer 17.

[0202] The common electrode CE may not be separated for each pixel region. For example, the common electrode CE may have an opening 15p in a region (pixel contact portion) where the pixel contact hole CHp is formed, and may be formed in the entire pixel region except for the pixel contact portion.

[0203] <Method for Manufacturing Active Matrix Substrate 101>

[0204] Next, an example of a method for manufacturing the active matrix substrate 101 of the present embodiment will be described with reference to the drawings. Hereinafter, the method for manufacturing one pixel region among a plurality of pixel regions in the active matrix substrate 101 will be described.

[0205] Figure 3A to Figure 3L These are schematic cross-sectional views of the steps for explaining the method for manufacturing the active matrix substrate 101. These drawings show a region where a TFT is formed (a TFT formation region) in one pixel region.

[0206] Step 1: Formation of the first metal layer M1 ( Figure 3A )

[0207] On the substrate 1, a first conductive film (thickness: for example, 50 nm to 500 nm) is formed by sputtering. Next, the first conductive film is patterned by a known photolithography process. Here, a resist film is formed on the first conductive film, and the resist film is exposed using a source photomask to form a resist layer (not shown). The first conductive film is etched (for example, wet etching) using the resist layer as a mask.

[0208] In this way, Figure 3A As shown in FIG. 1 , a first metal layer M1 including a source bus line SL and a light shielding layer 3 of a TFT is formed. The source bus line SL includes a portion functioning as a source electrode SE of the TFT.

[0209] As the substrate 1 , a transparent and insulating substrate such as a glass substrate, a silicon substrate, a heat-resistant plastic substrate (resin substrate), etc. can be used.

[0210] The material of the first conductive film is not particularly limited, and a film containing a metal such as aluminum (Al), tungsten (W), molybdenum (Mo), tantalum (Ta), chromium (Cr), titanium (Ti), copper (Cu), or an alloy thereof or a metal nitride thereof can be suitably used. In addition, a laminated film formed by laminating a plurality of such films can also be used.

[0211] Here, as the first conductive film, a single-layer film of a metal film (including an alloy film) containing Cu or Al is used. Alternatively, a stacked film having a metal film containing Cu or Al as the top layer may be used. As described above, in this embodiment, even if an ohmic conductive film such as a Ti film is not provided on the Cu film or the Al film, the contact resistance between the source bus SL (source electrode SE) and the oxide semiconductor can be reduced.

[0212] STEP 2: Formation of lower insulating layer 5 ( Figure 3B )

[0213] Next, if Figure 3B As shown, a lower insulating layer 5 (thickness: for example, not less than 200 nm and not more than 600 nm) is formed so as to cover the first metal layer M1.

[0214] The lower insulating layer 5 is formed, for example, by a CVD method. As the lower insulating layer 5, a silicon oxide (SiOx) layer, a silicon nitride (SiNx) layer, an oxynitride silicon (SiOxNy; x>y) layer, a silicon nitride oxide (SiNxOy; x>y) layer, etc. can be suitably used. The lower insulating layer 5 can be a single layer or have a stacked structure. For example, a silicon nitride (SiNx) layer, a silicon nitride oxide layer, etc. can be formed on the substrate side (lower layer) to prevent the diffusion of impurities from the substrate 1, and a silicon oxide (SiO2) layer, an oxynitride silicon layer, etc. can be formed on the layer thereon (upper layer) to ensure insulation. Here, for example, a silicon oxide (SiO2) layer (thickness: for example, 350nm) is formed as the lower insulating layer 5 by a CVD method. Alternatively, a stacked film having a silicon nitride (SiNx) layer (thickness: 50 to 600 nm) as a lower layer and a silicon oxide (SiO2) layer (thickness: 50 to 600 nm) as an upper layer may be formed as the lower insulating layer 5. When an oxide film such as a silicon oxide film is used as the lower insulating layer 5 (as the uppermost layer thereof when the lower insulating layer 5 has a stacked structure), oxidation defects generated in the channel region of the oxide semiconductor layer to be formed later can be reduced by the oxide film, thereby suppressing the low resistance of the channel region.

[0215] STEP 3: Formation of oxide semiconductor layer 7 ( Figure 3C )

[0216] Next, an oxide semiconductor film (thickness: for example, 15 nm to 200 nm) is formed on the lower insulating layer 5. After that, the oxide semiconductor film may be annealed. Next, the oxide semiconductor film is patterned by a known photolithography process. Figure 3C As shown, the oxide semiconductor layer 7 serving as the active layer of the TFT 20 is obtained.

[0217] The oxide semiconductor film can be formed by, for example, a sputtering method. Here, an In-Ga-Zn-O-based semiconductor film (thickness: 50 nm) containing In, Ga, and Zn is formed as the oxide semiconductor film.

[0218] The patterning of the oxide semiconductor film can be performed by wet etching using, for example, a PAN-based etching solution containing phosphoric acid, nitric acid, and acetic acid, or another etching solution such as an oxalic acid-based etching solution.

[0219] STEP 4: Formation of gate insulating film 90 ( Figure 3D )

[0220] Next, if Figure 3D As shown in FIG. 1 , a gate insulating film 90 is formed so as to cover the oxide semiconductor layer 7 .

[0221] The same insulating film as the lower insulating layer 5 (the insulating film exemplified as the lower insulating layer 5) can be used as the gate insulating film 90. Here, a silicon oxide (SiO2) film is formed as the gate insulating film 90. When an oxide film such as a silicon oxide film is used as the gate insulating film 90, oxidation defects generated in the channel region of the oxide semiconductor layer 7 can be reduced by the oxide film, so that the resistance of the channel region can be suppressed.

[0222] STEP 5: Formation of the second metal layer M2 ( Figure 3E )

[0223] Next, a second conductive film (thickness: for example, 50 nm to 500 nm) not shown is formed on the gate insulating film 90. Thereafter, the second conductive film is patterned by a known photolithography process. Here, a resist film is formed on the second conductive film, and the resist film is exposed using a gate photomask to form a resist layer R. Using the resist layer R as a mask, the second conductive film is etched (for example, wet etching). Thus, a second metal layer M2 including a gate bus GL is obtained. The gate bus GL includes a portion that functions as a gate electrode GE of a TFT.

[0224] As the second conductive film, for example, metals such as molybdenum (Mo), tungsten (W), aluminum (Al), copper (Cu), titanium (Ti), tantalum (Ta), or alloys thereof can be used. The second conductive film may also have a stacked structure including a plurality of layers formed of different conductive materials. Here, a Cu / Ti stacked film having a Ti film as a lower layer and a Cu film as an upper layer, or a Cu / Mo stacked film having a Mo film as a lower layer and a Cu film as an upper layer is used as the second conductive film.

[0225] STEP 6: Patterning of gate insulating layer 9 ( Figure 3F )

[0226] Next, the gate insulating film 90 is patterned using the resist layer R as a mask or the second metal layer M2 as a mask to form the gate insulating layer 9. According to this method, the side surfaces of the gate electrode GE and the gate insulating layer 9 are aligned when viewed from the normal direction of the substrate 1.

[0227] In addition, the gate insulating film 90 and the second conductive film may be patterned separately. Specifically, the gate insulating film 90 may be patterned before the second conductive film is formed to form the gate insulating layer 9. Next, the second conductive film is formed in a manner covering the gate insulating layer 9, and the second conductive film is patterned to form the second metal layer M2. Alternatively, the second conductive film may be formed after the gate insulating film 90 is formed, and the second conductive film may be patterned. Thereafter, the gate insulating film 90 may be patterned to form the gate insulating layer 9.

[0228] STEP 7: Resistance reduction treatment of oxide semiconductor layer 7 ( Figure 3G )

[0229] Next, the oxide semiconductor layer 7 is subjected to a resistance lowering treatment. For example, a plasma treatment may be performed as the resistance lowering treatment. Figure 3G As shown, when viewed from the normal direction of the main surface of the substrate 1, the region (exposed region) in the oxide semiconductor layer 7 that does not overlap with the gate bus GL (or gate electrode GE) and the gate insulating layer 9 becomes a low-resistance region having a resistivity lower than that of the region overlapping with them (here, the region that becomes the channel). The low-resistance region may also be a conductor region (for example, a sheet resistance: 200Ω / □ or less). In this way, an oxide semiconductor layer 7 including the first region 7s and the second region 7d as low-resistance regions, and the channel region 7c that is not made low-resistance and remains as a semiconductor region is obtained.

[0230] The method of low resistance treatment (plasma treatment) is not limited to the above method. For example, the exposed region of the oxide semiconductor layer 7 may be low-resistance by using reducing plasma or plasma containing doping elements (e.g., argon plasma). The method and conditions of low resistance treatment are described in, for example, Japanese Patent Publication No. 2008-40343. For reference, the disclosure of Japanese Patent Publication No. 2008-40343 is incorporated herein in its entirety.

[0231] STEP 8: Formation of interlayer insulating layer 10 ( Figure 3H )

[0232] Next, an interlayer insulating layer 10 is formed to cover the oxide semiconductor layer 7, the gate insulating layer 9, and the gate electrode GE. Then, the interlayer insulating layer 10 and the lower insulating layer 5 are patterned by a known photolithography process. Figure 3H As shown, a drain contact hole CHd is formed in the interlayer insulating layer 10 to expose a portion of the second region 7d of the oxide semiconductor layer 7, and a source contact hole CHs is formed in the interlayer insulating layer 10 and the lower insulating layer 5 to expose a portion of the source bus SL (or source electrode SE) and a portion of the first region 7s of the oxide semiconductor layer 7.

[0233] An inorganic insulating layer such as a silicon oxide film, a silicon nitride film, a silicon oxynitride film, or a silicon nitride oxide film can be formed as a single layer or stacked as an interlayer insulating layer 10. The thickness of the inorganic insulating layer can be greater than 100 nm and less than 500 nm. When an insulating film such as a silicon nitride film that reduces an oxide semiconductor is used to form the interlayer insulating layer 10, the resistivity of the region in contact with the interlayer insulating layer 10 in the oxide semiconductor layer 7 (here, a low resistance region) can be maintained low, so it is preferred. Here, for example, a SiNx layer (thickness: 300 nm) is formed as the interlayer insulating layer 10 by a CVD method.

[0234] When an insulating layer that can reduce the oxide semiconductor (for example, a hydrogen-donating layer such as a silicon nitride layer) is used as the interlayer insulating layer 10, even without performing the above-mentioned low-resistance treatment, the portion of the oxide semiconductor layer 7 that is in contact with the interlayer insulating layer 10 can be made lower in resistance than the portion that is not in contact with the interlayer insulating layer 10.

[0235] For example, the interlayer insulating layer 10 and the lower insulating layer 5 can be patterned by dry etching. The dry etching is performed under the condition that only these insulating layers are etched without etching the oxide semiconductor layer 7. Thus, the oxide semiconductor layer 7 functions as an etching stopper, so that in the source contact hole CHs, a part of the side surface of the lower opening 5s formed in the lower insulating layer 5 is aligned with the side surface of the oxide semiconductor layer 7, and the other part is aligned with the side surface of the upper opening 10s.

[0236] In the present embodiment, in the patterning process of the interlayer insulating layer 10 and the lower insulating layer 5, for example, carbon tetrachloride (CF4) gas and oxygen (O2) gas (CF4 / O2) are used as etching gases. Inert gases such as Ar gas may also be added appropriately. The etching conditions (type of etching gas, substrate temperature, vacuum degree in the chamber, etc.) are set to conditions that can suppress damage to the oxide semiconductor layer 7. As an example, when CF4 / O2 is used as the etching gas, when the flow rate of O2 gas is increased (for example, the flow rate ratio of O2 gas to CF4 gas is made to be, for example, 10% to 25%), the surface of the oxide semiconductor layer 7 is not easily stripped, so the damage to the oxide semiconductor layer 7 can be reduced.

[0237] STEP 9: Formation of the third metal layer M3 ( Fig. 3I )

[0238] Next, a third conductive film (thickness: for example, 50 nm to 500 nm) not shown is formed on the interlayer insulating layer 10, and the third conductive film is patterned. Fig. 3I As shown, a third metal layer M3 including a connection electrode 8 and a drain electrode DE is formed.

[0239] The connection electrode 8 is arranged on the interlayer insulating layer 10 and in the source contact hole CHs, and is connected to the source bus line SL (or source electrode SE) and the first region 7s of the oxide semiconductor layer 7 in the source contact hole CHs. In this example, the connection electrode 8 is in direct contact with the source bus line SL and the first region 7s.

[0240] The drain electrode DE is disposed on the interlayer insulating layer 10 and in the drain opening 10p, and is connected in the drain opening 10p to the second region 7d of the oxide semiconductor layer 7. In this example, the drain electrode DE is in direct contact with the second region 7d.

[0241] As the third conductive film, for example, an element selected from aluminum (Al), chromium (Cr), copper (Cu), tantalum (Ta), titanium (Ti), molybdenum (Mo) or tungsten (W), or an alloy containing these elements as components can be used. For example, it can have a three-layer structure of titanium film-aluminum film-titanium film, a three-layer structure of molybdenum film-aluminum film-molybdenum film, etc. In addition, the third conductive film is not limited to a three-layer structure, and can also have a single-layer or two-layer structure or a stacked structure of more than four layers. Here, a stacked film with a Ti film (thickness: 15 to 70 nm) as the lower layer and a Cu film (thickness: 50 to 400 nm) as the upper layer is used. When a stacked film with an ohmic conductive film such as a Ti film as the lower layer is used, the contact resistance of the source contact portion can be more effectively reduced.

[0242] STEP 10: Formation of the inorganic insulating layer 11 and the organic insulating layer 12 ( Figure 3J )

[0243] Next, if Figure 3J As shown, an upper insulating layer 13 is formed to cover the interlayer insulating layer 10 and the third metal layer M3. Here, an inorganic insulating layer 11 (thickness: for example, 100 nm to 500 nm) and an organic insulating layer 12 (thickness: for example, 1 to 4 μm, preferably 2 to 3 μm) are formed in this order as the upper insulating layer 13.

[0244] As the inorganic insulating layer 11, the same inorganic insulating film as the interlayer insulating layer 10 can be used. Here, for example, a SiNx layer (thickness: 300 nm) is formed by CVD as the inorganic insulating layer 11. The organic insulating layer 12 may be, for example, an organic insulating film (eg, acrylic resin film) made of a photosensitive resin material.

[0245] Thereafter, the organic insulating layer 12 is patterned. Thus, in each pixel region, an opening 12p is formed in the organic insulating layer 12 to expose a portion of the inorganic insulating layer 11. The opening 12p is arranged so as to overlap with the drain electrode DE when viewed from the normal direction of the substrate 1. The entire portion of the organic insulating layer 12 located in the non-display region may be removed by this patterning.

[0246] STEP 11: Formation of common electrode CE ( Figure 3K )

[0247] Then, if Figure 3K As shown, the common electrode CE is formed on the upper insulating layer 13 .

[0248] First, a first transparent conductive film (thickness: 20 to 300 nm) not shown is formed on the upper insulating layer 13 and in the opening 12p. Here, for example, an indium zinc oxide film is formed as the first transparent conductive film by sputtering. Metal oxides such as indium tin oxide (ITO), indium zinc oxide, and ZnO can be used as the material of the first transparent conductive film. Thereafter, the first transparent conductive film is patterned. In the patterning, for example, wet etching can be performed using an oxalic acid-based etching solution. Thus, a common electrode CE is obtained. The common electrode CE can have an opening 15p, for example, in the area where the pixel contact hole is formed.

[0249] STEP 12: Formation of dielectric layer 17 ( Figure 3L )

[0250] Next, if Figure 3L As shown, the dielectric layer 17 (thickness: 50 to 500 nm) is formed so as to cover the common electrode CE, and the dielectric layer 17 and the inorganic insulating layer 11 are patterned.

[0251] The dielectric layer 17 is formed on the organic insulating layer 12 and the common electrode CE and in the opening 12p in the pixel region. The material of the dielectric layer 17 may be the same as the material exemplified as the material of the inorganic insulating layer 11. Here, a SiN film is formed as the dielectric layer 17 by, for example, CVD.

[0252] After that, the dielectric layer 17 and the inorganic insulating layer 11 are etched by a known photolithography process to form a pixel contact hole CHp that exposes the drain electrode DE. The pixel contact hole CHp includes an opening 17p of the dielectric layer 17, an opening 12p of the organic insulating layer 12, and an opening 11p of the inorganic insulating layer 11. The opening 17p only needs to at least partially overlap with the opening 12p when viewed from the normal direction of the substrate 1. The opening 11p is etched using the resist layer (not shown) on the dielectric layer 17 and the organic insulating layer 12 as masks.

[0253] STEP 13: Formation of pixel electrode PE ( Figure 2A , Figure 2B )

[0254] Next, a second transparent conductive film (thickness: 20 to 300 nm) not shown is formed on the dielectric layer 17 and in the pixel contact hole CHp. The second transparent conductive film can be formed using the same material as the first transparent conductive film.

[0255] After that, the second transparent conductive film is patterned. Here, for example, the second transparent conductive film is wet-etched using an oxalic acid-based etching solution. Thus, a pixel electrode PE is formed in each pixel region. The pixel electrode PE is connected to the drain electrode DE in the pixel contact hole CHp. In this way, a pixel electrode PE is manufactured. Figure 2A and Figure 2B The active matrix substrate 101 is shown.

[0256] According to the active matrix substrate 101 of this embodiment, the contact resistance of the source contact portion can be reduced compared to the conventional lower source structure substrate. In addition, in the conventional lower source structure substrate, a part of the oxide semiconductor layer 7 may be lost due to the process of forming the source contact portion, but in this embodiment, such a problem does not occur. Moreover, in this embodiment, the source contact hole CHs is formed by the same etching process as the drain contact hole CHd, so the number of photomasks used can be reduced compared to the conventional method.

[0257] In order to explain the above-mentioned effects of the present embodiment in more detail, first, a method for manufacturing a lower source structure substrate according to a reference example will be described.

[0258] Figures 12A to 12E 1 is a cross-sectional view for explaining a step of forming a source contact in a lower source structure substrate of a reference example. In the reference example, the source contact has a structure in which the oxide semiconductor layer is in direct contact with the source bus line in a source opening formed in the lower insulating layer.

[0259] First, if Fig. 12A As shown in FIG. 1 , a first conductive film is formed on a substrate 91 and patterned to form a source bus line SL.

[0260] Then, if Fig. 12B As shown, a lower insulating layer 95 covering the source bus line SL is formed. Then, a resist layer 98 is formed on the lower insulating layer 95 by a known photolithography process. Using the resist layer 98 as a mask, the lower insulating layer 95 is etched to form a source opening 95s that exposes a surface m1 of a part of the source bus line SL.

[0261] As described above, the surface m1 of the source bus line SL is, for example, a low-resistance metal film such as a Cu film or an Al film. It is preferred that an ohmic conductive film such as a Ti film is not formed on the low-resistance metal film. This is because when forming a Ti film, it is necessary to pattern the low-resistance metal film by wet etching and pattern the Ti film by dry etching, respectively, which complicates the manufacturing process.

[0262] After etching of the lower insulating layer 95, as Fig. 12C As shown, the resist layer 98 is peeled off from the substrate 91. At this time, the resist layer 98 formed on the lower insulating layer 95 is not easily peeled off, and sometimes a part of the resist layer 98 is not peeled off and remains on the lower insulating layer 95. The remaining part 98R of the resist layer 98 is called "resist residue".

[0263] Then, if Fig.12D As shown, an oxide semiconductor film (e.g., an In-Ga-Zn-O-based semiconductor film) is formed on the lower insulating layer 95 and in the source opening 95s, and the oxide semiconductor film is patterned to obtain an oxide semiconductor layer 97. The oxide semiconductor layer 97 is in direct contact with the exposed surface m1 of the source bus line SL in the source opening 95s.

[0264] At this time, if the resist residue 98R is generated, the adhesion between the oxide semiconductor film and the resist residue 98R is low, so Fig.12E As shown, a portion of the oxide semiconductor film located on the resist residue 98R may be peeled off, resulting in a defect 99 in the oxide semiconductor film. As a result, an oxide semiconductor layer 97 having a predetermined shape cannot be obtained, and TFT characteristics may be degraded or disconnection may occur.

[0265] Fig.13 FIG. 1 is a plan view of an oxide semiconductor TFT according to a reference example, illustrating a case where a defect 99 is generated in an oxide semiconductor layer 97 .

[0266] In contrast, in the present embodiment, the lower insulating layer 5 is not patterned before the oxide semiconductor film is formed, so there is no need to form a resist layer on the lower insulating layer 5, and no resist residue is generated on the upper surface of the lower insulating layer 5. Therefore, there is no defect in the oxide semiconductor film caused by the resist residue, and thus the reliability can be improved compared to the reference example.

[0267] In addition, according to the manufacturing method of the reference example, the surface m1 of the low-resistance metal film such as the Cu film in the source bus line SL cannot form a good ohmic contact with the oxide semiconductor layer 97, so the contact resistance may increase. In addition, if the lower insulating layer 95 is heat-treated to ensure the reliability of the lower insulating layer 95, the surface m1 of the source bus line SL exposed in the source opening 95s may be damaged or oxidized, resulting in that the contact resistance may further increase.

[0268] In this regard, in the present embodiment, the source contact hole CHs of the source contact portion SC can be formed by etching the lower insulating layer 5 and the interlayer insulating layer 10 after forming the interlayer insulating layer 10. Therefore, the increase in contact resistance caused by process damage to the source bus line SL can be suppressed. In addition, in the present embodiment, in the source contact portion SC, the oxide semiconductor layer 7 is connected to the source bus line SL using the connecting electrode 8 in the third metal layer M3. Even if the upper surface of the source bus line SL is a low-resistance metal surface such as Cu or Al, the contact resistance of the source contact portion SC can be further reduced by using a conductive film (ohmic conductive film) that can form an ohmic junction with an oxide semiconductor such as a Ti film in the bottom layer of the connecting electrode 8. Therefore, even if an ohmic conductive film is not formed on the Cu film of the source bus line SL, a reduction in contact resistance can be achieved.

[0269] Furthermore, in the reference example, since the patterning process of the lower insulating layer 95 for forming the source opening 95s and the patterning process of the interlayer insulating layer for forming the drain contact portion (not shown) are performed separately, the number of manufacturing processes and the number of photomasks used increase. In contrast, in the present embodiment, the source contact hole CHs can be formed simultaneously in the etching process for forming the drain contact hole CHd. Therefore, the number of manufacturing processes and the number of photomasks can be reduced compared to the reference example.

[0270] <Wiring connection section>

[0271] The active matrix substrate 101 may also include a plurality of wiring connection portions provided in the peripheral region. The wiring connection portion is a connection portion that connects wirings in different metal layers to each other, for example, connecting wirings in the first metal layer M1 to wirings in the second metal layer M2 or the third metal layer M3. Among the wiring connection portions, the wiring connection portion that connects wirings in the first metal layer M1 to wirings in the second metal layer M2 is referred to as a "source-gate connection portion".

[0272] Figure 4A This is a cross-sectional view showing an example of a wiring connection portion (source-gate connection portion) in this embodiment.

[0273] In the wiring connection portion 31, the first wiring 3b formed in the first metal layer M1 is electrically connected to the second wiring 8b arranged in the second metal layer M2 via the wiring connection electrode 6b arranged in the third metal layer M3. For example, the second wiring 8b may be a gate bus GL, which is connected to the connection wiring (first wiring 3b) formed in the first metal layer M1 in the wiring connection portion 31, and is connected to the gate driver via the connection wiring.

[0274] The wiring connection portion 31 includes: a first wiring 3b; a lower insulating layer 5 extending on the first wiring 3b; a second wiring 8b; an insulating layer 9b disposed between the second wiring 8b and the lower insulating layer 5; an interlayer insulating layer 10 extending on the second wiring 8b; and a wiring connection electrode 6b. The insulating layer 9b is formed of the same insulating film as the gate insulating layer 9 and is patterned into a shape substantially the same as that of the second wiring 8b. A wiring contact hole CHb is formed in the lower insulating layer 5 and the interlayer insulating layer 10 to expose a portion of the second wiring 8b and a portion of the first wiring 3b. The wiring connection electrode 6b is disposed on the interlayer insulating layer 10 and in the wiring contact hole CHb, and is connected to both the second wiring 8b and the first wiring 3b in the wiring contact hole CHb.

[0275] The wiring contact hole CHb of the wiring connection portion 31 can be formed by a common etching process with the source contact hole CHs and the drain contact hole CHd. Therefore, the wiring connection portion 31 can be formed on the active matrix substrate 101 without increasing the number of manufacturing steps and the number of photomasks used.

[0276] Figure 4B This is a cross-sectional view showing another example of the wiring connection portion of the present embodiment.

[0277] The wiring connection portion 32 connects the first wiring 3c formed in the first metal layer M1 to the third wiring 6c formed in the third metal layer M3. The wiring connection portion 32 includes the first wiring 3c, the lower insulating layer 5 and the interlayer insulating layer 10 extending on the first wiring 3c, and the third wiring 6c. The third wiring 6c contacts the first wiring 3c in the wiring contact hole CHc formed in the interlayer insulating layer 10 and the lower insulating layer 5. The wiring contact hole CHc of the wiring connection portion 32 can also be formed by a common etching process with the source contact hole CHs and the drain contact hole CHd.

[0278] <Modification>

[0279] Figure 5A is a top view of a pixel region in an active matrix substrate 102 according to a modified example. Figure 5B is a cross-sectional view of the pixel region along the Vb-Vb' line crossing the TFT 20. Figure 2A and Figure 2BThe same components are denoted by the same reference numerals, and description thereof is omitted.

[0280] The active matrix substrate 102 of the modified example is different from the active matrix substrate 101 in that a first opening 71 is formed in the first region 7 s of the oxide semiconductor layer 7 in the source contact portion SC.

[0281] In the active matrix substrate 102, the source contact hole CHs includes a lower opening 5s of the lower insulating layer 5, a first opening 71 of the oxide semiconductor layer 7, and an upper opening 10s of the interlayer insulating layer 10. The upper opening 10s is configured to overlap at least partially with the first opening 71 of the oxide semiconductor layer 7 when viewed from the normal direction of the substrate 1. It is also possible that the first opening 71 and the lower opening 5s are located inside the upper opening 10s when viewed from the normal direction of the substrate 1. Thus, even when a misalignment occurs, the contact area between the connection electrode 8 and the oxide semiconductor layer 7 can be maintained. In addition, when the first opening 71 is located inside the upper opening 10s, the entire side surface of the lower opening 5s can be aligned with the side surface of the first opening 71. Such a structure can be formed by etching the lower insulating layer 5 and the interlayer insulating layer 10 using the oxide semiconductor layer 7 as an etching stopper.

[0282] In this variation, the proportion of the area of ​​the portion where the upper opening 10s overlaps with the oxide semiconductor layer 7 (i.e., the contact area between the connecting electrode 8 and the upper surface of the oxide semiconductor layer 7) S1 in the entire area of ​​the upper opening 10s when viewed from the normal direction of the substrate 1 can be, for example, greater than 1 / 3 and less than 2 / 3.

[0283] Alternatively, instead of providing the first opening 71 in the oxide semiconductor layer 7 , a cutout may be provided in the oxide semiconductor layer 7 . Figure 5C is a top view of a pixel region in another active matrix substrate of the present variation. Figure 5D is a cross-sectional view of the pixel region along the Vd-Vd' line crossing the TFT 20, Figure 5E It is a cross-sectional view along the Ve-Ve' line crossing the source contact portion SC. As shown in the figure, the first region 7s of the oxide semiconductor layer 7 has at least one (here, two) cutout portions 72. The upper opening 10s is configured so as to at least partially overlap with the cutout portion 72 of the oxide semiconductor layer 7 when viewed from the normal direction of the substrate 1. The shape, size, number, etc. of the cutout portion 72 are not limited to the example shown in the figure. The cutout portion 72 can be formed, for example, in a manner such that the ratio of the above-mentioned area S1 is greater than 1 / 3 and less than 2 / 3.

[0284] (Second embodiment)

[0285] Fig. 6A is a plan view illustrating a pixel region in an active matrix substrate 103 according to the second embodiment. Figure 6B is a cross-sectional view of the pixel region along the line VIb-VIb' crossing the TFT 20. Figure 2A and Figure 2B The same components are denoted by the same reference numerals, and description thereof is omitted.

[0286] The active matrix substrate 103 of this embodiment is different from the active matrix substrate 101 of the above-mentioned embodiment in that the lower insulating layer 5 has a thin film region 52 in the source contact portion SC that is thinner than other regions of the lower insulating layer 5. Hereinafter, the differences from the active matrix substrate 101 will be mainly described, and descriptions of the same configurations will be omitted.

[0287] like Figure 6B As shown, in the source contact portion SC, a thin film region 52 is provided in the lower insulating layer 5. The thickness d1 of the thin film region 52 is smaller than the thickness d2 of other regions of the lower insulating layer 5 (for example, the region overlapping with the channel region 7c when viewed from the normal direction of the substrate 1). The thickness d1 of the thin film region 52 may be, for example, less than 1 / 2 of the thickness d2. Here, the thin film region 52 is formed by providing a recess 51 having a predetermined depth on the surface of the lower insulating layer 5.

[0288] In the source contact portion SC, the oxide semiconductor layer 7 is arranged so as to partially cover the thin-film region 52. The upper opening 10s in the source contact hole CHs is arranged so as to at least partially overlap with the thin-film region 52. The lower opening 5s is formed in the thin-film region 52 of the lower insulating layer 5. In this example, the lower opening 5s is located inside the recess 51 when viewed from the normal direction of the substrate 1.

[0289] <Method for Manufacturing Active Matrix Substrate 103>

[0290] Figure 7A to Figure 7E Each of them is a cross-sectional view of a process for explaining an example of a method for manufacturing the active matrix substrate 103 of the present embodiment, and shows each TFT formation region.

[0291] Hereinafter, a method for manufacturing one pixel region among a plurality of pixel regions in the active matrix substrate 103 will be described. If the material, thickness, formation process, etc. of each layer are the same as those of the active matrix substrate 101, the description thereof will be omitted.

[0292] First, if Fig. 7A As shown in FIG. 1 , a first metal layer M1 including a source bus line SL and a light shielding layer 3 of a TFT is formed, and then a lower insulating layer 5 is formed so as to cover the first metal layer M1 .

[0293] Afterwards, if Figure 7B As shown, in each region where a source contact is to be formed (source contact formation region), a recess 51 is formed on the surface of the lower insulating layer 5, thereby forming a thin film region 52 in the lower insulating layer 5. The recess 51 can be formed by, for example, forming a resist layer on the lower insulating layer 5 by a known photolithography process and etching only the upper portion of the lower insulating layer 5 using the resist layer as a mask (half etching).

[0294] Then, if Figure 7C As shown, an oxide semiconductor layer 7 is formed on the lower insulating layer 5. Here, the oxide semiconductor layer 7 is arranged so as to cover only a part of the recessed portion 51 (that is, only a part of the thin-filmed region 52).

[0295] Next, if Fig.7D As shown, the gate insulating layer 9 and the gate electrode GE are formed on a portion of the oxide semiconductor layer 7. Thereafter, the oxide semiconductor layer 7 is subjected to a resistance lowering treatment to form the channel region 7c, the first region 7s, and the second region 7d.

[0296] Next, if Fig. 7E As shown, an interlayer insulating layer 10 covering the oxide semiconductor layer 7, the gate insulating layer 9, and the gate electrode GE is formed, and the interlayer insulating layer 10 is patterned. Thus, a drain contact hole CHd is formed in the interlayer insulating layer 10 to expose a portion of the second region 7d of the oxide semiconductor layer 7, and a source contact hole CHs is formed in the interlayer insulating layer 10 and the lower insulating layer 5 to expose a portion of the source bus line SL (or the source electrode SE) and a portion of the first region 7s of the oxide semiconductor layer 7. The source contact hole CHs includes a lower opening 5s formed in the thin-film region 52 of the lower insulating layer 5 and an upper opening 10s formed in the interlayer insulating layer 10. The upper opening 10s is configured so that a portion thereof overlaps with the oxide semiconductor layer 7 and the remaining portion overlaps with the thin-film region 52 when viewed from the normal direction of the substrate 1. Thus, only the thin-film region 52 in the lower insulating layer 5 is etched to form the lower opening 5s. A part of the side surface of the lower opening 5 s is aligned with the side surface of the oxide semiconductor layer 7 , and another part is aligned with the side surface of the upper opening 10 s .

[0297] Next, although not shown, a connection electrode 8 is formed on the interlayer insulating layer 10 and in the source contact hole CHs, and a drain electrode DE is formed on the interlayer insulating layer 10 and in the drain opening 10p. The connection electrode 8 is in direct contact with the source bus line SL and the first region 7s. The subsequent steps are the same as those of the active matrix substrate 101, and thus description thereof is omitted.

[0298] According to this embodiment, similarly to the above-mentioned embodiments, the contact resistance of the source contact portion SC can be reduced.

[0299] According to this embodiment, compared with the first embodiment ( Figure 3A to Figure 3L ), a thinning (half etching) step of the lower insulating layer 5 is added, and the number of photomasks used increases by one. However, there are the following advantages.

[0300] In the above-mentioned embodiment, in the patterning process for forming the source contact hole CHs and the drain contact hole CHd, the interlayer insulating layer 10 and the lower insulating layer 5 are etched using the same resist mask. After the interlayer insulating layer 10 is etched to expose a portion of the oxide semiconductor layer 7, until the etching of the lower insulating layer 5 is completed, the exposed portion of the oxide semiconductor layer 7 in the source contact hole CHs and the drain contact hole CHd is exposed to the etching gas and may be damaged. Figure 4A ), the exposed portion of the second wiring 8b in the wiring contact hole CHb is also damaged. In addition, the edge of the resist layer may retreat due to the etching gas during the etching of the lower insulating layer 5, and the contact hole size may become larger than the specified size. In this regard, according to the present embodiment, the lower insulating layer 5 in the area where the source contact hole CHs is formed is thinned, so that the etching time of the lower insulating layer 5 is shortened. As a result, it is possible to suppress damage to the oxide semiconductor layer 7 and the wiring exposed during the etching of the interlayer insulating layer 10, and it is also possible to reduce the deviation of the contact hole size.

[0301] Furthermore, if a through hole reaching the source bus line SL is formed in the lower insulating layer 5 before forming the oxide semiconductor layer 7, the exposed portion of the source bus line SL may be damaged by the etching solution of the oxide semiconductor film. In contrast, in the present embodiment, only the lower insulating layer 5 is thinned before forming the oxide semiconductor layer 7, and the source bus line SL is not exposed, thereby preventing damage to the source bus line SL caused by the etching solution of the oxide semiconductor film.

[0302] In this embodiment, the thinner the thin-film region 52 is, the shorter the time required for etching the lower insulating layer 5 in the etching process for forming the source contact hole CHs, so it is possible to more effectively suppress damage to the exposed portion of the oxide semiconductor layer 7 and deviation of the contact hole size. From this point of view, the thickness d1 of the thin-film region 52 can be, for example, less than 1 / 2 of the thickness d2 of other regions of the lower insulating layer 5 (for example, the thickness of the portion overlapping with the channel region 7c), preferably less than 1 / 3. The lower limit of the thickness d1 of the thin-film region 52 is not particularly limited as long as the source bus line SL is not exposed, but in consideration of etching accuracy, it is set to, for example, 100 nm or more (more than 30% of the thickness d2).

[0303] Although not shown in the figure, in this embodiment, it is also possible to refer to Figure 5A , Figure 5B As in the above-described modification, the first opening or cutout is provided in the oxide semiconductor layer 7. When viewed from the normal direction of the substrate 1, the first opening may be located inside the thin-filmed region 52 (inside the recessed portion 51).

[0304] <Wiring connection section>

[0305] Fig. 8A This is a cross-sectional view showing an example of a wiring connection portion according to the present embodiment. Figure 8B It is a cross-sectional view showing another example of the wiring connection portion.

[0306] like Fig. 8A As shown in the example, in the wiring connection portion (gate-source connection portion) 33, the first wiring 3b formed in the first metal layer M1 is electrically connected to the second wiring 8b arranged in the second metal layer M2 via the wiring connection electrode 6b arranged in the third metal layer M3. A wiring contact hole CHb is formed in the lower insulating layer 5 and the interlayer insulating layer 10 to expose a part of the first wiring 3b and a part of the second wiring 8b. The wiring contact hole CHb includes an upper opening portion 10b formed in the interlayer insulating layer and another lower opening portion 5b formed in the lower insulating layer. The wiring connection electrode 6b is arranged on the interlayer insulating layer 10 and in the wiring contact hole CHb, and is connected to the first wiring 3b and the second wiring 8b in the wiring contact hole CHb.

[0307] In the wiring connection portion 33, the surface of the lower insulating layer 5 has a recessed portion 53. The region 54 having the recessed portion 53 is a thin-film region thinner than other regions of the lower insulating layer 5. When viewed from the normal direction of the substrate 1, the lower opening 5b of the wiring contact hole CHb is located inside the recessed portion 53. In other words, the lower opening 5b is formed in the thin-film region 54 of the lower insulating layer 5. The other configurations are the same as those of the wiring connection portion 31 of the first embodiment.

[0308] like Figure 8B As shown in the example, in the wiring connection portion 34, the first wiring 3c formed in the first metal layer M1 is connected to the third wiring 6c formed in the third metal layer M3. A wiring contact hole CHc is formed in the lower insulating layer 5 and the interlayer insulating layer 10 to expose a portion of the first wiring 3c. The wiring contact hole CHc includes an upper opening 10c formed in the interlayer insulating layer and another lower opening 5c ​​formed in the lower insulating layer. The side surfaces of these openings are aligned with each other. The third wiring 6c is arranged on the interlayer insulating layer 10 and in the wiring contact hole CHc, and is connected to the first wiring 3c in the wiring contact hole CHc.

[0309] In the wiring connection portion 34, the surface of the lower insulating layer 5 has a recessed portion 55. The region 56 having the recessed portion 55 is a thin-film region thinner than other regions of the lower insulating layer 5. When viewed from the normal direction of the substrate 1, the lower opening 5c ​​of the wiring contact hole CHc is located inside the recessed portion 55. In other words, the lower opening 5c ​​is formed in the thin-film region 56 of the lower insulating layer 5. The other configurations are the same as those of the wiring connection portion 32 of the first embodiment.

[0310] The wiring contact holes CHb and CHc in the wiring connection parts 33 and 34 can be formed by a common etching process with the source contact hole CHs and the drain contact hole CHd. Therefore, the wiring connection part 33 and / or the wiring connection part 34 can be formed on the active matrix substrate 103 without increasing the number of manufacturing processes and the number of photomasks used. In addition, in the area where these contact holes are formed, the lower insulating layer 5 is thinned, so the etching time of the lower insulating layer 5 is shortened. Therefore, it is possible to reduce damage to the oxide semiconductor layer 7 and the like exposed during etching of the interlayer insulating layer 10. In addition, the offset of the contact hole size can be reduced.

[0311] (Third embodiment)

[0312] Fig.9A is a plan view illustrating a pixel region in an active matrix substrate 104 according to the third embodiment. Fig. 9B is a cross-sectional view of the pixel region along the line IXb-IXb' crossing the TFT 20. Figure 2A and Figure 2B The same components are denoted by the same reference numerals, and description thereof is omitted.

[0313] The active matrix substrate 104 of this embodiment also has multiple electrodes for touch sensors (hereinafter referred to as "touch sensor electrodes") TX, and multiple wirings (hereinafter referred to as "touch wirings") TL for driving and / or detecting the touch sensors, which is different from the active matrix substrate 101.

[0314] The structures of the TFT 20 and the source contact portion SC in the active matrix substrate 104 are the same as those of the active matrix substrate 101. Although not shown, the structure of the source contact portion SC may be the same as that of the other active matrix substrates 102 and 103.

[0315] The touch line TL is disposed on the upper insulating layer 13 at a distance from the pixel electrode PE. In this example, the touch line TL extends in the column direction so as to overlap with the source bus line SL when viewed from the normal direction of the substrate 1.

[0316] The touch wiring TL has a stacked structure of a lower layer 18 formed in the lower transparent conductive layer T1 and an upper layer 19 formed on the lower layer 18. The upper layer 19 is formed of a fourth conductive film (typically a metal film). The layer including the electrode / wiring formed by the fourth conductive film is referred to as the "fourth metal layer M4". The lower layer 18 and the upper layer 19 are patterned using the same resist mask and are aligned with each other when viewed from the normal direction of the substrate 1.

[0317] The fourth metal layer M4 and the lower transparent conductive layer T1 are covered by a dielectric layer 17. A common electrode CE is arranged on the dielectric layer 17. In this embodiment, the common electrode CE is divided into a plurality of segments, and each segment also functions as a touch sensor electrode TX. Each touch sensor electrode TX is arranged, for example, corresponding to a plurality of pixel regions.

[0318] Each touch sensor electrode TX is connected to a corresponding touch wiring TL. Here, the touch sensor electrode TX is connected to the upper layer 19 of the touch wiring TL in the touch contact hole CHt formed in the dielectric layer 17. The connection portion TC between the touch sensor electrode TX and the touch wiring TL is referred to as a "touch wiring contact portion". It is sufficient that at least one touch wiring TL is provided for one touch sensor electrode TX. It is also possible to provide two or more touch wirings TL for one touch sensor electrode TX.

[0319] The touch line TL extends to the peripheral region of the active matrix substrate 104 and is connected to a touch drive unit (not shown) provided (mounted or integrally) in the peripheral region.

[0320] The touch drive unit is configured to switch between a display mode in which a plurality of touch sensor electrodes TX function as a common electrode CE and a touch detection mode in which the touch sensor electrodes TX function in a time-division manner. For example, in the display mode, the touch drive unit applies a common signal to the touch sensor electrodes TX (common electrode CE) via the touch wiring TL. On the other hand, in the touch detection mode, the touch drive unit applies a touch drive signal to the touch sensor electrodes TX via the touch wiring TL.

[0321] The active matrix substrate 104 may also have a first electrode 21 formed of the same conductive film as the upper layer 19 (i.e., in the fourth metal layer M4) in the pixel contact portion. The first electrode 21 is arranged in contact with the pixel electrode PE on a portion of each pixel electrode PE. The first electrode 21 is an island electrode arranged in a manner overlapping with the pixel contact hole CHp when viewed from the normal direction of the substrate 1. In this example, the first electrode 21 overlaps with the entire pixel contact hole CHp (the entire bottom surface of the pixel contact hole CHp) when viewed from the normal direction of the substrate 1. By providing the first electrode 21, the pixel aperture ratio can be ensured and the surface of the drain electrode DE can be protected. The details will be described later.

[0322] The active matrix substrate 104 is applied to, for example, an embedded touch panel display device. The embedded touch panel display device may have a built-in self-capacitance touch sensor or a built-in mutual capacitance touch sensor. The specific structure, driving method, etc. of the mutual capacitance and self-capacitance touch sensors are described in, for example, Japanese Patent Publication No. 2018-5484, International Application No. 2018 / 092758, International Application No. 2017 / 126603, Japanese Patent Publication No. 2016-126336, etc., and are well known, so detailed descriptions are omitted. For reference, the disclosures of Japanese Patent Publication No. 2018-5484, International Application No. 2018 / 092758, International Application No. 2017 / 126603, and Japanese Patent Publication No. 2016-126336 are all cited in this specification.

[0323] In addition, in this specification, regardless of whether the touch sensor formed on the active matrix substrate 101 is a self-capacitance method or a mutual capacitance method, the electrode for the touch sensor configured on the active matrix substrate 101 side will be referred to as a "touch sensor electrode TX", and the wiring for the touch sensor electrically connected to the touch sensor electrode TX will be referred to as a "touch wiring."

[0324] <Method of Manufacturing Active Matrix Substrate 104>

[0325] Figures 10A to 10F Each of them is a cross-sectional view of a process for explaining an example of a method for manufacturing the active matrix substrate 104 of the present embodiment, and shows each TFT formation region.

[0326] First, if Fig. 10A As shown, the first metal layer M1, the lower insulating layer 5, the oxide semiconductor layer 7, the gate insulating layer 9, the second metal layer M2, the interlayer insulating layer 10 and the third metal layer M3 are formed on the substrate 1 by the same method as the active matrix substrate 101. Thus, the TFT 20 and the source contact portion SC are obtained.

[0327] Next, if Fig. 10BAs shown, an upper insulating layer 13 including an inorganic insulating layer 11 and an organic insulating layer 12 is formed to cover the third metal layer M3. Then, in each pixel region, an opening 12p is formed in the organic insulating layer 12 to expose a portion of the inorganic insulating layer 11.

[0328] Then, if Fig. 10C As shown, the inorganic insulating layer 11 is etched using the organic insulating layer 12 as a mask, and an opening 11p for exposing the drain electrode DE is provided in the inorganic insulating layer 11. In this way, a pixel contact hole CHp including the openings 11p and 12p is formed.

[0329] Next, a first transparent conductive film (not shown) and a fourth conductive film (not shown) are formed on the upper insulating layer 13 and in the pixel contact hole CHp. After that, for example, the fourth conductive film is patterned using a hydrogen peroxide-based etching solution, and then the first transparent conductive film is etched using oxalic acid. Alternatively, the first transparent conductive film and the fourth conductive film are patterned using a hydrogen peroxide-based etching solution containing a fluorine compound. Thus, as shown in FIG. Fig. 10D As shown, the touch wiring TL and the stacked film 40 including the pixel electrode PE are formed spaced apart from each other. The touch wiring TL has a stacked structure including a lower layer 18 formed of a first transparent conductive film and an upper layer 19 formed of a fourth conductive film. The stacked film 40 includes the pixel electrode PE and a conductive layer 41 formed of a fourth conductive film and located on the pixel electrode PE. When viewed from the normal direction of the substrate 1, the lower layer 18 and the upper layer 19 are aligned with each other, and the pixel electrode PE and the conductive layer 41 are aligned with each other.

[0330] The same conductive film as the gate conductive film or the source conductive film can be used as the fourth conductive film. The fourth conductive film may be a metal film (thickness: 50 to 500 nm) mainly composed of Cu or Al and having a single layer or a stacked structure.

[0331] Then, if Fig. 10E As shown, the conductive layer 41 is patterned to obtain the first electrode 21. The conductive layer 41 is patterned under the condition that the pixel electrode PE is not etched but only the conductive layer 41 is etched. Here, for example, the conductive layer 41 is wet-etched using a hydrogen peroxide-based etching solution that does not contain a fluorine compound.

[0332] Forming the first electrode 21 by the above-described method provides the following advantages.

[0333] If only the first transparent conductive film (for example, indium tin oxide (ITO)) is formed on the upper insulating layer 13 and in the pixel contact hole CHp and patterned, pinholes are easily formed in the pixel contact hole CHp because the first transparent conductive film is relatively thin. When a pinhole is formed in the first transparent conductive film in the pixel contact hole CHp, the surface of the drain electrode DE may be exposed and damaged due to the pinhole. In this regard, in the present embodiment, in a state where the fourth conductive film is formed on the first transparent conductive film, the first transparent conductive film and the fourth conductive film are patterned at the same time to form a stacked film 40 including the pixel electrode PE. As a result, it is not easy to generate pinholes in the first transparent conductive film (pixel electrode PE). In addition, even if a pinhole is generated, since the drain electrode DE is covered by the fourth conductive film, the surface of the drain electrode DE can be protected, and the increase in the contact resistance of the pixel contact portion caused by the pinhole can be suppressed. Then, the portion of the fourth conductive film (conductive layer 41) covering the entire pixel electrode PE other than the pixel contact portion (i.e., the portion located in the region contributing to display) is removed to form the first electrode 21. This can suppress the decrease in pixel aperture ratio caused by using the fourth conductive film.

[0334] Next, if Fig.10F As shown, a dielectric layer 17 (thickness: 50 to 500 nm) is formed to cover the touch wiring TL, the pixel electrode PE, and the first electrode 21. Then, the dielectric layer 17 is patterned to form a touch contact hole CHt that exposes a portion of the upper layer 19 of the touch wiring TL.

[0335] Next, a second transparent conductive film is formed on the dielectric layer 17 and in the touch contact hole CHt, and the second transparent conductive film is patterned. Fig.9A and Fig. 9B As shown in FIG. 1 , a common electrode CE including a plurality of segments each functioning as a touch sensor electrode TX is formed. Each touch sensor electrode TX is connected to a corresponding touch wiring TL in a touch contact hole CHt. In this way, an active matrix substrate 104 is manufactured.

[0336] The structure of the active matrix substrate for the embedded touch panel type display device of this embodiment is not limited to the above-mentioned structure. The source contact portion SC may also have the same structure as the source contact portion SC in the active matrix substrate 102 or the active matrix substrate 103. In addition, a common electrode CE (touch sensor electrode TX) may be formed in the lower transparent conductive layer T1, and a pixel electrode PE may be formed in the upper transparent conductive layer T2. The configuration of the touch wiring TL and the structure of the touch wiring contact portion TC are also not particularly limited.

[0337] In this embodiment, the touch wiring TL is formed in the fourth metal layer M4 using the same conductive film as the first electrode 21, but other electrodes / wirings may be formed instead. Such an active matrix substrate can also be applied to display devices other than embedded touch panel types. Although not shown, in the active matrix substrate of other embodiments, the fourth metal layer M4 including the first electrode 21 may be formed to protect the drain electrode DE.

[0338] (Fourth embodiment)

[0339] Fig.11A is a plan view illustrating a pixel region in an active matrix substrate 105 according to a fourth embodiment. Fig. 11B is a cross-sectional view of the pixel region along line XIb-XIb' crossing the TFT 20. Figure 2A and Figure 2B The same components are denoted by the same reference numerals, and description thereof is omitted.

[0340] The active matrix substrate 105 of this embodiment is different from the active matrix substrate 101 in that it does not include the third metal layer M3 and the organic insulating layer 12. In the active matrix substrate 105, the connection electrode of the source contact portion SC is formed in the lower transparent conductive layer T1.

[0341] In the active matrix substrate 105, a lower transparent conductive layer T1 including a pixel electrode PE and a connection electrode 23 is formed on the interlayer insulating layer 10. The pixel electrode PE is arranged on the interlayer insulating layer 10 and in the drain contact hole CHd formed in the interlayer insulating layer 10, and is arranged in a manner of contacting the second region 7d of the oxide semiconductor layer 7 in the drain contact hole CHd. That is, the oxide semiconductor layer 7 of the TFT 20 is electrically connected to the pixel electrode PE without passing through the drain electrode DE. The connection electrode 23 is arranged on the interlayer insulating layer 10 and in the source contact hole CHs formed in the lower insulating layer 5 and the interlayer insulating layer 10, and is connected to the second region 7d of the oxide semiconductor layer 7 and the source bus line SL in the source contact hole CHs.

[0342] The pixel electrode PE and the connection electrode 23 are covered by a dielectric layer 17. On the dielectric layer 17, an upper transparent conductive layer T2 including a common electrode CE is arranged.

[0343] Although not shown in the figure, the pixel electrode PE and the connection electrode 23 may be formed in the upper transparent conductive layer T2, and the common electrode CE may be formed in the lower transparent conductive layer T1. In addition, the structure of the source contact portion SC is not limited to the structure shown in the figure. Except that the connection electrode is formed using a transparent conductive film, it may have the same structure as the source contact portion SC in the active matrix substrate 102 and the active matrix substrate 103.

[0344] According to the present embodiment, by eliminating the third metal layer M3, the number of photomasks to be used can be reduced, thereby reducing the manufacturing cost.

[0345] The structure and manufacturing method of the active matrix substrate of the embodiment of the present invention are not limited to the structure and method exemplified above. In the above, an active matrix substrate having a top-gate pixel TFT is exemplified, but it may be replaced by a double-gate pixel TFT having two gates sandwiching an oxide semiconductor layer. For example, in the TFT 20 of the above embodiment, the light shielding layer 3 may also function as a lower gate electrode.

[0346] The embodiments of the present invention can be widely applied to devices and electronic devices equipped with TFTs, for example, circuit substrates such as active matrix substrates, display devices such as liquid crystal display devices, organic EL display devices, and micro-LED display devices, imaging devices such as radiation detectors and image sensors, image input devices, and electronic devices such as fingerprint readers.

[0347] <About Oxide Semiconductors>

[0348] The oxide semiconductor included in the oxide semiconductor layer 7 may be an amorphous oxide semiconductor or a crystalline oxide semiconductor having a crystalline portion. Examples of the crystalline oxide semiconductor include polycrystalline oxide semiconductors, microcrystalline oxide semiconductors, and crystalline oxide semiconductors with c-axis oriented substantially perpendicular to the layer surface.

[0349] The oxide semiconductor layer 7 may also have a stacked structure of more than two layers. In the case where the oxide semiconductor layer 7 has a stacked structure, the oxide semiconductor layer 7 may include an amorphous oxide semiconductor layer and a crystalline oxide semiconductor layer. Alternatively, it may include multiple crystalline oxide semiconductor layers with different crystal structures. In addition, it may also include multiple amorphous oxide semiconductor layers. In the case where the oxide semiconductor layer 7 has a two-layer structure including an upper layer and a lower layer, the energy gap of the oxide semiconductor included in the layer located on the gate electrode side of the two layers (if it is a bottom gate type, it is the lower layer, if it is a top gate type, it is the upper layer) may be smaller than the energy gap of the oxide semiconductor included in the layer located on the side opposite to the gate electrode (if it is a bottom gate type, it is the upper layer, if it is a top gate type, it is the lower layer). However, in the case where the difference in the energy gaps of these layers is relatively small, the energy gap of the oxide semiconductor of the layer located on the gate electrode side may also be larger than the energy gap of the oxide semiconductor of the layer located on the side opposite to the gate electrode.

[0350] The materials, structures, film formation methods, and configurations of oxide semiconductor layers having a stacked structure of amorphous oxide semiconductors and the above-mentioned crystalline oxide semiconductors are described in, for example, Japanese Patent Application Laid-Open No. 2014-007399, the disclosure of which is incorporated herein by reference in its entirety.

[0351] The oxide semiconductor layer 7 may contain, for example, at least one metal element selected from the group consisting of In, Ga, and Zn. In the present embodiment, the oxide semiconductor layer 7 may contain, for example, an In-Ga-Zn-O semiconductor (e.g., indium gallium zinc oxide). Here, the In-Ga-Zn-O semiconductor is a ternary oxide of In (indium), Ga (gallium), and Zn (zinc), and the ratio (composition ratio) of In, Ga, and Zn is not particularly limited, and may include, for example, In:Ga:Zn=2:2:1, In:Ga:Zn=1:1:1, In:Ga:Zn=1:1:2, etc. Such an oxide semiconductor layer 7 may be formed of an oxide semiconductor film containing an In-Ga-Zn-O semiconductor.

[0352] In-Ga-Zn-O semiconductors may be amorphous or crystalline. As crystalline In-Ga-Zn-O semiconductors, preferably, the c-axis is oriented substantially perpendicular to the plane.

[0353] In addition, the crystal structure of the semiconductor of the crystalline In-Ga-Zn-O system is disclosed in, for example, the above-mentioned Japanese Patent Publication No. 2014-007399, Japanese Patent Publication No. 2012-134475, Japanese Patent Publication No. 2014-209727, etc. For reference, the disclosures of Japanese Patent Publication No. 2012-134475 and Japanese Patent Publication No. 2014-209727 are all cited in this specification. The TFT having an In-Ga-Zn-O system oxide semiconductor layer has a high mobility (more than 20 times compared to a-SiTFT) and a low leakage current (less than one percent compared to a-SiTFT), and is therefore suitable for use as a driving TFT (for example, a TFT included in a driving circuit disposed on the same substrate as a display region around a display region including a plurality of pixels) and a pixel TFT (a TFT disposed in a pixel).

[0354] The oxide semiconductor layer 7 may also include other oxide semiconductors instead of the In-Ga-Zn-O semiconductor. For example, it may include an In-Sn-Zn-O semiconductor (e.g., In2O3-SnO2-ZnO; InSnZnO). The In-Sn-Zn-O semiconductor is a ternary oxide of In (indium), Sn (tin), and Zn (zinc). Alternatively, the oxide semiconductor layer 7 may also include In-Al-Zn-O based semiconductors, In-Al-Sn-Zn-O based semiconductors, Zn-O based semiconductors, In-Zn-O based semiconductors, Zn-Ti-O based semiconductors, Cd-Ge-O based semiconductors, Cd-Pb-O based semiconductors, CdO (cadmium oxide), Mg-Zn-O based semiconductors, In-Ga-Sn-O based semiconductors, In-Ga-O based semiconductors, Zr-In-Zn-O based semiconductors, Hf-In-Zn-O based semiconductors, Al-Ga-Zn-O based semiconductors, Ga-Zn-O based semiconductors, In-Ga-Zn-Sn-O based semiconductors, In-W-Zn-O based semiconductors, etc.

Claims

1. An active matrix substrate having a plurality of pixel regions, It is characterized in that have: substrate; A plurality of gate bus lines and a plurality of source bus lines supported on the main surface of the substrate, wherein the plurality of source bus lines are located closer to the substrate than the plurality of gate bus lines; a lower insulating layer, located between the plurality of source bus lines and the plurality of gate bus lines, and covering the plurality of source bus lines; an interlayer insulating layer covering the plurality of gate bus lines; A plurality of oxide semiconductor TFTs, which are arranged corresponding to the plurality of pixel regions; as well as A pixel electrode is disposed in each of the plurality of pixel regions. Each of the plurality of oxide semiconductor TFTs has: an oxide semiconductor layer, which is disposed on the lower insulating layer, and includes a channel region and a first region and a second region respectively located on both sides of the channel region, the first region being electrically connected to a corresponding one of the plurality of source bus lines, and the second region being electrically connected to the pixel electrode; a gate electrode disposed on a portion of the oxide semiconductor layer via a gate insulating layer and electrically connected to a corresponding one of the plurality of gate bus lines, wherein the gate electrode and the plurality of gate bus lines are formed of the same conductive film; as well as a source electrode formed between the substrate and the lower insulating layer and electrically connected to a corresponding one of the plurality of source bus lines, wherein the source electrode and the plurality of source bus lines are formed of the same conductive film, The active matrix substrate further includes a plurality of source contacts each electrically connecting one of the plurality of oxide semiconductor TFTs to the corresponding one of the source bus lines, each of the source contacts having: a source contact hole formed in the lower insulating layer and the interlayer insulating layer and exposing a portion of the first region of the oxide semiconductor layer and a portion of the source electrode in the one oxide semiconductor TFT, the source contact hole including a lower opening formed in the lower insulating layer and an upper opening formed in the interlayer insulating layer; as well as a connecting electrode disposed on the interlayer insulating layer and in the source contact hole, and connected to the portion of the first region and the portion of the source electrode in the source contact hole, In each of the source contacts, the lower insulating layer has a thin film region, a thickness d1 of the thin film region is smaller than a thickness d2 of a region of the lower insulating layer overlapping the channel region when viewed from a normal direction of the substrate, The lower opening of the source contact hole is formed in the thin-filmed region.

2. The active matrix substrate according to claim 1, In the source contact hole, a side surface of the oxide semiconductor layer is aligned with a side surface of the lower opening.

3. The active matrix substrate according to claim 1 or 2, In each of the source contact portions, when viewed in the normal direction of the substrate, an edge portion of the oxide semiconductor layer extends across the upper opening portion of the source contact hole.

4. The active matrix substrate according to claim 1 or 2, In each of the source contacts, the first region of the oxide semiconductor layer has a first opening. When viewed in a normal direction to the substrate, the first opening of the oxide semiconductor layer is located inside the upper opening of the source contact hole.

5. The active matrix substrate according to claim 1 or 2, Each of the oxide semiconductor TFTs further includes a drain electrode formed on the interlayer insulating layer and electrically connected to a corresponding one of the plurality of pixel electrodes. The connection electrode of each of the source contacts is formed of the same conductive film as the drain electrode of each of the oxide semiconductor TFTs.

6. The active matrix substrate according to claim 1 or 2, The connection electrode of each source contact portion is formed of the same transparent conductive film as the plurality of pixel electrodes.

7. The active matrix substrate according to claim 1, In each of the source contacts, the oxide semiconductor layer partially covers the thin-filmed region.

8. The active matrix substrate according to claim 1, The thickness d1 of the thin-film region is less than or equal to 1 / 2 of the thickness d2 of a region of the lower insulating layer that overlaps with the channel region when viewed in the normal direction of the substrate.

9. The active matrix substrate according to claim 1 or 2, The active matrix substrate comprises a display region including the plurality of pixel regions and a non-display region located around the display region. It also includes a plurality of wiring connection parts arranged in the non-display area. Each of the plurality of wiring connection portions has: a first wiring line formed of the same conductive film as the plurality of source bus lines; The lower insulating layer is extended on the first wiring; a second wiring line formed of the same conductive film as the plurality of gate bus lines; an insulating layer disposed between the second wiring and the lower insulating layer; The interlayer insulating layer is extended on the second wiring; a wiring contact hole formed in the lower insulating layer and the interlayer insulating layer to expose a portion of the first wiring and a portion of the second wiring; as well as The wiring connection electrode is arranged on the interlayer insulating layer and in the wiring contact hole, and is connected to the part of the first wiring and the part of the second wiring in the wiring contact hole.

10. The active matrix substrate according to claim 1, The active matrix substrate comprises a display region including the plurality of pixel regions and a non-display region located around the display region. It also includes a plurality of wiring connection parts arranged in the non-display area. Each of the plurality of wiring connection portions has: a first wiring line formed of the same conductive film as the plurality of source bus lines; The lower insulating layer is extended on the first wiring; a second wiring line formed of the same conductive film as the plurality of gate bus lines; an insulating layer disposed between the second wiring and the lower insulating layer; The interlayer insulating layer is extended on the second wiring; a wiring contact hole formed in the lower insulating layer and the interlayer insulating layer to expose a portion of the first wiring and a portion of the second wiring; as well as a wiring connection electrode, which is arranged on the interlayer insulating layer and in the wiring contact hole, and is connected to the part of the first wiring and the part of the second wiring in the wiring contact hole, The wiring contact hole of each wiring connection portion includes another lower opening formed in the lower insulating layer and another upper opening formed in the interlayer insulating layer. In each of the wiring connection portions, the lower insulating layer has another thin-film region. When viewed from the normal direction of the substrate, the other lower opening of the wiring contact hole is formed in the other thin-filmed region.

11. The active matrix substrate according to claim 5, The active matrix substrate further comprises an upper insulating layer covering the connection electrode and the drain electrode in each pixel region. The upper insulating layer has a pixel contact hole for exposing a portion of the drain electrode. The pixel electrode is disposed on the upper insulating layer and in the pixel contact hole, and is connected to the portion of the drain electrode in the pixel contact hole.

12. The active matrix substrate according to claim 11, Each of the pixel regions further includes a first electrode disposed on a portion of the pixel electrode so as to be in contact with an upper surface of the pixel electrode. The first electrode is formed of a metal film, and when viewed from a normal direction of the substrate, the first electrode overlaps the entire pixel contact hole.

13. The active matrix substrate according to claim 12, Also available: a plurality of touch wirings arranged on the upper insulating layer; and a plurality of touch sensor electrodes, each of which is electrically connected to any one of the plurality of touch wirings; Each of the plurality of touch wires has a stacked structure including a lower layer formed of the same transparent conductive film as the plurality of pixel electrodes and an upper layer formed of the same metal film as the first electrode.

14. The active matrix substrate according to claim 1 or 2, The oxide semiconductor layer includes an In—Ga—Zn—O-based semiconductor.

15. A method for manufacturing an active matrix substrate, The active matrix substrate has a plurality of pixel regions, a plurality of source bus lines and a plurality of gate bus lines, and a plurality of oxide semiconductor TFTs corresponding to the plurality of pixel regions. The method for manufacturing the active matrix substrate is characterized in that, in each TFT formation region where each of the plurality of oxide semiconductor TFTs is formed, the following is included: Step (a) of forming a first conductive film on a substrate and patterning the first conductive film to form a first metal layer including a source electrode of the oxide semiconductor TFT. in, The source electrode is formed integrally with a corresponding one of the plurality of source bus lines; Step (b), forming a lower insulating layer on the first metal layer; Step (c), forming an oxide semiconductor layer of the oxide semiconductor TFT on the lower insulating layer, wherein the oxide semiconductor layer includes a channel region; Step (d), forming a gate insulating film and a second conductive film so as to cover the oxide semiconductor layer, patterning the gate insulating film and the second conductive film, thereby forming a gate insulating layer from the gate insulating film, and forming a second metal layer including a gate electrode of the oxide semiconductor TFT from the second conductive film, wherein the gate electrode is formed integrally with a corresponding one of the plurality of gate bus lines, and is disposed on a portion of the oxide semiconductor layer via the gate insulating layer; Step (e), forming an interlayer insulating layer covering the second metal layer; Step (f), patterning the interlayer insulating layer and the lower insulating layer to form a source contact hole exposing a portion of the source electrode of the oxide semiconductor TFT and a portion of the oxide semiconductor layer, the source contact hole including a lower opening formed in the lower insulating layer; and step (g), forming a third conductive film on the interlayer insulating layer and in the source contact hole, and forming a connecting electrode in the source contact hole in contact with the portion of the source electrode and the portion of the oxide semiconductor layer by patterning the third conductive film, The lower insulating layer has a thin film region, and a thickness d1 of the thin film region is smaller than a thickness d2 of a region of the lower insulating layer overlapping the channel region when viewed from a normal direction of the substrate. The lower opening of the source contact hole is formed in the thin-filmed region.

16. The method for manufacturing an active matrix substrate according to claim 15, The method further includes, between the step (b) and the step (c), forming a thin-film region in the lower insulating layer. In the step (f), the source contact hole is formed by patterning the interlayer insulating layer and the thin-filmed region of the lower insulating layer.

17. The method for manufacturing an active matrix substrate according to claim 15 or 16, The step (f) includes forming a drain contact hole in the interlayer insulating layer to expose another portion of the oxide semiconductor layer. The step (g) includes the step of forming a drain electrode in contact with the other portion of the oxide semiconductor layer in the drain contact hole by patterning the third conductive film.

18. The method for manufacturing an active matrix substrate according to claim 17, Each of the plurality of pixel regions further includes: Step (h), forming an upper insulating layer on the interlayer insulating layer, and forming a pixel contact hole in the upper insulating layer to expose a portion of the drain electrode of the oxide semiconductor TFT; Step (i), forming a first transparent conductive film and a fourth conductive film on the upper insulating layer and in the pixel contact hole, and forming a laminated film including a pixel electrode formed of the first transparent conductive film and a conductive layer formed of the fourth conductive film by patterning the first transparent conductive film and the fourth conductive film; and Step (j), further patterning the conductive layer to form a first electrode disposed on a portion of the pixel electrode, in, When viewed from a normal direction of the substrate, the first electrode overlaps the entire pixel contact hole.

19. The method for manufacturing an active matrix substrate according to claim 18, The step (i) further includes forming a plurality of touch wirings by patterning the first transparent conductive film and the fourth conductive film.