Membrane electrode assembly, solid oxide fuel cell and electrochemical device
Patent Information
- Application Number
- CN202080008128.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-08-28
- Filing Date
- 2020-03-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-03-09
AI Technical Summary
特别是,在大量包含Co的镧锶钴氧化物的情况下,耐水蒸气稳定性的降低显著
[0020] The present disclosure is configured as described above, and exhibits the effects of high reaction efficiency and water vapor resistance stability at an operating temperature of 600° C. or lower.
Smart Images

Figure CN113272477B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a membrane electrode assembly, a solid oxide fuel cell, and an electrochemical device. Background Art
[0002] As electrochemical devices having an electrolyte membrane using a solid electrolyte containing a solid oxide and a membrane electrode assembly including electrodes, for example, solid oxide fuel cells, water electrolysis cells, and steam electrolysis cells are known. Among the solid electrolytes of electrochemical devices, oxide ions (O2) represented by stabilized zirconium oxide are widely used. 2- ) conductor. The lower the temperature of the oxide ion conductor, the lower the ion conductivity. Therefore, for example, the operating temperature of a solid oxide fuel cell using stabilized zirconium oxide as a solid electrolyte is preferably 700°C or higher. The operating temperature is particularly preferably a temperature in the range of 700°C or higher and 1000°C or lower.
[0003] In solid oxide fuel cells using stabilized zirconium oxide as a solid electrolyte, lanthanum strontium cobalt iron composite oxide is used as the most common air electrode material. 1-m Sr m Co n Fe 1-n O 3-δ The composition formula is represented by (0<m<1, 0<n<1, δ represents the oxygen deficiency, 0≤δ≤0.5), m=0.4, n=0.2 La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ The reason is that when the temperature is above 700℃, the electrode reaction in the air electrode (O2+4e - →2O 2- ) has a small reaction resistance, which improves the power generation efficiency; the material is relatively stable even at high temperatures; the difference in thermal expansion coefficient with the solid electrolyte is small, which can suppress the peeling of the electrode during the start-stop and temperature rise and fall.
[0004] However, when the operating temperature of the electrochemical device becomes a high temperature of 700°C or higher, there is a problem of increased manufacturing cost. That is, when the operating temperature becomes a high temperature of 700°C or higher, it is necessary to cover the periphery of the electrochemical device with a high-performance insulating material having a large thickness. As a result, the manufacturing cost becomes high. Furthermore, the components of the system including the electrochemical device require expensive special heat-resistant metals, so the manufacturing cost of the entire system also increases.
[0005] In addition, there is a problem that cracks are easily generated due to the difference in thermal expansion of the components when the system is started and stopped, and the reliability of the system is reduced. In addition, there is also a problem that the startup time becomes longer or the energy required at the time of startup increases.
[0006] Therefore, lowering the operating temperature of electrochemical devices such as solid oxide fuel cells using solid electrolytes containing solid oxides has become one of the major goals in their practical application. Therefore, solid oxide fuel cells that can lower the operating temperature to 600°C or less, especially 350°C or more and 600°C or less, and use proton conductors as solid electrolytes have attracted attention.
[0007] However, in solid oxide fuel cells that use proton conductors as solid electrolytes, the reaction (O2+4H + +4e - →2H2O) to generate water vapor. Therefore, it is necessary to consider the influence of water vapor in the air electrode.
[0008] For example, in Non-Patent Document 1, the stability to water vapor in the air is mentioned for lanthanum strontium cobalt iron composite oxide or lanthanum strontium cobalt composite oxide used as an air electrode material. That is, it is shown that the decomposition of lanthanum strontium cobalt iron composite oxide and lanthanum strontium cobalt oxide occurs due to the presence of water vapor in the air. In particular, in the case of lanthanum strontium cobalt oxide containing a large amount of Co, the water vapor resistance stability is significantly reduced.
[0009] Prior art literature
[0010] Non-patent literature
[0011] Non-patent document 1: I.Kivi et.al., "Influence of humidified synthetic airfeeding conditions on the stoichiometry of (La1-xSrx)yCoO3-δandLa0.6Sr0.4Co0.2Fe0.8O3-δcathodes under applied potential measured by electrochemical in situ high-temperature XRD method" J Solid StateElectrochem,2017,21,361-369 Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, conventionally, in a membrane electrode assembly including an electrolyte membrane using a solid electrolyte having proton conductivity and electrodes, sufficient studies have not been conducted on reaction efficiency and water vapor resistance stability at an operating temperature of 600° C. or lower.
[0014] Therefore, the present disclosure provides a membrane electrode assembly, a solid oxide fuel cell, and an electrochemical device having high reaction efficiency and water vapor resistance stability at an operating temperature of 600° C. or less.
[0015] Methods for solving problems
[0016] One form of the membrane electrode assembly disclosed in the present invention comprises: an electrolyte membrane comprising an oxide having proton conductivity; and an electrode disposed on the above-mentioned electrolyte membrane and comprising a lanthanum strontium cobalt iron composite oxide, wherein the ratio of the number of moles of cobalt in the above-mentioned electrode to the sum of the number of moles of cobalt and the number of moles of iron is a value in the range of greater than 0.35 and less than 0.6.
[0017] One mode of the solid oxide fuel cell disclosed herein has a membrane electrode assembly, which comprises: an electrolyte membrane comprising an oxide having proton conductivity; and an electrode disposed on the above-mentioned electrolyte membrane and comprising a lanthanum strontium cobalt iron composite oxide, wherein the ratio of the number of moles of cobalt in the above-mentioned electrode to the sum of the number of moles of cobalt and the number of moles of iron is a value in the range of greater than 0.35 and less than 0.6.
[0018] One mode of the electrochemical device disclosed in the present invention has a membrane electrode assembly, which comprises: an electrolyte membrane comprising an oxide having proton conductivity; and an electrode disposed on the above-mentioned electrolyte membrane and comprising a lanthanum strontium cobalt iron composite oxide, wherein the ratio of the number of moles of cobalt in the above-mentioned electrode to the sum of the number of moles of cobalt and the number of moles of iron is a value in the range of greater than 0.35 and less than 0.6.
[0019] Effects of the Invention
[0020] The present disclosure is configured as described above, and exhibits the effects of having high reaction efficiency and water vapor resistance stability at an operating temperature of 600° C. or lower. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a cross-sectional view schematically showing the structure of a membrane electrode assembly included in the electrochemical device according to the first embodiment of the present disclosure.
[0022] Figure 2 It is a cross-sectional view schematically showing the structure of a membrane electrode assembly included in an electrochemical device according to a second embodiment of the present disclosure.
[0023] Figure 3This is a diagram showing the measurement results obtained by the X-ray diffraction method regarding the LSCF according to Examples 2 and 3 of the present disclosure and the LSCF according to Comparative Examples 1 to 4.
[0024] Figure 4 This is a diagram showing an example of the results of AC impedance measurement in Examples of the present disclosure using a Cole-Cole plot.
[0025] Figure 5 This is a graph showing the relationship between the molar ratio of Co to the sum of the molar numbers of Co and Fe and the reaction resistance of the air electrodes according to Examples 1 to 3 and Comparative Examples 1 to 4 of the present disclosure. DETAILED DESCRIPTION
[0026] (A process of obtaining a method of the present disclosure)
[0027] When a membrane electrode assembly using stabilized zirconia as an electrolyte membrane is used at an operating temperature of 600°C, the ohmic resistance of the electrolyte membrane increases. Therefore, for example, the power generation efficiency of a solid oxide fuel cell having the membrane electrode assembly decreases. This is because the activation energy of oxide ion conduction in stabilized zirconia is large, and the oxide ion conductivity significantly decreases in a temperature range below 600°C.
[0028] In addition, in a solid oxide fuel cell having a membrane electrode assembly using stabilized zirconia as an electrolyte membrane, La, which is generally used as an air electrode, has been 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ (δ is the amount of oxygen deficiency. 0≤δ≤0.5) When the operation is performed at 600°C, the reaction resistance becomes larger than that of the operation at 700°C, thereby causing a decrease in power generation efficiency.
[0029] In order to obtain good power generation efficiency, for example, in a solid oxide fuel cell, the voltage in an open circuit state without applying current is 1.0 V and the current density is 0.2 A / cm 2 The above makes the voltage actually obtained during operation to be above 0.7V and the ohmic resistance of the electrolyte to be 0.1Ωcm 2 When the reaction resistance generated at the air electrode needs to be less than 1.4Ωcm 2 .
[0030] Therefore, as a material for an electrolyte membrane that can reduce ohmic resistance at an operating temperature of 600°C or less, the use of a proton conductor has been proposed. Among the proton conductors, barium zirconate oxides, barium cerate oxides, and barium zirconate cerate oxides are known to exhibit high proton conductivity. For example, BaZr 0.8 Y 0.2 O3 or BaZr 0.8 Yb 0.2 O3 has a 1.0×10 -2 High proton conductivity of more than S / cm.
[0031] In addition, for membrane electrode assemblies using proton conductors for electrolyte membranes, the water vapor resistance stability of the electrodes becomes important. For example, in the case of a solid oxide fuel cell composed of a membrane electrode assembly using proton conductors for electrolyte membranes, during power generation, (O2+4H + +4e - →2H2O) to generate water vapor. For example, when the air utilization rate is 30% during power generation of the solid oxide fuel cell, the water vapor concentration of the outlet air of the solid oxide fuel cell becomes about 12%. In addition, there is a possibility that the water vapor concentration may become even higher in the local electrode reaction. For example, oxygen (volume fraction 21%) in the air is converted into water vapor by O2+4H + 4e - → When all the water vapor is converted into water vapor by the reaction of 2H2O, the volume fraction of water vapor in the outlet air may become about 35%. Thus, in a membrane electrode assembly using a proton conductor as an electrolyte membrane, the electrode is exposed to air with a high water vapor concentration. Therefore, in the case of an electrode material with low water vapor resistance stability, there is a concern about electrode decomposition.
[0032] Here, non-patent document 1 discloses (La 0.6 Sr 0.4 ) x CoO 3-δ (0.99≤x≤1.01, 0≤δ≤0.5), and La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ(0≤δ≤0.5) The effect of the composition used for the air electrode material on the humidified air. That is, in Non-Patent Document 1, the effect of water vapor on the air electrode material is reported assuming the water vapor concentration in the normal air. However, in Non-Patent Document 1, there is no suggestion about the effect on the electrode material under the operating conditions of the membrane electrode assembly using the proton conductor for the electrolyte membrane (for example, at 600°C and high water vapor concentration (for example, the volume fraction of water vapor in the air is 35%)).
[0033] Therefore, the inventors of the present invention have conducted in-depth research on a membrane electrode assembly that can simultaneously satisfy high reaction efficiency and water vapor resistance stability at an operating temperature below 600°C. In addition, the so-called water vapor resistance stability refers to the property that the composition does not change even under high humidification conditions. That is, under conditions below 600°C and high humidification, in the electrode (hereinafter sometimes described as "air electrode"), decomposition products may be generated by the reaction of the substance contained in the electrode with water. Furthermore, sometimes the composition of the electrode changes.
[0034] Specifically, a membrane electrode assembly having an electrolyte membrane using a proton conductor and an electrode capable of maintaining high water vapor stability while reducing reaction resistance was studied. Furthermore, the molar ratio of cobalt (Co) relative to the sum of the molar numbers of cobalt (Co) and iron (Fe) in a lanthanum strontium cobalt iron composite oxide capable of forming an electrode capable of maintaining high water vapor stability while reducing reaction resistance at an operating temperature of 600°C or less was determined.
[0035] The present inventors have discovered a membrane electrode assembly, a solid oxide fuel cell, and an electrochemical device that have novel structures that have not been clearly understood so far. In the present disclosure, the following aspects are specifically provided.
[0036] The first embodiment of the present invention involves a membrane electrode assembly comprising: an electrolyte membrane comprising an oxide having proton conductivity; and an electrode disposed on the above-mentioned electrolyte membrane and comprising a lanthanum strontium cobalt iron composite oxide, wherein the ratio of the number of moles of cobalt in the above-mentioned electrode to the sum of the number of moles of cobalt and the number of moles of iron is a value in the range of greater than 0.35 and less than 0.6.
[0037] According to the above-mentioned configuration, since the ratio of the molar number of cobalt in the electrode to the sum of the molar number of cobalt and the molar number of iron is within the range of 0.35 to 0.6, for example, at an operating temperature of a solid electrolyte fuel cell using a proton conductor as a solid electrolyte of 600°C or less, the reaction efficiency (i.e., power generation efficiency) can be improved due to a reduction in reaction resistance, and the system has high water vapor resistance stability.
[0038] A membrane electrode assembly according to a second aspect of the present disclosure is the membrane electrode assembly according to the first aspect, wherein the electrolyte membrane and the electrode are arranged so as to be in contact with each other.
[0039] According to the above configuration, since the electrolyte membrane and the electrode can be arranged in contact with each other, the reaction resistance can be reduced, and thus the reaction efficiency can be improved.
[0040] The membrane electrode assembly according to the third aspect of the present disclosure is a membrane electrode assembly in the first or second aspect, wherein the electrolyte membrane may be a membrane electrode assembly comprising a material selected from BaZr 1-x1 M1 x1 O 3-γ ,BaCe 1-x2 M2 x2 O 3-γ , and BaZr 1-x3-y3 Ce x3 M3 y3 O 3-γ At least one compound in, M1, M2 and M3 are each independently at least one element selected from La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Y, Sc, Mn, Fe, Co, Ni, Al, Ga, In, and Lu, x1 satisfies 0<x1<1, x2 satisfies 0<x2<1, x3 satisfies 0<x3<1, and y3 satisfies 0<y3<1. In addition, γ is the oxygen deficiency, 0<γ≤0.5.
[0041] According to the above configuration, since the electrolyte membrane exhibits high proton conductivity, the ohmic resistance of the membrane electrode assembly can be reduced even in a temperature range where the operating temperature is 600° C. or less. Therefore, when the membrane electrode assembly is used as a solid oxide fuel cell, the power generation efficiency can be improved even in a temperature range where the operating temperature is 600° C. or less.
[0042] The membrane electrode assembly according to the fourth aspect of the present disclosure is a membrane electrode assembly according to the third aspect, wherein the electrolyte membrane may be BaZr 1-x1 Yb x1 O 3-γ The compounds shown.
[0043] According to the above configuration, the electrolyte membrane can have high proton conductivity and high durability against carbon dioxide. Therefore, when the membrane electrode assembly is used as a solid oxide fuel cell, even in a temperature range where the operating temperature is 600°C or less, the power generation efficiency can be improved and the stability against carbon dioxide can be improved.
[0044] A membrane electrode assembly according to a fifth aspect of the present disclosure is any one of the first to fourth aspects, wherein the electrode may be an air electrode.
[0045] According to the above configuration, when the electrode reaction is carried out as the air electrode in the membrane electrode assembly, the reaction resistance can be reduced, and even if the air electrode is exposed to a high water vapor concentration during the electrode reaction, it can have high water vapor resistance stability. That is, at an operating temperature of 600°C or less, it can have high reaction efficiency and water vapor resistance stability.
[0046] The sixth embodiment of the present disclosure relates to a solid oxide fuel cell having a membrane electrode assembly, which comprises: an electrolyte membrane comprising an oxide having proton conductivity; and an electrode disposed on the above-mentioned electrolyte membrane and comprising a lanthanum strontium cobalt iron composite oxide, wherein the ratio of the number of moles of cobalt in the above-mentioned electrode to the sum of the number of moles of cobalt and the number of moles of iron is a value in the range of greater than 0.35 and less than 0.6.
[0047] According to the above configuration, the solid oxide fuel cell can have high power generation efficiency and water vapor resistance stability at an operating temperature of 600° C. or lower.
[0048] The seventh embodiment of the present disclosure relates to an electrochemical device having a membrane electrode assembly, which comprises: an electrolyte membrane comprising an oxide having proton conductivity; and an electrode disposed on the above-mentioned electrolyte membrane and comprising a lanthanum strontium cobalt iron composite oxide, wherein the ratio of the number of moles of cobalt in the above-mentioned electrode to the sum of the number of moles of cobalt and the number of moles of iron is a value in the range of greater than 0.35 and less than 0.6.
[0049] According to the above configuration, the electrochemical device can have high reaction efficiency and water vapor resistance stability at an operating temperature of 600° C. or lower.
[0050] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0051] In addition, the embodiments described below are all embodiments showing inclusive or specific examples. The numerical values, shapes, materials, components, configuration positions and connection methods of the components shown in the following embodiments are examples and do not limit the subject matter of the present disclosure. In addition, among the components in the following embodiments, the components not recorded in the independent claims are described as arbitrary components.
[0052] In addition, each figure is a schematic diagram and is not necessarily a strict illustration. Therefore, for example, the scales in each figure are not necessarily the same. In addition, in each figure, the same symbols are attached to substantially the same structure, and repeated descriptions are omitted or simplified.
[0053] In addition, in this specification, terms such as parallel that indicate the relationship between elements, terms such as rectangle that indicate the shape of elements, and numerical ranges are not expressions that only express strict meanings, but are expressions that mean substantially the same range, for example, including differences of about several %. In addition, the so-called "thickness direction" in this specification refers to the direction in which the electrodes and the electrolyte membrane are stacked.
[0054] (First embodiment)
[0055] [Structure of membrane electrode assembly]
[0056] Figure 1 1 is a cross-sectional view schematically showing the structure of a membrane electrode assembly 10 provided in the electrochemical device according to the first embodiment of the present disclosure. Figure 1 FIG. 4 shows a cross section of a membrane electrode assembly 10 cut along its thickness direction. Figure 1 As shown, the membrane electrode assembly 10 includes an electrolyte membrane 11 including a solid electrolyte as a proton conductive oxide, and an air electrode 12 provided on the electrolyte membrane 11. That is, the membrane electrode assembly 10 has a stacked structure in which the electrolyte membrane 11 and the air electrode 12 are arranged in contact with each other.
[0057] Examples of the electrochemical device including the membrane electrode assembly 10 include a solid oxide fuel cell, a water electrolysis cell, a steam electrolysis cell, and an electrochemical reactor.
[0058] [Electrolyte membrane]
[0059] The electrolyte membrane 11 includes a solid electrolyte having proton conductivity as described above. The solid electrolyte can be represented by any of the following composition formulas (1) to (3).
[0060] BZ 1-x1 M1 x1 O 3-γ (1)
[0061] Bc 1-x2 M2 x2 O 3-γ (2)
[0062] BZ 1-x3-y3 Ce x3 M3 y3 O 3-γ (3)
[0063] Here, M1, M2, and M3 are each independently at least one element selected from La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Y, Sc, Mn, Fe, Co, Ni, Al, Ga, In, and Lu. These M1, M2, and M3 are sometimes referred to as dopants. In addition, x1, x2, x3, and y3 satisfy the following conditions (a) to (d), respectively.
[0064] 0<x1<1 (a)
[0065] 0<x2<1 (b)
[0066] 0<x3<1 (c)
[0067] 0<y3<1 (d)
[0068] 0<γ≤0.5 (e)
[0069] Among the above solid electrolytes, BaZr containing no Ce is particularly preferred. 1-x1 M1 x1 O 3-γ The compound represented by the composition formula (1) (hereinafter, sometimes referred to as "BZM") has high stability to carbon dioxide.
[0070] In the composition formulas (1) to (3), γ is a value corresponding to the amount of oxygen deficiency in the composition, and varies depending on the oxidation number of the dopant and the mixing ratios x1, x2, x3, and y3. O of H2O corresponding to the amount of oxygen deficiency γ can enter the oxygen deficiency position, and the minimum value can be γ = 0. The range of the possible values of γ is 0 < γ ≤ 0.5.
[0071] In composition formulas (1) to (3), if the values of x1, x2, x3, and y3 become larger, the performance of the solid electrolyte, that is, the proton conductivity, is likely to be improved. In addition, if the values of x1, x2, x3, and y3 become smaller, the crystal structure of the solid electrolyte is likely to be stabilized.
[0072] For example, in the composition formula (3), as the value of x3 increases, the performance improves, but the stability to carbon dioxide decreases.
[0073] In addition, regarding the composition formulas (1) and (2), when x1 and x2 have the same value, the performance of the composition formula (2) is generally improved. However, the stability to carbon dioxide is reduced.
[0074] From the perspective of simultaneously satisfying the improvement of the performance of the solid electrolyte (improvement of proton conductivity) and the improvement of the stability of the structure, for composition formulas (1) to (3), it is good to satisfy 0.05<x1<0.3, 0.05<x2<0.3, and 0.05<x3<0.3, respectively, and it is preferred to satisfy 0.1≤x1≤0.2, 0.1≤x2≤0.2, and 0.1≤x3≤0.2, respectively. It is further preferred to satisfy x1=0.2, x2=0.2, and x3=0.2, respectively. In composition formula (1), from the perspective of proton conductivity, M1 can be at least one element selected from Y, Tm, Yb, and Lu. From the perspective of proton conductivity and the difficulty in generating impurities when mixed and calcined with a compound containing Ni, in composition formula (1), M1 can be at least one element selected from Lu and Yb. That is, the solid electrolyte represented by the composition formula (1) may be, for example, BaZr wherein M1 is Yb and x is 0.2. 0.8 Yb 0.2 O 3-γ In making the solid electrolyte BaZr 0.8 Yb 0.2 O 3-γ In this case, a membrane electrode assembly 10 with improved power generation efficiency and durability can be obtained. In addition, BZM of composition formula (1), for example, when element M is Yb and the molar ratio of Zr to Yb is 8:2, has a proton conductivity of about 0.011 S / cm at 600°C.
[0075] Furthermore, in order to reduce the ohmic resistance (ie, IR resistance) of the electrolyte membrane 11 , the electrolyte membrane 11 may be made as thin as possible.
[0076] [Air pole]
[0077] The air electrode 12 is composed of an oxide ion / electron mixed conductor material. The oxide ion / electron mixed conductor material is a lanthanum strontium cobalt iron composite oxide (hereinafter, sometimes recorded as "LSCF".), and the ratio of the molar number of Co to the sum of the molar number of Co and the molar number of Fe is a value in the range of 0.4 or more and 0.6 or less. The air electrode 12 can be composed only of LSCF, or it can be a composition in which LSCF is combined with other oxide ion / electron mixed conductor materials. Furthermore, for example, the air electrode 12 can include a material (hereinafter, electrolyte material) such as BZM that constitutes a solid electrolyte of the electrolyte membrane 11.
[0078] When the air electrode 12 is used as the air electrode of a solid oxide fuel cell, for example, a reaction of electrochemically reducing oxygen in the gas phase occurs. Therefore, in order to ensure the diffusion path of oxygen and promote the reaction, the air electrode 12 may be a porous body. For example, it may be a porous body having a porosity of 20 to 50% by volume as measured by the Archimedean method or the mercury penetration method.
[0079] LSCF can be represented by the following composition formula (4).
[0080] La 1-m Sr m Co n Fe 1-n O 3-δ (4)
[0081] In the composition formula (4), n is a value in the range of 0.4≤n≤0.6. Therefore, for example, it is possible to prevent the generation of decomposition products (for example, Co oxides) in the air electrode 12 by reaction with water under the highly humidified conditions of the operating temperature range of the solid oxide fuel cell having proton conductivity (i.e., the temperature range below 600°C) and the volume fraction of water vapor in the air being about 35%. In addition, the reaction resistance of the electrode reaction in the air electrode 12 can be made small, and the power generation efficiency can be improved.
[0082] In the composition formula (4), m is preferably a value in the range of 0≤m≤0.5, and m is particularly preferably 0.4. In the composition formula (4), δ represents the oxygen deficiency. δ may vary in the range of 0 or more and 0.5 or less depending on the molar ratio of Sr (i.e., the value of m), the molar ratio of Co (i.e., the value of n), and the oxidation numbers of Co and Fe.
[0083] The membrane electrode assembly 10 according to the first embodiment including the electrolyte membrane 11 and the air electrode 12 is as follows: Figure 1 As shown in the figure, the air electrode 12 is arranged on one main surface of the electrolyte membrane 11 and the electrolyte membrane 11 is laminated.
[0084] Therefore, the membrane electrode assembly 10 can reduce the reaction resistance and improve the reaction efficiency of the electrochemical device. In particular, since the air electrode 12 has high water vapor resistance and low reaction resistance, the membrane electrode assembly 10 can simultaneously meet high reaction efficiency and water vapor resistance.
[0085] (Second embodiment)
[0086] Below, refer to Figure 2The membrane electrode assembly 100 provided in the electrochemical device according to the second embodiment of the present disclosure is described. In the description of the second embodiment, the differences from the first embodiment are mainly described, and the same reference numerals are attached to the same or corresponding components in all the figures, and the description thereof is sometimes omitted.
[0087] Figure 2 2 is a cross-sectional view schematically showing the structure of a membrane electrode assembly 100 provided in an electrochemical device according to a second embodiment of the present disclosure. Figure 2 FIG. 4 shows a cross section of the membrane electrode assembly 100 cut along the thickness direction. Figure 2 As shown, the membrane electrode assembly 100 according to the second embodiment is a structure in which the fuel electrode 13 is further provided in the structure of the membrane electrode assembly 10 according to the first embodiment. That is, the membrane electrode assembly 10 is provided with an air electrode 12 on one main surface side of the electrolyte membrane 11, and a fuel electrode 13 on the other main surface side. In other words, in the electrochemical device, the air electrode 12, the electrolyte membrane 11, and the fuel electrode 13 are stacked in this order.
[0088] The membrane electrode assembly 100 according to the second embodiment has the same configuration as the membrane electrode assembly 10 according to the first embodiment except that it further includes a fuel electrode 13. Therefore, the same reference numerals are given to the same components as those of the membrane electrode assembly 10, and detailed description thereof is omitted.
[0089] In addition, Figure 2 In the embodiment, the membrane electrode assembly 100 has a structure in which the electrolyte membrane 11 is stacked on the fuel electrode 13, and the air electrode 12 is stacked on the electrolyte membrane 11, but the present invention is not limited thereto. For example, another layer made of an ion conductive material different from that of the electrolyte membrane 11 may be formed between the fuel electrode 13 and the electrolyte membrane 11.
[0090] [Fuel pole]
[0091] The fuel electrode 13 is an electrode where electrochemical oxidation occurs, and is, for example, an electrode made of a cermet of Ni and an electrolyte material.
[0092] When the fuel electrode 13 is used as a fuel electrode of a solid oxide fuel cell, for example, a reaction of oxidizing hydrogen in the gas phase into protons occurs in the fuel electrode 13. Therefore, in order to promote the oxidation reaction from hydrogen to protons, the fuel electrode 13 can be formed as a joint of Ni having electron conductivity and hydrogen oxidation activity and an electrolyte material having proton conductivity. In addition, in order to ensure the diffusion path of the gas (for example, hydrogen), the fuel electrode 13 can be a porous body. For example, the fuel electrode 13 can be a porous body having a porosity of 20 to 50% by volume as measured by the Archimedean method or the mercury penetration method.
[0093] Furthermore, when the electrochemical device including the membrane electrode assembly 100 is a solid oxide fuel cell, air is supplied to the side of the electrolyte membrane 11 provided with the air electrode 12, and a gas containing hydrogen (i.e., fuel) is supplied to the side provided with the fuel electrode 13 to generate electricity. Therefore, when the electrochemical device including the membrane electrode assembly 100 is a solid oxide fuel cell, the electrolyte membrane 11 needs to be airtight.
[0094] As described above, the membrane electrode assembly 100 according to the second embodiment has a structure in which the air electrode 12, the electrolyte membrane 11, and the fuel electrode 13 are stacked in sequence. Therefore, similarly to the membrane electrode assembly 10 according to the first embodiment, the membrane electrode assembly 100 according to the second embodiment can reduce the reaction resistance and improve the reaction efficiency of the electrochemical device. In particular, since the air electrode 12 shows high water vapor resistance stability and low reaction resistance, the membrane electrode assembly 10 can simultaneously satisfy high reaction efficiency and water vapor resistance stability.
[0095] Therefore, when the electrochemical device including the membrane electrode assembly 100 is a solid oxide fuel cell, the solid oxide fuel cell can reduce reaction resistance to improve power generation efficiency and achieve high water vapor resistance stability.
[0096] When the electrochemical device including the membrane electrode assembly 100 is a steam electrolysis cell, the steam electrolysis cell can reduce reaction resistance to improve electrolysis efficiency and achieve high water vapor resistance stability.
[0097] When the membrane electrode assembly 100 according to the second embodiment is used in a solid oxide fuel cell, for example, it can be configured as a fuel cell system as follows: That is, the fuel cell system includes a raw material supply path (not shown) for supplying a raw material, a reformer (not shown) for reforming the raw material flowing through the raw material supply path to generate a gas containing hydrogen, and an air supply path (not shown) for supplying air (i.e., oxidant gas).
[0098] In the fuel cell system, a raw material such as hydrocarbon gas is supplied from the outside to the reformer through a raw material supply path. The reformer reforms the supplied raw material to generate a gas containing hydrogen. The hydrogen-containing gas generated in the reformer is supplied to the fuel electrode 13 of the solid oxide fuel cell including the membrane electrode assembly 100. Alternatively, a configuration may be adopted in which a reformer is not provided and a hydrogen-containing gas is directly supplied from the outside to the fuel electrode 13 through a raw material supply path.
[0099] On the other hand, the oxidant gas is supplied from the outside to the air electrode 12 of the solid oxide fuel cell (membrane electrode assembly 100) through the air supply path. The solid oxide fuel cell (membrane electrode assembly 100) generates electricity through an electrochemical reaction between hydrogen in the hydrogen-containing gas supplied in this way and oxygen in the oxidant gas.
[0100] (Example)
[0101] The following describes the embodiments (embodiments 1 and 2) of the present disclosure. In addition, embodiments 1 and 2 of the present disclosure are examples of the membrane electrode assembly 10 involved in the first embodiment of the present disclosure and the membrane electrode assembly 100 involved in the second embodiment, and the configuration of the membrane electrode assembly 10 involved in the first embodiment of the present disclosure and the membrane electrode assembly 100 involved in the second embodiment is not limited to the configuration of these embodiments.
[0102] First, the air electrode according to Example 1 represented by composition formula (5), the air electrode according to Example 2 represented by composition formula (6), and the air electrode according to Example 3 represented by composition formula (7) were prepared.
[0103] The ratio of the number of moles of Co to the sum of the number of moles of Co and the number of moles of Fe in each of the air electrodes according to Examples 1, 2, and 3 is a value in the range of 0.35 to 0.6.
[0104] La 0.6 Sr 0.4 Co 0.35 Fe 0.65 O 3-δ (5)
[0105] La 0.6 Sr 0.4 Co 0.4 Fe 0.6 O 3-δ (6)
[0106] La 0.6 Sr 0.4 Co 0.6 Fe 0.4 O 3-δ (7)
[0107] Furthermore, an air electrode according to Comparative Example 1 represented by the following composition formula (8), an air electrode according to Comparative Example 2 represented by the following composition formula (9), an air electrode according to Comparative Example 3 represented by the following composition formula (10), and an air electrode according to Comparative Example 4 represented by the following composition formula (11) were prepared respectively.
[0108] La 0.6 Sr 0.4 Co 0.2 Fe0.8 O 3-δ (8)
[0109] La 0.6 Sr 0.4 Co 0.3 Fe 0.7 O 3-δ (9)
[0110] La 0.6 Sr 0.4 Co 0.8 Fe 0.2 O 3-δ (10)
[0111] La 0.6 Sr 0.4 CoO 3-δ (11)
[0112] The ratio of the molar number of Co to the sum of the molar number of Co and the molar number of Fe in each of the air electrodes according to Comparative Examples 1 to 4 is less than 0.35 or greater than 0.6. In addition, δ in the above composition formula represents the oxygen deficiency. The value of δ satisfies 0≤δ≤0.5.
[0113] (Method for producing air electrode material)
[0114] Next, a method for producing LSCF (LSC in Comparative Example 4) which is the air electrode material in Examples 1 to 3 and Comparative Examples 1 to 4 will be described.
[0115] [Method for producing air electrode material of Example 1]
[0116] The air cathode material (LSCF) involved in Example 1 is produced by the citric acid coordination compound method using La(NO3)3·6H2O, Sr(NO3)2, Co(NO3)2·6H2O, and Fe(NO3)3·9H2O (each produced by Kanto Chemical) as starting materials.
[0117] Specifically, 23.27 g of La(NO3)3·6H2O powder, 7.58 g of Sr(NO3)2 powder, 9.12 g of Co(NO3)2·6H2O powder, and 23.52 g of Fe(NO3)3·9H2O powder were weighed. Furthermore, each weighed powder was dissolved in distilled water, and 34.42 g of citric acid monohydrate (manufactured by Kanto Chemical) and 26.17 g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical) were added respectively. Then, the pH was adjusted to 7 using ammonia water (28 wt%) (manufactured by Kanto Chemical). After the pH was adjusted, the solvent was removed at 90°C on a heated stirrer. Then, it was heated to about 300°C, and finally formally sintered at 1200°C in an air atmosphere to obtain a powder of LSCF.
[0118] [Method for producing air electrode material of Example 2]
[0119] The air cathode material (LSCF) involved in Example 2 is prepared by the same method as the air cathode material involved in Example 1, except for the differences in the amounts of the respective powders used as starting materials and the amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water to dissolve the powders.
[0120] In addition, for the air electrode material involved in Example 2, the amount of each powder used as the starting material is set to 23.25g of La(NO3)3·6H2O powder, 7.58g of Sr(NO3)2 powder, 10.42g of Co(NO3)2·6H2O powder, and 21.69g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical). In addition, 34.39g of citric acid monohydrate (manufactured by Kanto Chemical) and 26.16g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical) are used.
[0121] [Method for producing air electrode material of Example 3]
[0122] The air cathode material (LSCF) involved in Example 3 is prepared by the same method as the air cathode material involved in Example 1, except for the different amounts of the powders serving as the starting materials and the different amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water to dissolve the powders.
[0123] In addition, for the air electrode material involved in Example 3, the amount of each powder used as the starting material is set to 23.19g of La(NO3)3·6H2O powder, 7.55g of Sr(NO3)2 powder, 15.58g of Co(NO3)2·6H2O powder, and 14.42g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical). In addition, 34.30g of citric acid monohydrate (manufactured by Kanto Chemical) and 26.08g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical) are used.
[0124] [Method for producing air electrode material of Comparative Example 1]
[0125] The air cathode material (LSCF) involved in Comparative Example 1 is prepared by the same method as the air cathode material involved in Example 1, except for the different amounts of the powders serving as the starting materials and the different amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water to dissolve the powders.
[0126] In addition, for the air electrode material involved in Comparative Example 1, the amount of each powder used as the starting raw material is set to 23.32g of La(NO3)3·6H2O powder, 7.60g of Sr(NO3)2 powder, 5.22g of Co(NO3)2·6H2O powder, and 29.00g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical). In addition, 34.49g of citric acid monohydrate (manufactured by Kanto Chemical) and 26.19g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical) are used.
[0127] [Method for producing air electrode material of Comparative Example 2]
[0128] The air cathode material (LSCF) involved in Comparative Example 2 is prepared by the same method as the air cathode material involved in Example 1, except for the different amounts of the powders serving as the starting materials and the different amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water to dissolve the powders.
[0129] In addition, for the air electrode material involved in Comparative Example 2, the amount of each powder used as the starting raw material is set to 23.28g of La(NO3)3·6H2O powder, 7.59g of Sr(NO3)2 powder, 7.82g of Co(NO3)2·6H2O powder, and 25.34g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical). In addition, 34.44g of citric acid monohydrate (manufactured by Kanto Chemical) and 26.19g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical) are used.
[0130] [Method for producing air electrode material of Comparative Example 3]
[0131] The air cathode material (LSCF) involved in Comparative Example 3 is prepared by the same method as the air cathode material involved in Example 1, except for the different amounts of the powders serving as the starting materials and the different amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water to dissolve the powders.
[0132] In addition, for the air electrode material involved in Comparative Example 3, the amount of each powder used as the starting raw material was set to 23.12 g of La(NO3)3·6H2O powder, 7.53 g of Sr(NO3)2 powder, 20.72 g of Co(NO3)2·6H2O powder, and 7.19 g of Fe(NO3)3·9H2O powder (each manufactured by Kanto Chemical). In addition, 34.20 g of citric acid monohydrate (manufactured by Kanto Chemical) and 26.01 g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical) were used.
[0133] [Method for producing air electrode material of Comparative Example 4]
[0134] The air cathode material (LSC) involved in Comparative Example 4 is prepared by the same method as the air cathode material involved in Example 1, except for the different amounts of the powders serving as the starting materials and the amounts of citric acid monohydrate and ethylenediaminetetraacetic acid (EDTA) added to the distilled water to dissolve the powders.
[0135] In addition, for the air electrode material involved in Comparative Example 4, the amount of each powder used as the starting raw material was set to 23.06g of La(NO3)3·6H2O powder, 7.51g of Sr(NO3)2 powder, and 25.83g of Co(NO3)2·6H2O powder (each manufactured by Kanto Chemical). In addition, 34.11g of citric acid monohydrate (manufactured by Kanto Chemical) and 25.94g of ethylenediaminetetraacetic acid (EDTA) (manufactured by Kanto Chemical) were used.
[0136] [Water vapor resistance test of air electrode]
[0137] The LSCFs according to Examples 1 to 3 and the LSCFs according to Comparative Examples 1 to 4 obtained by the above-described production method were subjected to a water vapor resistance test as follows.
[0138] First, the LSCF involved in Examples 1 to 3 and the LSCF involved in Comparative Examples 1 to 4 obtained by the above-mentioned "Manufacturing Method of Air Electrode Material" are filled into the concave part of a quartz dish (1 mm thick, 1 cm in diameter). Furthermore, the surface of the LSCF powder is smoothed using a glass scraper. Then, the measurement results obtained by the X-ray diffraction method are analyzed at room temperature and set as a benchmark before the test (i.e., before the water vapor resistance test). In order to perform the measurement by the X-ray diffraction method, SmartLab manufactured by Rigaku was used. In addition, the X-rays irradiated to the sample are CuKα characteristic X-rays (wavelength ).
[0139] Next, the LSCF involved in Examples 1 to 3 and the LSCF involved in Comparative Examples 1 to 4 were placed in a quartz tube having a gas flow path in a tubular furnace. The tubular furnace was then heated so that the temperature near the LSCF powder reached 600°C. Then, a humidified gas having a volume fraction of 40% water vapor by bubbling synthetic air was circulated in the gas flow path at a rate of 160cc / min. In addition, the volume fraction of water vapor was set to be slightly higher than that of oxygen in air (volume fraction 21%). + +4e - →The ratio of the water vapor fraction (about 35%) when all of the 2H2O is converted into water vapor by the reaction.
[0140] After 1000 hours, the powder of LSCF was measured by X-ray diffraction at room temperature. In this way, the measurement results after the water vapor resistance test (i.e., the measurement results after the test) were obtained. The benchmark before the test and the obtained measurement results after the test were compared. In this comparison, when a peak not belonging to LSCF was detected, it was judged that decomposition products of LSCF were generated. Regarding the LSCF involved in Examples 1 to 3 and the LSCF involved in Comparative Examples 1 to 4, the presence or absence of decomposition products after 1000 hours is shown in the following Tables 1 and Figure 3 middle. Figure 3 This is a diagram showing the measurement results obtained by the X-ray diffraction method regarding the LSCF according to Examples 2 and 3 of the present disclosure and the LSCF according to Comparative Examples 1 to 4.
[0141] [Table 1]
[0142]
[0143] When the ratio of the number of moles of cobalt (Co) to the sum of the number of moles of cobalt (Co) and the number of moles of iron (Fe) was 0.2, 0.3, 0.4, and 0.6, no peak indicating decomposition products other than LSCF was detected. On the other hand, when the ratio of the number of moles of cobalt (Co) to the sum of the number of moles of cobalt (Co) and the number of moles of iron (Fe) was 0.8 and 1.0, a peak of cobalt oxide (Co3O4) was detected (see Figure 3 ).
[0144] From this result, it is clear that when the ratio of Co to the sum of Co and Fe is 0.6 or less, it has high stability to water vapor at 600°C. On the other hand, when the ratio of Co to the sum of Co and Fe is 0.8 or 1.0, it is found that it is unstable to water vapor at 600°C.
[0145] (Method for producing membrane electrode assembly)
[0146] The membrane electrode assembly using the LSCF involved in Examples 1 to 3 and Comparative Examples 1 to 4 was manufactured by the following manufacturing method. In addition, the membrane electrode assembly used here is configured to have an air electrode arranged on one main surface side of the electrolyte membrane and a fuel electrode arranged on the other main surface side. In addition, the electrolyte membranes of the membrane electrode assembly using the LSCF involved in Examples 1 to 3 and Comparative Examples 1 to 4 are all composed of the same electrolyte material, and the representative composition of the electrolyte material is BaZr 0.8 Yb 0.2 O 2.9 (hereinafter referred to as BZYb) The fuel electrodes included in the membrane electrode assemblies using the LSCF according to Examples 1 to 3 and Comparative Examples 1 to 4 were all the same, using a compound of BZYb and NiO.
[0147] [Method for producing electrolyte material]
[0148] First, a method for producing a BZYb green sheet material as an electrolyte material constituting an electrolyte membrane will be described.
[0149] BZYb was produced by the citric acid coordination compound method using powders of Ba(NO3)2 (manufactured by Kanto Chemical) and ZrO(NO3)2·2H2O (manufactured by Kanto Chemical) and powder of Yb(NO3)3·xH2O (manufactured by Kojun Chemical) as starting materials.
[0150] (Preparation of Electrolyte Powder)
[0151] First, the electrolyte powder is described. Specifically, first, regarding BZYb, 42.43 g of Ba(NO3)2 powder and 34.71 g of ZrO(NO3)2·2H2O powder were dissolved in distilled water. In addition, Yb(NO3)3·xH2O powder 180 g dissolved in 300 mL of distilled water was added. 3+ 187 mL of an aqueous solution having an ion concentration of 0.87 mol / L was added and the obtained aqueous solution was stirred. 3+ The ion concentration was calculated from the analysis results of inductively coupled plasma atomic emission spectrometry (ICP-AES). As an analysis apparatus, iCAP7400 Duo manufactured by Soundwave Science Inc. was used.
[0152] Next, 1.5 equivalents of citric acid monohydrate (produced by Kanto Chemical) and 1.5 equivalents of ethylenediaminetetraacetic acid (EDTA) (produced by Kanto Chemical) were added to the aqueous solution based on the metal cations contained in the aqueous solution. The aqueous solution was then stirred at 90°C.
[0153] Next, the aqueous solution was adjusted to pH 7 using aqueous ammonia (28% (weight ratio)) (manufactured by Kanto Chemical). After the pH adjustment, the solution was heated to 95° C. to 240° C. using a heating stirrer to remove the solvent, thereby obtaining a solid substance.
[0154] The obtained solid material was crushed in a mortar and then degreased at about 400°C. After degreasing, the obtained powder was pressed into a cylindrical shape and pre-fired at 900°C in an atmosphere for 10 hours. After pre-firing, the coarsely crushed powder was added to a plastic container together with zirconium oxide balls, and ethanol was further added and crushed by a ball mill for more than 4 days. After the crushing by the ball mill, the solvent was removed by lamp drying. Thus, a powder of the electrolyte material was obtained.
[0155] (Preparation of Electrolyte Powder for Green Sheet and Production of Green Sheet)
[0156] The above-mentioned "(Preparation of electrolyte powder)" operation is repeated several times. In this way, about 200 g of electrolyte powder for raw sheets is obtained. Green sheets are made using the powder of the obtained electrolyte material. Specifically, the powder of the electrolyte material, polyvinyl butyral as a resin, butyl benzyl phthalate as a plasticizer, and butyl acetate and 1-butanol as solvents are mixed. In this way, a mixture is obtained. The obtained mixture is processed by a tape casting method. In this way, a raw sheet of electrolyte is obtained.
[0157] [Method for producing fuel electrode material]
[0158] Next, a method for producing a fuel electrode material using BZYb and NiO will be described.
[0159] The powder of the electrolyte material obtained by the above-mentioned "method for producing the electrolyte material" and the powder of NiO (manufactured by Sumitomo Metal Mining) are weighed in a weight ratio of NiO:BZYb=80:20 (i.e., the volume ratio of Ni to BZYb is 69:31). Furthermore, a green sheet is produced using the weighed powder of the electrolyte material and the powder of NiO. Specifically, the powder of the electrolyte material, the powder of NiO, polyvinyl butyral as a resin, butyl benzyl phthalate as a plasticizer, and butyl acetate and 1-butanol as solvents are kneaded. In this way, a kneaded product is obtained. The obtained kneaded product is processed by a casting method. In this way, a green sheet of a fuel electrode is obtained.
[0160] [Method for producing laminate]
[0161] First, the method for manufacturing a laminate of a fuel electrode and an electrolyte membrane is described. Assuming a linear shrinkage of 22%, the fuel electrode green sheet obtained by the above-mentioned "manufacturing method of a fuel electrode material" is cut into a predetermined size after firing so as to become a square of 20 mm × 20 mm (the four corners are chamfered by 3 mm), and a plurality of sheets are stacked. Furthermore, the fuel electrode green sheets cut into a predetermined size and stacked are overlapped and stacked with the electrolyte green sheets obtained by the "manufacturing method of an electrolyte material", and a pressure of 50 MPa is applied by hot pressing to obtain a laminate.
[0162] The obtained laminate was sintered at 1475°C for 2 hours, and a half cell of 20 mm × 20 mm square (the four corners were chamfered with 3 mm) size was made from the laminate of the fuel electrode and the electrolyte membrane. In addition, the BZYb constituting the electrolyte membrane was confirmed to be a single phase by X-ray diffraction. The measurement was performed using SmartLab manufactured by Rigaku. In addition, the X-ray irradiated to the sample was set to CuKα characteristic X-ray (wavelength ).
[0163] Next, the method for forming the air electrode on the electrolyte membrane is described. The powders of the air electrode materials of Examples 1 to 3 and Comparative Examples 1 to 4 obtained by the above-mentioned "method for manufacturing air electrode materials" are mixed with a carrier mixed with alcohol and ether at a specified weight ratio, and kneaded with a rotation / revolution mixer to prepare a paste of the air electrode material. In addition, the powders of the air electrode materials of Examples 1 to 3 and Comparative Examples 1 to 4 are mixed with the carrier in a ratio of 3:2 (weight ratio).
[0164] The paste of the air electrode material involved in Examples 1 to 3 and Comparative Examples 1 to 4 was screen-printed on the electrolyte membrane of each half unit and applied as an air electrode with a diameter of 10 mm. Furthermore, the membrane electrode assembly involved in Examples 1 to 3 and Comparative Examples 1 to 4 was obtained by sintering at 950°C for 2 hours in an air atmosphere. In addition, the thickness of the electrolyte membrane, air electrode, and fuel electrode of the membrane electrode assembly involved in Examples 1 to 3 and Comparative Examples 1 to 4 obtained was 13 μm, 10 μm, and 0.6 mm, respectively.
[0165] (Measurement of Reaction Resistance of Membrane Electrode Assembly)
[0166] Next, the reaction resistance of the membrane electrode assemblies according to Examples 1 to 3 and Comparative Examples 1 to 4 was measured. The measurement was performed as follows by AC impedance measurement using a four-terminal method.
[0167] Ag mesh for current collection was bonded using Ag paste on the surfaces of the fuel electrode and air electrode of each of the membrane electrode assemblies involved in Examples 1 to 3 and Comparative Examples 1 to 4. In addition, two Pt wires were bonded to the Ag mesh as external extraction terminals for four-terminal method measurement on the fuel electrode side and the air electrode side, respectively.
[0168] First, the membrane electrode assembly is heated to 700°C, humidified air containing 3% water vapor is supplied to the air electrode side, and humidified hydrogen containing 3% water vapor is supplied to the fuel electrode side. The temperature is maintained for more than 4 hours to reduce the NiO in the mixture of NiO and BZYb in the fuel electrode to Ni.
[0169] The resistance measurement was performed after the reduction operation of the membrane electrode assembly at 600°C, with humidified air containing 3% (volume ratio) of water vapor supplied to the air electrode side and humidified hydrogen containing 3% of water vapor supplied to the fuel electrode side. The AC impedance measurement was performed using a ModulLab XM manufactured by Solatron, with an AC current applied with a frequency varying from 100 kHz to 0.01 Hz at an amplitude of 10 mV relative to the inter-terminal voltage at an external current of 0 A.
[0170] Figure 4 FIG. 1 is a diagram showing an example of the results of AC impedance measurement in the examples of the present disclosure using a Cole-Cole plot. Figure 4 The details of the resistance components obtained by AC impedance measurement are schematically shown in FIG. Figure 4As shown in FIG. 1 , the results of the AC impedance measurement can be graphically represented by a Cole plot using the real component Z' of the impedance Z (=Z'+jZ") on the horizontal axis and the imaginary component Z" on the vertical axis. In the Cole plot, for an arc drawn in the frequency range of about 10kHz to 0.01Hz, the length of the chord formed by the arc and the real axis (Z'), that is, the length of the two intersection points obtained by the arc cutting the real axis, becomes the reaction resistance. The results of the reaction resistance obtained by the measurement are shown in the above Table 1.
[0171] In addition, the relationship between the molar ratio of Co to the sum of the molar numbers of Co and Fe and the reaction resistance is shown in Figure 5 middle. Figure 5 This is a graph showing the relationship between the molar ratio of Co to the sum of the molar numbers of Co and Fe and the reaction resistance of the air electrodes according to Examples 1 to 3 and Comparative Examples 1 to 4 of the present disclosure. Figure 5 In the figure, the vertical axis is set as the reaction resistance (unit: Ωcm 2 ), the horizontal axis shows the ratio of Co in the air electrode to the sum of the molar numbers of Co and Fe.
[0172] As shown in Table 1 and Figure 5 As shown in FIG. 1 , when the molar ratio of Co to the sum of the molar numbers of Co and Fe in the air electrode material (LSCF) is 0.35 or more (the air electrodes involved in Examples 1 and 2 and the air electrodes involved in Comparative Example 3), the reaction resistance becomes 1.4 Ωcm 2 Therefore, when the membrane electrode assembly is used in a solid oxide fuel cell, the voltage does not fall below 0.7 V which is set as the minimum voltage actually obtained when the solid oxide fuel cell is operated.
[0173] On the other hand, when the molar ratio of Co to the sum of the molar numbers of Co and Fe in the air electrode material (LSCF) was 0.2 and 0.3 (the air electrodes of Comparative Examples 1 and 2), the reaction resistance was 2.1 cm 2 、1.8cm 2 , respectively, showed a significantly larger tendency than that of the air electrodes involved in Examples 1 and 2, and the reaction resistance became more than 1.4 Ωcm 2 The value of .
[0174] The above results clearly show that when the molar ratio of Co to the sum of the molar numbers of Co and Fe in the air electrode material (LSCF) is 0.35 or more, the reaction resistance of the membrane electrode assembly can be reduced. Therefore, when a membrane electrode assembly in which the molar ratio of Co to the sum of the molar numbers of Co and Fe in the air electrode material (LSCF) is 0.35 or more is used in a solid oxide fuel cell, high power generation efficiency can be achieved.
[0175] As shown in Table 1, regarding the water vapor resistance stability, it was confirmed that the membrane electrode assembly having a molar ratio of Co to the sum of the moles of Co and Fe in the air electrode material (LSCF) of 0.6 or less had high water vapor resistance stability.
[0176] From the above, it can be seen that in the air electrode material (LSCF), a membrane electrode assembly having a molar ratio of Co to the sum of the molar numbers of Co and Fe of 0.35 to 0.6 satisfies both high reaction efficiency and high water vapor resistance stability.
[0177] Industrial Availability
[0178] The membrane electrode assembly according to the present disclosure can be used in electrochemical devices such as solid oxide fuel cells, water electrolysis units, and steam electrolysis units.
[0179] Explanation of symbols
[0180] 10 Membrane Electrode Assembly
[0181] 11 Electrolyte membrane
[0182] 12 Air electrode
[0183] 13 Fuel electrode
[0184] 100 Membrane electrode assembly.
Claims
1. A membrane electrode assembly comprising: an electrolyte membrane comprising an oxide having proton conductivity; and an electrode provided on the electrolyte membrane and comprising a lanthanum strontium cobalt iron composite oxide, The lanthanum strontium cobalt iron composite oxide is represented by the following composition formula: Day 1-m Sr m Co n Feb 1-n O 3-δ in, 0.35≤n≤0.6, 0≤m≤0.5, 0≤δ≤0.
5. 2 . The membrane electrode assembly according to claim 1 , wherein the electrolyte membrane is arranged in contact with the electrode.
3. The membrane electrode assembly according to claim 1 or 2, wherein the electrolyte membrane comprises a member selected from BaZr 1-x1 M1 x1 O 3-γ ,BaCe 1-x2 M2 x2 O 3-γ , and BaZr 1-x3-y3 Ce x3 M3 y3 O 3-γ At least one compound of M1, M2 and M3 are each independently at least one element selected from La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Y, Sc, Mn, Fe, Co, Ni, Al, Ga, In, and Lu, x1 satisfies 0<x1<1, x2 satisfies 0<x2<1, x3 satisfies 0<x3<1, y3 satisfies 0<y3<1, and γ satisfies 0<γ≤0.
5.
4. The membrane electrode assembly according to claim 3, wherein the electrolyte membrane is BaZr 1-x1 Yb x1 O 3-γ The compounds shown. 5 . The membrane electrode assembly according to claim 1 , wherein the electrode is an air electrode. The membrane electrode assembly according to claim 3 , wherein the electrode is an air electrode. 7 . The membrane electrode assembly according to claim 1 , wherein n satisfies 0.4≤n≤0.
6. The membrane electrode assembly according to claim 3 , wherein n satisfies 0.4≤n≤0.
6. 9 . The membrane electrode assembly according to claim 5 , wherein n satisfies 0.4≤n≤0.
6. 10 . A solid oxide fuel cell comprising the membrane electrode assembly according to claim 1 . 11 . An electrochemical device comprising the membrane electrode assembly according to claim 1 .
Citation Information
Patent Citations
Proton conductor, solid electrolyte layer for fuel cell, cell structure, and fuel cell including the same
US20180037508A1