Semipermeable membrane support and method for producing the same

Through wet printing and hot pressing processing, the thickness difference of the semi-permeable membrane support is adjusted, which solves the problem of poor water permeability after modularization of the semi-permeable membrane support, and achieves high adhesion and adhesion, ensuring that Modular water permeability.

CN113272051BActive Publication Date: 2024-11-15MITSUBISHI PAPER MILLS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080008360.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-01-09
Filing Date
2020-01-06
Publication Date
2024-11-15
Estimated Expiration
2040-01-06

AI Technical Summary

Technical Problem

The existing semipermeable membrane support is poor in water permeability after modularization, mainly due to the low adhesion between the raw water spacer and the semipermeable membrane, the design of the spiral module cannot effectively exert water permeability.

Method used

The semi-permeable membrane support is manufactured by wet printing method, and the combination of metal rollers and elastic rollers is heat pressed and processed. The difference in the measured thickness is adjusted to be more than 1.0% and less than 5.0% to ensure good density between the raw water spacer and the semi-permeable membrane. Fitness and adhesion.

Benefits of technology

The high adhesion between the semi-permeable membrane and the semi-permeable membrane support and the excellent adhesion between the raw water spacer and the semi-permeable membrane are achieved, ensuring good water permeability after modularization and avoiding the problem of degradation of water permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113272051B_ABST
    Figure CN113272051B_ABST
Patent Text Reader

Abstract

A semipermeable membrane supporting body and a method for producing a semipermeable membrane supporting body subjected to heat pressing using an elastic roller having a hardness of 60 or more on a type A durometer and a hardness of 95 or less on a type D durometer, wherein the semipermeable membrane supporting body has a strength of 0.80 N / cm 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness measured under the conditions of is 1.0% to 5.0%, the semipermeable membrane has excellent adhesion to the semipermeable membrane supporting body, and the raw water spacer has excellent adhesion to the semipermeable membrane, thereby being expected to maintain good water permeability after modularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a semipermeable membrane support and a method for producing the semipermeable membrane support. Background Art

[0002] Semipermeable membranes are widely used in the fields of ultrapure water manufacturing for medical use and semiconductor cleaning represented by seawater desalination, water purifiers, food concentration, wastewater treatment, and blood filtration. As the separation functional layer of the semipermeable membrane, it is composed of porous resins such as cellulose resins, polysulfone resins, polyacrylonitrile resins, fluorine resins, and polyester resins. However, these porous resins have poor mechanical strength when they are alone, so a composite form in which a semipermeable membrane is provided on a single surface of a semipermeable membrane support body containing a fiber substrate such as a non-woven fabric or a woven fabric, i.e., a "filter membrane" is used. In the semipermeable membrane support body, the surface provided with the semipermeable membrane is called the "coated surface", and the surface without the semipermeable membrane is called the "non-coated surface".

[0003] For a "filtration membrane" in the form of a semipermeable membrane provided on a semipermeable membrane support, the following method is widely used: after dissolving a synthetic resin such as the above-mentioned polysulfone resin in an organic solvent to prepare a semipermeable membrane solution, the semipermeable membrane solution is applied to the semipermeable membrane support. In addition, the semipermeable membrane is required to have high adhesion to the semipermeable membrane support.

[0004] In addition, the filter membrane is used in a modular manner. Representative modules of sheet-like filter membranes are spiral modules and flat membrane modules. Representative modules of tubular filter membranes are tubular / tubular modules (see Patent Document 1). The spiral module has a structure in which the raw water supply side flow path material (hereinafter, "raw water supply side flow path material" is sometimes referred to as "raw water spacer"), the filter membrane and the treated water permeate side flow path material (hereinafter, "treated water permeate side flow path material" is sometimes referred to as "permeate water spacer") are rolled up together (see Patent Document 1). In addition, in the flat membrane module, the filter membrane is bonded and fixed to a frame material containing a resin such as polypropylene, acrylonitrile (Acrylonitrile)-butadiene (Butadiene)-styrene (Styrene) copolymer resin (ABS resin) for use. The bonding and fixing of the frame material is usually performed by heat welding treatment, ultrasonic welding treatment, etc.

[0005] As the semipermeable membrane support, paper made from pulp fibers, nonwoven fabrics made from polyester fibers and polypropylene fibers are generally used (see Patent Documents 2 and 3). In addition, for sheets made by wet papermaking, the strength, density and other properties of the semipermeable membrane support can be changed by adjusting the temperature, pressure, roll hardness, etc. by arbitrarily combining metal rolls and elastic rolls with a heating mechanism to perform hot pressing treatment (see Patent Document 4).

[0006] In recent years, in spiral modules using sheet-shaped filtration membranes, there has been a problem that after modularization, the water permeability calculated at the time of design is not achieved.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2001-252543

[0010] Patent Document 2: Japanese Patent Application Laid-Open No. 56-152705

[0011] Patent Document 3: Japanese Patent Application Publication No. 2002-95937

[0012] Patent Document 4: Japanese Patent Application Publication No. 2004-100047

[0013] Non-patent literature

[0014] Non-special static document 1: "Guidelines for the introduction of membrane treatment technology in sewage" compiled by the Sewage Membrane Treatment Technology Conference, [online], March 2011, [retrieved on January 6, 2011], Internet<URL:http: / / www.mlit.go.jp / common / 000146906.pdf> The inventors studied the reason why the semipermeable membrane supporting body used in the spiral module did not exhibit the water permeability calculated at the time of design after modularization, and found that the adhesion between the raw water spacer and the semipermeable membrane was low. Summary of the invention

[0015] Problems to be solved by the invention

[0016] An object of the present invention is to provide a semipermeable membrane supporting body having excellent adhesion between a semipermeable membrane and the semipermeable membrane supporting body and excellent adhesion between a raw water spacer and the semipermeable membrane, which can be expected to maintain good water permeability after modularization due to these properties.

[0017] Another object of the present invention is to provide an industrially advantageous production method for producing the semipermeable membrane supporting material of the present invention.

[0018] Other objects and advantages of the present invention will become apparent from the following description.

[0019] Means for solving problems

[0020] Means for Solving the Problems The present inventors have conducted intensive studies to solve the above-mentioned problems and have found the following invention.

[0021] (1) A semipermeable membrane supporting body characterized in that it is used with a semipermeable membrane, and the semipermeable membrane supporting body has a strength of 0.80 N / cm2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness under the conditions of 0.80N / cm 2 The measured thickness under the conditions of is 1.0% or more and 5.0% or less.

[0022] (2) The semipermeable membrane supporting material according to (1), characterized in that the semipermeable membrane supporting material has a strength of 0.80 N / cm 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness under the conditions of 0.80N / cm 2 The measured thickness under the conditions of is 1.4% or more and 3.0% or less.

[0023] (3) A method for producing a semipermeable membrane supporting body, characterized in that the method comprises subjecting a sheet produced by a wet papermaking method to a hot press treatment,

[0024] The hot pressing treatment is performed using a hot pressing treatment device having a combination of a metal roller and an elastic roller. At this time, an elastic roller having a hardness of 60 or more on a type A durometer and a hardness of 95 or less on a type D durometer is used as the elastic roller. The nip pressure between the metal roller and the elastic roller is set to 30 kN / m or more and 250 kN / m or less, and the processing speed is set to 20 m / min or more and 100 m / min or less. The hot pressing treatment is performed at 0.80 N / cm 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness under the conditions of 0.80N / cm 2 A semipermeable membrane supporting material having a measured thickness under the conditions of 1.0% to 5.0%.

[0025] (4) The method for producing a semipermeable membrane supporting material according to (3), wherein an elastic roller having a type A durometer hardness of 60 or more and 80 or less is used as the elastic roller.

[0026] Effects of the Invention

[0027] According to the semipermeable membrane supporting body of the present invention, the adhesion between the semipermeable membrane and the semipermeable membrane supporting body is excellent, and the adhesion between the raw water spacer and the semipermeable membrane is also excellent, so it can be expected that the water permeability after modularization is well maintained. In addition, according to the method for manufacturing a semipermeable membrane supporting body of the present invention, a semipermeable membrane supporting body having a more excellent adhesion between the semipermeable membrane and the semipermeable membrane supporting body can be manufactured.

[0028] BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1It is a schematic diagram showing the combination and arrangement of rollers used in the hot pressing process in the present invention, and the state of sheet passing.

[0030] Figure 2 It is a schematic diagram showing the combination and arrangement of rollers used in the hot pressing process in the present invention, and the state of sheet passing. DETAILED DESCRIPTION

[0031] The semipermeable membrane support of the present invention is preferably a wet nonwoven fabric comprising at least a main synthetic fiber and a binder synthetic fiber. The semipermeable membrane support of the present invention is characterized in that it is a semipermeable membrane support used with a semipermeable membrane provided on one surface, and the semipermeable membrane support has a strength of 0.80 N / cm 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness under the conditions of 0.80N / cm 2 The measured thickness under the conditions of is 1.0% or more and 5.0% or less.

[0032] More preferably, the semipermeable membrane support has a strength of 0.80 N / cm 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness under the conditions of 0.80N / cm 2 The measured thickness under the conditions of is 1.4% or more and 3.0% or less.

[0033] In this specification, “at 0.80 N / cm 2 The thickness measured under the conditions of 1.27 N / cm is abbreviated as "measured thickness (0.80)". 2 The thickness measured under the conditions of 0.80 N / cm is abbreviated as "measured thickness (1.27)". 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in measured thickness under the conditions of "measured thickness" is abbreviated as "measured thickness difference". "Measured thickness difference" is "{measured thickness (0.80) - measured thickness (1.27)} / measured thickness (0.80) × 100", and the unit is "%".

[0034] The results of the present invention are that by making the difference in measured thickness less than 5.0%, when a spiral module is formed and used, the raw water spacer and the semipermeable membrane are in good contact and close contact, and good turbulence is generated on the semipermeable membrane surface, so that water permeability can be well maintained. In the case where the difference in measured thickness is greater than 5.0%, a gap is generated at the interface between the raw water spacer and the semipermeable membrane due to the pressure applied to the semipermeable membrane support body when the spiral module is used, and good turbulence is not generated, thereby reducing water permeability. In addition, by making the difference in measured thickness more than 1.0%, when making a spiral module, the raw water spacer and the permeated water spacer can be well in close contact with the semipermeable membrane and the semipermeable membrane support body, and water permeability can be well maintained. In the case where the difference in measured thickness is less than 1.0%, when making a spiral module, the close contact between the raw water spacer or the permeated water spacer and the filtration membrane is reduced, and a gap is easily generated, and water permeability is reduced.

[0035] In the present invention, the difference in measured thickness is more preferably 3.0% or less. When the difference in measured thickness is 3.0% or less, when a spiral module is formed for use, even if pressure is applied to the semipermeable membrane support, a gap is less likely to be generated at the interface between the raw water spacer and the semipermeable membrane, and better turbulence is generated, thereby maintaining water permeability better. In addition, the difference in measured thickness is more preferably 1.4% or more. When the difference in measured thickness is 1.4% or more, when a spiral module is made, the raw water spacer and the permeated water spacer can be more closely fitted to the semipermeable membrane and the semipermeable membrane support, and water permeability can be maintained better.

[0036] The semipermeable membrane support of the present invention preferably contains main body fiber and bonding fiber.Main body fiber is the fiber that forms the skeleton of semipermeable membrane support.As main body fiber, synthetic fiber is mainly used.For example, the fiber of polyolefin system, polyamide system, polyacrylic acid system, vinylon system, vinylidene system, polyvinyl chloride system, polyester system, benzoate system, Polychlal system, phenol system etc. can be enumerated, it is not particularly limited, more preferably the fiber of polyester system with high heat resistance, further preferably the fiber of ethylene terephthalate (PET) system.In addition, acetate, triacetate, Promix (Promix), rayon of regenerated fiber, cuprammonium fiber, Lyocell (Lyocell) fiber etc. of semisynthetic fiber can also be used in combination.

[0037] As the bonding fiber, composite fibers such as core-sheath fibers (core-shell type), parallel fibers (side-by-side type), radially split fibers, and undrawn fibers can be cited. Composite fibers are not easy to form a coating, so they can improve the mechanical strength while maintaining the space of the semipermeable membrane support. More specifically, undrawn fibers such as a combination of polypropylene (core) and polyethylene (sheath), a combination of polypropylene (core) and ethylene vinyl alcohol (sheath), a combination of high melting point polyester (core) and low melting point polyester (sheath), and polyester can be cited. In addition, hot water-soluble binders such as single fibers (full melt type) composed only of low melting point resins such as polyethylene and polypropylene, and polyvinyl alcohol systems are easy to form a coating in the drying process of the semipermeable membrane support, and can be used within the range of not hindering the properties. In the present invention, the combination of high melting point polyester (core) and low melting point polyester (sheath) and undrawn fibers of polyester are preferred, and undrawn fibers of PET systems are more preferred.

[0038] In the semipermeable membrane supporting body of the present invention, as the main fiber, two or more fibers with different fiber diameters can be used together, and their average fiber diameter is not particularly limited. By arbitrarily and using two or more main fibers with different fiber diameters, it is possible to give changes to the fiber network, and it is possible to adjust the difference in measured thickness, measured thickness (0.80) and measured thickness (1.27).

[0039] The fiber diameter and fiber length of the fiber used in the semipermeable membrane support of the present invention are not particularly limited. From the perspective of nonwoven strength and manufacturability, the fiber diameter is preferably 1 μm or more and 30 μm or less, more preferably 3 μm or more and 25 μm or less, and particularly preferably 5 μm or more and 20 μm or less. The fiber length is preferably 1 mm or more and 20 mm or less, more preferably 1 mm or more and 12 mm or less, and particularly preferably 3 mm or more and 10 mm or less. The cross-sectional shape of the fiber is preferably circular, but in order to prevent penetration and surface smoothness, it is also possible to contain fibers with T-shaped, Y-shaped, triangular or other shaped cross-sections within the range of not hindering other characteristics such as fiber dispersibility. In addition, the split composite fiber can also be subdivided and used by water flow entanglement and refiner.

[0040] The air permeability of the semipermeable membrane supporting material of the present invention is preferably 0.5 to 25.0 cc / cm 2 · seconds, more preferably 1.0 to 20.0 cc / cm 2 · seconds, more preferably 1.5 to 16.0 cc / cm 2 · seconds, particularly preferably 2.0 to 15.0 cc / cm 2 When the length is within this range, the adhesion between the semipermeable membrane and the semipermeable membrane supporting body becomes good, and when the semipermeable membrane solution is applied, permeation is unlikely to occur, and the smoothness of the applied surface is also likely to become good.

[0041] The semipermeable membrane supporting material of the present invention may be a multilayer nonwoven fabric having two or more layers laminated thereon. The two or more layers may have the same formulation or different formulations.

[0042] In the method for producing a semipermeable membrane supporting material of the present invention, a sheet produced by a wet papermaking method is subjected to a hot press processing.

[0043] In the present invention, in the method for manufacturing a semipermeable membrane support body in which a sheet manufactured by a wet papermaking method is subjected to a hot pressing process, a hot pressing process is performed using a hot pressing process device having a combination of a metal roller and an elastic roller. With respect to the elastic roller, it is preferred that the A-type durometer hardness is 60 or more, the D-type durometer hardness is 95 or less, the clamping pressure is 30 kN / m or more and 250 kN / m or less, and the processing speed is 20 m / min or more and 100 m / min or less, so that a semipermeable membrane support body having better adhesion to the semipermeable membrane support body can be manufactured.

[0044] In the present invention, although the contribution ratios of various factors other than fiber blending are uncertain, the difference in measured thickness can be adjusted to a range of 1.0% to 5.0% by appropriately adjusting the wet paper making conditions, wet paper drying conditions, and hot press processing conditions in the wet papermaking method.

[0045] In the wet papermaking method, the fibers are first dispersed uniformly in water, and then, after screening (removing foreign matter, lumps, etc.), the final fiber concentration is adjusted to 0.01-0.50 mass% slurry by a papermaking machine to obtain wet paper. In order to make the fiber dispersion uniform, chemicals such as dispersants, defoamers, hydrophilic agents, antistatic agents, polymer adhesives, release agents, antibacterial agents, and fungicides are sometimes added during the process.

[0046] As the papermaking machine, for example, a papermaking machine that is individually provided with a papermaking net such as a long wire, a round wire, an inclined wire, etc.; a combined papermaking machine that is online provided with two or more papermaking nets of the same or different kinds, etc. can be used. In the case where the semipermeable membrane support of the present invention is a multi-layer nonwoven fabric, as its manufacturing method, there can be cited a "papermaking method" in which wet papers picked up by each papermaking machine are stacked; a "casting method" in which a slurry with dispersed fibers is cast on a previously formed layer to form other layers and stack them, etc. In the casting method, the previously formed layer can be in a wet paper state or in a dry state. In addition, two or more layers in a dry state can be thermally fused to form a multi-layer nonwoven fabric.

[0047] In addition, when wet paper is obtained by using a papermaking machine, the difference in measured thickness can be adjusted by adjusting the papermaking speed, fiber concentration, etc., even with the same fiber mix. For example, if the papermaking speed is increased, there is a tendency for the difference in measured thickness to become relatively smaller. If the fiber concentration of the slurry is reduced, there is a tendency for the difference in measured thickness to become relatively larger. By using these combinations and other methods in combination, the difference in measured thickness can be adjusted to more than 1.0% and less than 5.0%. Other methods are not particularly limited, and examples thereof include the adjustment of the slurry input speed, the vibration direction of the papermaking net, the vibration speed, and the amplitude.

[0048] The wet paper produced by the papermaking machine is dried by a Yankee dryer, an air dryer, a drum dryer, a suction drum dryer, an infrared dryer, etc., to obtain a sheet. When the wet paper is dried, it is brought into close contact with a hot roll of a Yankee dryer or the like to perform hot press drying, thereby improving the smoothness of the surface after the close contact. Hot press drying means that the wet paper is pressed against a hot roll by a touch roll or the like to dry it.

[0049] The surface temperature of the hot roller in the hot press drying is preferably 100 to 180°C, more preferably 100 to 160°C, and even more preferably 110 to 160°C. When the surface temperature of the hot roller is lower than 100°C, the moisture of the wet paper produced by the papermaking machine may not be fully evaporated, the thickness uniformity of the sheet may be deteriorated, and the difference in measured thickness may be greater than 5.0%. When the surface temperature of the hot roller exceeds 180°C, the wet paper produced by the papermaking machine may stick to the hot roller, the texture of the sheet may be deteriorated, and the difference in measured thickness may be less than 1.0%. The pressure is preferably 5 to 100 kN / m, more preferably 10 to 80 kN / m. When the pressure is lower than 5 kN / m, the moisture of the wet paper produced by the papermaking machine may not be fully removed, the thickness uniformity of the sheet may be deteriorated, and the difference in measured thickness may be greater than 5.0%. When the pressure exceeds 100 kN / m, the wet paper produced by the papermaking machine may stick to the hot roller, the texture of the sheet may be deteriorated, and the difference in measured thickness may be less than 1.0%.

[0050] In the method for manufacturing a semipermeable membrane support of the present invention, a sheet manufactured by a wet papermaking method is passed through the rollers of a hot pressing treatment device while being sandwiched therebetween, and hot pressing treatment is performed. As a combination of rollers, two metal rollers, a metal roller and a resin roller, a metal roller and a cotton roller, etc. can be cited. In addition, one or both rollers are heated. In addition, as required, the surface and back of the sheet can also be reversed, and the number of times passed through the clamping portion is set to more than 2 times. Hereinafter, "resin rollers" and "cotton rollers" are sometimes collectively referred to as "elastic rollers". Among them, a combination of a metal roller and an elastic roller is preferred.

[0051] Figure 1 and Figure 2It is a schematic diagram showing the combination and arrangement of rollers used in the hot pressing process of the present invention, and the state of sheet passing. Figure 1 and Figure 2 This is an example, but it is not limited to this. Figure 1 and Figure 2 In the figure, symbol 1 is a metal roller, and symbol 2 is an elastic roller. Both the metal roller and the elastic roller can be used as the hot roller, and preferably the metal roller and the elastic roller are used as the hot roller. More preferably, the metal roller is used as the hot roller. Figure 1 The invention is a hot press processing device in which a first roller nip consisting of a metal roller 1 and an elastic roller 2 and a second roller nip consisting of a metal roller 1 and an elastic roller 2 are continuously provided. Figure 2 The present invention is a hot press processing device in which a first roller nip portion consisting of two metal rollers 1 and a second roller nip portion consisting of one metal roller 1 and one elastic roller 2 are continuously provided.

[0052] The surface temperature of the roller used in the hot pressing process is preferably -60°C to +10°C, more preferably -40°C to ±0°C, relative to the melting point or softening point of the fiber measured by differential thermal analysis (DSC). If the surface temperature of the roller temperature is lower than the melting point or softening temperature of the fiber contained in the sheet by more than 60°C, fuzzing may occur easily, and it is difficult to obtain a semipermeable membrane of uniform thickness. On the other hand, if the surface temperature of the roller is higher than the melting point or softening temperature of the fiber contained in the sheet by more than 10°C, the molten component of the fiber may adhere to the metal roller, the semipermeable membrane support may become uneven, and it may be difficult to obtain a semipermeable membrane of uniform thickness, and the molten component in the semipermeable membrane support may become excessive, thereby reducing the cushioning property, and the difference in the measured thickness may be less than 1.0%.

[0053] The clamping pressure of the hot pressing process is preferably 30 to 250 kN / m, more preferably 40 to 200 kN / m. When the clamping pressure is lower than 30 kN / m, sufficient pressure is not applied, the surface smoothness of the semipermeable membrane support body is reduced, and uneven coating and defects are easily generated when the semipermeable membrane is set. On the other hand, if the clamping pressure exceeds 250 kN / m, the pressure is too high, and wrinkles are sometimes generated on the sheet. In addition, the surface smoothness of the semipermeable membrane support body becomes too high, and when the semipermeable membrane is set, the adhesion of the semipermeable membrane is sometimes reduced.

[0054] The processing speed of the hot press treatment is preferably 20 to 100 m / min, more preferably 30 to 60 m / min. When the processing speed is lower than 20 m / min, although the reason is not clear, it sometimes causes an increase in thickness and air permeability, and the difference in measured thickness is greater than 5.0%. It is presumed that this is probably because the residual heat time before clamping increases, causing the binder synthetic fiber to be inactivated. On the other hand, if the processing speed exceeds 100 m / min, the sheet is easily attached to the hot roller side near the exit of the clamping part, and stable operation becomes difficult.

[0055] The radius of the two rollers constituting the roller clamping portion may be the same or different. The roller radius is preferably 50 to 2000 mm, more preferably 100 to 1500 mm. When the roller radius is less than 50 mm, it is difficult to obtain the desired thickness. On the other hand, when the roller radius exceeds 2000 mm, it becomes difficult to control the surface temperature.

[0056] In the combination of the metal roller and the elastic roller, the materials of the elastic roller and the metal roller are not particularly limited, and the hardness has a preferred range. The A-type durometer hardness of the elastic roller is preferably 60 or more, and more preferably 70 or more. In addition, the D-type durometer hardness of the elastic roller is preferably 95 or less, and more preferably the A-type durometer hardness is 80 or less. The metal roller is not particularly limited, but is preferably a roller having a tungsten carbide spray coating and having a Shore hardness of HS60 or more and HS95 or less as measured by the method specified in JIS Z2246:2000.

[0057] When the A-type durometer hardness of the elastic roller is less than 60, the surface of the elastic roller is sometimes deformed and it is difficult to obtain the desired thickness, and the difference in the measured thickness is greater than 5.0%. If the D-type durometer hardness of the elastic roller exceeds 95, cracks are sometimes easily generated on the surface of the elastic roller when clamped with the metal roller, and the roller needs to be replaced frequently, which makes it difficult to operate stably. On the other hand, the surface of the metal roller with a Shore hardness exceeding HS95 is too hard, so wrinkles are sometimes generated on the sheet. If it is a metal roller with a Shore hardness lower than HS60, it is easy to deform and wrinkle when clamped, and the uniformity of the semipermeable membrane support body is easy to deteriorate.

[0058] The durometer hardness is measured by a durometer hardness test according to the method specified in JIS K6253-3: 2012. The hardness is measured by a type A durometer to a type D durometer, and the surface hardness of the elastic roller after the elastic roller is assembled is measured. The apparent hardness within 1 / second after the pressing surface of the durometer is in close contact with the surface of the elastic roller is read, and the median value of the 5-point measurement is defined as the "durometer hardness of the elastic roller".

[0059] When the semipermeable membrane support of the present invention is a multilayer nonwoven fabric and a multilayer nonwoven fabric is manufactured by a wet papermaking method, the fiber concentration of the slurry can be reduced by reducing the weight per unit area of ​​each layer, so the texture of the sheet becomes good, and as a result, the smoothness and uniformity of the coating surface are improved. In addition, even if the texture of each layer is uneven, it can be filled by stacking. In addition, the papermaking speed can be increased, and the operability is improved.

[0060] The weight per unit area of ​​the semipermeable membrane supporting material is preferably 20 to 150 g / m 2 , more preferably 30 to 110 g / m2 , more preferably 40 to 90 g / m 2 . Below 20g / m 2 In the case of more than 150 g / m, sufficient tensile strength cannot be obtained, and the semipermeable membrane solution may penetrate, and sometimes the adhesion of the semipermeable membrane becomes weak. 2 In this case, the drying load in the manufacturing process becomes large and the manufacturing stability is likely to decrease.

[0061] The semipermeable membrane support of the present invention can be a multilayer nonwoven fabric formed by laminating two or more nonwoven fabrics using the same method as the thermal processing treatment. The unit weight of each nonwoven fabric can be the same or different. In this case, the drying load in the manufacturing process can be suppressed, and the unit weight of 20 to 300 g / m 2 Semipermeable membrane support. 2 In this case, the load in the bonding process becomes large and the manufacturing stability is likely to decrease.

[0062] The thickness of the semipermeable membrane support is preferably 40 to 300 μm, more preferably 60 to 200 μm, and further preferably 80 to 150 μm. If the thickness of the semipermeable membrane support exceeds 300 μm, the area of ​​the filter membrane assembled in the unit sometimes becomes smaller, the number of filter membranes assembled in the unit will decrease, and as a result, the life of the semipermeable membrane sometimes becomes shorter. On the other hand, when it is less than 40 μm, sufficient tensile strength cannot be obtained sometimes, the permeability becomes low, and the life of the filter membrane becomes shorter.

[0063] Example

[0064] The present invention is further described in detail by way of examples.

[0065] (Example 1)

[0066] <Sheet production>

[0067] 70% by weight of stretched polyester fibers with a fiber diameter of 7.7 μm and a fiber length of 5 mm as main fibers and 30% by weight of unstretched polyester binder fibers with a fiber diameter of 10.9 μm, a fiber length of 5 mm and a melting point of 260° C. as binder fibers were dissociated and dispersed in water in a pulper and stirred to prepare a uniform papermaking slurry. The papermaking slurry was formed using a combination of an inclined screen and a cylinder screen at a papermaking speed of 60 m / min to obtain a papermaking slurry with a dry weight of 37.5 g / m2 for each layer. 2 After the wet paper was combined, the coated surface was brought into contact with a Yankee dryer at a surface temperature of 130°C and hot-pressed with a contact roll pressure of 100 kN / m to obtain a combined paper with a unit area weight of 75 g / m 2 of sheet.

[0068] <Hot Press Processing>

[0069] use Figure 1 The obtained sheet was subjected to hot pressing to obtain a semipermeable membrane supporting body. The conditions for the hot pressing treatment are shown in Table 1.

[0070] (Example 2)

[0071] <Sheet production>

[0072] Based on the preparation of the sheet in Example 1, the fiber composition was changed to 80% by mass of the main fiber and 20% by mass of the binder fiber, and the dry weight of each layer was changed to 40 g / m 2 The papermaking speed was changed to 45 m / min, and the pressure of the touch roll was changed to 5 kN / m. The same operation was performed except that the papermaking speed was changed to 45 m / min and the pressure of the touch roll was changed to 5 kN / m. The papermaking weight per unit area was 80 g / m 2 of sheet.

[0073] <Hot Press Processing>

[0074] The obtained sheet was subjected to hot pressing in the same manner as in <Hot Pressing> of Example 1, except that the conditions for the hot pressing were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0075] (Example 3)

[0076] <Sheet production>

[0077] On the basis of the <Preparation of Sheet Material> of Example 2, the fiber blending was carried out in the same manner as above, with the main fiber being a stretched polyester fiber with a fiber diameter of 7.9 μm and a fiber length of 5 mm being changed to 20% by mass, the stretched polyester fiber with a fiber diameter of 12.1 μm and a fiber length of 5 mm being changed to 30% by mass, the stretched polyester fiber with a fiber diameter of 17.5 μm and a fiber length of 5 mm being changed to 20% by mass, and the binder fiber being an unstretched polyester binder fiber with a fiber diameter of 10.5 μm, a fiber length of 5 mm and a melting point of 260°C being changed to 30% by mass, the papermaking speed being changed to 50 m / min, and the pressure of the contact roll being changed to 80 kN / m. Except for the above, the papermaking speed was changed to 50 m / min, and the pressure of the contact roll was changed to 80 kN / m. The papermaking weight per unit area of ​​80 g / m was obtained. 2 of sheet.

[0078] <Hot Press Processing>

[0079] use Figure 2The hot pressing treatment device continuously provided with a first roller clamping portion consisting of two metal rollers (radius 450mm) and a second roller clamping portion consisting of a metal roller (radius 450mm) and an elastic roller as shown, the obtained sheet is subjected to hot pressing to obtain a semipermeable membrane supporting body. The conditions of the hot pressing treatment are shown in Table 1.

[0080] (Example 4)

[0081] <Sheet production>

[0082] Based on the "Preparation of Sheet Material" in Example 2, the fiber mix was changed to 75% by mass of main fiber and 25% by mass of binder fiber, the pressure of the contact roll was changed to 10 kN / m, and the dry weight of each layer was changed to 37.5 g / m 2 , change the unit area weight of the copy to 75g / m 2 , except for this, the same operation was performed to obtain a sheet.

[0083] <Hot Press Processing>

[0084] The obtained sheet was subjected to heat pressing in the same manner as in <Hot Pressing> of Example 2 to obtain a semipermeable membrane supporting material.

[0085] (Example 5)

[0086] <Sheet production>

[0087] The same operation was performed as in Example 4, except that the papermaking speed was changed to 50 m / min and the pressure of the touch roll was changed to 30 kN / m, to obtain a sheet with a weight per unit area of ​​75 g / m 2 of sheet.

[0088] <Sheet production>

[0089] The obtained sheet was subjected to hot pressing in the same manner as in <Hot Pressing> of Example 4, except that the conditions for the hot pressing were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0090] (Examples 6 to 8)

[0091] The sheet obtained in <Preparation of Sheet> in Example 1 was subjected to hot pressing in the same manner as in <Hot Pressing> in Example 1, except that the hot pressing conditions were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0092] (Comparative Example 1)

[0093] On the basis of <Preparation of Sheet Material> in Example 3, as for the fiber blending, as the main fiber, the stretched polyester fiber with a fiber diameter of 7.9 μm and a fiber length of 5 mm was changed to 20% by mass, the stretched polyester fiber with a fiber diameter of 12.1 μm and a fiber length of 5 mm was changed to 30% by mass, the stretched polyester fiber with a fiber diameter of 17.5 μm and a fiber length of 5 mm was changed to 10% by mass, and as the bonding fiber, the unstretched polyester bonding fiber with a fiber diameter of 10.5 μm, a fiber length of 5 mm and a melting point of 260°C was changed to 40% by mass, the pressure of the contact roller was changed to 110 kN / m, and the dry mass of each layer was changed to 45 g / m 2 In addition, the weight per unit area of ​​the composite was 90 g / m 2 of sheet.

[0094] <Hot Press Processing>

[0095] The obtained sheet was subjected to hot pressing in the same manner as in <Hot Pressing> of Example 3, except that the conditions for the hot pressing were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0096] (Comparative Example 2)

[0097] <Sheet production>

[0098] The same method as in Example 2 was used for the preparation of the sheet, except that the pressure of the touch roll was changed to 4 kN / m and the dry weight of each layer was changed to 30 g / m 2 In addition, the same operation was performed to obtain a combined weight per unit area of ​​60 g / m 2 of sheet.

[0099] <Hot Press Processing>

[0100] The obtained sheet was subjected to hot pressing in the same manner as in <Hot Pressing> of Example 2, except that the conditions for the hot pressing were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0101] (Comparative Example 3)

[0102] <Sheet production>

[0103] On the basis of the "Preparation of Sheet Material" in Example 1, 35% by mass of stretched polyester fibers with a fiber diameter of 17.5 μm and a fiber length of 5 mm were used as the main fiber, and 65% by mass of unstretched polyester binder fibers with a fiber diameter of 10.5 μm, a fiber length of 5 mm and a melting point of 256°C were used as the binder fiber. The dry weight of each layer was changed to 50.0 g / m at a papermaking speed of 30 m / min. 2In addition, the same operation was performed to obtain a combined weight per unit area of ​​100 g / m 2 of sheet.

[0104] <Hot Press Processing>

[0105] The obtained sheet was subjected to hot pressing in the same manner as in <Hot Pressing> of Example 1, except that the conditions for the hot pressing were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0106] (Comparative Example 4)

[0107] <Sheet production>

[0108] The same operation was performed as in Comparative Example 3, except that the main fiber was changed to 50% by mass and the binder fiber was changed to 50% by mass, to obtain a sheet having a weight per unit area of ​​100 g / m 2 of sheet.

[0109] <Hot Press Processing>

[0110] The obtained sheet was subjected to hot pressing in the same manner as in <Hot Pressing> of Example 1, except that the conditions for the hot pressing were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0111] (Comparative Example 5)

[0112] <Sheet production>

[0113] The same operation was performed as in Comparative Example 3, except that the main fiber was changed to 65% by mass and the binder fiber was changed to 35% by mass, to obtain a sheet having a weight per unit area of ​​100 g / m 2 of sheet.

[0114] <Hot Press Processing>

[0115] The obtained sheet was subjected to hot pressing in the same manner as in <Hot Pressing> of Example 1, except that the conditions for the hot pressing were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0116] (Comparative Examples 6 to 7)

[0117] The sheet obtained in <Preparation of Sheet> in Example 1 was subjected to hot pressing in the same manner as in <Hot Pressing> in Example 1, except that the hot pressing conditions were changed to those described in Table 1, to obtain a semipermeable membrane supporting material.

[0118] The above-mentioned comparative examples 3 to 5 are prepared with reference to the examples 4 to 6 disclosed in the prior art document 4 (Japanese Patent Application Laid-Open No. 2004-100047).

[0119] The semipermeable membrane supporting materials obtained in Examples and Comparative Examples were subjected to the following measurements and evaluations. The results are shown in Table 1.

[0120] Measurement 1 (Measurement of thickness (1.27))

[0121] A precision thickness gauge (manufactured by Swiss Instruments, trade name: Tesa Micro-Hite 100) was used to measure the thickness at a pressure of 1.27 N / cm 2 The test piece adjustment, the test piece measurement position, and the number of measurements were in accordance with JIS P8118:2014, and the average of the measured values ​​was set to three significant figures by the method specified in JIS Z8401:1999, and the obtained value was defined as the measured thickness (1.27).

[0122] Measurement 2 (Measurement of thickness (0.80))

[0123] Based on measurement 1, change the measurement pressure to 0.80 N / cm 2 The measurement was performed in the same manner except for the above setting, and the obtained value was defined as the measured thickness (0.80).

[0124] Measurement 3 (Weight per unit area)

[0125] The weight per unit area was measured in accordance with JIS P8124:2011.

[0126] Measurement 4 (ventilation)

[0127] The air permeability tester (manufactured by Kato Tech Co., Ltd., trade name: KES-F8-AP1) was used to measure the air permeability according to the method described in JIS L1096:2010.

[0128] Evaluation 1 (Adhesion)

[0129] A comma coater with a certain gap was used to coat a DMF solution (concentration: 21% by mass) of a polysulfone resin (manufactured by SOLVAY, trade name: Udel (registered trademark) P-3500LCD MB3, molecular weight 78,000 to 84,000 g / mol (catalog value)) on the coating surface of the semipermeable membrane support, followed by washing with water and drying to form a polysulfone membrane on the surface of the semipermeable membrane support.

[0130] An aqueous solution containing 2.0 mass % of m-phenylenediamine and 0.15 mass % of sodium lauryl sulfate was applied to the obtained polysulfone membrane, and the polysulfone membrane was brought into contact with the aqueous solution for several seconds, and then excess aqueous solution was removed to form a coating layer of the aqueous solution on the polysulfone membrane.

[0131] A hexane solution containing 0.10% by mass of trimesoyl chloride and 2% by mass of acetone was applied to the obtained coating layer, and the coating layer was allowed to contact with the hexane solution for several seconds, then the hexane solution was removed and then kept in air for 10 minutes to form a polyamide layer on the polysulfone membrane, thereby obtaining a semipermeable membrane.

[0132] A raw water spacer of 0.71 mm was provided on the obtained semipermeable membrane, and the pressure dependency of the permeation flux was evaluated.

[0133] ◎ (Very Good): The permeation flux increases at a certain rate as the pressure increases, and no reduction due to the pressure increase is observed, which is a good level. The adhesion to the raw water spacer is good.

[0134] ○ (Good): The permeate flux showed a certain increase rate from low pressure to medium pressure, but the increase rate of the permeate flux decreased at high pressure, and a reduction due to the increase in pressure was observed, but it was a good level for practical use. The adhesion with the raw water spacer decreased at high pressure.

[0135] △ (Satisfactory): From low pressure to high pressure, the rate of increase of permeation flux decreases, and the loss caused by the pressure increase is clearly observed. It is a practical level. The tightness with the raw water spacer is low.

[0136] × (Unsatisfactory): The rate of increase of permeation flux decreases significantly from low pressure to high pressure, and the loss caused by the pressure increase is very obvious, which is the practical limit. The adhesion with the raw water spacer is poor.

[0137] Evaluation 2 (Polysulfone membrane adhesion)

[0138] One day after the polysulfone membrane produced in Evaluation 1, the polysulfone membrane and the semipermeable membrane support were slowly peeled off at the interface, and the degree of resistance during the peeling was evaluated.

[0139] ◎ (Excellent): The adhesion between the polysulfone membrane and the semipermeable membrane support is very high and cannot be peeled off. This is a very good level.

[0140] ○ (Very Good): The adhesion between the polysulfone membrane and the semipermeable membrane support is high, and a strong force is required for peeling. This is a good level.

[0141] ○△ (Good): There are some areas that are easily peeled off. This is a level that does not cause any practical problems.

[0142] △ (Satisfactory): The polysulfone membrane is adhered to the semipermeable membrane support, but is easily peeled off as a whole. This is the lower limit level for practical use.

[0143] × (Unsatisfactory): The polysulfone membrane peeled off or the semipermeable membrane support was damaged during the washing or drying process after the polysulfone membrane was coated. This level was unusable.

[0144] [Table 1]

[0145]

[0146] The semipermeable membrane supporting materials of Examples 1 to 8 were characterized in that the difference in measured thickness was 1.0% or more and 5.0% or less, and the adhesion between the raw water spacer and the semipermeable membrane was good.

[0147] In contrast, the difference in measured thickness of the semipermeable membrane supports of Comparative Examples 1 and 6 and 7 is less than 1.0%, and the difference in measured thickness of the semipermeable membrane supports of Comparative Examples 2 to 5 is greater than 5.0%. The adhesion between the raw water spacer and the semipermeable membrane of both is poor, which is at a practically limiting level.

[0148] Regarding the semipermeable membrane supports of Examples 3 to 8 in which the difference in measured thickness was greater than 1.4% and less than 3.0%, the adhesion between the raw water spacer and the semipermeable membrane was better than that of the semipermeable membrane support of Example 1 in which the difference in measured thickness was less than 1.4% and that of Example 2 in which the difference in measured thickness was greater than 3.0%.

[0149] Regarding the semipermeable membrane supports of Examples 6 to 8 manufactured by a method for manufacturing a semipermeable membrane support by performing hot pressing processing using a hot pressing processing device having a combination of a metal roller and an elastic roller, wherein the A-type durometer hardness of the elastic roller is greater than 60 and less than 80, the clamping pressure is greater than 30 kN / m and less than 250 kN / m, and the processing speed is greater than 20 m / min and less than 100 m / min, the polysulfone membrane adhesion is better than the semipermeable membrane supports of Examples 1 to 5.

[0150] Industrial Applicability

[0151] The semipermeable membrane supporting body of the present invention can be used in the fields of seawater desalination, water purifiers, food concentration, wastewater treatment, blood filtration, medical use, ultrapure water production for semiconductor cleaning, and the like.

[0152] Description of Reference Numerals

[0153] 1: Metal roller

[0154] 2: Elastic roller

Claims

1. A semipermeable membrane support, characterized in that A semipermeable membrane support is provided for use with a semipermeable membrane, the semipermeable membrane support being obtained by subjecting a sheet produced by a wet papermaking method to a hot press process, comprising a main fiber and a binder fiber, the main fiber being a synthetic fiber, the binder fiber being an unstretched fiber, The synthetic fiber is a polyester fiber, and the undrawn fiber is a polyester fiber. The synthetic fiber has a fiber diameter of 1 μm or more and 30 μm or less, and a fiber length of 1 mm or more and 20 mm or less. The weight per unit area of ​​each sheet of the semipermeable membrane support is 20 to 150 g / m 2 , The thickness of the semipermeable membrane support is 40 to 300 μm. The air permeability of the semipermeable membrane support is 0.5 to 25.0 cc / cm 2 ·Second, The semipermeable membrane support is at 0.80N / cm 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness under the conditions of 0.80N / cm 2 The measured thickness under the conditions of is 1.0% or more and 5.0% or less.

2. The semipermeable membrane support according to claim 1, characterized in that The semipermeable membrane support is at 0.80N / cm 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness under the conditions of 0.80N / cm 2 The measured thickness under the conditions of is 1.4% or more and 3.0% or less.

3. A method for producing a semipermeable membrane support according to claim 1, characterized in that: A method for producing a semipermeable membrane supporting body comprising subjecting a sheet produced by a wet papermaking method to a heat-pressing treatment. The hot pressing treatment is performed using a hot pressing treatment device having a combination of a metal roller and an elastic roller. At this time, an elastic roller having a hardness of 60 or more on a type A durometer and a hardness of 95 or less on a type D durometer is used as the elastic roller. The clamping pressure between the metal roller and the elastic roller is set to 30 kN / m or more and 250 kN / m or less, and the processing speed is set to 30 m / min or more and 60 m / min or less. The hot pressing treatment is performed at 0.80 N / cm 2 The measured thickness under the conditions of 1.27N / cm 2 The difference in thickness under the conditions of 0.80N / cm 2 A semipermeable membrane supporting material having a measured thickness under the conditions of 1.0% to 5.0%. 4 . The method for producing a semipermeable membrane supporting material according to claim 3 , wherein an elastic roller having a type A durometer hardness of 60 or more and 80 or less is used as the elastic roller.