Method for forming semiconductor device
By forming an opening and side wall layer on the layer to be etched of the fin field effect transistor and forming a cutting layer inside and outside it, the complex patterning operation in the prior art is solved, efficiency is improved and adapted to the needs of diversified processes .
Patent Information
- Application Number
- CN202010211643.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-03-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-03-24
AI Technical Summary
In the rear-stage process of fin field effect transistors, the existing patterned first mask layer method is complex to operate, reducing working efficiency.
By forming a plurality of openings on the layer to be etched and depositing a side wall layer on its side walls, a cutting layer is formed to simplify the patterning operation of the mask layer, reduce process steps and improve efficiency.
The process operation steps are simplified, work efficiency is improved, and the cutting layer size is allowed to be adjusted as needed to meet diverse process needs.
Smart Images

Figure CN113451131B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for forming a semiconductor device. Background Art
[0002] The traditional planar field-effect transistor has a weak ability to control the channel current, which has led to the emergence of a new complementary metal-oxide semiconductor transistor - the Fin Field-Effect Transistor (FinFET).
[0003] In a self-aligned double patterning (SADP) process of a back end of line (BEOL) manufacturing process of a fin field effect transistor, a first mask layer on a semiconductor substrate needs to be patterned.
[0004] However, the existing method for patterning the first mask layer has the problem of complex operation, which reduces the working efficiency. Summary of the invention
[0005] The technical problem solved by the present invention is how to simplify the patterning operation of the first mask layer and improve work efficiency.
[0006] In order to solve the above technical problems, an embodiment of the present invention provides a method for forming a semiconductor device, the method comprising:
[0007] Providing a layer to be etched;
[0008] forming a first mask layer on the layer to be etched;
[0009] forming a plurality of first openings extending along a first direction in the first mask layer;
[0010] forming a sidewall layer on the sidewall of the first opening;
[0011] After forming the spacer layer, forming a second opening extending along the first direction in the first mask layer between adjacent first openings;
[0012] A first cutting layer is formed in the first opening to cut the first opening along a second direction. In the process of forming the first cutting layer, a second cutting layer is formed in the second opening to cut the second opening along the second direction. The second direction is perpendicular to the first direction.
[0013] Optionally, before forming the first mask layer on the layer to be etched, it also includes: forming a second mask layer on the layer to be etched; the first mask layer is located on the second mask layer; after forming the first cutting layer and the second cutting layer, etching the second mask layer with the first mask layer, the side wall layer, the first cutting layer and the second cutting layer as masks, forming a third opening in the second mask layer at the bottom of the first opening, and forming a fourth opening in the second mask layer at the bottom of the second opening; after forming the third opening and the fourth opening in the second mask layer, removing the first mask layer, the side wall layer, the first cutting layer and the second cutting layer.
[0014] Optionally, the step of forming the first opening includes: forming a patterned third mask layer on the first mask layer; etching the first mask layer using the patterned third mask layer as a mask to form the first opening; after forming the first opening, removing the third mask layer.
[0015] Optionally, before forming the patterned third mask layer, it also includes: forming a first SOC layer and a first Si-ARC layer in sequence on the first mask layer; in the process of forming the first opening, etching the first Si-ARC layer, the first SOC layer and the first mask layer in sequence using the patterned third mask layer as a mask.
[0016] Optionally, the process of etching the first mask layer using the patterned third mask layer as a mask is a first plasma dry etching process, and an etching angle of the first plasma dry etching process is 90 degrees.
[0017] Optionally, during the process of forming the first opening, an etching selectivity ratio between the first mask layer and the second mask layer is greater than or equal to 100.
[0018] Optionally, the step of forming the sidewall layer includes: depositing a sidewall material layer on the top surface of the first mask layer, the sidewall and the bottom of the first opening; etching back the sidewall material layer to remove the sidewall material layer on the top surface of the first mask layer and the bottom of the first opening, and forming a sidewall layer located on the sidewall of the first opening.
[0019] Optionally, the material of the spacer layer includes titanium oxide.
[0020] Optionally, the process for forming the spacer material layer includes an atomic layer deposition process.
[0021] Optionally, the thickness of the sidewall layer is 100 angstroms to 150 angstroms.
[0022] Optionally, the step of forming the second opening includes: forming a patterned fourth mask layer on the first mask layer; etching the first mask layer between adjacent first openings using the patterned fourth mask layer as a mask to form the second opening, wherein the sidewall of the second opening exposes the sidewall layer; after forming the second opening, removing the fourth mask layer.
[0023] Optionally, before forming the patterned fourth mask layer, the method also includes: forming a second SOC layer and a second Si-ARC layer in sequence on the first mask layer; and in the process of forming the second opening, etching the second Si-ARC layer, the second SOC layer and the first mask layer in sequence using the patterned fourth mask layer as a mask.
[0024] Optionally, the process of etching the first mask layer between adjacent first openings using the patterned fourth mask layer as a mask is a second plasma dry etching process, and an etching angle of the second plasma dry etching process is 90 degrees.
[0025] Optionally, in the process of forming the second opening, an etching selectivity ratio between the first mask layer and the second mask layer is greater than or equal to 100, and an etching selectivity ratio between the first mask layer and the sidewall layer is greater than or equal to 20.
[0026] Optionally, the step of forming the first cutting layer and the second cutting layer includes: forming a sacrificial material layer covering the first mask layer, the first opening, the side wall layer and the second opening; flattening the sacrificial material layer until the top surface of the first mask layer and the top surface of the side wall are exposed to form a sacrificial layer filled in the first opening and the second opening; forming a first cutting groove located in the first opening and a second cutting groove located in the second opening in the sacrificial layer; forming a cutting material layer covering the first mask layer, the side wall layer, the sacrificial layer and filling the first cutting groove and the second cutting groove; removing the cutting material layer on the top surface of the first mask layer, the top surface of the sacrificial layer and part of the top surface of the side wall layer to form the first cutting layer and the second cutting layer; removing the sacrificial layer.
[0027] Optionally, the process of forming the first cutting layer and the second cutting layer is a third plasma dry etching process.
[0028] Optionally, the material of the cutting material layer includes low temperature oxide.
[0029] Optionally, for adjacent first openings and second openings, the first cutting layer located in the first opening and the second cutting layer located in the second opening are separated from each other in the first direction.
[0030] Optionally, a size of the first cutting layer in the first direction is 20 nanometers to 30 nanometers; a size of the second cutting layer in the first direction is 20 nanometers to 30 nanometers.
[0031] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:
[0032] In the above scheme, while forming the first cutting layer in the first opening in the first mask layer, the second cutting layer is formed in the second opening. Compared with the existing method of forming the first cutting layer and the second cutting layer in two steps, the process operation steps can be simplified and the work efficiency can be improved. In addition, when forming the second cutting layer, the size of the second cutting layer in the first direction can be adjusted according to actual needs, and then the distance from the head to the head of the second opening after cutting can be adjusted to meet diverse process requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a schematic flow chart of a method for forming a semiconductor device according to an embodiment of the present invention;
[0034] Figures 2 to 9 It is a schematic diagram of intermediate structures corresponding to each step of a method for forming a semiconductor device according to an embodiment of the present invention. DETAILED DESCRIPTION
[0035] As mentioned in the background technology, in the existing self-aligned double patterning (SADP) process of the back end of line (BEOL) of the fin field effect transistor, the segmentation operation of the first opening and the second opening in the first mask layer needs to be performed separately in two steps, which has the problem of complex operation and reduces work efficiency.
[0036] The technical solution in the embodiment of the present invention forms the first cutting layer in the first opening in the first mask layer and forms the second cutting layer in the second opening at the same time. Compared with the existing method of forming the first cutting layer and the second cutting layer separately in two processes, the process operation steps can be simplified and the work efficiency can be improved. In addition, when forming the second cutting layer, the size of the second cutting layer in the first direction can be adjusted according to actual needs, and then the distance from the end of the second opening after cutting can be adjusted to meet diverse process requirements.
[0037] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0038] Figure 1 1 is a schematic diagram of a method for forming a semiconductor device according to an embodiment of the present invention. Figure 1A method for forming a semiconductor device in an embodiment of the present invention may specifically include the following steps:
[0039] Step S101: providing a layer to be etched;
[0040] Step S102: forming a first mask layer on the layer to be etched;
[0041] Step S103: forming a plurality of first openings extending along a first direction in the first mask layer;
[0042] Step S104: forming a sidewall layer on the sidewall of the first opening;
[0043] Step S105: after forming the spacer layer, forming a second opening extending along the first direction in the first mask layer between adjacent first openings;
[0044] Step S106: forming a first cutting layer in the first opening for cutting the first opening along a second direction, and in the process of forming the first cutting layer, forming a second cutting layer in the second opening for cutting the second opening along the second direction; the second direction is perpendicular to the first direction.
[0045] The following will be combined Figures 2 to 9 A method for forming a semiconductor device in an embodiment of the present invention is described in further detail.
[0046] See also Figure 2 , providing a substrate, on which a layer 100 to be etched is formed.
[0047] In a specific implementation, the substrate provides a process platform for subsequently forming a fin field effect transistor. The fin field effect transistor may be an NMOS transistor or a PMOS transistor.
[0048] In a specific implementation, the substrate may be a silicon substrate or a germanium substrate, etc. In addition, other devices may be formed in the substrate, such as a PMOS transistor, an NMOS transistor, etc.; an isolation structure may also be formed in the substrate, and the isolation structure may be a shallow trench isolation (STI) structure or a local oxide of silicon (LOCOS) isolation structure. Similarly, a conductive member may also be formed in the substrate, and the conductive member may be a gate, source or drain of a transistor, or a metal interconnect structure electrically connected to the transistor, etc.
[0049] In the embodiment of the present invention, the layer to be etched 100 is a multi-layer structure, including a first etch stop layer, an interlayer dielectric layer located on the first etch stop layer, a second etch stop layer located on the interlayer dielectric layer, and an underlying hard mask layer located on the second etch stop layer. In this embodiment, the material of the first etch stop layer is aluminum nitride, the material of the interlayer dielectric layer is black diamond (BD) or a low-K dielectric material, the material of the second etch stop layer is silicon oxycarbide (SiOC), and the material of the underlying hard mask layer includes titanium nitride (TiN).
[0050] See also Figure 3 , a second mask layer 110 and a first mask layer 120 located on the second mask layer 110 are sequentially formed on the layer to be etched 100 .
[0051] In this embodiment, the second mask layer 110 is located on the bottom hard mask layer.
[0052] The second mask layer 110 is used to form a third opening and a fourth opening therein by etching later.
[0053] The first mask layer 120 is used as an etching mask for subsequently etching the second mask layer 110 .
[0054] The material of the first mask layer 120 includes: amorphous silicon.
[0055] The material of the second mask layer 110 includes silicon oxide or SiOC. The second mask layer 110 can also increase the adhesion between the underlying hard mask layer and the first mask layer 120 .
[0056] The second etch stop layer can also increase the adhesion between the underlying hard mask layer and the interlayer dielectric layer.
[0057] See also Figure 4 , the first mask layer 120 is etched to form a plurality of first openings 121 extending along a first direction in the first mask layer 120 , and the bottoms of the first openings 121 expose the material of the second mask layer 110 .
[0058] In a specific implementation, the first opening 121 is used to define the position and width of a third opening subsequently formed in the first mask layer.
[0059] In a specific implementation, the step of forming the first opening may include: forming a first SOC layer, a first Si-ARC layer and a third mask layer on the first mask layer in sequence; performing a photolithography process on the third mask layer using a mask plate to form a patterned third mask layer, wherein the patterned third mask layer has a pattern defining a plurality of openings extending along a first direction; etching the first Si-ARC layer, the first SOC layer and the first mask layer 120 in sequence using the patterned third mask layer as a mask until the top surface of the second mask layer 110 is exposed, and forming a plurality of first openings 121 extending along the first direction in the first mask layer 120; and then removing the first SOC layer, the first Si-ARC layer and the third mask layer. In this embodiment, the process of etching the first mask layer using the patterned third mask layer as a mask is a first plasma dry etching process, and the etching angle of the first plasma dry etching process is 90 degrees.
[0060] In order to retain the second mask layer 110 in the step of forming the first opening 121, the etching selectivity rate of the second mask layer 110 should be lower than the etching selectivity rate of the first mask layer 120. In the embodiment of the present invention, in the process of etching the first mask layer 120 to form the first opening 121, the etching selectivity ratio of the first mask layer to the second mask layer is greater than or equal to 100, such as 150, 200, etc.
[0061] In this embodiment, the material of the third mask layer is photoresist.
[0062] See also Figure 5 , a spacer layer 130 is formed on the sidewall of the first opening 121 .
[0063] The spacer layer 130 is used to define the spacing distance between the first opening and the second opening formed subsequently in a second direction; the second direction is perpendicular to the first direction. The spacer layer 130 separates the first opening from the second opening.
[0064] In a specific implementation, the sidewall layer may be made of a material having a higher etching selectivity rate relative to the second hard mask layer. In an embodiment of the present invention, the material of the sidewall layer includes titanium oxide. In other embodiments, the material of the sidewall layer may also be AlO, AlN, AlON, TaN, SiO, or SiN, or other materials such as nitrides, oxides, oxynitrides, carbides, borides, and combinations thereof.
[0065] The step of forming the sidewall layer may include: depositing a sidewall material layer on the top surface of the second mask layer and the sidewall and bottom of the first opening; etching back the sidewall material layer to remove the sidewall material layer above the top surface of the first mask layer and the bottom surface of the first opening, thereby forming a sidewall layer located on the sidewall of the first opening.
[0066] The process for forming the spacer material layer is a deposition process, such as an atomic layer deposition process.
[0067] In a specific implementation, the size of the spacer layer in the second direction can be determined according to the spacing distance between the first opening formed subsequently and the second opening formed subsequently in the second direction, that is, according to the spacing distance between the first metal line and the second metal line formed subsequently in the interlayer dielectric layer of the to-be-etched layer 100 in the second direction. In the embodiment of the present invention, the thickness of the spacer layer is 100 angstroms to 150 angstroms.
[0068] See also Figure 6 After forming the spacer layer 130 , a second opening 122 extending along the first direction is formed in the first mask layer 120 between adjacent first openings 121 .
[0069] In this embodiment, the bottom of the second opening 122 exposes the material of the second mask layer 110 .
[0070] The second opening is used to define a position of a fourth opening subsequently formed in the second mask layer.
[0071] The step of forming the second opening may include: forming a second SOC layer, a second Si-ARC layer, and a patterned fourth mask layer on the first hard mask layer; using the patterned fourth mask layer as a mask, sequentially etching the second Si-ARC layer, the second SOC layer, and the first mask layer between adjacent first openings, and forming a second opening 122 extending along the first direction in the first mask layer between adjacent first openings 121; after forming the second opening 122, removing the second SOC layer, the second Si-ARC layer, and the patterned fourth mask layer. In this embodiment, the process of sequentially etching the second Si-ARC layer, the second SOC layer, and the first mask layer using the patterned fourth mask layer as a mask is a second plasma dry etching process, and the etching angle of the second plasma dry etching process is 90 degrees.
[0072] In a specific implementation, the positions, sizes, and numbers of the first openings 121 and the second openings 122 can be determined according to actual process requirements. In this embodiment, the numbers of the first openings 121 and the second openings 122 are 3 and 2, respectively.
[0073] In order to retain the second mask layer 110 and the sidewall 130 in the step of forming the second opening 122, the etching rate of the first mask layer 120 should be greater than the etching rate of the second mask layer 110 and the sidewall 130. In the embodiment of the present invention, in the process of etching the first mask layer to form the second opening 122, the etching selectivity ratio of the first mask layer to the second mask layer is greater than or equal to 100, such as 150, 200, etc., and the etching selectivity ratio of the first mask layer to the sidewall layer is greater than or equal to 20, such as 50, 100, etc.
[0074] See also Figure 7 A first cutting layer 141 is formed in the first opening 121 for cutting the first opening 121 along a second direction. In the process of forming the first cutting layer 141, a second cutting layer 142 is formed in the second opening 122 for cutting the second opening 122 along the second direction; the second direction is perpendicular to the first direction.
[0075] For the adjacent first opening 121 and second opening 122 , the first cutting layer 141 located in the first opening 121 and the second cutting layer 142 located in the second opening 122 are separated from each other in the first direction.
[0076] The first cutting layer 141 is used to define the segmentation position and size of the third opening subsequently formed in the second mask layer 110 ; the second cutting layer 142 is used to define the segmentation position and size of the fourth opening subsequently formed in the second mask layer 110 .
[0077] In this embodiment, the materials of the first cutting layer 141 and the second cutting layer 142 are low temperature oxide (LTO).
[0078] The steps of forming a first cutting layer 141 and a second cutting layer 142 may include: forming a sacrificial material layer covering the first mask layer 120, the first opening 121, the sidewall layer 130 and the second opening 122; flattening the sacrificial material layer until the top surface of the first mask layer 120 and the top surface of the sidewall layer 130 are exposed to form a sacrificial layer filled in the first opening 121 and the second opening 122; forming a first cutting groove in the first opening 121 and a second cutting groove in the second opening 122 in the sacrificial layer 122, the first cutting groove and the second cutting groove in adjacent sacrificial layers being separated from each other in a first direction; forming a first cutting layer 141 in the first cutting groove, and forming a second cutting layer 142 in the second cutting groove.
[0079] The sacrificial material layer provides a process basis for subsequently forming a first cutting groove in the first opening and a second cutting groove in the second opening.
[0080] The process of forming the sacrificial material layer includes chemical vapor deposition, physical vapor deposition and atomic layer deposition.
[0081] The first cutting groove is used to define a process position of a first cutting layer 141 subsequently formed in the first opening 121 ; the second cutting groove is used to define a process position of a second cutting layer 142 subsequently formed in the second opening 122 .
[0082] The steps of forming the first cutting groove 141 and the second cutting groove 142 may include: forming a third SOC layer, a third Si-ARC layer and a patterned fifth mask layer in sequence on the upper surfaces of the first mask layer 120, the sidewall layer 130 and the sacrificial layer; the patterned fifth mask layer has a pattern defining the first cutting groove and the second cutting groove; etching the third SOC layer, the third Si-ARC layer and the sacrificial layer in sequence using the patterned fifth mask layer as a mask until the top surface of the first mask layer is exposed, and forming a first cutting groove located in the first opening 121 and a second cutting groove located in the second opening 122 in the sacrificial layer; after forming the first cutting groove and the second cutting groove, removing the patterned third mask layer, the third SOC layer and the third Si-ARC layer.
[0083] The subsequent steps also include the step of removing the sacrificial layer. In order to retain the first mask layer 120, the side wall layer 130, the first cutting layer 141 and the second cutting layer 142 in the step of removing the sacrificial layer, the etching rate of the sacrificial layer should be greater than the etching rate of the first mask layer 120, the side wall layer 130, the first cutting layer 141 and the second cutting layer 142, respectively.
[0084] The method for forming the first cutting layer 141 and the second cutting layer 142 may include: forming a cutting material layer covering the first mask layer 120, the sidewall layer 130, the sacrificial layer and filling the first cutting groove and the second cutting groove; etching back the cutting material layer to remove the top surface of the first mask layer 120, the top surface of the sacrificial layer and then part of the cutting material layer on the top surface of the sidewall layer to form the first cutting layer 141 and the second cutting layer 142, wherein the first cutting layer 141 also extends along the second direction to the sidewall layers on both sides of the first cutting groove, and the second cutting layer 142 also extends along the second direction to the sidewall layers on both sides of the second cutting groove.
[0085] In this embodiment, the first cutting layer 141 extends along the second direction to the sidewall layers on both sides of the first cutting groove, but the first cutting layer 141 does not extend into the adjacent second opening, and the first cutting layer 141 does not cut the second opening.
[0086] In this embodiment, the second cutting layer 142 also extends along the second direction to the sidewall layers on both sides of the second cutting groove, but the second cutting layer 142 does not extend into the adjacent first opening, and the second cutting layer 142 does not cut the first opening.
[0087] Since the first cutting layer 141 extends along the second direction to the sidewall layers on both sides of the first cutting groove, the size of the first cutting layer 141 in the second direction increases, so that while limiting the first cutting layer 141 to have a smaller size in the first direction, the restriction on the size of the first cutting layer 141 in the second direction is reduced. Therefore, the difficulty of forming the first cutting layer 141 is reduced.
[0088] Since the second cutting layer 142 also extends along the second direction to the sidewall layers on both sides of the second cutting groove, the size of the second cutting layer 142 in the second direction increases, so that while limiting the second cutting layer 142 to have a smaller size in the first direction, the restriction on the size of the second cutting layer 142 in the second direction is reduced. Therefore, the difficulty of forming the second cutting layer 142 is reduced.
[0089] In one embodiment, the size of the first cutting layer 141 in the first direction is 20 nanometers to 30 nanometers, such as 26 nanometers.
[0090] In one embodiment, the size of the second cutting layer 142 in the first direction is 20 nanometers to 30 nanometers, such as 26 nanometers.
[0091] A size of the first cutting layer 141 in the first direction is the same as or different from a size of the second cutting layer 142 in the first direction.
[0092] The process of forming the cutting material layer includes a deposition process, such as a plasma chemical vapor deposition process, a low pressure chemical vapor deposition process or an atomic layer deposition process.
[0093] In the embodiment of the present invention, after forming the first cutting layer and the second cutting layer, a step of removing the sacrificial layer is further included. In this embodiment, the sacrificial layer in the first opening and the second opening is etched away using a third plasma dry etching process.
[0094] See also Figure 8 The second mask layer 110 is etched using the first mask layer 120, the sidewall layer 130, the first cutting layer 141 and the second cutting layer 142 as masks to form a third opening 111 in the second mask layer 110 at the bottom of the first opening, and a fourth opening 112 in the second mask layer at the bottom of the second opening.
[0095] Due to the existence of the first cutting layer 141 and the second cutting layer, the second mask layer 110 under the first cutting layer 141 and the second cutting layer 142 is retained, so that the third opening 111 and the fourth opening 112 are respectively divided by the second mask layer 110 retained under the first cutting layer and the second cutting layer.
[0096] See also Fig. 9 After forming the third opening 111 and the fourth opening 112 , the first cutting layer 141 , the second cutting layer 142 , the spacer layer 130 , and the first mask layer 120 are removed.
[0097] In a specific implementation, the process of removing the first cutting layer 141 and the second cutting layer 142 , the spacer layer 130 and the first mask layer 120 includes a dry etching process and a wet etching process.
[0098] In order to retain the layer to be etched 100, in the process of removing the first cutting layer 141 and the second cutting layer 142, the spacer layer 130 and the first mask layer 120, the etching rate of the layer to be etched 100 should be respectively lower than the etching rates of the first cutting layer 141 and the second cutting layer 142, the spacer layer 130 and the first mask layer 120. The material of the layer to be etched 100 should be selected to have an etching selectivity rate lower than the etching selectivity rates of the first cutting layer 141 and the second cutting layer 142, the spacer layer 130 and the first mask layer 120.
[0099] In an embodiment of the present invention, the first cutting layer 141 and the second cutting layer 142, the sidewall layer 130 and the first mask layer 120 are removed, so that the third opening and the fourth opening patterns formed in the second mask layer are continuously transferred downward to the interlayer dielectric layer in the layer to be etched 100, corresponding openings are formed in the interlayer dielectric layer, and metal materials are filled in the corresponding openings formed in the interlayer dielectric layer to form corresponding multiple conductive layers.
[0100] Specifically, in this embodiment, the second mask layer is used as a mask to etch the layer 100 to be etched at the bottom of the third opening and the fourth opening, and a first intermediate opening is formed in the underlying hard mask layer at the bottom of the third opening, and a second intermediate opening is formed in the underlying hard mask layer at the bottom of the fourth opening; then, the second mask layer is removed; then, the second etching stop layer and the interlayer dielectric layer at the bottom of the first intermediate opening and the second intermediate opening are etched using the underlying hard mask layer as a mask, and a first interconnect opening is formed in the interlayer dielectric layer at the bottom of the first intermediate opening, and a second interconnect opening is formed in the interlayer dielectric layer at the bottom of the second intermediate opening; a first conductive layer is formed in the first interconnect opening; and a second conductive layer is formed in the second interconnect opening.
[0101] In one embodiment, the second conductive layer is formed during the process of forming the first conductive layer, thereby simplifying the process.
[0102] By adopting the above scheme in the implementation of the present invention, by forming the first cutting layer in the first opening in the first mask layer and forming the second cutting layer in the second opening at the same time, the process operation steps can be simplified and the work efficiency can be improved compared with the existing two processes of forming the first cutting layer and the second cutting layer respectively. In addition, when forming the second cutting layer, the size of the second cutting layer in the first direction can be adjusted according to actual needs, and then the distance from the end of the second opening after cutting can be adjusted to meet diverse process requirements.
[0103] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor device, characterized in that: include: Providing a layer to be etched; forming a first mask layer on the layer to be etched; forming a plurality of first openings extending along a first direction in the first mask layer; forming a sidewall layer on the sidewall of the first opening; After forming the spacer layer, forming a second opening extending along the first direction in the first mask layer between adjacent first openings; forming a first cutting layer in the first opening for cutting the first opening along a second direction, and forming a second cutting layer in the second opening for cutting the second opening along the second direction during the process of forming the first cutting layer; The second direction is perpendicular to the first direction; The steps of forming the first cutting layer and the second cutting layer include: forming a sacrificial material layer covering the first mask layer, the first opening, the sidewall layer and the second opening; planarizing the sacrificial material layer until the top surface of the first mask layer and the top surface of the sidewall are exposed, so as to form a sacrificial layer filled in the first opening and the second opening; forming a first cutting groove located in the first opening and a second cutting groove located in the second opening in the sacrificial layer; forming a cutting material layer covering the first mask layer, the sidewall layer, the sacrificial layer and filling the first cutting groove and the second cutting groove; Removing the cutting material layer on the top surface of the first mask layer, the top surface of the sacrificial layer and a portion of the top surface of the spacer layer to form the first cutting layer and the second cutting layer; The sacrificial layer is removed.
2. The method for forming a semiconductor device according to claim 1, wherein: Before forming the first mask layer on the layer to be etched, it also includes: forming a second mask layer on the layer to be etched; the first mask layer is located on the second mask layer; after forming the first cutting layer and the second cutting layer, etching the second mask layer with the first mask layer, the side wall layer, the first cutting layer and the second cutting layer as masks, forming a third opening in the second mask layer at the bottom of the first opening, and forming a fourth opening in the second mask layer at the bottom of the second opening; after forming the third opening and the fourth opening in the second mask layer, removing the first mask layer, the side wall layer, the first cutting layer and the second cutting layer.
3. The method for forming a semiconductor device according to claim 1, wherein: The step of forming the first opening comprises: forming a patterned third mask layer on the first mask layer; Using the patterned third mask layer as a mask, etching the first mask layer to form the first opening; After forming the first opening, the third mask layer is removed.
4. The method for forming a semiconductor device according to claim 3, wherein: Before forming the patterned third mask layer, it also includes: forming a first SOC layer and a first Si-ARC layer in sequence on the first mask layer; in the process of forming the first opening, etching the first Si-ARC layer, the first SOC layer and the first mask layer in sequence using the patterned third mask layer as a mask.
5. The method for forming a semiconductor device according to claim 3, wherein: The process of etching the first mask layer using the patterned third mask layer as a mask is a first plasma dry etching process, and the etching angle of the first plasma dry etching process is 90 degrees.
6. The method for forming a semiconductor device according to claim 2, wherein: In the process of forming the first opening, an etching selection ratio of the first mask layer to the second mask layer is greater than or equal to 100.
7. The method for forming a semiconductor device according to claim 1, wherein: The steps of forming the sidewall layer include: Depositing a spacer material layer on a top surface of the first mask layer, and on a sidewall and a bottom of the first opening; The sidewall material layer is etched back to remove the top surface of the first mask layer and the sidewall material layer at the bottom of the first opening, so as to form a sidewall layer located on the sidewall of the first opening.
8. The method for forming a semiconductor device according to claim 1, wherein: The material of the spacer layer includes titanium oxide.
9. The method for forming a semiconductor device according to claim 7, wherein: The process for forming the spacer material layer includes an atomic layer deposition process.
10. The method for forming a semiconductor device according to claim 1, wherein: The thickness of the sidewall layer is 100 angstroms to 150 angstroms.
11. The method for forming a semiconductor device according to claim 1, wherein: The step of forming the second opening comprises: forming a patterned fourth mask layer on the first mask layer; Using the patterned fourth mask layer as a mask, etching the first mask layer between adjacent first openings to form the second openings, wherein the sidewalls of the second openings expose the spacer layer; After forming the second opening, the fourth mask layer is removed.
12. The method for forming a semiconductor device according to claim 11, wherein: Before forming the patterned fourth mask layer, it also includes: forming a second SOC layer and a second Si-ARC layer in sequence on the first mask layer; in the process of forming the second opening, etching the second Si-ARC layer, the second SOC layer and the first mask layer in sequence using the patterned fourth mask layer as a mask.
13. The method for forming a semiconductor device according to claim 11, wherein: The process of etching the first mask layer between adjacent first openings using the patterned fourth mask layer as a mask is a second plasma dry etching process, and the etching angle of the second plasma dry etching process is 90 degrees.
14. The method for forming a semiconductor device according to claim 2, wherein: In the process of forming the second opening, an etching selectivity ratio between the first mask layer and the second mask layer is greater than or equal to 100, and an etching selectivity ratio between the first mask layer and the sidewall layer is greater than or equal to 20.
15. The method for forming a semiconductor device according to claim 1, wherein: The process of forming the first cutting layer and the second cutting layer is a third plasma dry etching process.
16. The method for forming a semiconductor device according to claim 1, wherein: The material of the cutting material layer includes low temperature oxide.
17. The method for forming a semiconductor device according to claim 1, wherein: For the adjacent first opening and the second opening, the first cutting layer located in the first opening and the second cutting layer located in the second opening are separated from each other in the first direction.
18. The method for forming a semiconductor device according to claim 1, wherein: The size of the first cutting layer in the first direction is 20 nanometers to 30 nanometers; the size of the second cutting layer in the first direction is 20 nanometers to 30 nanometers.