A flame retardant electric heating cable

By using a combination of organic and inorganic mixed flame retardants, fiber flame retardants and auxiliary flame retardants on the electric heating tape, a dense flame retardant material layer is formed, which solves the problem of insufficient flame retardant performance of the traditional electric heating tape and achieves Stronger temperature control and protection effect.

CN113556833BActive Publication Date: 2024-10-18ANBANG ELECTRICAL GRP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202110834428.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-23
Publication Date
2024-10-18
Estimated Expiration
2041-07-23

AI Technical Summary

Technical Problem

The peripheral flame retardant performance of traditional electric heating tape is not ideal and cannot effectively limit the heating temperature and prevent burning.

Method used

It uses an organic-inorganic hybrid flame retardant composed of antimony trioxide, aluminum hydroxide and organic halide flame retardant, combined with modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber. Similar flame retardants, as well as auxiliary flame retardants such as diatomite, calcined clay, silicone oil and zinc borate, form a dense flame retardant material layer to enhance the flame retardant performance of the electric heating tape.

Benefits of technology

The flame retardant performance of the electric heating tape is significantly improved, which can effectively limit the heating temperature and prevent burning. It has a stronger protective effect than the traditional electric heating tape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003176577360000161
    Figure BDA0003176577360000161
  • Figure BDA0003176577360000171
    Figure BDA0003176577360000171
  • Figure BDA0003176577360000172
    Figure BDA0003176577360000172
Patent Text Reader

Abstract

The present invention discloses a flame-retardant electric heating tape, comprising two tinned copper wires located in the innermost layer, a PTC conductive heating layer wrapped around the outer periphery of the tinned copper wires, an insulating layer wrapped around the outer periphery of the PTC conductive heating layer, a metal shielding layer wrapped around the outer periphery of the insulating layer, and a reinforced protective flame-retardant layer located in the outermost layer, wherein the reinforced protective flame-retardant layer located in the outermost layer is composed of a reinforced metal mesh and a flame-retardant material layer wrapped around the surface of the reinforced metal mesh. The present invention can effectively improve the flame-retardant properties of the flame-retardant material layer on the surface of the electric heating tape by using an organic-inorganic mixed flame retardant composed of antimony trioxide, aluminum hydroxide, and an organic halide flame retardant; the present invention can effectively improve the flame-retardant properties of the flame-retardant material layer on the surface of the electric heating tape by using a fiber-type flame retardant composed of modified basalt fiber, polyphenylsulfone terephthalamide fiber, and polycrystalline mullite fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention and the technical field of electric heating belts specifically relate to a flame retardant electric heating belt. Background Art

[0002] The electric heating cable is composed of a conductive polymer and two parallel metal wires and an insulating sheath. Its characteristics are that the conductive polymer has a very high positive temperature coefficient characteristic, and is connected in parallel with each other, and can automatically adjust the output power with the temperature change of the heated system, automatically limit the heating temperature, can be arbitrarily shortened or extended within a certain range, and allows multiple cross-overlaps without the worry of high-temperature hot spots and burning; the flame retardant performance of the outer layer of the general electric heating cable is not very ideal. In view of this, we propose a flame-retardant electric heating cable. Summary of the invention

[0003] In order to make up for the above deficiencies, the present invention provides a flame retardant electric heating tape.

[0004] The technical solution of the present invention is:

[0005] A flame retardant electric heating tape comprises two tinned copper wires in the innermost layer, a PTC conductive heating layer wrapped around the tinned copper wires, an insulating layer wrapped around the PTC conductive heating layer, a metal shielding layer wrapped around the insulating layer, and a reinforced protective flame retardant layer in the outermost layer, wherein the reinforced protective flame retardant layer in the outermost layer is composed of a reinforced metal mesh and a flame retardant material layer wrapped around the surface of the reinforced metal mesh.

[0006] As a preferred embodiment of the present invention, the flame retardant material layer is prepared from an organic-inorganic mixed flame retardant, a fiber flame retardant and an auxiliary flame retardant, wherein the composition ratio of the three is: 45% organic-inorganic mixed flame retardant, 40% fiber flame retardant, and 15% auxiliary flame retardant.

[0007] As a preferred embodiment of the present invention, the organic-inorganic hybrid flame retardant includes an organic flame retardant material and an inorganic flame retardant material, and the composition ratio of the two is: 45% organic flame retardant material, 55% inorganic flame retardant material, wherein the inorganic flame retardant material uses antimony trioxide and aluminum hydroxide, and the composition ratio of the two is: 45% antimony trioxide, 55% aluminum hydroxide, and the organic flame retardant material uses an organic halide flame retardant, and the organic halide flame retardant is selected from one or more of decabromobiphenyl acid, tetrabromobisphenol, brominated polystyrene, chlorinated paraffin and chlorinated polyethylene.

[0008] As a preferred embodiment of the present invention, the fiber flame retardant includes the following components: modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber, wherein the composition ratio of the three is: 40% of modified basalt fiber, 35% of polyphenylsulfone terephthalamide fiber and 25% of polycrystalline mullite fiber.

[0009] As a preferred embodiment of the present invention, the auxiliary flame retardant includes the following components: diatomaceous earth, calcined clay, silicone oil, zinc borate and pure water, wherein the composition ratio of the five is: 30% diatomaceous earth, 25% calcined clay, 20% silicone oil, 18% zinc borate and 7% pure water.

[0010] As a preferred embodiment of the present invention, the method for preparing the flame retardant material layer comprises the following steps:

[0011] Step 1: Prepare the corresponding amount of each ingredient according to its composition ratio, and place them separately for later use after preparation;

[0012] Step 2: After aluminum hydroxide is micronized, it is fully mixed with antimony trioxide to form an inorganic flame retardant material, and then an organic halide flame retardant is added to the mixed inorganic flame retardant material, and the two are fully mixed to form an organic-inorganic mixed flame retardant;

[0013] Step 3: The modified basalt fiber, the polyphenylsulfone terephthalamide fiber and the polycrystalline mullite fiber are fully minced to form powder particles, and then the powder particles formed by the three minced particles are put into a mixing device for full mixing to form a fiber flame retardant;

[0014] Step 4: Place diatomaceous earth, calcined clay, and zinc borate together and stir them thoroughly, then pour a mixed liquid of silicone oil and pure water into the mixture, and stir them thoroughly to form an auxiliary flame retardant;

[0015] Step 5: Mix the organic-inorganic mixed flame retardant, the fiber flame retardant and the auxiliary flame retardant together, and stir them fully to make the three mixed fully and evenly to form a viscous flame retardant material;

[0016] Step 6: Apply the viscous flame retardant material evenly on the outermost reinforced metal mesh surface of the electric heating cable, apply three layers in total, until a dense flame retardant material layer is formed on the reinforced metal mesh surface, place the electric heating cable coated with the flame retardant material in a drying equipment for drying, and wait until the flame retardant material layer is completely dry and formed.

[0017] As a preferred embodiment of the present invention, when aluminum hydroxide and antimony trioxide are mixed in step 2, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained between 25°C and 35°C, and the mixing time is 15min to 25min. When the organic halide flame retardant and the inorganic flame retardant material are mixed, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained between 22°C and 38°C, and the mixing time is 18min to 28min.

[0018] As a preferred embodiment of the present invention, in step three, the temperature of the modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber in the grinding process is maintained between 35°C and 45°C, and the grinding time is 20min to 30min. When the powder particles formed by the three are mixed, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained between 32°C and 42°C, and the mixing time is 20min to 30min.

[0019] As a preferred embodiment of the present invention, in step 4, when diatomaceous earth, calcined clay and zinc borate are mixed, the stirring speed of the mixing equipment is 250r / min, the temperature in the mixing equipment is maintained between 28°C and 36°C, and the mixing time is 18min to 26min. When mixing with silicone oil and pure water, the stirring speed of the mixing equipment is 250r / min, the temperature in the mixing equipment is maintained between 32°C and 38°C, and the mixing time is 22min to 28min.

[0020] As a preferred embodiment of the present invention, when the organic-inorganic mixed flame retardant, fiber flame retardant and auxiliary flame retardant are mixed in step five, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained between 35°C and 40°C, and the mixing time is 30min to 40min; in step six, the coating thickness of each layer of flame retardant material is not less than 0.05mm, the drying temperature of the electric heating after coating the flame retardant material is maintained between 55°C and 75°C, and the drying time is 35min to 55mim.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention can effectively improve the flame retardant performance of the flame retardant material layer on the surface of the electric heating belt through the organic-inorganic mixed flame retardant composed of antimony trioxide, aluminum hydroxide and organic halide flame retardant;

[0023] 2. The present invention can effectively improve the flame retardant properties of the flame retardant material layer on the surface of the electric heating cable by using the fiber flame retardant composed of modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber;

[0024] 3. The present invention can effectively improve the flame retardant properties of the flame retardant material layer on the surface of the electric heating cable by using the auxiliary flame retardant composed of diatomaceous earth, calcined clay, silicone oil, zinc borate and pure water. DETAILED DESCRIPTION

[0025] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1

[0027] The present embodiment provides a flame-retardant electric heating tape, including two tinned copper wires located in the innermost layer, a PTC conductive heating layer wrapped around the tinned copper wires, an insulating layer wrapped around the PTC conductive heating layer, a metal shielding layer wrapped around the insulating layer, and a reinforced protective flame-retardant layer located in the outermost layer, wherein the reinforced protective flame-retardant layer located in the outermost layer is composed of a reinforced metal mesh and a flame-retardant material layer wrapped around the surface of the reinforced metal mesh.

[0028] As a preferred embodiment of this embodiment, the flame retardant material layer is prepared from an organic-inorganic mixed flame retardant, a fiber flame retardant and an auxiliary flame retardant, wherein the composition ratio of the three is: 45% organic-inorganic mixed flame retardant, 40% fiber flame retardant, and 15% auxiliary flame retardant.

[0029] As a preferred embodiment of the present invention, the organic-inorganic hybrid flame retardant includes an organic flame retardant material and an inorganic flame retardant material, and the composition ratio of the two is: 45% organic flame retardant material, 55% inorganic flame retardant material, wherein the inorganic flame retardant material uses antimony trioxide and aluminum hydroxide, and the composition ratio of the two is: 45% antimony trioxide, 55% aluminum hydroxide, and the organic flame retardant material uses an organic halide flame retardant, and the organic halide flame retardant is decabromobiphenyl acid.

[0030] Antimony trioxide and aluminum hydroxide are both inorganic compounds, which have a high melting point. Organic halide flame retardants also have a high melting point. The combination of antimony trioxide, aluminum hydroxide and organic halide flame retardants can effectively combine the chemical properties of the three and achieve better flame retardant properties.

[0031] As a preferred embodiment of this embodiment, the fiber flame retardant includes the following components: modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber, wherein the composition ratio of the three is: modified basalt fiber 40%, polyphenylsulfone terephthalamide fiber 35%, polycrystalline mullite fiber 25%.

[0032] Modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber all have high melting points. Not only that, the strength of the three materials is also high, but they also have many excellent properties such as electrical insulation, corrosion resistance, and high temperature resistance. The fiber flame retardant formed by combining the three together can effectively improve the flame retardant properties of the entire electric heating belt.

[0033] As a preferred embodiment of this embodiment, the auxiliary flame retardant includes the following ingredients: diatomaceous earth, calcined clay, silicone oil, zinc borate and pure water, wherein the composition ratio of the five is: 30% diatomaceous earth, 25% calcined clay, 20% silicone oil, 18% zinc borate and 7% pure water.

[0034] The density of diatomite is 1.9-2.3g / cm3, the bulk density is 0.34-0.65g / cm3, the specific surface area is 40-65㎡ / g, and the pore volume is 0.45-0.98cm 3 / g, water absorption is 2-4 times of its own volume, melting point is 1650℃-1750℃, special porous structure can be observed under electron microscope, these excellent physical properties determine its excellent flame retardant performance; calcined clay has excellent freeze-thaw resistance, it can freeze and thaw 50 times at -45℃ without cracks, good weathering and corrosion resistance, its internal structure is not easily affected by acidic substances, and calcined clay also has a high melting point and excellent flame retardant performance; silicone oil has a very small vapor pressure, high With a flash point and ignition point, and a relatively low freezing point, silicone oil has heat resistance, electrical insulation, weather resistance, hydrophobicity, physiological inertness, and a relatively small surface tension. In addition, it has a low viscosity-temperature coefficient and high compression resistance. Zinc borate can be used as a multifunctional synergistic additive for antimony oxide or other halogen flame retardants, which can effectively improve the flame retardant properties, reduce the generation of smoke during combustion, and adjust the chemical, mechanical, and electrical properties of rubber and plastic products. Combining these four substances to form an auxiliary flame retardant can achieve excellent flame retardant properties for electric heating cables.

[0035] As a preferred embodiment of the present invention, the method for preparing the flame retardant material layer comprises the following steps:

[0036] Step 1: Prepare the corresponding amount of each ingredient according to its composition ratio, and place them separately for later use after preparation;

[0037] Step 2: After aluminum hydroxide is micronized, it is fully mixed with antimony trioxide to form an inorganic flame retardant material, and then an organic halide flame retardant is added to the mixed inorganic flame retardant material, and the two are fully mixed to form an organic-inorganic mixed flame retardant;

[0038] Step 3: The modified basalt fiber, the polyphenylsulfone terephthalamide fiber and the polycrystalline mullite fiber are fully minced to form powder particles, and then the powder particles formed by the three minced particles are put into a mixing device for full mixing to form a fiber flame retardant;

[0039] Step 4: Place diatomaceous earth, calcined clay, and zinc borate together and stir them thoroughly, then pour a mixed liquid of silicone oil and pure water into the mixture, and stir them thoroughly to form an auxiliary flame retardant;

[0040] Step 5: Mix the organic-inorganic mixed flame retardant, the fiber flame retardant and the auxiliary flame retardant together, and stir them fully to make the three mixed fully and evenly to form a viscous flame retardant material;

[0041] Step 6: Apply the viscous flame retardant material evenly on the outermost reinforced metal mesh surface of the electric heating cable, apply three layers in total, until a dense flame retardant material layer is formed on the reinforced metal mesh surface, place the electric heating cable coated with the flame retardant material in a drying equipment for drying, and wait until the flame retardant material layer is completely dry and formed.

[0042] As a preferred embodiment of the present invention, when aluminum hydroxide and antimony trioxide are mixed in step 2, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained at 25°C, and the mixing time is 15 min. When the organic halide flame retardant and the inorganic flame retardant material are mixed, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained at 22°C, and the mixing time is 18 min.

[0043] As a preferred embodiment of the present invention, in step three, the temperature of the modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber in the grinding process is maintained at 35°C, and the grinding time is 20 minutes. When the powder particles formed by the three are mixed, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 32°C, and the mixing time is 20 minutes.

[0044] As a preferred embodiment of the present invention, in step 4, when diatomaceous earth, calcined clay and zinc borate are mixed, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 28°C, and the mixing time is 18 min. When mixed with silicone oil and pure water, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 32°C, and the mixing time is 22 min.

[0045] As a preferred embodiment of the present invention, when the organic-inorganic mixed flame retardant, fiber flame retardant and auxiliary flame retardant are mixed in step five, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 35°C, and the mixing time is 30min; in step six, the coating thickness of each layer of flame retardant material is not less than 0.05mm, the drying temperature of the electric heating after coating the flame retardant material is maintained at 55°C, and the drying time is 35min.

[0046] Example 2

[0047] The present embodiment provides a flame-retardant electric heating tape, including two tinned copper wires located in the innermost layer, a PTC conductive heating layer wrapped around the tinned copper wires, an insulating layer wrapped around the PTC conductive heating layer, a metal shielding layer wrapped around the insulating layer, and a reinforced protective flame-retardant layer located in the outermost layer, wherein the reinforced protective flame-retardant layer located in the outermost layer is composed of a reinforced metal mesh and a flame-retardant material layer wrapped around the surface of the reinforced metal mesh.

[0048] As a preferred embodiment of this embodiment, the flame retardant material layer is prepared from an organic-inorganic mixed flame retardant, a fiber flame retardant and an auxiliary flame retardant, wherein the composition ratio of the three is: 45% organic-inorganic mixed flame retardant, 40% fiber flame retardant, and 15% auxiliary flame retardant.

[0049] As a preferred embodiment of the present invention, the organic-inorganic hybrid flame retardant includes a synergistic mixture of organic flame retardant materials and inorganic flame retardant materials, and the composition ratio of the two is: 45% organic flame retardant material, 55% inorganic flame retardant material, wherein the inorganic flame retardant material uses antimony trioxide and aluminum hydroxide, and the composition ratio of the two is: 45% antimony trioxide, 55% aluminum hydroxide, and the organic flame retardant material uses an organic halide flame retardant, and the organic halide flame retardant uses brominated polystyrene.

[0050] Antimony trioxide and aluminum hydroxide are both inorganic compounds, which have a high melting point. Organic halide flame retardants also have a high melting point. The combination of antimony trioxide, aluminum hydroxide and organic halide flame retardants can effectively combine the chemical properties of the three and achieve better flame retardant properties.

[0051] As a preferred embodiment of this embodiment, the fiber flame retardant includes the following components: modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber, wherein the composition ratio of the three is: modified basalt fiber 40%, polyphenylsulfone terephthalamide fiber 35%, polycrystalline mullite fiber 25%.

[0052] Modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber all have high melting points. Not only that, the strength of the three materials is also high, but they also have many excellent properties such as electrical insulation, corrosion resistance, and high temperature resistance. The fiber flame retardant formed by combining the three together can effectively improve the flame retardant properties of the entire electric heating belt.

[0053] As a preferred embodiment of this embodiment, the auxiliary flame retardant includes the following ingredients: diatomaceous earth, calcined clay, silicone oil, zinc borate and pure water, wherein the composition ratio of the five is: 30% diatomaceous earth, 25% calcined clay, 20% silicone oil, 18% zinc borate and 7% pure water.

[0054] The density of diatomite is 1.9-2.3g / cm3, the bulk density is 0.34-0.65g / cm3, the specific surface area is 40-65㎡ / g, and the pore volume is 0.45-0.98cm 3 / g, water absorption is 2-4 times of its own volume, melting point is 1650℃-1750℃, special porous structure can be observed under electron microscope, these excellent physical properties determine its excellent flame retardant performance; calcined clay has excellent freeze-thaw resistance, it can freeze and thaw 50 times at -45℃ without cracks, good weathering and corrosion resistance, its internal structure is not easily affected by acidic substances, and calcined clay also has a high melting point and excellent flame retardant performance; silicone oil has a very small vapor pressure, high With a flash point and ignition point, and a relatively low freezing point, silicone oil has heat resistance, electrical insulation, weather resistance, hydrophobicity, physiological inertness, and a relatively small surface tension. In addition, it has a low viscosity-temperature coefficient and high compression resistance. Zinc borate can be used as a multifunctional synergistic additive for antimony oxide or other halogen flame retardants, which can effectively improve the flame retardant properties, reduce the generation of smoke during combustion, and adjust the chemical, mechanical, and electrical properties of rubber and plastic products. Combining these four substances to form an auxiliary flame retardant can achieve excellent flame retardant properties for electric heating cables.

[0055] As a preferred embodiment of the present invention, the method for preparing the flame retardant material layer comprises the following steps:

[0056] Step 1: Prepare the corresponding amount of each ingredient according to its composition ratio, and place them separately for later use after preparation;

[0057] Step 2: After aluminum hydroxide is micronized, it is fully mixed with antimony trioxide to form an inorganic flame retardant material, and then an organic halide flame retardant is added to the mixed inorganic flame retardant material, and the two are fully mixed to form an organic-inorganic mixed flame retardant;

[0058] Step 3: The modified basalt fiber, the polyphenylsulfone terephthalamide fiber and the polycrystalline mullite fiber are fully minced to form powder particles, and then the powder particles formed by the three minced particles are put into a mixing device for full mixing to form a fiber flame retardant;

[0059] Step 4: Place diatomaceous earth, calcined clay, and zinc borate together and stir them thoroughly, then pour a mixed liquid of silicone oil and pure water into the mixture, and stir them thoroughly to form an auxiliary flame retardant;

[0060] Step 5: Mix the organic-inorganic mixed flame retardant, the fiber flame retardant and the auxiliary flame retardant together, and stir them fully to make the three mixed fully and evenly to form a viscous flame retardant material;

[0061] Step 6: Apply the viscous flame retardant material evenly on the outermost reinforced metal mesh surface of the electric heating cable, apply three layers in total, until a dense flame retardant material layer is formed on the reinforced metal mesh surface, place the electric heating cable coated with the flame retardant material in a drying equipment for drying, and wait until the flame retardant material layer is completely dry and formed.

[0062] As a preferred embodiment of the present invention, when aluminum hydroxide and antimony trioxide are mixed in step 2, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained at 30°C, and the mixing time is 20 min. When the organic halide flame retardant and the inorganic flame retardant material are mixed, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained at 30°C, and the mixing time is 24 min.

[0063] As a preferred embodiment of the present invention, in step three, the temperature of the modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber in the grinding process is maintained at 40°C, and the grinding time is 25 minutes. When the powder particles formed by the three are mixed, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 36°C, and the mixing time is 25 minutes.

[0064] As a preferred embodiment of the present invention, in step 4, when diatomaceous earth, calcined clay and zinc borate are mixed, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 33°C, and the mixing time is 22 min. When mixed with silicone oil and pure water, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 35°C, and the mixing time is 25 min.

[0065] As a preferred embodiment of this embodiment, when the organic-inorganic mixed flame retardant, fiber flame retardant and auxiliary flame retardant are mixed in step five, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 37°C, and the mixing time is 35min; in step six, the coating thickness of each layer of flame retardant material is not less than 0.05mm, the drying temperature of the electric heating after coating the flame retardant material is maintained at 65°C, and the drying time is 45mim.

[0066] Example 3

[0067] The present embodiment provides a flame-retardant electric heating tape, including two tinned copper wires located in the innermost layer, a PTC conductive heating layer wrapped around the tinned copper wires, an insulating layer wrapped around the PTC conductive heating layer, a metal shielding layer wrapped around the insulating layer, and a reinforced protective flame-retardant layer located in the outermost layer, wherein the reinforced protective flame-retardant layer located in the outermost layer is composed of a reinforced metal mesh and a flame-retardant material layer wrapped around the surface of the reinforced metal mesh.

[0068] As a preferred embodiment of this embodiment, the flame retardant material layer is prepared from an organic-inorganic mixed flame retardant, a fiber flame retardant and an auxiliary flame retardant, wherein the composition ratio of the three is: 45% organic-inorganic mixed flame retardant, 40% fiber flame retardant, and 15% auxiliary flame retardant.

[0069] As a preferred embodiment of the present invention, the organic-inorganic hybrid flame retardant includes an organic flame retardant material and an inorganic flame retardant material mixed in a ratio of 45% for organic flame retardant material and 55% for inorganic flame retardant material. Among them, the inorganic flame retardant material adopts antimony trioxide and aluminum hydroxide, and the ratio of the two is 45% for antimony trioxide and 55% for aluminum hydroxide. The organic flame retardant material adopts an organic halide flame retardant, and the organic halide flame retardant selects chlorinated paraffin and chlorinated polyethylene.

[0070] Antimony trioxide and aluminum hydroxide are both inorganic compounds, which have a high melting point. Organic halide flame retardants also have a high melting point. The combination of antimony trioxide, aluminum hydroxide and organic halide flame retardants can effectively combine the chemical properties of the three and achieve better flame retardant properties.

[0071] As a preferred embodiment of this embodiment, the fiber flame retardant includes the following components: modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber, wherein the composition ratio of the three is: modified basalt fiber 40%, polyphenylsulfone terephthalamide fiber 35%, polycrystalline mullite fiber 25%.

[0072] Modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber all have high melting points. Not only that, the strength of the three materials is also high, but they also have many excellent properties such as electrical insulation, corrosion resistance, and high temperature resistance. The fiber flame retardant formed by combining the three together can effectively improve the flame retardant properties of the entire electric heating belt.

[0073] As a preferred embodiment of this embodiment, the auxiliary flame retardant includes the following ingredients: diatomaceous earth, calcined clay, silicone oil, zinc borate and pure water, wherein the composition ratio of the five is: 30% diatomaceous earth, 25% calcined clay, 20% silicone oil, 18% zinc borate and 7% pure water.

[0074] The density of diatomite is 1.9-2.3g / cm3, the bulk density is 0.34-0.65g / cm3, the specific surface area is 40-65㎡ / g, and the pore volume is 0.45-0.98cm 3 / g, water absorption is 2-4 times of its own volume, melting point is 1650℃-1750℃, special porous structure can be observed under electron microscope, these excellent physical properties determine its excellent flame retardant performance; calcined clay has excellent freeze-thaw resistance, it can freeze and thaw 50 times at -45℃ without cracks, good weathering and corrosion resistance, its internal structure is not easily affected by acidic substances, and calcined clay also has a high melting point and excellent flame retardant performance; silicone oil has a very small vapor pressure, high With a flash point and ignition point, and a relatively low freezing point, silicone oil has heat resistance, electrical insulation, weather resistance, hydrophobicity, physiological inertness, and a relatively small surface tension. In addition, it has a low viscosity-temperature coefficient and high compression resistance. Zinc borate can be used as a multifunctional synergistic additive for antimony oxide or other halogen flame retardants, which can effectively improve the flame retardant properties, reduce the generation of smoke during combustion, and adjust the chemical, mechanical, and electrical properties of rubber and plastic products. Combining these four substances to form an auxiliary flame retardant can achieve excellent flame retardant properties for electric heating cables.

[0075] As a preferred embodiment of the present invention, the method for preparing the flame retardant material layer comprises the following steps:

[0076] Step 1: Prepare the corresponding amount of each ingredient according to its composition ratio, and place them separately for later use after preparation;

[0077] Step 2: After aluminum hydroxide is micronized, it is fully mixed with antimony trioxide to form an inorganic flame retardant material, and then an organic halide flame retardant is added to the mixed inorganic flame retardant material, and the two are fully mixed to form an organic-inorganic mixed flame retardant;

[0078] Step 3: The modified basalt fiber, the polyphenylsulfone terephthalamide fiber and the polycrystalline mullite fiber are fully minced to form powder particles, and then the powder particles formed by the three minced particles are put into a mixing device for full mixing to form a fiber flame retardant;

[0079] Step 4: Place diatomaceous earth, calcined clay, and zinc borate together and stir them thoroughly, then pour a mixed liquid of silicone oil and pure water into the mixture, and stir them thoroughly to form an auxiliary flame retardant;

[0080] Step 5: Mix the organic-inorganic mixed flame retardant, the fiber flame retardant and the auxiliary flame retardant together, and stir them fully to make the three mixed fully and evenly to form a viscous flame retardant material;

[0081] Step 6: Apply the viscous flame retardant material evenly on the outermost reinforced metal mesh surface of the electric heating cable, apply three layers in total, until a dense flame retardant material layer is formed on the reinforced metal mesh surface, place the electric heating cable coated with the flame retardant material in a drying equipment for drying, and wait until the flame retardant material layer is completely dry and formed.

[0082] As a preferred embodiment of the present invention, when aluminum hydroxide and antimony trioxide are mixed in step 2, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained at 35°C, and the mixing time is 25 min. When the organic halide flame retardant and the inorganic flame retardant material are mixed, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained at 38°C, and the mixing time is 28 min.

[0083] As a preferred embodiment of the present invention, in step three, the temperature of the modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber in the grinding process is maintained at 45°C, and the grinding time is 30 minutes. When the powder particles formed by the three are mixed, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 42°C, and the mixing time is 30 minutes.

[0084] As a preferred embodiment of the present invention, in step 4, when diatomaceous earth, calcined clay and zinc borate are mixed, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 36°C, and the mixing time is 26 min. When mixed with silicone oil and pure water, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 38°C, and the mixing time is 28 min.

[0085] As a preferred embodiment of this embodiment, when the organic-inorganic mixed flame retardant, fiber flame retardant and auxiliary flame retardant are mixed in step five, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 40°C, and the mixing time is 40min; in step six, the coating thickness of each layer of flame retardant material is not less than 0.05mm, the drying temperature of the electric heating after coating the flame retardant material is maintained at 75°C, and the drying time is 55mim.

[0086] Comparative Example 1

[0087] The present comparative example provides a flame-retardant electric heating tape, comprising two tinned copper wires located in the innermost layer, a PTC conductive heating layer wrapped around the tinned copper wires, an insulating layer wrapped around the PTC conductive heating layer, a metal shielding layer wrapped around the insulating layer, and a reinforced protective flame-retardant layer located in the outermost layer, wherein the reinforced protective flame-retardant layer located in the outermost layer is composed of a reinforced metal mesh and a flame-retardant material layer wrapped around the surface of the reinforced metal mesh.

[0088] As a preferred embodiment of this comparative example, the flame retardant material layer is prepared from an organic-inorganic mixed flame retardant and a fiber flame retardant, wherein the composition ratio of the two is: 50% of the organic-inorganic mixed flame retardant and 50% of the fiber flame retardant.

[0089] As the preferred embodiment of this comparative example, the organic-inorganic hybrid flame retardant includes an organic flame retardant material and an inorganic flame retardant material, and the composition ratio of the two is: 45% organic flame retardant material, 55% inorganic flame retardant material, wherein the inorganic flame retardant material adopts antimony trioxide and aluminum hydroxide, and the composition ratio of the two is: 45% antimony trioxide, 55% aluminum hydroxide, and the organic flame retardant material adopts an organic halide flame retardant, and the organic halide flame retardant selects decabromobiphenyl acid.

[0090] As a preferred example of this comparative example, the fiber flame retardant includes the following components: modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber, wherein the composition ratio of the three is: 40% of modified basalt fiber, 35% of polyphenylsulfone terephthalamide fiber and 25% of polycrystalline mullite fiber.

[0091] As a preferred embodiment of this comparative example, the method for preparing the flame retardant material layer comprises the following steps:

[0092] Step 1: Prepare the corresponding amount of each ingredient according to its composition ratio, and place them separately for later use after preparation;

[0093] Step 2: After aluminum hydroxide is micronized, it is fully mixed with antimony trioxide to form an inorganic flame retardant material, and then an organic halide flame retardant is added to the mixed inorganic flame retardant material, and the two are fully mixed to form an organic-inorganic mixed flame retardant;

[0094] Step 3: The modified basalt fiber, the polyphenylsulfone terephthalamide fiber and the polycrystalline mullite fiber are fully minced to form powder particles, and then the powder particles formed by the three minced particles are put into a mixing device for full mixing to form a fiber flame retardant;

[0095] Step 4: Mix the organic-inorganic mixed flame retardant and the fiber flame retardant together, add water and stir them thoroughly to make the three mixed thoroughly and evenly to form a viscous flame retardant material;

[0096] Step 5: Apply the viscous flame retardant material evenly on the outermost reinforced metal mesh surface of the electric heating cable, apply three layers in total, until a dense flame retardant material layer is formed on the reinforced metal mesh surface, place the electric heating cable coated with the flame retardant material in a drying equipment for drying, and wait until the flame retardant material layer is completely dry and formed.

[0097] As the preferred embodiment of this comparative example, when aluminum hydroxide and antimony trioxide are mixed in step 2, the stirring speed of the mixing equipment is 300r / min, the temperature in the mixing equipment is maintained at 29°C, and the mixing time is 19min. When the organic halide flame retardant and the inorganic flame retardant material are mixed, the stirring speed of the mixing equipment is 300r / min, the temperature in the mixing equipment is maintained at 30°C, and the mixing time is 24min.

[0098] As the preferred embodiment of this comparative example, in step three, the temperature of the modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber in the grinding process is maintained at 39°C, and the grinding time is 26 minutes. When the powder particles formed by the three are mixed, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 36°C, and the mixing time is 24 minutes.

[0099] As the preferred embodiment of this comparative example, when the organic-inorganic mixed flame retardant, fiber flame retardant and auxiliary flame retardant are mixed in step 4, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 37°C, and the mixing time is 36min; in step 5, the coating thickness of each layer of flame retardant material is not less than 0.05mm, the drying temperature of the electric heating after coating the flame retardant material is maintained at 62°C, and the drying time is 46mim.

[0100] Comparative Example 2

[0101] The present comparative example provides a flame-retardant electric heating tape, comprising two tinned copper wires located in the innermost layer, a PTC conductive heating layer wrapped around the tinned copper wires, an insulating layer wrapped around the PTC conductive heating layer, a metal shielding layer wrapped around the insulating layer, and a reinforced protective flame-retardant layer located in the outermost layer, wherein the reinforced protective flame-retardant layer located in the outermost layer is composed of a reinforced metal mesh and a flame-retardant material layer wrapped around the surface of the reinforced metal mesh.

[0102] As a preferred embodiment of this comparative example, the flame retardant material layer is prepared from an organic-inorganic mixed flame retardant and an auxiliary flame retardant, wherein the composition ratio of the three is: 75% of the organic-inorganic mixed flame retardant and 25% of the auxiliary flame retardant.

[0103] As the preferred embodiment of this comparative example, the organic-inorganic hybrid flame retardant includes an organic flame retardant material and an inorganic flame retardant material, and the composition ratio of the two is: 45% organic flame retardant material, 55% inorganic flame retardant material, wherein the inorganic flame retardant material adopts antimony trioxide and aluminum hydroxide, and the composition ratio of the two is: 45% antimony trioxide, 55% aluminum hydroxide, and the organic flame retardant material adopts an organic halide flame retardant, and the organic halide flame retardant selects chlorinated paraffin and chlorinated polyethylene.

[0104] As a preferred embodiment of this comparative example, the auxiliary flame retardant includes the following ingredients: diatomaceous earth, calcined clay, silicone oil, zinc borate and pure water, wherein the composition ratio of the five is: 30% diatomaceous earth, 25% calcined clay, 20% silicone oil, 18% zinc borate and 7% pure water.

[0105] As a preferred embodiment of this comparative example, the method for preparing the flame retardant material layer comprises the following steps:

[0106] Step 1: Prepare the corresponding amount of each ingredient according to its composition ratio, and place them separately for later use after preparation;

[0107] Step 2: After aluminum hydroxide is micronized, it is fully mixed with antimony trioxide to form an inorganic flame retardant material, and then an organic halide flame retardant is added to the mixed inorganic flame retardant material, and the two are fully mixed to form an organic-inorganic mixed flame retardant;

[0108] Step 3: Place diatomaceous earth, calcined clay, and zinc borate together and stir them thoroughly, then pour a mixed liquid of silicone oil and pure water into the mixture, and stir them thoroughly to form an auxiliary flame retardant;

[0109] Step 4: Mix the organic-inorganic mixed flame retardant, the fiber flame retardant and the auxiliary flame retardant together, and stir them fully to make the three mixed fully and evenly to form a viscous flame retardant material;

[0110] Step 5: Apply the viscous flame retardant material evenly on the outermost reinforced metal mesh surface of the electric heating cable, apply three layers in total, until a dense flame retardant material layer is formed on the reinforced metal mesh surface, place the electric heating cable coated with the flame retardant material in a drying equipment for drying, and wait until the flame retardant material layer is completely dry and formed.

[0111] As the preferred embodiment of this comparative example, in step 2, when aluminum hydroxide and antimony trioxide are mixed, the stirring speed of the mixing equipment is 300r / min, the temperature in the mixing equipment is maintained at 30°C, and the mixing time is 30min. When the organic halide flame retardant and the inorganic flame retardant material are mixed, the stirring speed of the mixing equipment is 300r / min, the temperature in the mixing equipment is maintained at 30°C, and the mixing time is 25min.

[0112] As a preferred embodiment of this comparative example, in step 3, when diatomaceous earth, calcined clay and zinc borate are mixed, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 32°C, and the mixing time is 22 min. When mixed with silicone oil and pure water, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 35°C, and the mixing time is 24.5 min.

[0113] As the preferred embodiment of this comparative example, when the organic-inorganic mixed flame retardant, fiber flame retardant and auxiliary flame retardant are mixed in step 4, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 38°C, and the mixing time is 36min; in step 5, the coating thickness of each layer of flame retardant material is not less than 0.05mm, the drying temperature of the electric heating after coating the flame retardant material is maintained at 63°C, and the drying time is 46mim.

[0114] Comparative Example 3

[0115] The present comparative example provides a flame-retardant electric heating tape, comprising two tinned copper wires located in the innermost layer, a PTC conductive heating layer wrapped around the tinned copper wires, an insulating layer wrapped around the PTC conductive heating layer, a metal shielding layer wrapped around the insulating layer, and a reinforced protective flame-retardant layer located in the outermost layer, wherein the reinforced protective flame-retardant layer located in the outermost layer is composed of a reinforced metal mesh and a flame-retardant material layer wrapped around the surface of the reinforced metal mesh.

[0116] As a preferred embodiment of this comparative example, the flame retardant material layer is prepared from a fiber flame retardant and an auxiliary flame retardant, wherein the composition ratio of the three is: 75% of the fiber flame retardant and 25% of the auxiliary flame retardant.

[0117] As a preferred example of this comparative example, the fiber flame retardant includes the following components: modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber, wherein the composition ratio of the three is: 40% of modified basalt fiber, 35% of polyphenylsulfone terephthalamide fiber and 25% of polycrystalline mullite fiber.

[0118] As a preferred embodiment of this comparative example, the auxiliary flame retardant includes the following ingredients: diatomaceous earth, calcined clay, silicone oil, zinc borate and pure water, wherein the composition ratio of the five is: 30% diatomaceous earth, 25% calcined clay, 20% silicone oil, 18% zinc borate and 7% pure water.

[0119] As a preferred embodiment of this comparative example, the method for preparing the flame retardant material layer comprises the following steps:

[0120] Step 1: Prepare the corresponding amount of each ingredient according to its composition ratio, and place them separately for later use after preparation;

[0121] Step 2: The modified basalt fiber, the polyphenylsulfone terephthalamide fiber and the polycrystalline mullite fiber are fully minced to form powder particles, and then the powder particles formed by the three minced particles are put into a mixing device for full mixing to form a fiber flame retardant;

[0122] Step 3: Place diatomaceous earth, calcined clay, and zinc borate together and stir them thoroughly, then pour a mixed liquid of silicone oil and pure water into the mixture, and stir them thoroughly to form an auxiliary flame retardant;

[0123] Step 4: Mix the organic-inorganic mixed flame retardant, the fiber flame retardant and the auxiliary flame retardant together, and stir them fully to make the three mixed fully and evenly to form a viscous flame retardant material;

[0124] Step 5: Apply the viscous flame retardant material evenly on the outermost reinforced metal mesh surface of the electric heating cable, apply three layers in total, until a dense flame retardant material layer is formed on the reinforced metal mesh surface, place the electric heating cable coated with the flame retardant material in a drying equipment for drying, and wait until the flame retardant material layer is completely dry and formed.

[0125] As the preferred embodiment of this comparative example, in step 2, the temperature of the modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber in the grinding process is maintained at 40°C, and the grinding time is 25 minutes. When the powder particles formed by the three are mixed, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 37°C, and the mixing time is 26 minutes.

[0126] As a preferred embodiment of this comparative example, in step 3, when diatomaceous earth, calcined clay and zinc borate are mixed, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 32°C, and the mixing time is 22 min. When mixed with silicone oil and pure water, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained at 35°C, and the mixing time is 24 min.

[0127] As the preferred embodiment of this comparative example, when the organic-inorganic mixed flame retardant, fiber flame retardant and auxiliary flame retardant are mixed in step 4, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained at 37.5°C, and the mixing time is 35min; in step 5, the coating thickness of each layer of flame retardant material is not less than 0.05mm, the drying temperature of the electric heating after coating the flame retardant material is maintained at 60°C, and the drying time is 45mim.

[0128] The electric heating cables prepared in Examples 1 to 3 and the electric heating cables prepared in Comparative Example 1 were tested and the experimental data obtained were as follows:

[0129]

[0130]

[0131] It can be seen from the above experimental data that the flame retardant performance of the electric heating tape without auxiliary flame retardants is significantly lower than that of the electric heating tape with auxiliary flame retardants. Therefore, the auxiliary flame retardant is one of the key factors for flame retardant performance in the present invention, but it still has obvious flame retardant performance advantages compared to traditional electric heating tapes.

[0132] The electric heating cables prepared in Examples 1 to 3 and the electric heating cables prepared in Comparative Example 2 were tested and the experimental data were as follows:

[0133]

[0134]

[0135] It can be seen from the above experimental data that the flame retardant performance of the electric heating tape without fiber flame retardants is significantly lower than that of the electric heating tape with fiber flame retardants added. Therefore, the fiber flame retardant is one of the key factors for flame retardant performance in the present invention, but it still has a very obvious flame retardant advantage compared to traditional electric heating tapes.

[0136] The electric heating cables prepared in Examples 1 to 3 and the electric heating cables prepared in Comparative Example 3 were tested and the experimental data were as follows:

[0137]

[0138]

[0139] It can be seen from the above experimental data that the flame retardant performance of the electric heating tape lacking the organic-inorganic mixed flame retardant is significantly lower than that of the electric heating tape added with the organic-inorganic mixed flame retardant. Therefore, the organic-inorganic mixed flame retardant is one of the key factors that play a role in flame retardant performance in the present invention, but it still has a very obvious flame retardant advantage compared to the traditional electric heating tape.

[0140] In summary, the flame retardant electric heating tape provided by the present invention has more obvious advantages in flame retardant performance than traditional electric heating tapes.

[0141] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A flame-retardant electric heating cable, comprising two tinned copper wires in the innermost layer, a PTC conductive heating layer wrapped around the tinned copper wires, an insulating layer wrapped around the PTC conductive heating layer, a metal shielding layer wrapped around the insulating layer, and a reinforced protective flame-retardant layer in the outermost layer, characterized in that: The outermost reinforced protective flame retardant layer is composed of a reinforced metal mesh and a flame retardant material layer wrapped on the surface of the reinforced metal mesh; the flame retardant material layer is prepared from an organic-inorganic mixed flame retardant, a fiber flame retardant and an auxiliary flame retardant, wherein the composition ratio of the three is: 45% of the organic-inorganic mixed flame retardant, 40% of the fiber flame retardant and 15% of the auxiliary flame retardant; The organic-inorganic mixed flame retardant includes an organic flame retardant material and an inorganic flame retardant material in a synergistic mixture, the composition ratio of the two being: 45% of organic flame retardant material and 55% of inorganic flame retardant material, wherein the inorganic flame retardant material uses antimony trioxide and aluminum hydroxide, the composition ratio of the two being: 45% of antimony trioxide and 55% of aluminum hydroxide, the organic flame retardant material uses an organic halide flame retardant, and the organic halide flame retardant is selected from one or more of decabromobiphenyl acid, tetrabromobisphenol, brominated polystyrene, chlorinated paraffin and chlorinated polyethylene; The fiber flame retardant includes the following components: modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber, wherein the composition ratio of the three is: 40% of modified basalt fiber, 35% of polyphenylsulfone terephthalamide fiber and 25% of polycrystalline mullite fiber; The auxiliary flame retardant includes the following components: diatomaceous earth, calcined clay, silicone oil, zinc borate and pure water, wherein the composition ratio of the five is: 30% of diatomaceous earth, 25% of calcined clay, 20% of silicone oil, 18% of zinc borate and 7% of pure water.

2. The flame retardant electric heating cable according to claim 1, characterized in that: The method for preparing the flame retardant material layer comprises the following steps: Step 1: Prepare the corresponding amount of each ingredient according to its composition ratio, and place them separately for later use after preparation; Step 2: After aluminum hydroxide is micronized, it is fully mixed with antimony trioxide to form an inorganic flame retardant material, and then an organic halide flame retardant is added to the mixed inorganic flame retardant material, and the two are fully mixed to form an organic-inorganic mixed flame retardant; Step 3: The modified basalt fiber, the polyphenylsulfone terephthalamide fiber and the polycrystalline mullite fiber are fully minced to form powder particles, and then the powder particles formed by the three minced particles are put into a mixing device for full mixing to form a fiber flame retardant; Step 4: Place diatomaceous earth, calcined clay, and zinc borate together and stir them thoroughly, then pour a mixed liquid of silicone oil and pure water into the mixture, and stir them thoroughly to form an auxiliary flame retardant; Step 5: Mix the organic-inorganic mixed flame retardant, the fiber flame retardant and the auxiliary flame retardant together, and stir them fully to make the three mixed fully and evenly to form a viscous flame retardant material; Step 6: Apply the viscous flame retardant material evenly on the outermost reinforced metal mesh surface of the electric heating cable, apply three layers in total, until a dense flame retardant material layer is formed on the reinforced metal mesh surface, place the electric heating cable coated with the flame retardant material in a drying equipment for drying, and wait until the flame retardant material layer is completely dry and formed.

3. The flame retardant electric heating tape according to claim 2, characterized in that: In step 2, when aluminum hydroxide and antimony trioxide are mixed, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained between 25°C and 35°C, and the mixing time is 15min to 25min. When the organic halide flame retardant and the inorganic flame retardant material are mixed, the stirring speed of the mixing equipment is 300 r / min, the temperature in the mixing equipment is maintained between 22°C and 38°C, and the mixing time is 18min to 28min.

4. The flame retardant electric heating cable according to claim 3, characterized in that: In step 3, during the mincing process of the modified basalt fiber, polyphenylsulfone terephthalamide fiber and polycrystalline mullite fiber, the temperature in the mincing equipment is maintained between 35°C and 45°C, and the mincing time is 20min to 30min. When the powder particles formed by the three are mixed, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained between 32°C and 42°C, and the mixing time is 20min to 30min.

5. The flame retardant electric heating tape according to claim 4, characterized in that: In step 4, when diatomaceous earth, calcined clay and zinc borate are mixed, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained between 28°C and 36°C, and the mixing time is 18min to 26min. When mixing with silicone oil and pure water, the stirring speed of the mixing equipment is 250 r / min, the temperature in the mixing equipment is maintained between 32°C and 38°C, and the mixing time is 22min to 28min.

6. The flame retardant electric heating tape according to claim 5, characterized in that: In step 5, when the organic-inorganic mixed flame retardant, fiber flame retardant and auxiliary flame retardant are mixed, the stirring speed of the mixing equipment is 350r / min, the temperature in the mixing equipment is maintained between 35°C and 40°C, and the mixing time is 30min to 40min; in step 6, the coating thickness of each layer of flame retardant material is not less than 0.05mm, the drying temperature of the electric heating after coating the flame retardant material is maintained between 55°C and 75°C, and the drying time is 35min to 55mim.

Citation Information

Patent Citations

  • Halogen-free flame-retardant PET (polyethylene terephthalate) composite material and preparation method thereof

    CN103333469A

  • Inflaming retarding typed carbon fiber heating cable

    CN103547002A

  • Insulating flame-retardant bulk molding compound and preparation method thereof

    CN109575548A

  • Flame-retardant cable and preparation method thereof

    CN110229443A

  • Constant temperature self -regulating electric heat tracing area

    CN205902116U