Semiconductor structure and method for forming the same

By forming a source-drain opening and a silicon germanium doped layer with a specific structure in the semiconductor device, the problem of low performance in the prior art is solved, and the driving current is improved and the interface reliability is improved.

CN113394271BActive Publication Date: 2024-11-19SEMICON MFG INT (BEIJING) CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010177157.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-03-13
Publication Date
2024-11-19
Estimated Expiration
2040-03-13

AI Technical Summary

Technical Problem

The existing semiconductor devices have low performance and are difficult to meet the demand for driving current increase by integrated circuit manufacturing technology.

Method used

By forming a source and drain opening of a specific structure in the substrate and forming a silicon germanium doped layer therein, the size of the source and drain opening is increased to increase the volume and stress of the doped layer while keeping the channel length unchanged, ions are used The injection and annealing process forms a multilayer stress structure to optimize interface and carrier diffusion.

Benefits of technology

It improves the driving current and performance of semiconductor devices, increases the stress of the doped layer, reduces the carrier diffusion distance, and improves the interface reliability and overall performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113394271B_ABST
    Figure CN113394271B_ABST
Patent Text Reader

Abstract

A semiconductor structure and a method for forming the same, wherein the method comprises: providing a substrate, wherein the substrate surface has a gate structure; forming initial source-drain openings in the substrate on both sides of the gate structure, wherein the initial source openings comprise: a first region and a second region located on the first region; increasing the size of the first region of the initial source-drain openings in a direction perpendicular to the sidewall surface of the gate structure to form source-drain openings; and forming source-drain doping layers in the source-drain openings. The semiconductor structure formed by the method has good performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a forming method thereof. Background Art

[0002] With the rapid development of integrated circuit manufacturing technology, the size of semiconductor devices in the integrated circuit is continuously reduced, so that the operating speed of the entire integrated circuit can be effectively improved.

[0003] In a very large scale integrated circuit, stress is usually formed on a transistor to increase the carrier mobility of the transistor and thus increase the driving current of the transistor.

[0004] However, the performance of semiconductor devices formed by the prior art needs to be improved. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the performance of semiconductor devices.

[0006] To solve the above technical problems, the technical solution of the present invention provides a semiconductor structure, including: a substrate, a surface of the substrate having a gate structure; source and drain openings in the substrate on both sides of the gate structure, the source and drain openings including: a first region and a second region located on the first region, and the sidewalls of the second region are recessed relative to the sidewalls of the first region; and a source and drain doping layer located in the source and drain openings.

[0007] Optionally, a dimension of the first region of the source / drain opening in a direction perpendicular to the sidewall surface of the gate structure ranges from 50 nanometers to 130 nanometers.

[0008] Optionally, the source-drain doping layer includes: a first stress structure located on the sidewall surfaces and the top surface of the source-drain opening; and a second stress structure located on the surface of the first stress structure, and the second stress structure completely fills the source-drain opening.

[0009] Optionally, the material of the first stress structure includes: germanium silicon, and the germanium in the germanium silicon material has a first concentration; the material of the second stress structure includes: germanium silicon, and the germanium in the germanium silicon material has a second concentration, and the first concentration is less than the second concentration.

[0010] Optionally, the first concentration ranges from 10% to 25%; the second concentration ranges from 35% to 60%.

[0011] Optionally, the first stress structure includes: a first stress layer located on the side wall surfaces and the top surface of the source and drain openings, and a second stress layer located on the surface of the first stress layer; the second stress structure includes: a third stress layer located on the surface of the second stress layer, and a fourth stress layer located on the surface of the third stress layer, and the fourth stress layer fills the source and drain openings.

[0012] Optionally, the first stress layer, the second stress layer, the third stress layer and the fourth stress layer are doped with first conductive type ions.

[0013] Optionally, the first conductive type ions in the first stress layer and the second stress layer have a third concentration; the first conductive type ions in the third stress layer and the fourth stress layer have a fourth concentration, and the third concentration is less than the fourth concentration.

[0014] Optionally, the second stress layer and the third stress layer are also doped with second conductive type ions; the second conductive type ions in the second stress layer have a fifth concentration, and the fifth concentration is less than the third concentration; the second conductive type ions in the third stress layer have a sixth concentration, and the sixth concentration is less than the third concentration.

[0015] Optionally, the base includes a substrate and a fin located on a surface of the substrate, the gate structure covers a portion of a top surface and a sidewall surface of the fin; and the source and drain openings are located in the fins on both sides of the gate structure.

[0016] Correspondingly, the technical solution of the present invention also provides a method for forming the semiconductor structure described in any of the above items, including: providing a substrate, the surface of the substrate having a gate structure; forming initial source and drain openings in the substrate on both sides of the gate structure, the initial source openings including: a first region and a second region located on the first region; increasing the size of the first region of the initial source and drain openings in a direction perpendicular to the side wall surface of the gate structure to form a source and drain opening; and forming a source and drain doping layer in the source and drain openings.

[0017] Optionally, the method for forming the initial source opening includes: using the gate structure as a mask, etching the substrate, and forming initial source and drain openings in the substrate.

[0018] Optionally, the method for increasing the size of the first area of ​​the initial source and drain opening in a direction perpendicular to the side wall surface of the gate structure includes: performing amorphization treatment on the substrate exposed by the first area of ​​the initial source and drain opening to form an amorphized layer on the side wall and bottom of the first area of ​​the initial source and drain opening; removing the amorphized layer to increase the size of the first area of ​​the initial source and drain opening in a direction perpendicular to the side wall surface of the gate structure to allow the initial source and drain opening to form the source and drain opening.

[0019] Optionally, the amorphization treatment process includes: an ion implantation process; the parameters of the ion implantation process include: an implantation angle range of 5 degrees to 25 degrees, the implanted ions include: boron ions and nitrogen ions, or boron ions and germanium ions, the implantation angle is the angle between the ion implantation direction and a reference plane, and the reference plane is a plane perpendicular to the substrate surface and parallel to the channel width direction.

[0020] Optionally, the process of removing the amorphous layer includes: a dry etching process or a wet etching process, or a combination of the two.

[0021] Optionally, the base includes a substrate and a fin located on the surface of the substrate; the method for forming the initial source and drain openings includes: using the gate structure as a mask, etching the fin until the substrate surface is exposed, and forming the initial source and drain openings in the fins on both sides of the gate structure.

[0022] Optionally, the method for forming the source-drain doping layer includes: forming a first stress structure on the sidewall surfaces and bottom surface of the source-drain opening; and forming a second stress structure on the surface of the first stress structure.

[0023] Optionally, the first stress structure includes: a first stress layer located on the side wall surface and the bottom surface of the source and drain opening, and a second stress layer located on the surface of the first stress layer; the second stress structure includes: a third stress layer located on the surface of the second stress layer, and a fourth stress layer located on the surface of the third stress layer; the method for forming the first stress layer, the second stress layer, the third stress layer and the fourth stress layer includes: forming a first initial stress layer on the side wall surface and the bottom surface of the source and drain opening, wherein the first initial stress layer is doped with first conductive type ions; performing an ion implantation process on the first initial stress layer to form an inverse doped layer in the first initial stress layer. A region is formed, wherein the inversion doping region is doped with second conductive type ions, and the conductive type of the second conductive type ions is opposite to that of the first conductive type ions; a second initial stress layer is formed on the surface of the first initial stress layer, and the second initial stress layer is doped with first conductive type ions; an annealing process is adopted to diffuse the second conductive type ions in the inversion doping region toward the first initial stress layer and the second initial stress layer, the ions diffuse into the first initial stress layer to form a second stress layer, and the first initial stress layer where no diffusion occurs forms a second stress layer, the ions diffuse into the second initial stress layer to form a third stress layer, and the second initial stress layer where no diffusion occurs forms a fourth stress layer.

[0024] Optionally, a first epitaxial growth process is used to form the first initial stress layer, and an in-situ doping process is used to dope the first conductive type ions into the first initial stress layer; a second epitaxial growth process is used to form the second initial stress layer, and an in-situ doping process is used to dope the first conductive type ions into the second initial stress layer.

[0025] Optionally, the ion implantation process includes: an implantation energy range of 1KeV to 5KeV; an implantation dose range of 5e13atm / cm2 to 5e14atm / cm2; an implantation angle of 0 degrees to 5 degrees; and parameters of the annealing process include: an annealing temperature of 800 degrees Celsius to 950 degrees Celsius, and an annealing time of 30 seconds to 30 minutes.

[0026] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:

[0027] In the method for forming a semiconductor structure provided by the technical solution of the present invention, a source-drain opening is formed by increasing the size of the first area of ​​the initial source-drain opening in a direction perpendicular to the surface of the sidewall of the gate structure, so that the size of the first area of ​​the source-drain opening is increased. The size of the first area of ​​the source-drain opening is relatively large, and the source-drain opening is used to provide space for the subsequent formation of a source-drain doped layer, so that the volume of the source-drain doped layer subsequently formed in the source-drain opening is increased, and the source-drain doped layer with a larger volume has a greater stress, which is beneficial to improving the driving current of the formed device. At the same time, the size of the second area of ​​the source-drain opening remains unchanged, which is beneficial to ensure that the effective length of the channel located below the gate structure is not affected. In summary, the semiconductor structure formed by the method has high performance.

[0028] Furthermore, the material of the first stress structure includes: germanium silicon, in which germanium has a first concentration; the material of the second stress structure includes: germanium silicon, in which germanium has a second concentration, and the first concentration is less than the second concentration. The first stress structure with a smaller concentration is conducive to making the interface defects between the first stress structure and the substrate smaller, thereby serving as a buffer layer between the substrate and the second stress structure, which is conducive to improving the interface reliability. The second stress structure with a larger concentration has a larger stress, which is conducive to improving the driving current of the device. In summary, the first stress structure and the second stress structure are conducive to improving the performance of the semiconductor structure.

[0029] Furthermore, an inversion doping region is formed in the first initial stress layer, and the inversion doping region is doped with second conductive type ions, and the conductivity type of the second conductive type ions is opposite to that of the first conductive type ions. Through the annealing process, the second conductive type ions in the inversion doping region diffuse to the first initial stress layer and the second initial stress layer, and the second conductive type ions diffused into the first initial stress layer can neutralize part of the first conductive type ions, so that the concentration of carriers is small, which is beneficial to reduce the diffusion distance of carriers, thereby reducing the impact on the channel length. Similarly, the second conductive type ions diffused into the second initial stress layer can neutralize part of the first conductive type ions, so that the concentration of carriers is small, which is beneficial to reduce the diffusion distance of carriers, thereby reducing the impact on the channel length. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figures 1 to 3 It is a schematic structural diagram of each step of a method for forming a semiconductor structure;

[0031] Figures 4 to 11 It is a structural schematic diagram of each step of a method for forming a semiconductor structure in one embodiment of the present invention. DETAILED DESCRIPTION

[0032] As described in the background art, semiconductor structures have poor performance.

[0033] The following is a detailed description of the reasons for the poor performance of the semiconductor structure with reference to the accompanying drawings. Figure 1 It is a structural diagram of a semiconductor structure.

[0034] Please refer to Figure 1 , providing a substrate 100, wherein a gate structure 110 is provided on a surface of the substrate 100.

[0035] Please refer to Figure 2 , source and drain openings 120 are formed in the substrate 100 on both sides of the gate structure 110 .

[0036] Please refer to Figure 3 , a source-drain doping layer 130 is formed in the source-drain opening 120 .

[0037] In the above method, the semiconductor structure is a PMOS transistor, and the source-drain doped layer 130 is formed by an epitaxial growth process, and the material of the source-drain doped layer 130 is usually silicon germanium or silicon carbide. The source-drain doped layer 130 formed of the silicon germanium or silicon carbide material has a large stress, which is conducive to improving the driving current of the formed semiconductor structure.

[0038] However, the source-drain opening 120 formed in the substrate 100 by etching process is generally in the shape of an inverted trapezoid with a large top and a small bottom. Since the bottom of the source-drain opening 120 is small in size, the volume of the source-drain opening 120 is small, resulting in that the stress generated by the source-drain doping layer 130 in the source-drain opening 120 with a small volume on the channel is still small, and therefore, the driving current of the semiconductor structure is still small.

[0039] In order to solve the above technical problems, the size of the source-drain opening 120 is enlarged by further etching, so that the source-drain doping layer 130 located in the larger source-drain opening 120 has a larger stress, thereby improving the driving current of the formed semiconductor structure.

[0040] However, when the size of the source and drain openings 120 is increased by further etching, the top and bottom sizes of the source and drain openings 120 are both increased. Since the fins between the source and drain openings 120 form a channel, and as the semiconductor structure develops toward higher and higher integration, when the top size of the source and drain openings 120 is larger, the size of the channel between the source and drain openings 120 is smaller, which easily causes a short channel effect.

[0041] To solve the technical problem, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate, the surface of the substrate having a gate structure; forming initial source and drain openings in the substrate on both sides of the gate structure, the initial source openings comprising: a first region and a second region located on the first region; increasing the size of the first region of the initial source and drain openings in a direction perpendicular to the sidewall surface of the gate structure to form source and drain openings; forming source and drain doping layers in the source and drain openings. The semiconductor structure formed by the method has high performance.

[0042] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0043] Figures 4 to 11 It is a structural schematic diagram of each step of a method for forming a semiconductor structure in one embodiment of the present invention.

[0044] Please refer to Figure 4 , providing a substrate 200, wherein the surface of the substrate 200 has a gate structure 210.

[0045] In this embodiment, the base 200 includes a substrate 201 and a fin 202 located on a surface of the substrate 201 , and the gate structure 210 covers a portion of a top surface and a sidewall surface of the fin 202 .

[0046] In this embodiment, the method for forming the base 200 includes: providing an initial substrate (not shown); the initial substrate has a first patterned layer, and the first patterned layer exposes a portion of the surface of the initial substrate; using the first patterned layer as a mask, etching the initial substrate to form the substrate 201 and the fin 202 located on the surface of the substrate 201.

[0047] In this embodiment, the material of the initial substrate is silicon. Accordingly, the material of the substrate 201 and the fin 202 is silicon.

[0048] In other embodiments, the material of the initial substrate includes: germanium, silicon germanium, silicon on insulator or germanium on insulator. Correspondingly, the material of the substrate includes: germanium, silicon germanium, silicon on insulator or germanium on insulator. The material of the fin includes: germanium, silicon germanium, silicon on insulator or germanium on insulator.

[0049] In this embodiment, the gate structure 210 includes a gate dielectric layer 211 and a gate electrode layer 212 located on the surface of the gate dielectric layer 211 .

[0050] In this embodiment, the process of forming the gate dielectric layer 211 includes: a deposition process; the material of the gate dielectric layer 211 is silicon oxide.

[0051] In another embodiment, the material of the gate dielectric layer includes a material with a K value greater than 3.9, such as titanium oxide, aluminum oxide, hafnium oxide, tantalum oxide or lanthanum oxide.

[0052] In this embodiment, the material of the gate electrode layer 212 includes polysilicon.

[0053] In another embodiment, the material of the gate electrode layer includes a metal material, such as a combination of one or more of tungsten, cobalt, copper, nickel, titanium and titanium nitride.

[0054] In this embodiment, the gate structure 210 further includes: a barrier layer 213 located on the top surface of the gate electrode layer 212. The barrier layer 213 is used to protect the gate structure 210 from being affected by the subsequent processes, so as to maintain a good morphology.

[0055] In this embodiment, the gate structure 210 further includes: a sidewall 214 located on the sidewall surface of the gate dielectric layer 211 and the sidewall surface of the gate electrode layer 212. The sidewall 214 is used, on the one hand, to protect the gate structure from being affected by the process in the subsequent process steps, so as to maintain a good morphology; on the other hand, to control the position of the source and drain doping layer formed subsequently, so as to avoid the source and drain doping layer being too close to the gate structure 210.

[0056] Please refer to Figure 5, initial source-drain openings 220 are formed in the substrate 200 on both sides of the gate structure 210 , and the initial source-drain openings 220 include: a first region I and a second region II located on the first region I.

[0057] In this embodiment, the initial source and drain openings 220 are formed in the fins 202 on both sides of the gate structure 210 .

[0058] It should be noted that the second region II is located on the first region I, so that the source and drain openings formed by subsequently processing the initial source and drain openings 220 include: the first region I and the second region II, and the second region II is located on the first region I.

[0059] The method for forming the initial source opening 220 includes: using the gate structure 210 as a mask, etching the substrate 200 , and forming the initial source and drain opening 220 in the substrate 200 .

[0060] In this embodiment, the size of the top of the initial source / drain opening 220 is greater than the size of the bottom of the initial source / drain opening 220 .

[0061] The dimension refers to the distance along a direction perpendicular to the sidewall surface of the gate structure 210 .

[0062] In other embodiments, the size of the top of the initial source and drain openings is consistent with the size of the bottom of the initial source and drain openings, that is, the sidewalls of the initial source and drain openings are perpendicular to the substrate surface. Specifically, in this embodiment, the method for forming the initial source and drain openings 220 includes: using the gate structure 210 as a mask, etching the fins 202 until the surface of the substrate 201 is exposed, and forming the initial source and drain openings 220 in the fins 202 on both sides of the gate structure 210.

[0063] The process of etching the fin 202 using the gate structure 210 as a mask includes: an anisotropic dry etching process.

[0064] Please refer to Figure 6 , the first region I of the initial source / drain opening 220 is amorphized, and an amorphized layer 230 is formed on the sidewalls and bottom of the first region I of the initial source / drain opening 220 .

[0065] The amorphization process includes: an ion implantation process.

[0066] The parameters of the ion implantation process include: an implantation angle range of 5 to 25 degrees, the implanted ions include: boron ions and nitrogen ions, or boron ions and germanium ions, the implantation angle is the angle between the ion implantation direction and a reference plane, and the reference plane is a plane perpendicular to the surface of the substrate 200 and parallel to the channel width direction.

[0067] The reason for selecting the injection angle within the range is that the smaller injection angle can enable the injected ions to be partially blocked by the gate structure 210 located on the top surface of the fin 202, so that the substrate 200 close to the side wall of the initial source and drain opening 220 at the bottom of the gate structure 210, that is, the substrate 200 around the initial source and drain opening 220 of the second region II is not easily injected with ions or even not injected with ions, and at the same time, the substrate 200 exposed by the initial source and drain opening 220 away from the bottom of the gate structure 210, that is, the substrate 200 on the side wall and bottom of the first region I of the initial source and drain opening 220 is easily injected with ions, thereby achieving amorphization treatment of the substrate 200 exposed by the first region I of the initial source and drain opening 220, forming an amorphization layer 230 on the side wall and bottom of the first region I of the initial source and drain opening 220, and at the same time, having no impact on the substrate 200 around the initial source and drain opening 220 of the second region II.

[0068] In this embodiment, through the amorphization treatment, ions are implanted into the fin 202 located at the sidewall of the first region I of the initial source / drain opening 220 and the substrate 201 located at the bottom of the first region I of the initial source / drain opening 220 to form an amorphization layer 230 .

[0069] Due to the different properties of the materials of the amorphous layer 230 and the fin 202, the subsequent etching process can have different etching rates for the amorphous layer 230 and the fin 202, thereby removing the amorphous layer 230 to increase the size of the first region I of the initial source and drain opening 220 in the direction perpendicular to the side wall surface 202 of the gate structure, while not causing etching to the initial source and drain opening 220 in the second region II.

[0070] Please refer to Figure 7 , removing the amorphous layer 230 , so that the initial source-drain opening 220 forms the source-drain opening 240 .

[0071] Specifically, by removing the amorphized layer 230, the amorphized layer 230 is located on the sidewall and bottom of the first region I of the initial source and drain opening to form a source and drain opening 240, so that the size of the first region I of the formed source and drain opening 240 is increased in a direction perpendicular to the sidewall surface of the gate structure 210.

[0072] In this embodiment, the sidewalls of the second region II of the source / drain opening 240 are recessed relative to the sidewalls of the first region I. Specifically, in this embodiment, by removing the amorphized layer 230, the size of the first region I of the initial source / drain opening 220 is increased, so that the size of the bottom of the second region II of the source / drain opening 240 is smaller than the size of the top of the first region I of the source / drain opening 240.

[0073] The process of removing the amorphous layer 230 includes: a dry etching process or a wet etching process, or a combination of the two.

[0074] In this embodiment, the process of removing the amorphous layer 230 is a wet etching process; the parameters of the wet etching process include: the etching solution used is a tetramethylammonium hydroxide solution.

[0075] The source-drain opening 240 is formed by increasing the size of the first region I of the initial source-drain opening 220 in a direction perpendicular to the sidewall surface of the gate structure 210, so that the size of the first region I of the source-drain opening 240 is increased. The size of the first region I of the source-drain opening 240 is relatively large, and the source-drain opening 240 is used to provide space for the subsequent formation of the source-drain doping layer, so that the volume of the source-drain doping layer subsequently formed in the source-drain opening 240 is increased. The source-drain doping layer with a larger volume has a greater stress, which is beneficial to improving the driving current of the formed device. At the same time, the size of the second region II of the source-drain opening 240 remains unchanged, which is beneficial to ensure that the effective length of the channel located below the gate structure 210 is not affected. In summary, the semiconductor structure formed by the method has high performance.

[0076] After the source-drain opening 240 is formed, a source-drain doping layer is formed in the source-drain opening 240. For details on the process of forming the source-drain doping layer, please refer to Figures 8 to 11 .

[0077] Please refer to Figure 8 A first initial stress layer 250 is formed on the sidewall surface and the bottom surface of the source / drain opening 240 , and the first initial stress layer 250 is doped with first conductive type ions.

[0078] The first initial stress layer 250 is formed by a first epitaxial growth process, and the first initial stress layer 250 is doped with first conductive type ions by an in-situ doping process.

[0079] In this embodiment, the semiconductor structure is used to form a PMOS transistor, the material of the first initial stress layer 250 includes: germanium silicon, and the first conductive type ions doped in the first initial stress layer 241 include: boron ions or BF 2+ ion.

[0080] The germanium in the silicon germanium material of the first initial stress layer 250 formed by the first epitaxial growth process has a first concentration.

[0081] The first concentration ranges from 10% to 25%.

[0082] In other embodiments, the semiconductor structure is used to form an NMOS transistor, and the material of the first initial stress layer includes: silicon carbide or silicon phosphide.

[0083] Please refer to Fig. 9 , an ion implantation process is performed on the first initial stress layer 250 to form an inversion doping region (not shown in the figure) in the first initial stress layer, wherein the inversion doping region is doped with second conductive type ions, and the conductive types of the second conductive type ions and the first conductive type ions are opposite.

[0084] The ion implantation process includes: an implantation energy range of 1KeV to 5KeV; an implantation dose range of 5e 13 atm / cm 2 ~5e 14 atm / cm 2 ; The injection angle is 0 degrees to 5 degrees.

[0085] Specifically, a portion of the first initial stress layer 250 exposed by the source / drain opening 240 is doped with ions of the second conductive type.

[0086] In this embodiment, the second conductive type ions include phosphorus ions, arsenic ions or antimony ions.

[0087] Please refer to Fig.10 A second initial stress layer 260 is formed on the surface of the first initial stress layer 250 , and the second initial stress layer 260 is doped with first conductive type ions.

[0088] The second initial stress layer 260 is formed by a second epitaxial growth process, and the second initial stress layer 260 is doped with first conductive type ions by an in-situ doping process.

[0089] In this embodiment, the semiconductor structure is used to form a PMOS transistor, the material of the first initial stress layer 250 includes: germanium silicon, and the first conductive type ions doped in the second initial stress layer 250 include: boron ions or BF 2+ ion.

[0090] In this embodiment, the semiconductor structure is used to form a PMOS transistor, the material of the first initial stress layer 250 includes: germanium silicon, and the first conductive type ions doped in the first initial stress layer 241 include: boron ions or BF 2+ ion.

[0091] The germanium in the germanium silicon material of the second initial stress layer 260 formed by the second epitaxial growth process has a second concentration, and the second concentration is greater than the first concentration.

[0092] The second concentration ranges from 35% to 60%.

[0093] In other embodiments, the semiconductor structure is used to form an NMOS transistor, and the material of the second initial stress layer includes: silicon carbide or silicon phosphide.

[0094] The first initial stress layer 250 forms a first stress structure after a subsequent process, and the second initial stress layer 260 forms a second stress structure after a subsequent process. Since the germanium in the germanium silicon material of the first initial stress layer 250 has a first concentration, and the silicon in the germanium silicon material of the second initial stress layer 260 has a second concentration, and the second concentration is greater than the first concentration, correspondingly, the germanium in the germanium silicon material of the first stress structure has a first concentration, and the germanium in the germanium silicon material of the second stress structure has a second concentration, and the first concentration is less than the second concentration. The first stress structure with a smaller concentration is conducive to making the interface defects between the first stress structure and the substrate smaller, thereby serving as a buffer layer between the substrate and the second stress structure, which is conducive to improving the interface reliability. The second stress structure with a larger concentration has a larger stress, which is conducive to improving the driving current of the device. In summary, the first stress structure and the second stress structure are conducive to improving the performance of the semiconductor structure.

[0095] Please refer to Fig.11 An annealing process is used to diffuse the second conductive type ions in the inversion doping region into the first initial stress layer 250 and the second initial stress layer 260. The ions diffuse into the first initial stress layer 250 to form a second stress layer 272, and the first initial stress layer 250 where no diffusion occurs forms a first stress layer 271. The ions diffuse into the second initial stress layer 260 to form a third stress layer 273, and the second initial stress layer 260 where no diffusion occurs forms a fourth stress layer 274.

[0096] The parameters of the annealing process include: an annealing temperature of 800 degrees Celsius to 950 degrees Celsius, and an annealing time of 30 seconds to 30 minutes.

[0097] After the annealing process, the first stress layer 271 and the second stress layer 272 located on the surface of the first stress layer 271 constitute a first stress structure (not shown), the first stress layer 271 is located on the side wall surface and the bottom surface of the source / drain opening 240, and the germanium in the germanium silicon material of the first stress structure has a first concentration; the third stress layer 273 and the fourth stress layer 274 located on the surface of the third stress layer 273 constitute a second stress structure (not shown), and the germanium in the germanium silicon material of the second stress structure has a second concentration, and the second concentration is greater than the first concentration.

[0098] The source-drain doping layer 270 includes a first stress structure and a second stress structure.

[0099] Through the annealing process, the second conductive type ions in the inversion doping region diffuse toward the first initial stress layer 250 and the second initial stress layer 260. The second conductive type ions diffused into the first initial stress layer 250 can neutralize part of the first conductive type ions, so that the concentration of carriers is small, which is beneficial to reduce the diffusion distance of carriers, thereby reducing the impact on the channel length. Similarly, the second conductive type ions diffused into the second initial stress layer 260 can neutralize part of the first conductive type ions, so that the concentration of carriers is small, which is beneficial to reduce the diffusion distance of carriers, thereby reducing the impact on the channel length.

[0100] Specifically, the high temperature of the annealing process can promote the diffusion of the second conductive type ions in the inversion doping region, that is, the second conductive type ions in the inversion doping region not only diffuse into the first initial stress layer 250 to form the second stress layer 272, the second stress layer 272 not only has the first conductive type ions, but also has the second conductive type ions, the second conductive type ions can neutralize part of the first conductive type ions, so that the concentration of carriers is small, which is conducive to reducing the diffusion distance of carriers, thereby reducing the impact on the channel length. At the same time, the second conductive type ions in the inversion doping region diffuse into the second initial stress layer 260 to form the third stress layer 273, the third stress layer 273 not only has the first conductive type ions, but also has the second conductive type ions, and the second conductive type ions can neutralize part of the first conductive type ions, so that the concentration of carriers is small, which is conducive to reducing the diffusion distance of carriers, thereby reducing the impact on the channel length.

[0101] Accordingly, the present invention also provides a semiconductor structure formed by the above method, please continue to refer to Fig.11 , including: a substrate 200, wherein the surface of the substrate 200 has a gate structure 210; source-drain openings 240 in the substrate 200 located on both sides of the gate structure 210, wherein the source-drain openings 240 include: a first region I and a second region II located on the first region I, and the sidewalls of the second region II are recessed relative to the sidewalls of the first region I; and a source-drain doping layer 270 located in the source-drain openings 240.

[0102] The source-drain opening 240 is formed by increasing the size of the first region I of the initial source-drain opening in a direction perpendicular to the sidewall surface of the gate structure 210, and the size of the first region I of the source-drain opening 240 is relatively large. The size of the first region I of the source-drain opening 240 is relatively large, and the volume of the source-drain doped layer 270 in the source-drain opening 240 is increased. The source-drain doped layer 270 with a larger volume has a larger stress, which is beneficial to improving the driving current of the formed device. At the same time, the size of the second region of the source-drain opening 240 remains unchanged, which is beneficial to ensure that the effective length of the channel located below the gate structure 210 is not affected. In summary, the semiconductor structure formed by the method has high performance.

[0103] The following is a detailed description with reference to the accompanying drawings.

[0104] In this embodiment, the base 200 includes a substrate 201 and a fin 202 located on the surface of the substrate 201 , and the gate structure 210 covers part of the top surface and sidewall surface of the fin 202 ; the source and drain openings 240 are located in the fin 202 on both sides of the gate structure 240 .

[0105] In this embodiment, the sidewall of the second region II of the source / drain opening 240 is recessed relative to the sidewall of the first region I. Specifically, the size of the bottom of the second region II of the source / drain opening 240 is smaller than the size of the top of the first region I of the source / drain opening 240 .

[0106] The size of the first region I of the source / drain opening 240 along a direction perpendicular to the sidewall surface of the gate structure 210 ranges from 50 nanometers to 130 nanometers.

[0107] The source-drain doping layer 270 includes: a first stress structure (not shown) located on the sidewall surface and top surface of the source-drain opening 240 ; a second stress structure (not shown) located on the surface of the first stress structure, and the second stress structure fills the source-drain opening 240 .

[0108] The material of the first stress structure includes: germanium silicon, in which germanium has a first concentration; the material of the second stress structure includes: germanium silicon, in which germanium has a second concentration, and the first concentration is less than the second concentration.

[0109] The first concentration ranges from 10% to 25%; the second concentration ranges from 35% to 60%.

[0110] The first stress structure includes: a first stress layer 271 located on the side wall surface and the top surface of the source-drain opening 240, and a second stress layer 272 located on the surface of the first stress layer 271; the second stress structure includes: a third stress layer 273 located on the surface of the second stress layer 272, and a fourth stress layer 274 located on the surface of the third stress layer 273, and the fourth stress layer 274 fills the source-drain opening 240.

[0111] The material of the first stress structure includes: germanium silicon, in which germanium has a first concentration; the material of the second stress structure includes: germanium silicon, in which germanium has a second concentration, and the first concentration is less than the second concentration. The first stress structure with a smaller concentration is conducive to making the interface defects between the first stress structure and the substrate 200 smaller, thereby serving as a buffer layer between the substrate 200 and the second stress structure, which is conducive to improving the interface reliability. The second stress structure with a larger concentration has a larger stress, which is conducive to improving the driving current of the device. In summary, the first stress structure and the second stress structure are conducive to improving the performance of the semiconductor structure.

[0112] The first stress layer 271 , the second stress layer 272 , the third stress layer 273 , and the fourth stress layer 274 are doped with first conductive type ions.

[0113] The first conductive type ions in the first stress layer 271 and the second stress layer 272 have a third concentration; the first conductive type ions in the third stress layer 273 and the fourth stress layer 274 have a fourth concentration, and the third concentration is less than the fourth concentration.

[0114] The second stress layer 272 and the third stress layer 273 are also doped with second conductive type ions; the second conductive type ions in the second stress layer 272 have a fifth concentration, and the fifth concentration is less than the third concentration; the second conductive type ions in the third stress layer 273 have a sixth concentration, and the sixth concentration is less than the third concentration.

[0115] The second stress layer 272 has ions of the first conductive type in it, and the second stress layer 272 has ions of the second conductive type, and the second conductive type ions can neutralize part of the first conductive type ions, so that the concentration of carriers is small, which is beneficial to reduce the diffusion distance of carriers, thereby reducing the impact on the channel length. Similarly, the third stress layer 273 has ions of the first conductive type in it, and the third stress layer 273 also has ions of the second conductive type in it, and the second conductive type ions can neutralize part of the first conductive type ions, so that the concentration of carriers is small, which is beneficial to reduce the diffusion distance of carriers, thereby reducing the impact on the channel length.

[0116] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A semiconductor structure, characterized in that: include: A substrate, wherein a surface of the substrate has a gate structure; Source and drain openings in the substrate located at both sides of the gate structure, the source and drain openings comprising: a first region and a second region located on the first region, and a sidewall of the second region is recessed relative to a sidewall of the first region; a source-drain doping layer located in the source-drain opening; The source-drain doping layer comprises: a first stress structure located on the sidewall surface and the top surface of the source-drain opening; a second stress structure located on the surface of the first stress structure, and the second stress structure fills the source-drain opening; The first stress structure comprises: a first stress layer located on the sidewall surface and the top surface of the source / drain opening, and a second stress layer located on the surface of the first stress layer; the second stress structure comprises: a third stress layer located on the surface of the second stress layer, and a fourth stress layer located on the surface of the third stress layer, wherein the fourth stress layer fills the source / drain opening; The second stress layer is doped with first conductive type ions; the first conductive type ions in the second stress layer have a third concentration; the second conductive type ions are also doped in the second stress layer and the third stress layer; the second conductive type ions in the second stress layer have a fifth concentration, and the fifth concentration is less than the third concentration; the second conductive type ions in the third stress layer have a sixth concentration, and the sixth concentration is less than the third concentration.

2. The semiconductor structure according to claim 1, wherein: The size of the first region of the source / drain opening in a direction perpendicular to the sidewall surface of the gate structure ranges from 50 nanometers to 130 nanometers.

3. The semiconductor structure according to claim 1, wherein: The material of the first stress structure includes: germanium silicon, in which germanium has a first concentration; the material of the second stress structure includes: germanium silicon, in which germanium has a second concentration, and the first concentration is less than the second concentration.

4. The semiconductor structure according to claim 3, characterized in that The first concentration ranges from 10% to 25%; the second concentration ranges from 35% to 60%.

5. The semiconductor structure according to claim 1, wherein: The first stress layer, the third stress layer and the fourth stress layer are doped with first conductive type ions.

6. The semiconductor structure according to claim 5, characterized in that The first conductive type ions in the first stress layer have a third concentration; the first conductive type ions in the third stress layer and the fourth stress layer have a fourth concentration, and the third concentration is less than the fourth concentration.

7. The semiconductor structure according to any one of claims 1 to 6, characterized in that: The base comprises a substrate and a fin located on the surface of the substrate, the gate structure covers a portion of the top surface and the sidewall surface of the fin; the source and drain openings are located in the fins on both sides of the gate structure.

8. A method for forming a semiconductor structure according to any one of claims 1 to 7, characterized in that: include: Providing a substrate, wherein a surface of the substrate has a gate structure; forming initial source-drain openings in the substrate at both sides of the gate structure, the initial source-drain openings comprising: a first region and a second region located on the first region; Enlarging the dimension of the first region of the initial source / drain opening in a direction perpendicular to the sidewall surface of the gate structure to form a source / drain opening; forming a source-drain doping layer in the source-drain opening; The method for forming the source-drain doping layer comprises: forming the first stress structure on the sidewall surface and the bottom surface of the source-drain opening; and forming the second stress structure on the surface of the first stress structure.

9. The method for forming a semiconductor structure according to claim 8, wherein: The method for forming the initial source-drain openings includes: using the gate structure as a mask, etching the substrate, and forming initial source-drain openings in the substrate.

10. The method for forming a semiconductor structure according to claim 8, wherein: The method for increasing the size of the first area of ​​the initial source and drain opening in a direction perpendicular to the side wall surface of the gate structure includes: amorphizing the substrate exposed by the first area of ​​the initial source and drain opening to form an amorphized layer on the side walls and bottom of the first area of ​​the initial source and drain opening; and removing the amorphized layer to form the source and drain opening from the initial source and drain opening.

11. The method for forming a semiconductor structure according to claim 10, wherein: The amorphization treatment process includes: an ion implantation process; the parameters of the ion implantation process include: an implantation angle range of 5 degrees to 25 degrees, the implanted ions include: boron ions and nitrogen ions, or boron ions and germanium ions, the implantation angle is the angle between the ion implantation direction and a reference plane, and the reference plane is a plane perpendicular to the substrate surface and parallel to the channel width direction.

12. The method for forming a semiconductor structure according to claim 10, wherein: The process of removing the amorphous layer includes: a dry etching process or a wet etching process, or a combination of the two.

13. The method for forming a semiconductor structure according to claim 10, wherein: The base comprises a substrate and a fin located on the surface of the substrate; The method for forming the initial source and drain openings includes: using the gate structure as a mask, etching the fins until the substrate surface is exposed, and forming the initial source and drain openings in the fins on both sides of the gate structure.

14. The method for forming a semiconductor structure according to claim 8, wherein: The method for forming the first stress layer, the second stress layer, the third stress layer and the fourth stress layer includes: forming a first initial stress layer on the side wall surface and the bottom surface of the source and drain opening, wherein the first initial stress layer is doped with first conductive type ions; performing an ion implantation process on the first initial stress layer to form an inversion doping region in the first initial stress layer, wherein the inversion doping region is doped with second conductive type ions, and the conductive types of the second conductive type ions and the first conductive type ions are opposite; forming a second initial stress layer on the surface of the first initial stress layer, wherein the second initial stress layer is doped with first conductive type ions; and using an annealing process to diffuse the second conductive type ions in the inversion doping region toward the first initial stress layer and the second initial stress layer, wherein the ions diffuse into the first initial stress layer to form the second stress layer, and the first initial stress layer where no diffusion occurs forms the second stress layer, wherein the ions diffuse into the second initial stress layer to form the third stress layer, and the second initial stress layer where no diffusion occurs forms the fourth stress layer.

15. The method for forming a semiconductor structure according to claim 14, wherein: The first initial stress layer is formed by a first epitaxial growth process, and the first conductive type ions are doped into the first initial stress layer by an in-situ doping process; the second initial stress layer is formed by a second epitaxial growth process, and the first conductive type ions are doped into the second initial stress layer by an in-situ doping process.

16. The method for forming a semiconductor structure according to claim 14, wherein: The ion implantation process includes: an implantation energy range of 1KeV to 5KeV; an implantation dose range of 5e 13 atm / cm 2 ~5e 14 atm / cm 2 ; The injection angle is 0 degrees to 5 degrees; the parameters of the annealing process include: the annealing temperature is 800 degrees Celsius to 950 degrees Celsius, and the annealing time is 30 seconds to 30 minutes.