Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element

By using a liquid crystal aligning agent containing an oxazoline skeleton polymer and a diamine, the problem of mechanical strength and residual image characteristics of the liquid crystal alignment film in the liquid crystal display is solved, and high mechanical strength and excellent residual image performance are achieved.

CN113474725BActive Publication Date: 2024-10-29NISSAN CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202080016622.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-02-26
Publication Date
2024-10-29
Estimated Expiration
2040-02-26

AI Technical Summary

Technical Problem

In the current manufacturing of liquid crystal displays, it is difficult for the liquid crystal alignment film to meet the requirements for mechanical strength and other properties at the same time. In particular, the afterimage properties are poor under long-term AC driving under a lateral electric field.

Method used

A liquid crystal aligning agent containing a specific polymer (A) and a polymer (B) is used, wherein the polymer (A) is obtained by reacting a diamine with an oxazoline skeleton and a tetracarboxylic acid derivative, and the polymer (B) is obtained by a specific Diamine is formed by reacting with tetracarboxylic acid derivatives. Combining these compounds can improve the mechanical strength of the liquid crystal alignment film and its performance under a lateral electric field.

Benefits of technology

It achieves high mechanical strength of the liquid crystal alignment film and excellent afterimage characteristics under long-term AC driving, and reduces display defects and afterimage problems of liquid crystal display elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113474725B_ABST
    Figure CN113474725B_ABST
Patent Text Reader

Abstract

The present invention provides a liquid crystal alignment agent containing the following polymer (A) and polymer (B). Polymer (A): at least one polymer selected from a polyimide precursor and a polyimide as an imide product of the polyimide precursor, wherein the polyimide precursor is a reaction product of a diamine component containing a diamine having a skeleton of the following formula (1) and a tetracarboxylic acid derivative component. The definitions of the symbols in the formula are as described in the specification. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal aligning film obtained from the liquid crystal aligning agent, and a liquid crystal display element having the liquid crystal aligning film; and novel diamines and polymers suitable for use therewith. Background Art

[0002] Liquid crystal display elements are known to be light, thin, and low-power display devices. Liquid crystal display elements are composed of a pair of transparent substrates with electrodes sandwiching a liquid crystal layer. In liquid crystal display elements, in order to make the liquid crystals in a desired orientation state between the substrates, an organic film composed of an organic material is used as a liquid crystal alignment film.

[0003] In recent years, high-definition liquid crystal display elements for smartphones and tablet terminals have been pursued to have high display quality, and various properties other than liquid crystal orientation have been required for liquid crystal alignment films at high levels.

[0004] In order to achieve these requirements, a method of adding low molecular weight compounds having various characteristics to a liquid crystal alignment agent for making a liquid crystal alignment film is widely used. For example, in order to improve the mechanical strength of the obtained liquid crystal alignment film, a liquid crystal alignment agent containing a low molecular weight compound that improves the hardness of the liquid crystal alignment film is proposed (see patent documents 1 and 2). The low molecular weight compound contains a group that causes a cross-linking reaction in the heating process performed in the liquid crystal alignment film production process, and is linked to each other through a cross-linked polymer, thereby improving the mechanical strength of the obtained liquid crystal alignment film.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2010-544185

[0008] Patent Document 2: Japanese Patent No. 617911 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, in recent years, in the manufacture of liquid crystal displays, a liquid crystal alignment film that not only satisfies the mechanical strength of the liquid crystal alignment film, but also satisfies other characteristics. The problem to be solved by the present invention is to provide a liquid crystal alignment film with excellent mechanical strength of the film; further provide a liquid crystal alignment film with excellent afterimage characteristics based on long-term AC drive, especially in a liquid crystal display element for a lateral electric field; and provide a liquid crystal alignment agent that can obtain the liquid crystal alignment film.

[0011] Solutions for solving problems

[0012] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention as a result. The present invention has the following solutions.

[0013] 1. A liquid crystal aligning agent comprising the following polymer (A) and polymer (B).

[0014] Polymer (A): at least one polymer selected from a polyimide precursor which is a reaction product of a diamine component including a diamine having a skeleton of the following formula (1) and a tetracarboxylic acid derivative component, and a polyimide which is an imidation product of the polyimide precursor.

[0015]

[0016] In formula (1), R 1 represents hydrogen or a monovalent organic group, and * represents a site bonded to another group.

[0017] Polymer (B): at least one polymer selected from a polyimide precursor and a polyimide which is an imide product of the polyimide precursor, wherein the polyimide precursor is a reaction product of a diamine component containing at least one diamine selected from the following formulas (3) and (4) and a tetracarboxylic acid derivative component.

[0018]

[0019] In formula (3) and (4), A1 is a single bond, an ether bond, an ester bond, an amide bond, a thioether bond, a thioester bond, an alkylene group having 2 to 20 carbon atoms (wherein any -CH2- of the alkylene group is optionally substituted by an ether group, an ester group, a cyclohexylene group or a phenylene group), or a phenylene group. A2 is a halogen atom, a hydroxyl group, or an alkyl or alkoxy group having 1 to 5 carbon atoms (wherein any hydrogen atom of the alkyl or alkoxy group is optionally substituted by a halogen atom). a is an integer of 0 to 4, and when a is 2 or more, A2 may be the same or different. b and c are each independently an integer of 1 to 2.

[0020] Effects of the Invention

[0021] According to the present invention, a liquid crystal alignment film having excellent mechanical strength of the film can be obtained. In other words, by using a polymer having an oxazoline skeleton as a component of a liquid crystal alignment agent, a liquid crystal alignment film that is difficult to peel off or damage the film during brushing can be obtained. In addition, by using a polymer composed of a diamine of the above formula (3) or (4) having excellent liquid crystal orientation, a liquid crystal alignment film having excellent afterimage characteristics after long-term AC driving, especially in a liquid crystal display element for a transverse electric field, can be obtained.

[0022] The liquid crystal display element including the liquid crystal aligning film obtained from the liquid crystal aligning agent of the present invention has few display defects due to scraping and scratching of the liquid crystal aligning film and is excellent in the afterimage characteristics after long-term AC driving. DETAILED DESCRIPTION

[0023] The liquid crystal aligning agent of the present invention is a liquid crystal aligning agent containing the above-mentioned polymers (A) and (B). Hereinafter, each structural requirement will be described in detail.

[0024] <Polymer (A)>

[0025] The polymer (A) contained in the liquid crystal aligning agent of the present invention is at least one polymer selected from a polyimide precursor which is a reaction product of a diamine component containing a diamine having a skeleton of the following formula (1) and a tetracarboxylic acid derivative component, and a polyimide which is an imidate of the polyimide precursor.

[0026]

[0027] In the above formula (1), R 1 represents hydrogen or a monovalent organic group, and * represents a site bonded to another group. The specific polymer of the present invention is preferably a polymer obtained from a diamine having a structure of the above formula (1).

[0028] If the amount of the diamine having a skeleton of formula (1) used is too small relative to the total amount of the diamine components used to produce the polymer (A), the mechanical strength of the film will be weak. If the amount is too large, the afterimage characteristics based on long-term AC driving will be poor. Therefore, it is 1 to 80 mol%, more preferably 3 to 65 mol%, and even more preferably 5 to 50 mol%.

[0029] <Specific diamine>

[0030] Examples of the diamine having an oxazoline skeleton represented by the above formula (1) (hereinafter also referred to as a specific diamine) include diamines selected from the group represented by the following formulas (2-1) to (2-3).

[0031]

[0032] In the above formulas (2-1) to (2-3), R 1 The definition of R is the same as that in the above formula (1). 2 is selected from a single bond, -O-, -COO-, -OCO-, -(CH2) l -, -O(CH2) l O-、-CONR 11 -, -NR 11 CO- and -NR 11-, or a divalent organic group consisting of a combination of these, W 1 represents a structure selected from the following group (3-1), W 2 represents a structure selected from the following group (3-2), W 3 represents a structure selected from the following group (3-3), W 4 represents a structure selected from the following group (3-4). 11 represents hydrogen or a monovalent organic group, l is an integer of 1 to 12, and a represents an integer of 0 or 1.

[0033]

[0034]

[0035] In the above group (3-1), *1 represents the site bonded to the amino group in formula (2-1) to (2-3), and *2 represents the site bonded to the oxazoline ring. In the group (3-2), *1 represents the site bonded to the amino group in formula (2-1) to (2-3), and *3 represents the site bonded to R 2 In group (3-3), *3 indicates the bonding site with R 2 Bonding site. In group (3-4), *2 represents the bonding site to the oxazoline ring. X represents a substituent, which represents a hydrogen atom; a halogen atom; an alkyl group having 1 to 6 carbon atoms, such as methyl, ethyl, and propyl; a halogenated alkyl group having 1 to 6 carbon atoms, such as trifluoromethyl; a substituted amino group, such as dimethylamino; an alkoxy group having 1 to 6 carbon atoms, such as methoxy and ethoxy; an amide group, such as NHCOCH3, NHCOCH2CH3, and NHCOOtBu. tBu represents a tert-butyl group.

[0036] As specific examples of the diamines of the above formulae (2-1) to (2-3), the following examples are given.

[0037]

[0038]

[0039] In the above formula, R 1 The definition of R is the same as that in the above formula (1), and is particularly preferably a hydrogen atom, a methyl group (Me) or an ethyl group (Et). 11 The definition of is the same as in the above formula (1), and is particularly preferably a hydrogen atom, a Me group or an Et group. n represents an integer of 1 to 6, and m represents an integer of 1 to 12.

[0040] <Method for synthesizing specific diamine>

[0041] The method for synthesizing the specific diamine of the present invention includes, for example, synthesizing a dinitro compound represented by the following formulas (4-1) to (4-3), and further reducing the nitro group to convert it into an amino group.

[0042]

[0043] In the above formulas (4-1) to (4-3), R 1 , R 2 , W 1 , W 2 , W 3 , W 4 The definition of a is the same as in the above formulas (2-1) to (2-3).

[0044] The catalyst used in the reduction reaction of the nitro group is preferably an activated carbon-supported metal that can be obtained as a commercial product, for example, palladium-activated carbon, platinum-activated carbon, rhodium-activated carbon, etc. In addition, palladium hydroxide, platinum oxide, Raney nickel, etc., may not necessarily be an activated carbon-supported metal catalyst. Among them, palladium-activated carbon is preferred.

[0045] In order to make the above reduction reaction more effective, the reaction may be carried out in the presence of activated carbon. At this time, the amount of activated carbon used is preferably 1 to 30% by mass, more preferably 10 to 20% by mass relative to the dinitro compound. Sometimes the reaction may be carried out under pressure for the same reason. In this case, in order to avoid the reduction of the benzene nucleus, the reaction is preferably carried out at a pressure of less than 20 atmospheres, more preferably at a pressure of up to 10 atmospheres.

[0046] The solvent used in the reduction reaction can be used without limitation as long as it does not react with the raw materials. For example, the following can be used: aprotic polar organic solvents (N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), etc.); ethers (diethyl ether (Et2O), diisopropyl ether (i-Pr2O), tert-butyl methyl ether (TBME), cyclopentyl methyl ether (CPME), tetrahydrofuran (THF), 1,4-dioxane, etc.); aliphatic hydrocarbons (pentane, hexane, heptane, petroleum ether, etc.); aromatic hydrocarbons (benzene, toluene, xylene, mesitylene, chlorobenzene, dichlorobenzene, nitrobenzene, tetralin, etc.); halogenated hydrocarbons (chloroform, dichloromethane, carbon tetrachloride, ethylene dichloride, etc.); lower fatty acid esters (methyl acetate, ethyl acetate, butyl acetate, methyl propionate, etc.); nitriles (acetonitrile, propionitrile, butyronitrile, etc.); etc. These solvents can be appropriately selected considering the ease of reaction, and two or more solvents can be mixed and used. It is also possible to use a suitable dehydrating agent or drying agent to dry the solvent and use it as a non-aqueous solvent as needed. The amount of the solvent used (reaction concentration) is 0.1 to 100 times by mass, preferably 0.5 to 30 times by mass, and more preferably 1 to 10 times by mass relative to the dinitro compound.

[0047] The reaction temperature is in the range of -100° C. to the boiling point of the solvent used, and is preferably -50 to 150° C. The reaction time is usually 0.05 to 350 hours, and preferably 0.5 to 100 hours.

[0048] [Method for preparing dinitro compounds of formula (4-1) and formula (4-3)]

[0049] The method for synthesizing the compounds of formula (4-1) and (4-3) is, for example, as shown in the following reaction formula, by reacting the compound represented by formula (5-1) or (5-2) with halogenated nitrobenzene in the presence of a base to obtain (4-1-1) or (4-3-1).

[0050]

[0051] The above reaction is preferably carried out in the presence of a base. As the base, for example, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, alkali metal carbonates such as sodium carbonate and potassium carbonate, alkali metal bicarbonates such as sodium hydrogen carbonate and potassium hydrogen carbonate, and organic bases such as potassium phosphate, 1,8-diazabicyclo[5,4,0]-7-undecene and triethylamine can be used in an amount preferably 1 to 4 equivalents relative to (5-1) or (5-2).

[0052] The reaction solvent is preferably an aprotic polar organic solvent (DMF, DMSO, DMAc, NMP, etc.). The amount of the solvent used (reaction concentration) is preferably 0.1 to 100 times by mass, more preferably 0.5 to 30 times by mass relative to (5-1) or (5-2).

[0053] The reaction temperature is preferably in the range of -10°C to the boiling point of the solvent used, and more preferably 0 to 150°C. The reaction time is usually 0.05 to 350 hours, and preferably 0.5 to 100 hours.

[0054] As another method for producing the above-mentioned dinitro compound, a leaving group (LG) can be introduced into the alcohol compound represented by (5-1-1) or (5-2-1), and after obtaining (5-1-1a) or (5-2-1a), the compound is reacted with a phenol compound or an amine compound in the presence of a base to obtain the compound of formula (4-1-2) or (4-3-2).

[0055]

[0056] The leaving group (LG) can be introduced by reacting with methanesulfonyl chloride, ethylsulfonyl chloride, p-toluenesulfonyl chloride or the like in the presence of a base such as triethylamine or pyridine.

[0057] The reaction of (5-1-1a) or (5-2-1a) with a phenol compound or an amine compound is preferably carried out in the presence of a base. As the base, for example, an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide; or an alkali metal carbonate such as sodium carbonate or potassium carbonate can be used in an amount preferably 1 to 4 equivalents relative to (5-1-1a) or (5-2-1a).

[0058] (4-1-2) or (4-3-3) can be obtained by reacting the compound represented by (5-1) or (5-2) with an acid chloride in the presence of a base such as triethylamine or pyridine.

[0059]

[0060] [Preparation method of formula (4-2)]

[0061] The method for synthesizing the compound of formula (4-2) is not particularly limited. For example, as shown in the following reaction formula, (4-2-1) or (4-2-2) can be obtained by reacting the compound represented by formula (5-1) with an acid chloride in the presence of a base such as triethylamine or pyridine.

[0062]

[0063] [Preparation methods of formulas (5-1) and (5-2)]

[0064] The method for synthesizing Formula (5-1) and Formula (5-2) is not particularly limited. For example, according to reference (J. Org. Chem. 2014, 79, 8668-8677), as shown in the following reaction formula, (5-1-1) or (5-2-1) can be obtained by reacting a cyano compound with an aminoethanol compound in the presence of a base.

[0065]

[0066] The above reaction is preferably carried out in the presence of a base. As the base, for example, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, preferably 1 to 4 equivalents relative to the cyano compound; alkali metal carbonates such as sodium carbonate and potassium carbonate; inorganic compounds such as sodium phosphate and potassium phosphate; organic bases such as 1,8-diazabicyclo[5,4,0]-7-undecene; etc. can be used. Among them, alkali metal carbonates such as sodium carbonate and potassium carbonate are preferred.

[0067] As reaction solvents, the following can be used: aprotic polar organic solvents (DMF, DMSO, DMAc, NMP, etc.); ethers (Et2O, i-Pr2O, TBME, CPME, THF, 1,4-dioxane, etc.); aliphatic hydrocarbons (pentane, hexane, heptane, petroleum ether, etc.); aromatic hydrocarbons (benzene, toluene, xylene, mesitylene, chlorobenzene, dichlorobenzene, nitrobenzene, tetralin, etc.); halogen hydrocarbons (chloroform, dichloromethane, carbon tetrachloride, dichloroethane, etc.); lower fatty acid esters (methyl acetate, ethyl acetate, butyl acetate, methyl propionate, etc.); nitriles (acetonitrile, propionitrile, butyronitrile, etc.); alcohols (methanol, ethanol, 2-propanol, etc.), etc. These solvents can be appropriately selected in consideration of the ease of reaction, etc., and can be used alone or in combination of two or more. If necessary, the solvent can be dried using an appropriate dehydrating agent or drying agent to use as a non-aqueous solvent. Alcohols (methanol, ethanol, 2-propanol, etc.) are particularly preferred.

[0068] (5-1-2) or (5-2-2) can be obtained by reacting (5-1-1a) or (5-2-1a) with potassium phthalimide to obtain (5-1-1b) or (5-2-1b), and then deprotecting using hydrazine-hydrate. Alternatively, (5-1-3) or (5-2-3) can be obtained by reacting (5-1-1a) or (5-2-1a) with an excess of a secondary amine compound.

[0069]

[0070] It should be noted that in the formulas in the manufacturing flow charts so far, R 1 , W 1 , W 2 , W 3 , W 4The definition of is the same as that in the above formulas (2-1) to (2-3), R 1 Preferably, it is a hydrogen atom, a Me group or an Et group. Y represents OH, NH2 or NHR 11 , Y 1 Indicates O, NH or NR 11 , R 11 The definition of is the same as in the above formula (1), and preferably a hydrogen atom, a Me group, and an Et group. Z represents F, Cl, Br, or I, n represents an integer of 1 to 6, and m represents an integer of 1 to 12.

[0071] <Polymer>

[0072] The polymer (A) of the present invention has a structure represented by the above formula (1). Specific examples include polyamic acid, polyamic acid ester, polyimide, polyurea, polyamide, etc. From the perspective of a liquid crystal aligning agent, it is more preferably selected from at least one of a polyimide precursor comprising a structural unit represented by the following formula (6) and a polyimide as an imide product of the polyimide precursor. More preferably, it is polyamic acid.

[0073]

[0074] In the above formula (6), X1 is a tetravalent organic group derived from a tetracarboxylic acid derivative, Y1 is a divalent organic group derived from a diamine having a structure of formula (1), and R4 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. In view of the ease of imidization by heating, R4 is preferably a hydrogen atom, a methyl group or an ethyl group.

[0075] <Tetracarboxylic acid derivatives>

[0076] X1 in the polyimide precursor of the above formula (6) is a tetravalent organic group derived from a tetracarboxylic acid derivative. As tetracarboxylic acid derivatives, not only tetracarboxylic dianhydride but also tetracarboxylic acids, tetracarboxylic acid dihalide compounds, tetracarboxylic acid dialkyl esters, and tetracarboxylic acid dialkyl ester dihalides as derivatives thereof can be listed. Among them, the tetracarboxylic acid derivatives shown in the following formula (7) are preferred.

[0077]

[0078] In formula (7), X1 has the same definition as X1 in formula (6), and its structure is not particularly limited. Preferred specific examples include the following formulae (X1-1) to (X1-44).

[0079]

[0080]

[0081] In formulas (X1-1) to (X1-4), R3 to R23 Each of R3 to R4 is independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, a monovalent organic group having 1 to 6 carbon atoms and containing a fluorine atom, or a phenyl group. 23 Preferred is a hydrogen atom, a halogen atom, a methyl group or an ethyl group, and preferred is a hydrogen atom or a methyl group.

[0082] Specific examples of the formula (X1-1) include the following formulas (X1-1-1) to (X1-1-6). (X1-1-1) is particularly preferred from the viewpoint of liquid crystal orientation and photoreaction sensitivity.

[0083]

[0084] The tetracarboxylic acid derivative used for the polymer (A) can be appropriately selected according to the solubility of the polymer in the solvent, the coating property of the liquid crystal aligning agent, the orientation of the liquid crystal when it is made into a liquid crystal aligning film, the voltage holding ratio, the degree of required characteristics such as the stored charge, and can be one kind or a mixture of two or more kinds in the same polymer. However, if it contains a tetracarboxylic dianhydride component containing an aromatic structure, it is preferred from the viewpoint of quickly relaxing the stored charge.

[0085] <Diamine>

[0086] In the above formula (6), specific examples of Y1 include a structure in which two amino groups are removed from the diamine of the above formula (2-1), (2-2) or (2-3).

[0087] <Other structural units of polymer (A)>

[0088] The polyimide precursor containing the structural unit represented by the formula (6) may contain the structural unit represented by the following formula (7) within a range not impairing the effects of the present invention.

[0089]

[0090] In formula (7), X2 is a tetravalent organic group derived from a tetracarboxylic acid derivative, Y2 is a divalent organic group derived from a diamine that does not include the structure of formula (1), R4 has the same definition as in formula (6), and R5 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. In addition, it is preferred that at least one of the two R4s is a hydrogen atom.

[0091] As specific examples of X2, including preferred examples, the same structures as those exemplified by X1 in formula (6) can be cited. In addition, Y2 in the polyimide precursor is a divalent organic group derived from a diamine (hereinafter also referred to as other diamines) that does not include the structure of formula (1), and its structure is not particularly limited.

[0092] Another diamine used for the production of the polyimide precursor is represented by the following formula (8).

[0093]

[0094] In the above formula (8), A1 and A2 are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, or an alkynyl group having 2 to 5 carbon atoms.

[0095] In addition, Y2 can be appropriately selected based on the solubility of the polymer in the solvent, the coating properties of the liquid crystal alignment agent, the orientation of the liquid crystal when it is made into a liquid crystal alignment film, the voltage retention rate, the degree of required characteristics such as the accumulated charge, and more than two types can be mixed in the same polymer.

[0096] Specific examples of Y2 are shown below.

[0097]

[0098]

[0099]

[0100]

[0101]

[0102]

[0103] <Polymer (B)>

[0104] The polymer (B) contained in the liquid crystal aligning agent of the present invention refers to at least one polymer selected from a polyimide precursor and a polyimide which is an imide product of the polyimide precursor, wherein the polyimide precursor is a reaction product of a diamine component containing at least one diamine selected from the following formulas (3) and (4) and a tetracarboxylic acid derivative component.

[0105]

[0106] In formula (3) and (4), A1 is a single bond, an ether bond, an ester bond, an amide bond, a thioether bond, a thioester bond, an alkylene group having 2 to 20 carbon atoms (wherein any -CH2- of the alkylene group is optionally substituted by an ether group, an ester group, a cyclohexylene group or a phenylene group), or a phenylene group. A2 is a halogen atom, a hydroxyl group, or an alkyl or alkoxy group having 1 to 5 carbon atoms (wherein any hydrogen atom of the alkyl or alkoxy group is optionally substituted by a halogen atom). a is an integer of 0 to 4, and when a is 2 or more, A2 may be the same or different. b and c are each independently an integer of 1 to 2.

[0107] (Diamine component for producing polymer (B))

[0108] The diamine component used for producing the polymer (B) contains at least one diamine selected from the group consisting of diamines represented by the above formula (3) to (4).

[0109] In the above formulae (3) to (4), A1 is a single bond, an alkylene group having 1 to 8 carbon atoms (wherein at least one -CH2- of the alkylene group is substituted by an ether group or an ester group), or a phenylene group. Preferably, A2 is CH3, a is an integer of 0 to 1, b is 1, and c is an integer of 1 to 2.

[0110] Examples of the diamines represented by formula (3) to (4) include the following.

[0111]

[0112]

[0113]

[0114]

[0115]

[0116] In addition, as the diamine component for producing the polymer (B) contained in the liquid crystal aligning agent of the present invention, any diamine other than the diamines represented by formulas (3) and (4) can be used. Specific examples thereof include examples excluding the diamine having the skeleton of the above-mentioned formula (1) and the diamine represented by formulas (3) and (4) from the examples of the above-mentioned other diamines.

[0117] The diamine component used to produce the polymer (B) of the present invention may be used alone or in combination of two or more, depending on the solubility of the polymer (B) in a solvent, the coating properties of a liquid crystal aligning agent, the liquid crystal orientation when formed into a liquid crystal aligning film, the voltage holding ratio, the stored charge and other properties.

[0118] The tetracarboxylic acid derivative component used for producing the polymer (B) of the present invention can be the same tetracarboxylic acid derivative as that used for the polymer (A). Among them, tetracarboxylic dianhydride having the following structure is preferably used from the viewpoint of good mechanical strength of the film.

[0119]

[0120] <Liquid crystal alignment agent>

[0121] The liquid crystal alignment agent of the present invention contains the above-mentioned specific polymer, but may also contain two or more specific polymers of different structures. In addition, in addition to the specific polymer, other polymers may also be contained, that is, polymers that do not have a divalent group represented by formula (1). As the form of the polymer, there can be listed: polyamic acid, polyimide, polyamic acid ester, polyester, polyamide, polyurea, polyorganosiloxane, cellulose derivatives, polyacetals, polystyrene or its derivatives, poly(styrene-phenylmaleimide) derivatives, poly(meth)acrylates, etc. In the case where the liquid crystal alignment agent of the present invention contains other polymers, the proportion of the specific polymer relative to the total polymer component is preferably 5% by mass or more, for example, 5 to 95% by mass can be listed.

[0122] The preferred abundance ratio (mass ratio) of the polymer (A) to the polymer (B) is 1:99 to 99:1, and more preferably 1:99 to 50:50.

[0123] From the perspective of forming a uniform film, the liquid crystal aligning agent generally takes the form of a coating liquid. The liquid crystal aligning agent of the present invention is also preferably a coating liquid containing the above-mentioned polymer component and an organic solvent that dissolves the polymer component. At this time, the concentration of the polymer in the liquid crystal aligning agent can be appropriately changed according to the setting of the thickness of the coating film to be formed. From the perspective of forming a uniform and defect-free coating film, it is preferably more than 1% by mass, and from the perspective of the storage stability of the solution, it is preferably less than 10% by mass. The concentration of the particularly preferred polymer is 2 to 8% by mass.

[0124] The organic solvent contained in the liquid crystal alignment agent is not particularly limited as long as it uniformly dissolves the polymer component. Specific examples include: N, N-dimethylformamide, N, N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethyl sulfoxide, γ-butyrolactone, 1, 3-dimethyl-imidazolidinone, methyl ethyl ketone, cyclohexanone, cyclopentanone, etc. Among them, it is preferred to use N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone or γ-butyrolactone.

[0125] Moreover, the organic solvent contained in the liquid crystal aligning agent of the present invention may use a solvent which improves coating property when applying the liquid crystal aligning agent and surface smoothness of the coating film in addition to the above-mentioned solvents. Specific examples of the organic solvent are given below.

[0126] For example, ethanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, isopentanol, tert-pentanol, 3-methyl-2-butanol, neopentyl alcohol, 1-hexanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-ethyl-1-butanol, 1-heptanol, 2-heptanol, 3-heptanol, 1-octanol, 2-octanol, 2-ethyl-1-hexanol, cyclohexanol, 1-methylcyclohexanol, 2-methylcyclohexanol, 3-methylcyclohexanol, 2,6-dimethyl-4-heptanol, 1,2-ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2 , 3-butanediol, 1,5-pentanediol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, diisopropyl ether, dipropyl ether, dibutyl ether, dihexyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, 1,2-butoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, 4-hydroxy-4-methyl-2-pentanone, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, 2-pentanone, 3-pentanone, 2-hexanone, 2-heptanone, 4-heptanone, 2,6-dimethyl-4-heptanone, 4,6-dimethyl-2-heptanone, 3-ethoxybutyl acetate, 1-methylpentyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate Acid esters, ethylene glycol monoacetate, ethylene glycol diacetate, propylene carbonate, ethylene carbonate, 2-(methoxymethoxy)ethanol, ethylene glycol monobutyl ether, ethylene glycol monoisoamyl ether, ethylene glycol monohexyl ether, 2-(hexyloxy)ethanol, furfuryl alcohol, diethylene glycol, propylene glycol, propylene glycol monobutyl ether, 1-(butoxyethoxy)propanol, propylene glycol monomethyl ether acetate, dipropylene glycol, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, ethylene glycol monoacetate, ethylene glycol diacetate, diethylene glycol monoethyl ether Acetate, diethylene glycol monobutyl ether acetate, 2-(2-ethoxyethoxy)ethyl acetate, diethylene glycol acetate, triethylene glycol, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol acetate monoethyl ether, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isoamyl lactate, and solvents represented by the following formulas [D-1] to [D-3].

[0127]

[0128] (D 1 ~D 3 represents an alkyl group having 1 to 4 carbon atoms. )

[0129] Among them, the organic solvent is preferably 1-hexanol, cyclohexanol, 1,2-ethylene glycol, 1,2-propylene glycol, propylene glycol monobutyl ether, diethylene glycol diethyl ether, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monobutyl ether or dipropylene glycol dimethyl ether. The type and content of the solvent are appropriately selected according to the coating device, coating conditions, coating environment, etc. of the liquid crystal alignment agent.

[0130] The liquid crystal aligning agent of the present invention may also contain additional components other than the polymer component and the organic solvent. As such additional components, there can be listed: a bonding aid for improving the adhesion between the liquid crystal aligning film and the substrate, and the adhesion between the liquid crystal aligning film and the sealant; a cross-linking agent for improving the strength of the liquid crystal aligning film; a dielectric, a conductive material, etc. for adjusting the dielectric constant and resistance of the liquid crystal aligning film. As specific examples of these additional components, there can be listed the poor solvents and cross-linking compounds disclosed in paragraphs

[0104] on page 53 to

[0116] on page 60 of International Publication No. 2015 / 060357.

[0131] Examples of compounds for improving the adhesion between the liquid crystal alignment film and the substrate include compounds containing functional silanes and compounds containing epoxy groups, such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2 -aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltriethoxysilane, N-triethoxysilylpropyltriethylenetriamine, N-trimethoxysilylpropyltriethylenetriamine, 10-trimethoxysilyl-1,4,7-triazadecane, 10-triethoxysilyl-1,4,7-triazadecane, 9-trimethoxysilyl- 3,6-diazanonyl acetate, 9-triethoxysilyl-3,6-diazanonyl acetate, N-benzyl-3-aminopropyl trimethoxysilane, N-benzyl-3-aminopropyl triethoxysilane, N-phenyl-3-aminopropyl trimethoxysilane, N-phenyl-3-aminopropyl triethoxysilane, N-bis(oxyethylene)-3-aminopropyl trimethoxysilane, N-bis(oxyethylene)-3-aminopropyl triethoxysilane, ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether Water glyceryl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol diglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, 1,3,5,6-tetraglycidyl-2,4-hexanediol, N,N,N',N'-tetraglycidyl-m-xylene diamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane or N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, etc.

[0132] Moreover, in order to improve the mechanical strength of a liquid crystal alignment film, the liquid crystal aligning agent of this invention may contain the following additives.

[0133]

[0134] The additive is preferably 0.1 to 30 parts by mass based on 100 parts by mass of the polymer component contained in the liquid crystal aligning agent. If it is less than 0.1 parts by mass, no effect can be expected, and if it exceeds 30 parts by mass, the orientation of the liquid crystal is reduced, so it is more preferably 0.5 to 20 parts by mass.

[0135] In addition to the above, the liquid crystal alignment agent of the present invention may also contain: a polymer other than the specific polymer described in the present invention, a dielectric for the purpose of changing the electrical properties of the liquid crystal alignment film, such as the dielectric constant and conductivity, a silane coupling agent for the purpose of improving the adhesion between the liquid crystal alignment film and the substrate, a cross-linking compound for the purpose of improving the hardness and density of the film when the liquid crystal alignment film is prepared, an imidization accelerator for the purpose of more efficiently performing imidization by heating the polyimide precursor when the coating film is fired, and the like.

[0136] <Liquid crystal alignment film>

[0137] The liquid crystal alignment film of the present invention is obtained from the liquid crystal alignment agent. If an example of a method for obtaining a liquid crystal alignment film from a liquid crystal alignment agent is given, it can be listed as a method of applying a liquid crystal alignment agent in the form of a coating liquid to a substrate, drying it, and firing it, and then performing an alignment treatment by a brushing treatment method or a photo-alignment treatment method.

[0138] As a substrate for coating a liquid crystal alignment agent, there is no particular limitation as long as it is a substrate with high transparency. In addition to glass substrates and silicon nitride substrates, plastic substrates such as acrylic substrates and polycarbonate substrates can also be used. In this case, if a substrate is formed with an ITO electrode for driving a liquid crystal, it is preferred from the perspective of simplifying the process. In addition, in a reflective liquid crystal display element, if it is only a single-sided substrate, an opaque object such as a silicon wafer can also be used, and the electrode in this case can also use a light-reflecting material such as aluminum.

[0139] The coating method of the liquid crystal aligning agent is generally screen printing, gravure printing, flexographic printing, inkjet method, etc. Other coating methods include dipping method, roll coating method, slit coating method, spin coating method, spray coating method, etc., and these can be used according to the purpose.

[0140] After the liquid crystal alignment agent is applied to the substrate, the solvent is evaporated and fired by a heating unit such as a heating plate, a heat circulation oven, an IR (infrared) oven, etc. The drying and firing processes after the liquid crystal alignment agent is applied can select any temperature and time. Although a drying process is not necessarily required, in the case where the time from coating to firing on each substrate is not constant, or when firing is not performed immediately after coating, it is preferred to perform a drying process. The drying can be performed to remove the solvent to the extent that the shape of the coating film is not deformed by the transportation of the substrate, etc. For its drying method, for example, the following method can be cited: drying on a heating plate at a temperature of 40°C to 150°C, preferably 60°C to 100°C for 0.5 minutes to 30 minutes, preferably drying for 1 minute to 5 minutes.

[0141] The firing temperature of the coating formed by applying the liquid crystal alignment agent is, for example, 100 to 350° C., preferably 120 to 300° C., and more preferably 150 to 250° C. The firing time is 5 to 240 minutes, preferably 10 to 90 minutes, and more preferably 20 to 90 minutes. Heating can usually be performed by a known method, such as a hot plate, a hot air circulation furnace, an infrared furnace, etc.

[0142] Since the reliability of a liquid crystal display element may fall when the thickness of the liquid crystal aligning film after baking is too thin, it is preferably 5-300 nm, and more preferably 10-200 nm.

[0143] When manufacturing a TN type, STN type, IPS type or FFS type liquid crystal display element, a process for imparting liquid crystal orientation ability to the coating film formed in the above process is performed. Examples of the orientation ability imparting process include a brushing process in which the coating film is rubbed in a certain direction using a roller wound with a cloth made of fibers such as nylon, rayon, and cotton, and a photo-orientation process in which the coating film is irradiated with polarized light or non-polarized light radiation.

[0144] In the photo-alignment treatment, as the radiation irradiated to the coating film, for example, ultraviolet rays and visible light containing light with a wavelength of 150 to 800 nm can be used. In the case where the radiation is polarized light, it can be linearly polarized light or partially polarized light. In addition, in the case where the radiation used is linearly polarized light or partially polarized light, the irradiation can be performed from a direction perpendicular to the substrate surface, from an oblique direction, or in combination. In the case of irradiating non-polarized radiation, the irradiation direction is set to an oblique direction.

[0145] As the light source used, for example, a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, an LED lamp, etc. can be used. Ultraviolet rays in a preferred wavelength range can be obtained by using a light source, for example, with a filter, a diffraction grating, etc. The irradiation amount of the radiation is preferably 100 to 50,000 J / m 2 , more preferably 300 to 20000 J / m 2 .

[0146] Furthermore, the coating film may be irradiated with light while being heated to improve reactivity. The temperature during heating is usually 30 to 250°C, preferably 40 to 200°C, and more preferably 50 to 150°C.

[0147] As for the photo-alignment treatment, the heat treatment can be performed during the light irradiation, or the heat treatment can be performed after the photo-alignment treatment. The heating temperature at this time is preferably 80 to 300°C, more preferably 120 to 250°C. The heating time is preferably 5 to 200 minutes, more preferably 10 to 100 minutes. In addition, the heating treatment can be replaced by washing with an organic solvent or water, and the washing treatment and the heating treatment can be combined.

[0148] The liquid crystal alignment film after the brushing treatment can be further subjected to a treatment of changing the pretilt angle of a part of the liquid crystal alignment film by irradiating a part of the liquid crystal alignment film with ultraviolet rays, and after forming an anti-etching film on a part of the surface of the liquid crystal alignment film, a brushing treatment in a direction different from the previous brushing treatment can be performed to remove the anti-etching film, so that each area of ​​the liquid crystal alignment film has a different liquid crystal orientation ability. In this case, the field of view characteristics of the obtained liquid crystal display element can be improved.

[0149] The liquid crystal aligning film of the present invention is preferably used as a liquid crystal aligning film for a liquid crystal display element of a transverse electric field system such as an IPS system or an FFS (Fringe Field Switching) system.

[0150] <Liquid crystal display device>

[0151] The liquid crystal display element of the present invention is obtained by obtaining a substrate with a liquid crystal alignment film obtained by the above-mentioned liquid crystal alignment agent, and then making a liquid crystal box by a known method, and using the liquid crystal box to make an element. As a specific example of a liquid crystal display element that can be made, it is a liquid crystal display element with a liquid crystal box, and the liquid crystal box has: two substrates arranged to be opposite; a liquid crystal layer provided between the substrates; and the above-mentioned liquid crystal alignment film formed by the liquid crystal alignment agent of the present invention provided between the substrate and the liquid crystal layer. More specifically, it is a liquid crystal display element as follows: a liquid crystal alignment film is formed by applying the liquid crystal alignment agent of the present invention on two substrates and firing them, two substrates are arranged in a manner that the liquid crystal alignment film is opposite, and a liquid crystal layer composed of liquid crystals is sandwiched between the two substrates, that is, the liquid crystal layer is arranged in a manner in contact with the liquid crystal alignment film.

[0152] As an example of a method for making a liquid crystal box, a liquid crystal display element with a passive matrix structure is used as an example for description. Specifically, a transparent substrate is prepared, and then, under the above-mentioned conditions, a liquid crystal alignment film is formed on each substrate. As described above, the substrate is usually a substrate on which a transparent electrode for driving liquid crystal is formed. As a specific example, the same substrate as the substrate described in the above-mentioned liquid crystal alignment film can be cited.

[0153] A common electrode is provided on one substrate, and a segmented electrode is provided on the other substrate. These electrodes can be, for example, ITO electrodes, and are patterned in a manner that enables a desired image display. Next, an insulating film is provided on each substrate in a manner that covers the common electrode and the segmented electrode. The insulating film can be, for example, a film composed of SiO2-TiO2 formed by a sol-gel method.

[0154] In the case of manufacturing an IPS type or FFS type liquid crystal display element, a liquid crystal alignment agent is applied to the electrode forming surface of a substrate provided with an electrode composed of a transparent conductive film or a metal film patterned into a comb shape and to one side of an opposing substrate without an electrode, and then each coated surface is heated to form a coating film. As the metal film, for example, a film containing a metal such as chromium can be used.

[0155] In addition, a high-performance element such as a TFT type element is used in which an element such as a transistor is formed between an electrode for driving liquid crystal and a substrate.

[0156] In the case of a transmissive liquid crystal display element, the above-mentioned substrate is usually used, but in a reflective liquid crystal display element, if only a single-sided substrate is used, an opaque substrate such as a silicon wafer may also be used. In this case, a material such as aluminum that reflects light may also be used in the electrode formed on the substrate.

[0157] On the other hand, the liquid crystal material constituting the liquid crystal layer of the liquid crystal display element of the horizontal alignment method such as IPS and FFS can also use the liquid crystal material used in the existing horizontal alignment method, for example, negative and positive liquid crystals such as MLC-2003 and MLC-2041 manufactured by MERCK, and negative liquid crystals such as MLC-6608.

[0158] As a method for sandwiching the liquid crystal layer between two substrates, known methods can be cited. For example, the following method can be cited: prepare a pair of substrates formed with liquid crystal alignment films, scatter spacers such as beads on the liquid crystal alignment film of one substrate, adhere the other substrate in a manner that the surface of the side formed with the liquid crystal alignment film becomes the inner side, and inject liquid crystal under reduced pressure for sealing. In addition, a liquid crystal box can also be made by the following method: prepare a pair of substrates formed with liquid crystal alignment films, scatter spacers such as beads on the liquid crystal alignment film of one substrate, and then drip liquid crystal, and then, adhere the other substrate in a manner that the surface of the side formed with the liquid crystal alignment film becomes the inner side for sealing. The thickness of the above-mentioned spacer is preferably 1 to 30 μm, and more preferably 2 to 10 μm.

[0159] After the above steps are completed, a polarizing plate is placed on the liquid crystal cell. Specifically, it is preferable that a pair of polarizing plates are bonded to the surfaces of the two substrates on the opposite side to the liquid crystal layer.

[0160] It should be noted that the liquid crystal alignment film and the liquid crystal display element of the present invention are not limited as long as the liquid crystal alignment agent of the present invention is used, and can also be produced by other known methods. The process until the liquid crystal display element is obtained from the liquid crystal alignment agent is disclosed, for example, in paragraphs

[0074] on page 17 to

[0081] on page 19 of Japanese Patent Application Laid-Open No. 2015-135393.

[0161] The liquid crystal display element of the present invention can be effectively applied to various devices, for example, it can be used in various display devices such as watches, portable game consoles, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smart phones, various monitors, LCD televisions, and information displays.

[0162] Example

[0163] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited thereto. The abbreviations of the following compounds and the methods for measuring the properties are as follows.

[0164] (Solvent)

[0165] NMP: N-methyl-2-pyrrolidone.

[0166] GBL: gamma-butyrolactone.

[0167] BCS: Butyl Cellosolve.

[0168] (Diamine)

[0169] DA-1: p-phenylenediamine.

[0170] DA-2: 1,2-bis(4-aminophenoxy)ethane.

[0171] DA-3: Refer to the following formula (DA-3).

[0172] DA-4: N-tert-butyloxycarbonyl-N-(2-(4-aminophenyl)ethyl)-N-(4-aminobenzyl)amine

[0173] DA-5: 4,4'-diaminodiphenylamine.

[0174] DA-6: 1,3-bis(4-aminophenethyl)urea.

[0175] DA-O1: Refer to the following formula (DA-O1).

[0176] DA-O2: Refer to the following formula (DA-O2).

[0177] DA-O3: Refer to the following formula (DA-O3).

[0178] DA-O4: Refer to the following formula (DA-O4).

[0179] (Acid dianhydride)

[0180] TA-1: 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride.

[0181] TA-2: 3,3',4,4'-biphenyltetracarboxylic dianhydride.

[0182]

[0183] [Viscosity]

[0184] The viscosity of the solution was measured at 25° C. using an E-type viscometer TVE-22H (manufactured by Toki Sangyo Co., Ltd.) with a sample volume of 1.1 mL and a conical rotor TE-1 (1°34′, R24).

[0185] [Production of Liquid Crystal Cell]

[0186] A liquid crystal cell having a structure of a fringe field switching (FFS) mode liquid crystal display element is produced.

[0187] First, prepare a substrate with electrodes. The substrate is a glass substrate with a size of 30 mm × 35 mm and a thickness of 0.7 mm. On the substrate, as the first layer, an ITO electrode with a dense pattern constituting a counter electrode is formed. On the counter electrode of the first layer, as the second layer, a SiN (silicon nitride) film formed by a CVD method is formed. The film thickness of the second layer of the SiN film is 500 nm, and it functions as an interlayer insulating film. On the second layer of the SiN film, as the third layer, a comb-shaped pixel electrode formed by patterning the ITO film is arranged to form two types of pixels, the first pixel and the second pixel. The size of each pixel is 6 mm in length and about 5 mm in width. At this time, the counter electrode of the first layer and the pixel electrode of the third layer are electrically insulated due to the action of the SiN film of the second layer.

[0188] The pixel electrode of the third layer has a comb-like shape formed by arranging a plurality of electrode elements in the shape of a "< symbol" with the central portion bent at an internal angle of 160°. The width of each electrode element in the short dimension direction is 3μm, and the interval between the electrode elements is 6μm. The pixel electrode forming each pixel is composed of an arrangement of a plurality of electrode elements in the shape of a "< symbol" with a bent central portion, so the shape of each pixel has a shape similar to the bold "< symbol" bent in the central portion like the electrode elements, rather than a rectangular shape. In addition, each pixel is divided into upper and lower parts with the bent portion in the center as the boundary, and has a first area on the upper side of the bent portion and a second area on the lower side.

[0189] Next, after filtering the liquid crystal alignment agent with a 1.0 μm filter, the liquid crystal alignment agent was applied to the prepared substrate with electrodes and a glass substrate with a columnar spacer having a height of 4 μm and an ITO film formed on the back by spin coating. After drying on a hot plate at 80°C for 2 minutes, the liquid crystal alignment agent was fired in a hot air circulation oven at 230°C for 30 minutes to form a coating film with a thickness of 100 nm. The coating film surface was irradiated with a linearly polarized ultraviolet light with an extinction ratio of 10:1 or more at a wavelength of 254 nm through a polarizing plate.

[0190] It should be noted that the liquid crystal orientation film formed on the first glass substrate is oriented in a manner that the direction of dividing the inner angle of the pixel bending portion into equal parts is orthogonal to the orientation direction of the liquid crystal, and the liquid crystal orientation film formed on the second glass substrate is oriented in a manner that the orientation direction of the liquid crystal on the first substrate is consistent with the orientation direction of the liquid crystal on the second substrate when making a liquid crystal box. The substrate was further fired in a hot air circulation oven at 230°C for 30 minutes to obtain a substrate with a liquid crystal orientation film. The above two substrates were set as a group, and a sealant was printed on the substrate. After bonding another substrate with the liquid crystal orientation film surface facing each other and the orientation direction being 0°, the sealant was cured to produce an empty box. Liquid crystal MLC-3019 (manufactured by MERCK) was injected into the empty box by a reduced pressure injection method, and the injection port was sealed to obtain an FFS driven liquid crystal box. Then, the obtained liquid crystal box was heated at 110°C for 1 hour, left overnight and used for each evaluation.

[0191] [Evaluation of afterimage based on long-term AC drive]

[0192] Using the above liquid crystal cell, an AC voltage of ±5 V was applied at a frequency of 60 Hz for 120 hours in a constant temperature environment of 60° C. Then, the pixel electrode and the counter electrode of the liquid crystal cell were short-circuited and left at room temperature for one day.

[0193] After placement, the liquid crystal box is set between two polarizing plates arranged in a manner that the polarization axes are orthogonal, the backlight is turned on in advance without applying voltage, and the configuration angle of the liquid crystal box is adjusted to minimize the brightness of the transmitted light. Then, the rotation angle when the liquid crystal box is rotated from the angle at which the second area of ​​the first pixel becomes the darkest until the angle at which the first area becomes the darkest is calculated as angle Δ. Similarly, in the second pixel, the second area is compared with the first area, and the same angle Δ is calculated. The case where the calculated angle Δ value is less than 0.3 degrees is evaluated as "good", and the case where the calculated angle Δ value exceeds 0.3 degrees is evaluated as "poor".

[0194] [Evaluation of brush abrasion resistance]

[0195] The liquid crystal alignment agent was applied on the prepared ITO substrate by spin coating, dried on a hot plate at 80°C for 2 minutes, and then fired in a hot air circulation oven at 230°C for 30 minutes to form a coating with a thickness of 100nm. Ultraviolet rays with a linear polarization wavelength of 254nm with an extinction ratio of 10:1 or more were irradiated to the coating surface through a polarizing plate. The substrate was further fired in a hot air circulation oven at 230°C for 30 minutes to obtain a substrate with a liquid crystal alignment film. The liquid crystal alignment film was brushed with rayon cloth (roller speed: 1000rpm, stage moving speed: 20mm / sec, pressing length: 0.4mm). The substrate was observed under a microscope, and the case where no line marks caused by brushing were observed on the film surface was evaluated as "good", and the case where line marks were seen was evaluated as "poor".

[0196] Compounds DA-O1 to DA-O4 are novel compounds and were synthesized as follows.

[0197] The products obtained from the following monomer synthesis examples 1 to 4 were identified by 1H-NMR analysis. The analysis conditions are as follows.

[0198] Apparatus: Varian NMR System 400NB (400 MHz).

[0199] Determination solvent: dimethyl sulfoxide (DMSO)-d6.

[0200] Reference material: Tetramethylsilane (TMS) (δ0.0ppm for 1 H).

[0201] <<Synthesis Example 1: Synthesis of DA-O1>>

[0202]

[0203] <Synthesis of compound [1]>

[0204] Methanol (320 g), p-nitrobenzonitrile (40.0 g, 270 mmol), 2-amino-2-methyl-1,3-propanediol (142.3 g) and sodium carbonate (28.6 g) were placed in a flask and reacted for 22 hours under a nitrogen atmosphere and reflux conditions. After the reaction was completed, the reaction solution was poured into pure water (960 g) to precipitate crystals, which were filtered and washed with methanol. Next, the obtained crude product was slurry-washed with a mixed solvent of ethyl acetate (260 g) and hexane (40 g), and compound [1] was obtained as white crystals by filtering and drying (yield: 46.8 g, yield: 73%).

[0205] 1H-NMR(400MHz)in DMSO-d6: 8.29-8.33ppm (m, 2H), 8.07-8.11ppm (m, 2H) 4.97ppm (t, J=6.0Hz, 1H), 4.46p pm (d, J=8.4Hz, 1H), 4.07ppm (d, J=8.4Hz, 1H), 3.36-3.47ppm (m, 2H), 1.25ppm (s, 3H).

[0206] <Synthesis of Compound [2]>

[0207] N-methyl-2-pyrrolidone (380 g), compound [1] (44.7 g, 189 mmol), 4-fluoronitrobenzene (45.9 g) and sodium hydroxide (12.6 g) were placed in a flask and reacted at room temperature for about 5 days. After the reaction was completed, the reaction solution was poured into pure water (1124 g) to precipitate crystals, and the crude crystals were recovered by filtration. Then, room temperature slurry washing was performed with methanol (179 g), and then slurry washing was performed with ethyl acetate (560 g). After slurry washing, compound [2] was obtained as light yellow crystals by filtration and drying (yield: 51.4 g, yield: 76%).

[0208] 1 H-NMR(400MHz)in DMSO-d6: 8.30-8.32ppm (m, 2H), 8.15-8.19ppm (m, 2H), 8.09-8.12ppm (m, 2H), 7.13-7.18ppm (m, 2H), 4.56ppm (d , J=8.8Hz, 1H), 4.27ppm (d, J=8.4Hz, 1H), 4.26ppm (d, J=9.6Hz, 1H), 4.21ppm (d, J=10.0Hz, 1H) 1.25ppm (s, 3H).

[0209] <Synthesis of DA-O1>

[0210] Tetrahydrofuran (397 g), methanol (99 g), compound [2] (49.7 g, 139 mmol), and 5% palladium-carbon (about 50% water-wet product) (3.46 g) were placed in a flask and reacted for 24 hours under a hydrogen atmosphere at room temperature. After the reaction was completed, 5% palladium-carbon was removed by filtration, and the internal mass was set to 73.4 g by vacuum concentration. Then, 2-propanol (250 g) was added, heated at 50°C to dissolve, and crystals were precipitated under ice-cooling conditions. DA-O1 was obtained as white crystals by filtration and drying (yield: 30.2 g, yield: 73%).

[0211] 1H-NMR(400MHz)in DMSO-d6: 7.50-7.54ppm (m, 2H), 6.62-6.66ppm (m, 2H), 6.53-6.56ppm (m, 2H), 6.45-6.49ppm (m, 2H), 5.7ppm (s, 2 H), 4.61ppm (s, 2H), 4.31ppm (d, J=8.4Hz, 1H), 4.00ppm (d, J=8.40Hz, 1H), 3.74-3.79ppm (m, 2H), 1.30ppm (s, 3H).

[0212] <<Synthesis Example 2: Synthesis of DA-O2>>

[0213]

[0214] <Synthesis of compound [3]>

[0215] Methanol (240 g), p-nitrobenzonitrile (30.0 g, 203 mmol), 2-amino-1,3-propanediol (55.6 g) and sodium carbonate (21.6 g) were placed in a flask and reacted for 23 hours under a nitrogen atmosphere and reflux conditions. After the reaction was completed, the reaction solution was poured into pure water (720 g) to precipitate crystals, which were filtered and washed with methanol. Next, the obtained crude product was slurry-washed with a mixed solvent of ethyl acetate (150 g) and hexane (30 g), and the compound [3] was obtained as light yellow crystals by filtering and drying (yield: 30.9 g, yield: 69%).

[0216] 1 H-NMR(400MHz)in DMSO-d6: 8.11-8.33ppm (m, 2H), 8.09-8.12ppm (m, 2H), 4.90ppm (t, J=5.6Hz, 1H), 4.48-4.90ppm (m, 1H), 4.33-4.41ppm (m, 2H), 3.36-3.64ppm (m, 2H).

[0217] <Synthesis of compound [4]>

[0218] N-methyl-2-pyrrolidone (138 g), compound [3] (27.8 g, 126 mmol), 4-fluoronitrobenzene (28.8 g) and sodium hydroxide (7.6 g) were placed in a flask and reacted at room temperature for about 4 days. After the reaction was completed, ethyl acetate (504 g) and pure water (224 g) were added to the reaction solution, resulting in the precipitation of crystals. The crystals were recovered by filtration and the recovered crystals were slurry-washed at room temperature with a mixed solvent of methanol (140 g) and pure water (140 g). After slurry washing, the compound [4] was obtained as light yellow crystals by filtration, methanol washing and drying (yield: 31.3 g, yield: 72%).

[0219] 1 H-NMR(400MHz)in DMSO-d6: 8.31-8.33ppm (m, 2H) 8.17-8.21ppm (m, 2H), 8.11-8.14ppm (m, 2H), 7.15-7.19ppm (m, 2H), 4.76-4.83ppm (m, 1H), 4.66-4.70ppm (m, 1H), 4.42-4.46ppm (m, 1H), 4.32-4.38ppm (m, 1H).

[0220] <Synthesis of DA-O2>

[0221] Tetrahydrofuran (217 g), methanol (62.6 g), compound [4] (31.3 g, 91.2 mmol) and 5% palladium-carbon (about 50% water-wet product) (2.34 g) were placed in a flask and reacted for 4 days under a hydrogen atmosphere at 40°C. After the reaction was completed, 5% palladium-carbon was removed by filtration, and the solvent was removed by vacuum concentration to obtain a crude product. Then, the room temperature slurry was washed with methanol (243 g), and DA-O2 was obtained as light pink crystals by filtration and drying (yield: 17.5 g, yield: 68%).

[0222] 1 H-NMR(400MHz)in DMSO-d6: 7.53-7.56ppm (m, 2H), 6.64-6.68ppm (m, 2H), 6.54-6.57ppm (m, 2H), 6.47-6.51ppm (m, 2H), 5.73ppm (s, 2H), 4.62ppm (s, 2H), 4.41-4.47ppm (m, 2H), 4.15-4.18ppm (m, 1H), 3.96-3.99ppm (m, 1H), 3.79-3.83ppm (m, 1H).

[0223] <<Synthesis Example 3: Synthesis of DA-O3>>

[0224]

[0225] <Synthesis of compound [5]>

[0226] Methanol (400 g), terephthalonitrile (50.2 g, 392 mmol), 2-amino-2-methyl-1,3-propanediol (165 g) and sodium carbonate (83.9 g) were placed in a flask and reacted for 20 hours under a nitrogen atmosphere and reflux conditions. After the reaction was completed, the reaction solution was poured into pure water (1200 g) to precipitate crystals, and the crude product was recovered by filtration. The obtained crude product was washed with pure water (300 g × 6 times) and then washed with methanol (200 g × 2 times) to obtain compound [5] as white crystals (crude yield: 109.6 g, crude yield: 100%).

[0227] 1 H-NMR(400MHz)in DMSO-d6: 7.92ppm (s, 4H), 4.94ppm (t, J=5.2Hz, 2H), 4.41ppm (d, J=8.0Hz, 2H), 4.01ppm (d, J=8.0Hz, 2H), 3.36-3.44ppm (m, 4H), 1.23ppm (s, 6H).

[0228] <Synthesis of compound [6]>

[0229] N-methyl-2-pyrrolidone (327 g), compound [5] (40.8 g, 146 mmol) and potassium hydroxide (21.2 g) were placed in a flask, and 4-fluoronitrobenzene (45.7 g) dissolved in N-methyl-2-pyrrolidone (19.9 g) was added dropwise under nitrogen atmosphere and water cooling. After the addition was completed, the dropping funnel was washed with N-methyl-2-pyrrolidone (21.4 g), and the reaction was carried out at room temperature for 2 hours. After the reaction was completed, the reaction solution was poured into pure water (1200 g), crystals were precipitated, and filtered, washed with pure water, and washed with methanol. Then, the obtained crude crystals were slurried and washed with methanol (300 g) at room temperature. Then, the crude crystals were heated and dissolved in chloroform (10009 g), methanol (466 g) was added, crystals were precipitated, and the compound [6] was obtained as pale yellow crystals by filtration and drying (yield: 63.2 g, yield: 79%).

[0230] 1 H-NMR (400MHz) in DMSO-d6: 8.16-8.19ppm (m, 4H), 7.95ppm (s, 4H), 7.13-7.16ppm (m, 4H), 4.52ppm (d, J=8.4Hz, 2H), 4.19-4.22ppm (m, 6H), 1.42ppm (s, 6H).

[0231] <Synthesis of DA-O3>

[0232] Tetrahydrofuran (509 g), methanol (62.3 g), compound [6] (62.7 g, 115 mmol) and 5% palladium-carbon (about 50% water-wet product) (3.66 g) were placed in a flask and reacted for 4 days under a hydrogen atmosphere at 40°C. After the reaction was completed, the 5% palladium-carbon was removed by filtration. Then, the filtrate was washed with excess N,N-dimethylformamide. The obtained filtrate was concentrated under reduced pressure, methanol (660 g) was added, crystals precipitated, and DA-O3 was obtained by filtration as light pink crystals (yield: 20.9 g, yield: 38%).

[0233] 1 H-NMR(400MHz)in DMSO-d6: 7.96ppm (s, 4H), 6.62-6.65ppm (m, 4H), 6.46-6.49ppm (m, 4H), 4.61ppm (s, 4H), 4.47ppm (d, J=8. 4Hz, 2H), 4.16ppm (d, J=8.4Hz, 2H), 3.87ppm (d, J=9.2Hz, 2H), 3.60ppm (d, J=9.2Hz, 2H), 1.36ppm (s, 6H).

[0234] <<Synthesis Example 4: Synthesis of DA-O4>>

[0235]

[0236] <Synthesis of Compound [7]>

[0237] N-methyl-2-pyrrolidone (400 g), compound [5] (40.0 g, 143 mmol) and triethylamine (38.0 g) were placed in a flask, and 4-nitrobenzoyl chloride (60.7 g) was added in four portions under a nitrogen atmosphere and water cooling. After the addition, poor stirring occurred, so N-methyl-2-pyrrolidone (160 g) was added to ensure stirring, and the reaction was carried out at room temperature for about 15 hours. After the reaction was completed, the reaction solution was poured into pure water (1500 g) to precipitate crystals, which were filtered, washed with pure water and washed with methanol. Then, the obtained crude product was dissolved in tetrahydrofuran (560 g) by heating at 50°C, and methanol (400 g) was added to precipitate crystals. The further obtained crystals were slurry-washed with tetrahydrofuran (160 g), filtered and dried to obtain compound [7] as white crystals (yield: 47.4 g, yield: 55%).

[0238] 1H-NMR(400MHz)in DMSO-d6: 8.24-8.30ppm (m, 4H), 8.06-8.11ppm (m, 4H), 7.93ppm (s, 4H), 4.58- 4.60ppm (m, 2H), 4.35-4.43ppm (m, 4H), 4.19-4.22ppm (m, 2H), 1.43ppm (s, 6H).

[0239] <Synthesis of DA-O4>

[0240] Tetrahydrofuran (453 g), methanol (95.6 g), N,N-dimethylformamide (400 g), compound [7] (47.4 g, 78.6 mmol) and 5% palladium-carbon (about 50% water-wet product) (2.90 g) were placed in a flask and reacted for about 3 days under a hydrogen atmosphere at room temperature. The 5% palladium-carbon was removed by filtration and the internal mass was reduced to 130 g by vacuum concentration. Methanol (390 g) was added to the obtained homogeneous solution to precipitate crystals, which were filtered and dried to obtain DA-O4 as white crystals (yield: 17.3 g, yield: 41%).

[0241] 1 H-NMR(400MHz)in DMSO-d6: 7.96ppm (s, 4H), 7.52-7.55ppm (m, 4H), 6.46-6.50ppm (m, 4H), 5.96 ppm (s, 4H), 4.48ppm (d, J = 8.8Hz, 2H), 4.16-4.22ppm (m, 6H), 1.39ppm (s, 6H).

[0242] <Synthesis Example 1 of PAA>

[0243] In a 200 ml four-necked flask equipped with a stirrer and a nitrogen inlet tube, 1.08 g (10.0 mmol) of DA-1, 3.66 g (15.0 mmol) of DA-2, 4.81 g (15.0 mmol) of DA-3, and 3.41 g (15.0 mmol) of DA-4 were weighed, 132.0 g of NMP was added, and the mixture was dissolved by stirring while nitrogen was supplied. While stirring the diamine solution, 10.54 g (47.0 mmol) of TA-1 was added, and NMP was further added to make the solid content concentration 12% by mass, and the mixture was stirred at 40° C. for 20 hours to obtain a polyamic acid solution (PAA-1).

[0244] The viscosity of the polyamic acid solution at a temperature of 25°C is 380 mPa·s. 60.0 g of the polyamic acid solution (PAA-1) was taken out into a 200 ml conical flask, 20.0 g of NMP was added thereto, and then 4.56 g of acetic anhydride and 1.18 g of pyridine were added, and the mixture was reacted at 55°C for 3 hours. The reaction solution was injected into 300 g of methanol, and the resulting precipitate was filtered out. The precipitate was washed with methanol and dried under reduced pressure at 80°C to obtain a polyimide powder. The imidization rate of the polyimide was 66%. 13.2 g of NMP and 13.2 g of GBL were added to 3.6 g of the obtained polyimide powder, and the mixture was dissolved by stirring at 70°C for 20 hours to obtain a polyimide solution (SPI-1).

[0245] <Synthesis Example 2 of PAA>

[0246] In a 50 ml four-necked flask equipped with a stirrer and a nitrogen inlet tube, 1.594 g (8.00 mmol) of DA-5 and 0.595 g (2.00 mmol) of DA-O1 were weighed, 33.1 g of NMP was added, and the mixture was dissolved by stirring while nitrogen was supplied. While stirring the diamine solution, 2.824 g (9.60 mmol) of TA-2 was added, and NMP was further added so that the solid content concentration became 12% by mass, and the mixture was stirred at 40° C. for 20 hours to obtain a polyamic acid solution (PAA-2).

[0247] The viscosity of the polyamic acid solution at 25° C. was 363 mPa·s.

[0248] <Synthesis Example 3 of PAA>

[0249] In a 50 ml four-necked flask equipped with a stirrer and a nitrogen inlet tube, 1.594 g (8.00 mmol) of DA-5 and 0.973 g (2.00 mmol) of DA-O3 were weighed, 35.4 g of NMP was added, and the mixture was dissolved by stirring while nitrogen was supplied. While stirring the diamine solution, 2.824 g (9.60 mmol) of TA-2 was added, and NMP was further added so that the solid content concentration became 12% by mass, and the mixture was stirred at 40° C. for 20 hours to obtain a polyamic acid solution (PAA-3).

[0250] The viscosity of the polyamic acid solution at 25° C. was 348 mPa·s.

[0251] <Synthesis Example 4 of PAA>

[0252] In a 50 ml four-necked flask equipped with a stirrer and a nitrogen inlet tube, 1.594 g (8.00 mmol) of DA-5 and 1.085 g (2.00 mmol) of DA-O4 were weighed, and 35.9 g of NMP was added, and stirred while nitrogen was supplied to dissolve. While stirring the diamine solution, 2.751 g (9.35 mmol) of TA-2 was added, and NMP was further added so that the solid content concentration became 12% by mass, and stirred at 40°C for 20 hours to obtain a polyamic acid solution (PAA-4).

[0253] The viscosity of the polyamic acid solution at 25° C. was 438 mPa·s.

[0254] <Synthesis Example 5 of PAA>

[0255] In a 100 ml four-necked flask equipped with a stirrer and a nitrogen inlet tube, 3.99 g (20.0 mmol) of DA-5 and 1.49 g (5.0 mmol) of DA-6 were weighed, and 78.0 g of NMP was added, and stirred while nitrogen was supplied to dissolve. While stirring the diamine solution, 6.77 g (23.0 mmol) of TA-2 was added, and NMP was further added so that the solid content concentration became 12% by mass, and stirred at 70° C. for 20 hours to obtain a polyamic acid solution (PAA-5).

[0256] The viscosity of the polyamic acid solution at 25° C. was 420 mPa·s.

[0257] <Example 1>

[0258] 1.88 g of the 12 mass % polyimide solution (SPI-1) obtained in Synthesis Example 5 and 4.38 g of the 12 mass % polyamic acid solution (PAA-2) obtained in Synthesis Example 6 were added to a 30 ml conical flask, 2.08 g of NMP, 3.67 g of GBL, and 3.00 g of BCS were added, and stirred at 25° C. for 2 hours to obtain a liquid crystal aligning agent (A1). It was confirmed that the liquid crystal aligning agent was a uniform solution without abnormalities such as turbidity and precipitation.

[0259] <Examples 2 and 3>

[0260] Liquid crystal aligning agents (A2) and (A3) were obtained in the same manner as in Example, except that the polyamic acid solutions (PAA-3) and (PAA-4) were used instead of the polyamic acid solution (PAA-2).

[0261] <Comparative Example 1>

[0262] 1.88 g of the 12 mass % polyimide solution (SPI-1) obtained in Synthesis Example 5 and 4.38 g of the 12 mass % polyamic acid solution (PAA-5) obtained in Synthesis Example 8 were added to a 30 ml conical flask, 2.08 g of NMP, 3.67 g of GBL, and 3.00 g of BCS were added, and stirred at 25° C. for 2 hours to obtain a liquid crystal aligning agent (B1). It was confirmed that the liquid crystal aligning agent was a uniform solution without abnormalities such as turbidity and precipitation.

[0263] [Table 1]

[0264]

[0265] <Example 4>

[0266] The liquid crystal aligning agent (A1) obtained in Example 1 was filtered through a 1.0 μm filter and then applied to the prepared substrate with electrodes and a glass substrate with a columnar spacer having an ITO film on the back and a height of 4 μm. After drying on a hot plate at 80°C for 2 minutes, it was fired in a hot air circulation oven at 230°C for 30 minutes to form a coating with a thickness of 100 nm. The coating surface was irradiated with 0.3 J / cm2 through a polarizing plate. 2 The ultraviolet light with a wavelength of 254 nm of linear polarization having an extinction ratio of 26:1 was calcined in a hot air circulation oven at 230°C for 30 minutes to obtain a substrate with a liquid crystal alignment film.

[0267] The two substrates thus obtained were set as a group, a sealant was applied on one substrate, and the other substrate was bonded with the liquid crystal alignment film facing each other and the alignment direction being 0°, and the sealant was cured to produce an empty box. Liquid crystal MLC-3019 (manufactured by MERCK) was injected into the empty box by a reduced pressure injection method, and the injection port was sealed to obtain an FFS driven liquid crystal box.

[0268] [Evaluation of afterimage based on long-term AC drive]

[0269] In a constant temperature environment of 60°C, an AC voltage of ±5V was applied to the above-mentioned liquid crystal box at a frequency of 60Hz. After applying the AC voltage for 120 hours, the pixel electrode and the counter electrode of the liquid crystal box were short-circuited and left at room temperature for one day. Then, the angle Δ of the liquid crystal box was measured, and the result was that the value of the angle Δ was 0.08 degrees.

[0270] [Evaluation of brush abrasion resistance]

[0271] The liquid crystal alignment agent was applied on the ITO substrate by spin coating, dried on a hot plate at 80°C for 2 minutes, and then baked in a hot air circulation oven at 230°C for 30 minutes to form a coating film with a thickness of 100 nm. The coating film surface was irradiated with 0.3 J / cm 2 The extinction ratio of the substrate was 26:1, and the linearly polarized ultraviolet light of wavelength 254nm was used. The substrate was fired in a hot air circulation oven at 230°C for 30 minutes to obtain a substrate with a liquid crystal alignment film. The brushing resistance of the obtained liquid crystal alignment film was evaluated according to the above evaluation method. As a result, no line marks caused by brushing were observed on the film surface, and the brushing resistance was good.

[0272] <Examples 5 and 6, Comparative Example 2>

[0273] Except that the liquid crystal aligning agents shown in Table 1 were used instead of the liquid crystal aligning agent (A1), the residual image evaluation and the brushing resistance evaluation based on long-term AC driving were carried out in the same manner as in Example 4. The evaluation results of the residual image caused by long-term AC driving and the evaluation results of the brushing resistance in each example are shown in Table 2.

[0274] [Table 2]

[0275]

[0276] Industrial Applicability

[0277] By using the liquid crystal alignment agent of the present invention, a liquid crystal alignment film having high mechanical strength and suppressing afterimages caused by AC driving in a liquid crystal display element of an IPS or FFS driving mode can be obtained. Therefore, it is expected to be used in a liquid crystal display element that pursues high display quality.

Claims

1. A liquid crystal aligning agent comprising the following polymer (A) and polymer (B), Polymer (A): at least one polymer selected from a polyimide precursor and a polyimide which is an imide product of the polyimide precursor, wherein the polyimide precursor is a reaction product of a diamine component including a diamine having a skeleton of the following formula (1) and a tetracarboxylic acid derivative component, The diamine having the skeleton of the formula (1) is at least one selected from the following formulas (2-1) to (2-3), The amount of the diamine having the skeleton of the formula (1) used is 5 to 50 mol% based on the total amount of the diamine components used to produce the polymer (A). In formula (1), R 1 represents hydrogen or a monovalent organic group, * represents a site bonded to other groups, In formula (2-1) to formula (2-3), R 1 represents hydrogen or a monovalent organic group, R 2 is selected from a single bond, -O-, -COO-, -OCO-, -(CH2) l -, -O(CH2) l O-、-CONR 11 -, -NR 11 CO- and -NR 11 -, or a divalent organic group consisting of a combination of these, W 1 represents a structure selected from the following group (3-1), W 2 represents a structure selected from the following group (3-2), W 3 represents a structure selected from the following group (3-3), W 4 represents a structure selected from the following group (3-4), wherein R 11 represents hydrogen or a monovalent organic group, l is an integer from 1 to 12, a represents an integer of 0 or 1, In the group (3-1), *1 represents the site bonded to the amino group in the formulae (2-1) to (2-3), and *2 represents the site bonded to the oxazoline ring. In the group (3-2), *1 represents the site bonded to the amino group in the formulae (2-1) to (2-3), and *3 represents the site bonded to R 2 Bonding site, group (3-3), *3 indicates R 2 The bonding site, in group (3-4), *2 represents the bonding site to the oxazoline ring, X represents a substituent, and represents a hydrogen atom; a halogen atom; an alkyl group having 1 to 6 carbon atoms; a halogenated alkyl group having 1 to 6 carbon atoms; a substituted amino group; an alkoxy group having 1 to 6 carbon atoms; an amide group, Polymer (B): at least one polymer selected from a polyimide precursor and a polyimide which is an imide product of the polyimide precursor, wherein the polyimide precursor is a reaction product of a diamine component containing at least one diamine selected from the following formulas (3) and (4) and a tetracarboxylic acid derivative component, In formulas (3) and (4), A1 is a single bond, an ether bond, an ester bond, an amide bond, a thioether bond, a thioester bond, an alkylene group having 2 to 20 carbon atoms, or a phenylene group, wherein any -CH2- of the alkylene group is optionally substituted by an ether group, an ester group, a cyclohexylene group, or a phenylene group; A2 is a halogen atom, a hydroxyl group, or an alkyl or alkoxy group having 1 to 5 carbon atoms, wherein any hydrogen atom of the alkyl or alkoxy group is optionally substituted by a halogen atom; a is an integer of 0 to 4; when a is greater than 2, A2 may be the same or different; and b and c are each independently an integer of 1 to 2.

2. The liquid crystal alignment agent according to claim 1, wherein The polymer (A) is polyamic acid.

3. The liquid crystal aligning agent according to claim 1 or 2, wherein: The mass ratio of polymer (A) to polymer (B) is 95:5 to 50:

50.

4. The liquid crystal aligning agent according to claim 1 or 2, wherein The tetracarboxylic acid derivative component of the polymer (A) contains aromatic tetracarboxylic dianhydride.

5. The liquid crystal aligning agent according to claim 1 or 2, wherein The diamine having a skeleton of the formula (1) is at least one selected from the following formulas (2-1-1) to (2-3-4), In formulas (2-1-1) to (2-3-4), R 1 represents hydrogen or a monovalent organic group, R 11 represents hydrogen or a monovalent organic group, n represents an integer of 1 to 6, and m represents an integer of 1 to 12.

6. The liquid crystal aligning agent according to claim 1 or 2, wherein: The tetracarboxylic acid derivative component of the polymer (B) contains a tetracarboxylic acid derivative having the following structure:

7. The liquid crystal aligning agent according to claim 1 or 2, wherein: The polymer (B) is a polyimide. 8 . A liquid crystal alignment film obtained from the liquid crystal alignment agent according to claim 1 . 9 . A liquid crystal display element comprising the liquid crystal alignment film according to claim 8 .

Citation Information

Patent Citations

  • Power source turning-on and-off circuit

    JP1986007911A

  • Liquid crystal alignment agent, liquid crystal alignment film, liquid crystal display element, retardation film, and manufacturing method of retardation film

    JP2015135393A

  • Liquid crystal alignment agent, liquid crystal alignment film, liquid crystal display, polymer, and compound

    JP2016118574A