Method for manufacturing nonvolatile magnetic memory and magnetic memory unit

By depositing a dielectric layer on the wafer and selective atomic layer deposition to form a magnetic nanowire track, the problem of difficulty in preparing high aspect ratio magnetic nanowire tracks in the existing technology is solved, and efficient memory density and capacity improvements are achieved.

CN113540343BActive Publication Date: 2024-10-15POSAI MICRO TECH (HANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110636393.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-08
Publication Date
2024-10-15
Estimated Expiration
2041-06-08

AI Technical Summary

Technical Problem

It is difficult to effectively prepare high-aspect-ratio magnetic nanowire tracks with existing technology, and traditional etching processes may damage magnetic materials and affect memory performance.

Method used

By depositing a dielectric layer on the wafer and forming a deep trench, filling and planarizing it, and then using selective atomic layer deposition to form a magnetic nanowire track on the magnetic nanowire track template to avoid etching of the magnetic material, Achieving high aspect ratio magnetic nanowire racetracks.

Benefits of technology

The preparation of magnetic nanowire tracks with a high aspect ratio is achieved, which avoids performance degradation caused by the etching process and improves the density and capacity of the memory.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113540343B_ABST
    Figure CN113540343B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for manufacturing a non-volatile magnetic memory and a magnetic memory unit, comprising the following steps: depositing a dielectric layer 1 on a wafer, and forming a deep groove in the dielectric layer 1 by an etching method; filling the deep groove with a dielectric layer 2, and performing a flattening treatment; forming a magnetic nanowire racetrack template in the dielectric layer 1 and the dielectric layer 2 by an etching method; forming a magnetic nanowire racetrack on the magnetic nanowire racetrack template by a selective atomic layer deposition method; completing the preparation of a read device and a write device. The present invention forms a dielectric template required for depositing a nanowire racetrack by an etching and deposition process, and then forms a magnetic nanowire racetrack by a selective atomic layer deposition method, thereby achieving a high aspect ratio without damaging the material properties of the magnetic nanowire racetrack, being able to prepare a magnetic nanowire racetrack with a high aspect ratio, and during the preparation process, it is not necessary to etch the magnetic material of the magnetic nanowire racetrack, thereby avoiding performance degradation caused by the etching process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of non-volatile magnetic memory, in particular to a method for manufacturing a non-volatile magnetic memory. Background Art

[0002] Magnetic racetrack memory is a non-volatile memory consisting of a magnetic nanowire racetrack connected by a circuit and corresponding read and write devices. The magnetic nanowire racetrack may contain multiple different magnetic domains, and adjacent magnetic domains are separated by magnetic domain walls. The arrangement of the magnetic domains (walls) represents the information stored in the magnetic nanowire racetrack. The new magnetic domain state can be written into the magnetic nanowire racetrack by the write device, and the arrangement of the magnetic domains can be read out by the read device to extract the stored information. The magnetic domains in the magnetic nanowire racetrack can move under the action of an external current. When the direction of the external current is changed, the direction of the movement of the magnetic domain also changes accordingly. Therefore, the magnetic domain pattern storing information can be driven by an external current to pass through the read device or the write device in sequence along the magnetic nanowire racetrack, and the magnetic domain is read or written bit by bit.

[0003] In order to increase the capacity and density of the memory, the magnetic nanowire track needs to have a higher aspect ratio so that more information can be stored on a smaller wafer area. It is difficult to prepare a magnetic nanowire track with a high aspect ratio through traditional etching and filling processes. At the same time, the etching process of the magnetic material may cause damage to the magnetic material, affecting the performance of the magnetic track memory. Therefore, it is necessary to find a new process method that can prepare a magnetic nanowire track with a high aspect ratio without damaging its performance. Summary of the invention

[0004] The object of the present invention is to provide a method for manufacturing a non-volatile magnetic memory to solve the above-mentioned deficiencies in the prior art.

[0005] In order to achieve the above object, the present invention provides the following technical solution: a method for manufacturing a non-volatile magnetic memory, comprising the following steps;

[0006] Depositing a dielectric layer 1 on a wafer, and forming a deep groove in the dielectric layer 1 by an etching method;

[0007] Filling the deep trench with a dielectric layer 2 and performing a planarization process;

[0008] A magnetic nanowire racetrack template is formed in dielectric layer 1 and dielectric layer 2 by an etching method;

[0009] A magnetic nanowire racetrack is formed on a magnetic nanowire racetrack template by a selective atomic layer deposition method;

[0010] Complete the preparation of read devices and write devices.

[0011] As a further description of the above technical solution: before the deposition of the magnetic nanowire racetrack, the surfaces of the dielectric layer 1 and the dielectric layer 2 are also treated to obtain better selectivity, wherein the treatment methods include but are not limited to wet cleaning and plasma treatment.

[0012] As a further description of the above technical solution: the dielectric layer 1 is any one of silicon oxide, silicon oxide containing doped elements, and silicon oxide containing voids.

[0013] As a further description of the above technical solution: the dielectric layer 2 is any one of silicon nitride or silicon nitride containing doped elements, and silicon nitride containing voids.

[0014] As a further description of the above technical solution: the deposition method of the dielectric layer 1 on the wafer is any one of a chemical vapor deposition process, an atomic layer deposition process, a spin coating process and a physical vapor deposition process.

[0015] As a further description of the above technical solution: forming a magnetic nanowire racetrack on a magnetic nanowire racetrack template is specifically to sequentially form a seed layer, a magnetic layer and a covering layer by a selective atomic layer deposition method.

[0016] As a further description of the above technical solution: the method of sequentially forming a seed layer, a magnetic layer and a covering layer by selective atomic layer deposition is to select suitable medium surface characteristics and precursors of the atomic layer deposition process so that the magnetic nanowire racetrack will only be deposited on the surface of the medium layer 2 and cannot be deposited on the surface of the medium layer 1, thereby finally forming a magnetic nanowire racetrack of a preset shape and size.

[0017] As a further description of the above technical solution: In the deposition process of the magnetic nanowire racetrack, one or more reduction reactions are required to remove excess oxygen elements in the film.

[0018] As a further description of the above technical solution: the preparation of the reading device and the writing device can be before the deposition of the magnetic nanowire racetrack or after the deposition of the magnetic nanowire racetrack.

[0019] A magnetic memory unit includes a magnetic nanowire racetrack, a writing device and a reading device; the magnetic nanowire racetrack is in a U-shaped structure, and the magnetization direction of the magnetic nanowire racetrack is perpendicular to the film surface, or parallel to the film surface, or forms an arbitrary angle with the film surface; the writing device and the magnetic nanowire racetrack form a magnetic tunnel junction structure; the reading device and the magnetic nanowire racetrack form a magnetic tunnel junction structure.

[0020] In the above technical scheme, the method for manufacturing a non-volatile magnetic memory provided by the present invention forms a dielectric template required for depositing a nanowire racetrack through etching and deposition processes, and then forms a magnetic nanowire racetrack through a selective atomic layer deposition method, thereby achieving a high aspect ratio without damaging the material properties of the magnetic nanowire racetrack. A magnetic nanowire racetrack with a high aspect ratio can be prepared, and the magnetic material of the magnetic nanowire racetrack does not need to be etched during the preparation process, thereby avoiding performance degradation caused by the etching process.

[0021] Since the above-mentioned method for manufacturing the non-volatile magnetic memory has the above-mentioned technical effects, the magnetic memory unit corresponding to the method naturally has the corresponding technical effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.

[0023] Figure 1 A schematic flow chart of a method for manufacturing a non-volatile magnetic memory provided by an embodiment of the present invention;

[0024] Figure 2 A schematic diagram of the structure of a deposited dielectric layer 1 provided in an embodiment of the present invention;

[0025] Figure 3 A schematic diagram of a structure for forming a deep trench in a dielectric layer 1 according to an embodiment of the present invention;

[0026] Figure 4 A schematic diagram of a structure in which a dielectric layer 2 is filled in a deep trench according to an embodiment of the present invention;

[0027] Figure 5 A schematic diagram of a structure of a magnetic nanowire racetrack template formed in dielectric layer 1 and dielectric layer 2 according to an embodiment of the present invention;

[0028] Figure 6 A schematic diagram of a structure for forming a magnetic nanowire racetrack on a magnetic nanowire racetrack template provided by an embodiment of the present invention;

[0029] Figure 7 A schematic diagram of a structure for completing the preparation of a read device and a write device provided in an embodiment of the present invention;

[0030] Figure 8 A schematic structural diagram of a nonvolatile magnetic memory provided by another embodiment of the present invention;

[0031] Fig. 9A schematic structural diagram of a nonvolatile magnetic memory provided by yet another embodiment of the present invention;

[0032] Fig.10 A schematic diagram of the structure of a non-volatile magnetic memory unit provided by an embodiment of the present invention;

[0033] Fig.11 A schematic diagram of the structure of a magnetic nanowire racetrack provided by an embodiment of the present invention;

[0034] Fig.12 A schematic diagram of the structure of the arrangement of the read / write device provided in an embodiment of the present invention;

[0035] Fig.13 A schematic structural diagram of a nonvolatile magnetic memory unit provided by another embodiment of the present invention;

[0036] Fig.14 A schematic structural diagram of a nonvolatile magnetic memory unit provided by yet another embodiment of the present invention;

[0037] Fig.15 A schematic structural diagram of a nonvolatile magnetic memory unit provided in yet another embodiment of the present invention.

[0038] Description of reference numerals:

[0039] 100, magnetically selected nanowire racetrack; 1100, covering layer; 1200, magnetic layer; 1300, seed layer; 200, writing device; 300, reading device; 220, reading and writing device; 440, magnetic domain a; 441, magnetic domain b; 442, magnetic domain c; 443, magnetic domain d; 450, magnetic domain e; 451, magnetic domain f;. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.

[0041] See also Figure 1-9 , an embodiment of the present invention provides a technical solution: a method for manufacturing a non-volatile magnetic memory, comprising the following steps;

[0042] Depositing a dielectric layer 1 on a wafer, and forming a deep groove in the dielectric layer 1 by an etching method;

[0043] Filling the deep trench with a dielectric layer 2 and performing a planarization process;

[0044] A magnetic nanowire racetrack template is formed in dielectric layer 1 and dielectric layer 2 by an etching method;

[0045] A magnetic nanowire racetrack is formed on a magnetic nanowire racetrack template by a selective atomic layer deposition method;

[0046] Complete the preparation of read devices and write devices.

[0047] Specifically, a dielectric layer 1 is deposited on a wafer, and a deep groove is formed in the dielectric layer 1 by an etching method, wherein the wafer contains part of the circuits and interconnection structures required for the magnetic racetrack memory, including but not limited to transistors, selection devices, resistors, capacitors, inductors, wires, contacts, power supplies, etc. A dielectric layer 2 is filled in the deep groove and flattened. The flattening process is performed by chemical mechanical polishing or etching. A magnetic nanowire racetrack template is formed in the dielectric layer 1 and the dielectric layer 2 by an etching method. More specifically, a deep groove is formed in the dielectric layer 2 by an etching method. At this time, the shape and size of the dielectric layer 2 are consistent with the desired magnetic racetrack. The shape and size of the nanowire track are matched. The magnetic nanowire track uses the patterned dielectric layer 2 as a template. After the selective atomic layer deposition method is used, by selecting the appropriate dielectric surface properties and the precursor of the atomic layer deposition process, the magnetic nanowire track will only be deposited on the surface of the dielectric layer 2, and cannot be deposited on the surface of the dielectric layer 1, thereby forming the desired shape and size, and then the read device and the write device are prepared, wherein the read device and the write device can be located at different positions of the magnetic nanowire track, such as the top, side, bottom, etc. Further, the read device is composed of a magnetic tunnel junction or a magnetic sensor. The write device is composed of a magnetic tunnel junction or a current conductor. The magnetic tunnel junction or the magnetic sensor is formed by processes such as thin film deposition, photolithography, etching and chemical mechanical polishing. Further, the read device and the write device may be the same device, both of which are magnetic tunnel junctions.

[0048] Before the deposition of the magnetic nanowire racetrack, the surfaces of the dielectric layer 1 and the dielectric layer 2 are treated to obtain better selectivity, wherein the treatment methods include but are not limited to wet cleaning and plasma treatment.

[0049] The dielectric layer 1 is any one of silicon oxide, silicon oxide containing doped elements, and silicon oxide containing voids. The dielectric layer 2 is any one of silicon nitride, silicon nitride containing doped elements, and silicon nitride containing voids. The doped silicon oxide and the doped silicon nitride are doped with elements such as carbon, hydrogen, and phosphorus.

[0050] The deposition method of the dielectric layer 1 on the wafer is any one of a chemical vapor deposition process, an atomic layer deposition process, a spin coating process and a physical vapor deposition process. The magnetic nanowire racetrack is formed on the magnetic nanowire racetrack template by selective atomic layer deposition. The method of sequentially forming the seed layer, the magnetic layer and the covering layer by selective atomic layer deposition is to select suitable dielectric surface properties and precursors of the atomic layer deposition process so that the magnetic nanowire racetrack will only be deposited on the surface of the dielectric layer 2, and cannot be deposited on the surface of the dielectric layer 1, and finally form a magnetic nanowire racetrack of a preset shape and size. Specifically, the seed layer material includes W, WNx, Hf, Ti, TiNx, Ru, Ir, Pt, Ta, TaNx, etc., and the corresponding precursors include WF 6 +SiH 4 , W.F. 6 +B 2 H 6 , Hf(NMe 2 ) 4 +H 2 O, Ti(O i Pr) 4 , TiCl 4 +H 2 O,RuCp 2 +O2,Ir(acac)3+O,MeCpPtMe 2 , Ta(N t Bu)(NEt 2 ) 3 , Ta(N t Bu)(NEt 2 ) 2 , and the thickness of the seed layer is 1-10nm; the magnetic layer material includes Co, Ni, etc., and the corresponding precursors include (C 5 H 5 )Co(η 4 -CH 2 CHC(Me)CH 2 ), Co 2 (CO) 8 ,CCTBA,Co(Cp) 2 ,Co(Cp)(CO) 2 ,Ni(dmamp) 2 , Ni(acac) 2 ,Ni(Me i PrCOCN t Bu) 2, Ni(Cp)allyl, etc. The thickness of the magnetic layer ranges from 1-50nm; the covering layer materials include W, WNx, Hf, Ti, TiNx, Ru, Ir, Pt, Ta, TaNx, etc., and the corresponding precursors include WF 6 +SiH 4 , W.F. 6 +B 2 H 6 , W.F. 6 +NH 3 , Hf(NMe 2 ) 4 +H 2 O, Ti(O i Pr) 4 , TiCl 4 +H 2 O,RuCp 2 +O 2 ,Ir(acac) 3 +O,MeCpPtMe 2 , Ta(N t Bu)(NEt 2 ) 3 , Ta(N t Bu)(NEt 2 ) 2 etc., the thickness of the covering layer ranges from 2-10 nm.

[0051] In the deposition process of the magnetic nanowire track, one or more reduction reaction treatments are required. Reducing gases, such as hydrogen and deuterium, are used to reduce the thin film formed by atomic layer deposition to remove excess oxides in the film. Furthermore, after the reduction reaction, the properties of the magnetic thin film material are measured, such as resistivity, saturation magnetic moment, coercive force, various anisotropic properties, etc. The testing equipment includes a four-point probe station, a BH Loop tester, an AGM tester, a VSM tester, and a SQUID tester. If the above characteristics are similar to those of the unoxidized magnetic thin film material, it can be considered that the reduction reaction has achieved the expected effect and the reduction reaction treatment is stopped.

[0052] The preparation of the read device and the write device can be before or after the deposition of the magnetic nanowire racetrack.

[0053] like Fig.10As shown, the magnetic memory unit includes a magnetic nanowire racetrack 100, a writing device 200 and a reading device 300; the magnetic nanowire racetrack 100 is in a U-shaped structure, and the magnetization direction of the magnetic nanowire racetrack 100 is perpendicular to the film surface, or parallel to the film surface, or forms an arbitrary angle with the film surface; the reading device 300 can form a magnetic tunnel junction structure with the magnetic nanowire racetrack 100, wherein the magnetic domain in the magnetic nanowire racetrack 100 constitutes a magnetic electrode of the "read MTJ", and the reading device 300 includes a tunneling barrier layer and a second magnetic electrode of the read MTJ. When the magnetization direction of the magnetic domain in the magnetic nanowire racetrack 100 changes, the resistance value of the read MTJ changes, and the stored information can be read by the change of the resistance value. The reading device 300 can also be an independent magnetic sensor, which may or may not have direct electrical contact with the magnetic nanowire racetrack 100, and reads the stored information by sensing the magnetic field generated by the magnetic domain (wall). The writing device 200 can form a "write MTJ" structure with the magnetic nanowire racetrack 100. The magnetic domains in the magnetic nanowire racetrack 100 constitute a magnetic electrode of the write MTJ, and the write device 200 includes a tunneling barrier layer and a second magnetic electrode of the write MTJ. When a write current is applied to the write MTJ, the spin transfer torque effect, the spin Hall effect, or a combination of the two generated by the current can change the magnetization direction of the magnetic domains in the magnetic nanowire racetrack 100, thereby writing data. The write device 200 can also be a metal wire. When the current passes through the metal wire, the magnetic field generated by the current causes the direction of the magnetic domains in the magnetic nanowire racetrack 100 to change, thereby writing data. The write device 200 may or may not have direct electrical contact with the magnetic nanowire racetrack 100. Each magnetic nanowire racetrack 100 can have a separate write device 200, or multiple magnetic nanowire racetracks can share one write device 200. The write device 200 and the read device 300 can be located on the top, side, or bottom of the magnetic nanowire racetrack 100.

[0054] In another embodiment provided by the present invention, Fig.11As shown, the non-volatile magnetic memory cell includes a magnetic nanowire racetrack 100, a writing device 200 and a reading device 300. The magnetic nanowire racetrack 100 includes a seed layer 1300, a magnetic layer 1200 and a covering layer 1100 and other multi-layer materials. The magnetic layer 1200 may include multiple layers of magnetic and non-magnetic films. Each magnetic film may be separated by different non-magnetic films and have mutual exchange coupling. Common mutual exchange coupling exists in artificial antiferromagnetic (SAF) structures. In this structure, adjacent magnetic films are exchange-coupled through non-magnetic films (such as Ru, Ir, Rh, Re, Os, Cr, etc.) between each other to achieve reverse arrangement of the magnetic moment directions of adjacent magnetic films. Another common mutual exchange coupling exists in artificial ferromagnetic structures. In this structure, adjacent magnetic films are exchange-coupled through non-magnetic films (such as Ru, Ir, Rh, Re, Os, Mo, Ta, W, Ti, Cr, Hf, Nb, Zr, Pt, Pd, Al, Mg, V, etc.) between each other, so as to achieve the same direction arrangement of the magnetic moments of adjacent magnetic films. There may be one or more of the following actions or effects between the magnetic layer 1200 and the seed layer 1300 and the cover layer 1100 in the magnetic nanowire racetrack 100: exchange bias, spin Hall effect, DM interaction, and Rashba effect. Under the action of an external current, one or more of the above actions or effects can affect the movement of the magnetic domains in the magnetic nanowire racetrack 100 together with the spin transfer torque (STT) effect generated by the current.

[0055] In another embodiment provided by the present invention, Fig.12 As shown, the non-volatile magnetic memory unit includes a magnetic nanowire racetrack 100 and a read-write device 220. The read device and the write device are the same device, namely the read-write device 220. The read-write device 220 and the magnetic nanowire racetrack 100 constitute a "read-write MTJ" structure. The magnetic domains in the magnetic nanowire racetrack 100 constitute a magnetic electrode of the read-write MTJ, and the read-write device 220 includes a tunneling barrier layer and a second magnetic electrode of the read-write MTJ. When the magnetization direction of the magnetic domains in the magnetic nanowire racetrack 100 changes, the resistance value of the read-write MTJ changes, and the stored information can be read by the change of the resistance value. When a write current is applied to the read-write MTJ, the spin transfer torque effect, the spin Hall effect, or a combination of the two generated by the current can change the magnetization direction of the magnetic domains in the magnetic nanowire racetrack 100, thereby writing data and completing the write operation. The read-write device 220 can be located at the top, side, or bottom of the magnetic nanowire racetrack 100.

[0056] In another embodiment provided by the present invention, Fig.13As shown, the non-volatile magnetic memory unit includes a magnetic nanowire racetrack 100, a writing device 200 and a reading device 300. The magnetic nanowire racetrack 100 is in the shape of a plurality of "U"s connected in sequence. The magnetization direction of the magnetic nanowire racetrack 100 can be perpendicular to the film surface, parallel to the film surface, or form any angle with the film surface.

[0057] In another embodiment provided by the present invention, Fig.14 As shown, the magnetic nanowire racetrack 100 contains multiple magnetic domains, such as magnetic domain a440 and magnetic domain b441. The reading device 300 can form a reading MTJ structure with the magnetic nanowire racetrack 100. The magnetic domain 441 in the magnetic nanowire racetrack 100 constitutes a magnetic electrode for reading the MTJ, and the reading device 300 includes a tunneling barrier layer and a second magnetic electrode for reading the MTJ. When the magnetization direction of the magnetic domain b441 in the magnetic nanowire racetrack 100 changes, the resistance value of the reading MTJ changes, and the stored information can be read by the change in the resistance value. The reading device 300 can also be an independent magnetic sensor, which may or may not have direct electrical contact with the magnetic nanowire racetrack 100, and reads the stored information by sensing the magnetic field generated by the magnetic domain (wall).

[0058] The writing device 200 can form a writing MTJ structure with the magnetic nanowire racetrack 100. The magnetic domain a440 in the magnetic nanowire racetrack 100 constitutes a magnetic electrode of the writing MTJ, and the writing device 100 includes a tunneling barrier layer and a second magnetic electrode of the writing MTJ. When a writing current is applied to the writing MTJ, the spin transfer torque effect, the spin Hall effect, or a combination of the two generated by the current can change the magnetization direction of the magnetic domain a440, thereby writing data. The writing device 200 can also be a metal wire. When the current passes through the metal wire, the magnetic field generated by the current causes the magnetic moment direction of the magnetic domain a440 to change, thereby writing data. The writing device 200 may or may not have direct electrical contact with the magnetic nanowire racetrack 100. Each magnetic nanowire racetrack 100 can have a separate writing device 200, or a plurality of magnetic nanowire racetracks can share a writing device 200. The writing device 200 and the reading device 300 can be located at the top, side, or bottom of the magnetic nanowire racetrack 100. Adjacent magnetic domains within the magnetic nanowire racetrack may have the same magnetic moment direction, such as magnetic domain c442 and magnetic domain d443.

[0059] In another embodiment provided by the present invention, Fig.15As shown, the magnetic nanowire racetrack 100 contains multiple magnetic domains, such as magnetic domain e450 and magnetic domain f451. When an external current 3000 flows through the magnetic nanowire racetrack 100, the magnetic domain can move as a whole along the magnetic nanowire racetrack 100, and the direction of movement is related to the direction of the current. The reading device 300 can form a reading MTJ structure with the magnetic nanowire racetrack 100. The magnetic domain f451 in the magnetic nanowire racetrack 100 constitutes a magnetic electrode for reading MTJ, and the reading device 300 includes a tunneling barrier layer and a second magnetic electrode for reading MTJ. When the magnetization direction of the magnetic domain f451 in the magnetic nanowire racetrack 100 changes, the resistance value of the reading MTJ changes, and the stored information can be read by the change in the resistance value. The reading device 300 can also be an independent magnetic sensor, which may or may not have direct electrical contact with the magnetic nanowire racetrack 100, and reads the stored information by sensing the magnetic field generated by the magnetic domain (wall).

[0060] The writing device 200 can form a writing MTJ structure with the magnetic nanowire racetrack 100. The magnetic domain e450 in the magnetic nanowire racetrack 100 constitutes a magnetic electrode of the writing MTJ, and the writing device 200 includes a tunneling barrier layer and a second magnetic electrode of the writing MTJ. When a writing current is applied to the writing MTJ, the spin transfer torque effect, or the spin Hall effect, or a combination of the two generated by the current can change the magnetization direction of the magnetic domain e450, thereby writing data. The writing device 200 can also be a metal wire. When the current passes through the metal wire, the magnetic field generated by the current causes the magnetic moment direction of the magnetic domain e450 to change, thereby writing data. The writing device 200 may or may not have direct electrical contact with the magnetic nanowire racetrack 100. Each magnetic nanowire racetrack 100 can have a separate writing device 200, or a plurality of magnetic nanowire racetracks can share a writing device 200.

[0061] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the above drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.

Claims

1. A method for manufacturing a non-volatile magnetic memory, characterized in that: The steps include: Depositing a dielectric layer 1 on a wafer, and forming a deep groove in the dielectric layer 1 by an etching method; Filling the deep trench with a dielectric layer 2 and performing a planarization process; A magnetic nanowire racetrack template is formed in dielectric layer 1 and dielectric layer 2 by an etching method; A magnetic nanowire racetrack is formed on a magnetic nanowire racetrack template by a selective atomic layer deposition method; Complete the preparation of read devices and write devices; Before the magnetic nanowire racetrack is deposited, the surface of the dielectric layer 1 and the dielectric layer 2 is treated to obtain better selectivity, wherein the treatment method is selected from wet cleaning and plasma treatment; The dielectric layer 1 is silicon oxide or silicon oxide containing doped elements; The dielectric layer 2 is silicon nitride or silicon nitride containing doped elements; The magnetic nanowire racetrack is formed on the magnetic nanowire racetrack template by sequentially forming a seed layer, a magnetic layer and a covering layer by a selective atomic layer deposition method; The method of sequentially forming a seed layer, a magnetic layer and a covering layer by selective atomic layer deposition is as follows: by selecting appropriate medium surface characteristics and precursors of the atomic layer deposition process, the magnetic nanowire racetrack is only deposited on the surface of the medium layer 2, but not on the surface of the medium layer 1, thereby finally forming a magnetic nanowire racetrack of a preset shape and size.

2. The method for manufacturing a non-volatile magnetic memory according to claim 1, characterized in that: The deposition method of the dielectric layer 1 on the wafer is any one of a chemical vapor deposition process, an atomic layer deposition process, a spin coating process and a physical vapor deposition process.

3. The method for manufacturing a non-volatile magnetic memory according to claim 1, characterized in that: In the deposition process of the magnetic nanowire racetrack, one or more reduction reactions are performed to remove excess oxygen elements in the film.

4. The method for manufacturing a non-volatile magnetic memory according to claim 1, characterized in that: The preparation of the reading device and the writing device can be before the deposition of the magnetic nanowire racetrack or after the deposition of the magnetic nanowire racetrack.

5. The magnetic memory unit manufactured by the method for manufacturing a non-volatile magnetic memory according to claim 1, characterized in that: Including magnetic nanowire racetrack, writing device and reading device; The magnetic nanowire racetrack has a U-shaped structure, and the magnetization direction of the magnetic nanowire racetrack is perpendicular to the film surface, or parallel to the film surface, or forms an arbitrary angle with the film surface; The writing device and the magnetic nanowire racetrack form a magnetic tunnel junction structure; The reading device and the magnetic nanowire racetrack form a magnetic tunnel junction structure.