Method for manufacturing printed circuit board
By electroless plating the insulating base material of the printed circuit board to form an electroless plating layer with specific surface parameters, combined with the use of a photoresist layer, the problems of poor patterning and reduced etching properties are solved, and the miniaturization of the printed circuit board is achieved. and high adhesion.
Patent Information
- Application Number
- CN202080022027.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-03-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-03-17
AI Technical Summary
In the manufacturing process of printed circuit boards, when copper foil with a smooth surface and small roughened particles is used and thin electroless plating is performed, pattern defects and difficulties in circuit miniaturization are likely to occur, leading to problems such as reduced etching properties and short circuits.
By performing electroless plating on an insulating base material with a rough surface, an electroless plating layer with prescribed surface parameters is formed, including a surface with an arithmetic mean waviness Wa of 0.10 μm or more and 0.25 μm or less, and a kurtosis Sku of 2.0 or more and 3.5 or less. A photoresist layer is laminated, exposed and developed to form a resist pattern, and unnecessary chemical plating is removed by etching to form a wiring pattern.
Effectively suppresses pattern defects, improves the formability and etching properties of fine circuits, and ensures high adhesion and miniaturization of printed circuit boards.
Smart Images

Figure CN113574977B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for manufacturing a printed circuit board. Background Art
[0002] In recent years, with the miniaturization and high density required for printed circuit boards, there is a demand for finer circuits (fine pitch). As a method for manufacturing printed circuit boards suitable for finer circuits, the semi-additive process (SAP process) is widely used. The SAP process is a method suitable for forming extremely fine circuits. As an example, the SAP process is performed using a roughened copper foil with a carrier. For example, Fig.10 and 11 As shown, using prepreg 112 and primer layer 113, roughened copper foil 110 is pressed and tightly bonded to insulating resin substrate 111 having lower circuit 111b on bottom substrate 111a (process (a)); after peeling off the carrier (not shown), via 114 is formed by laser perforation as needed (process (b)). Then, roughened copper foil 110 is removed by etching to expose primer layer 113 with roughened surface profile (process (c)). After the roughened surface is given chemical copper plating layer 115 (process (d)), it is masked with a prescribed pattern by exposure and development using dry film 116 (process (e)); and electroplated copper layer 117 is given (process (f)). After the dry film 116 is removed to form the wiring portion 117a (step (g)), the unnecessary chemical copper plating layer 115 between adjacent wiring portions 117a and 117a is removed by etching (step (h)), thereby obtaining wiring 118 formed in a predetermined pattern.
[0003] In such a SAP method using a roughened copper foil, the roughened copper foil itself is removed by etching after laser perforation (process (c)). Thus, the concavo-convex shape of the roughened surface of the roughened copper foil is transferred to the surface of the laminate from which the roughened copper foil has been removed, so that the adhesion between the insulating layer (e.g., the primer layer 113 or the prepreg 112 when there is no primer layer 113) and the plated circuit (e.g., wiring 118) can be ensured in the subsequent process. However, the surface profile suitable for improving the adhesion with the plated circuit generally tends to become rough concavo-convex, so in process (h), the etching property of the chemically plated copper layer is easily reduced. That is, more etching is required to remove the residual copper in accordance with the amount of rough concavo-convex embedded in the chemically plated copper layer.
[0004] Therefore, the following method is proposed: by reducing the roughened particles and making them have a middle tapered shape, when used in the SAP method, it is possible to ensure the required plated circuit adhesion and achieve good etching properties. For example, Patent Document 1 (International Publication No. 2016 / 158775) discloses a roughened copper foil having a roughened surface on at least one side, and the roughened surface has a plurality of roughly spherical protrusions formed by copper particles, and the average height of the roughly spherical protrusions is less than 2.60 μm. In addition, Patent Document 2 (International Publication No. 2018 / 211951) discloses a roughened copper foil having a roughened surface on at least one side, and the roughened copper foil is composed of primary roughened particles with a middle tapered portion and secondary roughened particles on the surface of the primary roughened particles, and the microscopic roughness of the roughened surface has a low roughness of less than 1.7 μm at a ten-point height Rz.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2016 / 158775
[0008] Patent Document 2: International Publication No. 2018 / 211951 Summary of the invention
[0009] In recent years, with the further miniaturization of circuits required by the SAP method, in order to achieve excellent etching properties, as mentioned above, it is conceivable to use a copper foil with a smooth surface and small roughening particles to give a roughened surface profile to the insulating substrate. In addition, if a thin chemical plating (for example, less than 1.0 μm) can be applied to the surface of the insulating substrate to which the roughened surface profile is applied, the etching amount can be reduced and further miniaturization of the circuit can be achieved, which is ideal. However, in the SAP method, when attempting to form a circuit using a copper foil with a smooth surface and small roughening particles and applying a thin chemical plating, it is found that problems such as short circuits and convex portions may occur in the formed circuit.
[0010] The present inventors have now found that a method for manufacturing a printed wiring board that can effectively suppress pattern defects and has excellent fine circuit formability can be provided by performing chemical plating on an insulating substrate having a rough surface to form a chemically plated layer having predetermined surface parameters and a thickness of less than 1.0 μm.
[0011] Therefore, an object of the present invention is to provide a method for producing a printed wiring board which can effectively suppress pattern defects and has excellent fine circuit formability.
[0012] According to one embodiment of the present invention, a method for manufacturing a printed circuit board is provided, comprising:
[0013] (a) a step of preparing an insulating substrate having a rough surface;
[0014] (b) a step of performing chemical plating on the rough surface of the insulating substrate to form a chemical plating layer having a thickness of less than 1.0 μm, wherein the chemical plating layer has a surface having an arithmetic mean waviness Wa of 0.10 μm or more and 0.25 μm or less as measured in accordance with JIS B0601-2001 and a kurtosis Sku of 2.0 or more and 3.5 or less as measured in accordance with ISO25178;
[0015] (c) a step of laminating a photoresist layer on the surface of the chemically plated layer;
[0016] (d) exposing and developing the photoresist layer to form a resist pattern;
[0017] (e) a step of electroplating the chemical plating layer through the resist pattern;
[0018] (f) a step of peeling off the resist pattern; and
[0019] (g) A step of removing unnecessary portions of the chemical plating layer exposed by peeling off the resist pattern by etching to form a wiring pattern. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a process flow chart showing the first half of the steps (steps (a) to (c)) in one example of the production method of the present invention.
[0021] Figure 2 This is a process flow chart showing the latter half of the steps (steps (d) to (g)) in one example of the production method of the present invention.
[0022] Figure 3 This is a process flow chart showing an example of the steps of preparing an insulating substrate having a rough surface.
[0023] Figure 4 This is a diagram for explaining the influence of surface foreign matter during exposure and development when there is not a sufficient concavo-convex shape on the surface after chemical plating.
[0024] Figure 5 This is a diagram for explaining the influence of surface foreign matter during exposure and development when a sufficient concavo-convex shape is present on the surface after chemical plating.
[0025] Figure 6 1 and 10 are diagrams for explaining the procedure of evaluating the number of dust detections in the embodiment.
[0026] Figure 7This is a diagram for explaining the load curve and load area ratio determined in accordance with ISO25178.
[0027] Figure 8 This is a diagram for explaining the load area ratio Smr2 of the protruding valley portion and the center portion determined in accordance with ISO25178.
[0028] Fig. 9 This is a diagram for explaining the void volume Vvv of the valley portion determined in accordance with ISO25178.
[0029] Fig.10 This is a process flow chart for explaining the SAP method, and is a diagram showing the first half of the processes (process (a) to process (d)).
[0030] Fig.11 This is a process flow chart for explaining the SAP method, and is a diagram showing the latter half of the processes (process (e) to process (h)). DETAILED DESCRIPTION
[0031] definition
[0032] The definitions of parameters used to define the present invention are shown below.
[0033] In this specification, "arithmetic mean waviness Wa" is the arithmetic mean height in the reference length of the waviness curve as a profile curve measured in accordance with JIS B0601-2001. The waviness curve is not the fine concavities and convexities represented by the roughness curve, but rather represents concavities and convexities of a larger scale (i.e., waviness). The arithmetic mean waviness Wa can be calculated by measuring the surface profile of a predetermined measurement length (e.g., a one-dimensional region of 64.124 μm) on the rough surface using a commercially available laser microscope.
[0034] In this specification, "kurtosis" refers to a parameter indicating the sharpness of the height distribution measured in accordance with ISO25178, and is also called kurtosis. Sku = 3 indicates that the height distribution is a normal distribution, Sku>3 indicates that the surface has many sharp peaks and valleys, and Sku<3 indicates that the surface is flat. The kurtosis Sku can be measured by using a commercially available laser microscope to measure a specified measurement area (e.g., 6811.801 μm 2 The surface profile of the two-dimensional area is measured and calculated.
[0035] In this specification, "maximum height Sz" refers to a parameter indicating the distance from the highest point to the lowest point on the surface measured in accordance with ISO 25178. The maximum height Sz can be measured by using a commercially available laser microscope to measure a predetermined area (e.g., 6811.801 μm 2The surface profile of the two-dimensional area is measured and calculated.
[0036] In this specification, the "surface load curve" (hereinafter referred to as "load curve") refers to a curve indicating the height of the load area ratio from 0% to 100% measured in accordance with ISO25178. Figure 7 As shown in Figure 2, the load area ratio is a parameter that represents the area of a region above a certain height c. The load area ratio at height c is equivalent to Figure 7 Smr(c) in Figure 8 As shown, along the load curve, starting from the load area ratio of 0%, take the load area ratio difference as 40% and draw a secant of the load curve, move the secant of the load curve from the load area ratio of 0%, and the position where the slope of the secant is the gentlest is called the central part of the load curve. Relative to the central part, the straight line with the smallest sum of the squares of deviations from the vertical axis direction is called the equivalent straight line. The part included in the range of heights of the load area ratio of 0% to 100% of the equivalent straight line is called the central part. The part higher than the central part is called the protruding peak, and the part lower than the central part is called the protruding valley. The central part indicates the height of the area that contacts other objects after the initial wear is over. In addition, in this specification, "the load area ratio Smr2 separating the protruding valley and the central part" means such as Figure 8 The parameter shown is the load area ratio at the intersection of the height of the lower part of the center and the load curve (i.e., the load area ratio separating the center and the protruding valley) measured in accordance with ISO 25178. The larger the value, the larger the proportion of the protruding valley.
[0037] In this specification, the "void volume Vvv of the valley" is a parameter indicating the volume of the space protruding from the valley measured in accordance with ISO 25178. Fig. 9 The volume of the space part is calculated from the load curve from the load area ratio Smr2 to the load area ratio of 100%. The void volume Vvv of the valley can be obtained by using a commercially available laser microscope to measure a predetermined area (e.g., 6811.801 μm 2 In this specification, the void volume Vvv of the valley portion is calculated by setting the load area ratio Smr2 separating the protruding valley portion and the center portion to 80%.
[0038] Method for manufacturing printed circuit board
[0039] The present invention relates to a method for manufacturing a printed circuit board, which comprises the following steps: (a) preparing an insulating substrate, (b) forming a chemical plating layer, (c) laminating a photoresist layer, (d) forming a resist pattern, (e) forming an electroplating layer, (f) stripping the resist pattern, and (g) forming a wiring pattern.
[0040] Below, refer to Figures 1 to 5 , while explaining steps (a) to (g) respectively.
[0041] (a) Preparation of insulating substrate
[0042] like Figure 1 As shown in (a), an insulating substrate 20 having a rough surface 20a is prepared. The insulating substrate 20 may have a rough surface 20a on both sides or only on one side. The insulating substrate 20 preferably contains an insulating resin. In addition, the insulating substrate 20 is preferably a prepreg and / or a resin sheet. Prepreg is a general term for composite materials obtained by impregnating synthetic resins into substrates such as synthetic resin plates, glass plates, glass woven fabrics, glass non-woven fabrics, and paper. Preferred examples of insulating resins impregnated into prepregs include epoxy resins, cyanate resins, bismaleimide triazine resins (BT resins), polyphenylene ether resins, phenolic resins, and the like. In addition, examples of insulating resins constituting resin sheets include insulating resins such as epoxy resins, polyimide resins, and polyester resins. From the viewpoint of improving insulation, filler particles formed of various inorganic particles such as silica and alumina may also be included in the insulating substrate 20. The thickness of the insulating base material 20 is not particularly limited, but is preferably 1 μm to 1000 μm, more preferably 2 μm to 400 μm, and further preferably 3 μm to 200 μm. The insulating base material 20 may be composed of multiple layers.
[0043] The rough surface 20a of the insulating substrate 20 can be formed by any method, typically by transferring the concavo-convex shape of the treated surface of the surface-treated copper foil to the surface of the insulating substrate 20. According to a preferred embodiment of the present invention, the rough surface 20a using the surface-treated copper foil is formed by the following method: (a-1) preparing a surface-treated copper foil having a predetermined treated surface, (a-2) laminating an insulating substrate on the treated surface of the surface-treated copper foil, transferring the surface shape of the treated surface to the surface of the insulating substrate, and then, (a-3) removing the surface-treated copper foil by etching to obtain an insulating substrate having a rough surface. The specific steps of each process are as follows.
[0044] (a-1) Preparation of surface-treated copper foil
[0045] like Figure 3As shown in (a-1), a surface treated copper foil 10 having a treated surface 10a on at least one side is prepared. The treated surface 10a is a surface to which certain surface treatments are applied, typically a roughened surface. The treated surface 10a is typically formed with a plurality of protrusions (e.g., roughened particles). In either case, the surface treated copper foil 10 may have treated surfaces 10a on both sides, or may have treated surfaces 10a only on one side. In the case where the treated surfaces 10a are on both sides, when used in the SAP method, the surface on the laser irradiated side (the surface on the opposite side to the surface in close contact with the insulating substrate) is also subjected to surface treatment, so the laser absorptivity is improved, and as a result, the laser permeability can also be improved. In addition, the surface treated copper foil 10 may also be in the form of a copper foil with a carrier. At this time, the copper foil with a carrier is typically formed with a carrier, a peeling layer disposed on the carrier, and a surface treated copper foil 10 disposed on the peeling layer with the treated surface 10a as the outer side. Of course, in addition to using the surface treated copper foil 10, the copper foil with a carrier may adopt a known layer structure.
[0046] The arithmetic mean waviness Wa of the treated surface 10a of the surface treated copper foil 10 is preferably 0.20 μm or more and 0.35 μm or less, and more preferably 0.25 μm or more and 0.32 μm or less. In addition, the maximum height Sz of the treated surface 10a of the surface treated copper foil 10 is preferably 3.0 μm or more and 4.0 μm or less, and more preferably 3.1 μm or more and 3.9 μm or less. Furthermore, the void volume Vvv of the valley portion of the treated surface 10a of the surface treated copper foil 10 is preferably 0.030 μm or more. 3 / μm 2 Above and 0.050μm 3 / μm 2 Below, more preferably 0.035 μm 3 / μm 2 Above and 0.045μm 3 / μm 2 Below. The treated surface 10a having such surface parameters can be said to be a shape with large waviness and small protrusions (such as roughened particles). By using the surface-treated copper foil 10 having the treated surface 10a to give the insulating substrate 20 a concave-convex shape, it is easy to form a chemical plating layer 22 having the specific surface parameters described later on the rough surface 20a of the insulating substrate 20. The treated surface 10a having the above-mentioned surface parameters can be formed by subjecting the copper foil surface to a surface treatment (typically a roughening treatment) under known / desired conditions. In addition, commercially available copper foil having a treated surface 10a that satisfies the above-mentioned conditions can also be selectively obtained.
[0047] (a-2) Transfer of concavo-convex shape to insulating substrate
[0048] like Figure 3As shown in (a-2), an insulating substrate 20' (i.e., an insulating substrate 20 without a rough surface 20a) is stacked on the treated surface 10a of the surface-treated copper foil 10 to form a copper-clad laminate 12. As a result, the surface shape of the treated surface 10a can be transferred to the surface of the insulating substrate 20'. The stacking of the insulating substrate 20' is preferably accompanied by hot pressing, and the processing temperature and processing time of the hot pressing can be appropriately determined based on the type of the insulating substrate 20' to be stacked, etc., based on known conditions. The preferred types of the insulating substrate 20' are as described above for the insulating substrate 20. It should be noted that the insulating substrate 20' can also be stacked on the surface-treated copper foil 10 with a primer layer (not shown) pre-coated on the treated surface 10a of the surface-treated copper foil 10. At this time, the primer layer can be regarded as a part of the insulating substrate. The primer layer is preferably composed of a resin, and the resin is preferably an insulating resin. If desired, via holes (not shown) may be formed in the copper-clad laminate 12 by laser drilling before the removal of the surface-treated copper foil 10 as the next step.
[0049] (a-3) Removal of surface treated copper foil
[0050] like Figure 3 As shown in (a-3), the surface treated copper foil 10 of the copper clad laminate 12 is removed by etching to obtain an insulating substrate 20 having a rough surface 20a. The etching of the surface treated copper foil 10 can be carried out by an etching method and conditions commonly used in the manufacture of printed circuit boards, for example, using an etching solution such as a sulfuric acid-hydrogen peroxide system, without particular limitation.
[0051] (b) Formation of chemical plating layer
[0052] like Figure 1 As shown in (b), the rough surface 20a of the insulating substrate 20 is chemically plated (for example, chemical copper plating) to form a chemical plating layer 22 with a thickness of less than 1.0 μm. The chemical plating can be carried out using a commercially available chemical plating solution and in accordance with the methods and conditions commonly used in the manufacture of printed circuit boards, without any particular limitation. The arithmetic mean waviness Wa of the surface of the chemical plating layer 22 is greater than 0.10 μm and less than 0.25 μm, and the kurtosis Sku is greater than 2.0 and less than 3.5. In this way, chemical plating is performed on the insulating substrate 20 having a rough surface 20a to form a chemical plating layer 22 having the above-mentioned specified surface parameters and a thickness of less than 1.0 μm, thereby providing a method for manufacturing a printed circuit board that can effectively suppress pattern defects and has excellent fine circuit formability.
[0053] As mentioned above, in recent years, as the circuit required by the SAP method has been further miniaturized, in order to achieve excellent etching properties, it is thought of to use a copper foil with a smooth surface and small roughening particles to give a roughened surface profile to an insulating substrate. In addition, if a thin chemical plating (for example, less than 1.0 μm) can be applied to the surface of the insulating substrate to which the roughened surface profile is applied, the etching amount can be reduced and further miniaturization of the circuit can be achieved, which is ideal. However, in the SAP method, when attempting to use a copper foil with a smooth surface and small roughening particles and applying a thin chemical plating to form a circuit, it is found that problems such as short circuits and convex portions may occur in the formed circuit. The mechanism of occurrence of this pattern defect has not yet been determined, and it is speculated to be the following mechanism.
[0054] That is, when the surface shape is transferred to an insulating substrate using a surface-treated copper foil, the rough surface of the insulating substrate will roughly reflect the surface contour of the surface-treated copper foil. Next, when the rough surface of the insulating substrate is chemically plated with a thickness of less than 1.0 μm, the surface shape of the chemically plated layer will roughly reflect the surface shape of the rough surface of the insulating substrate. Therefore, if a copper foil with a smooth surface and small roughening particles (in other words, a copper foil with fine concave-convex shapes) is used as a copper foil for transferring the surface contour to an insulating substrate, it can be said that it is difficult to give the surface of the chemically plated layer a sufficient concave-convex shape. On the other hand, in the conventional manufacturing process of printed circuit boards, in order to form circuits in a prescribed pattern, Figure 4 As shown in (i) to (iv) of FIG. 1 , a photoresist layer 24 (for example, including a dry film resist layer 24a and a support film 24b) is further laminated on the surface of the chemical plating layer 22 laminated on the insulating substrate 20, and exposure and development are performed to form a resist pattern 26. Here, as shown in FIG. Figure 4 As shown in (i), when the photoresist layer 24 is laminated / exposed, foreign matter F (such as dust / scratches on the surface of the photoresist layer, air entrainment during the lamination of the photoresist layer, etc.) may be attached / mixed on the surface of the photoresist layer 24. In contrast, if the photoresist layer 24 laminated on the surface of the chemical plating layer 22 that is not given a sufficient concavo-convex shape is exposed, Figure 4 As shown in (ii) of FIG. 1 , the exposure incident light I entering from a direction perpendicular to the main surface of the laminate is directly reflected at the chemical plating layer 22 and emitted as exposure reflected light R in a direction 180° opposite to the exposure incident light I. As a result, the portion of the photoresist layer 24 (e.g., the dry film resist layer 24a) that is supposed to be exposed directly below the foreign matter F remains unexposed (see FIG. 1 ). Figure 4 (iii)) state, after development, a hole H will be formed (refer to Figure 4As a result, electroplating is performed at locations where the circuit should not be formed, and it is believed that the unnecessary electroplated portion causes short circuits and protrusions in the above-mentioned circuits, thereby causing a problem of pattern defects.
[0055] The inventors of the present invention focused on this point and studied the relationship between the surface of the chemical plating layer and the unexposed part caused by foreign matter, and the relationship between the surface of the chemical plating layer and the fine circuit formability. As a result, it was found that in the surface of the chemical plating layer, by making the arithmetic mean waviness Wa greater than 0.10μm and less than 0.25μm, and making the kurtosis Sku greater than 2.0 and less than 3.5, the pattern defect is effectively suppressed and a fine circuit can be well formed, thereby completing the present invention. It can be considered that the above-mentioned suppression of pattern defects and excellent fine circuit formability are achieved in the following manner. That is, by setting the arithmetic mean waviness Wa of the surface of the chemical plating layer 22 to be greater than 0.10μm, the surface of the chemical plating layer 22 becomes sufficiently concave and convex (refer to Figure 5 Therefore, during exposure, the exposure incident light I entering from a direction perpendicular to the main surface of the stack will be diffusely reflected when it reaches the surface of the chemical plating layer 22 due to the waviness of the surface of the chemical plating layer 22 (refer to Figure 5 (ii)). In addition, from the viewpoint that strong light is not easily reflected when the exposure incident light I penetrates into the deep valleys of the uneven surface of the chemical plating layer 22, the sharpness of the valleys of the uneven surface of the chemical plating layer 22 is suppressed by setting the kurtosis Sku of the surface of the chemical plating layer 22 to less than 3.5. Therefore, the exposure incident light I can be diffusely reflected in the shallow valleys of the surface of the chemical plating layer 22, and the light intensity of the exposure reflected light R is maintained relatively strong. In other words, the chemical plating layer 22 with the above parameters has a surface with large waviness and shallow valleys (no large holes), so it can be said that the exposure incident light I can be diffusely reflected while maintaining a strong light intensity. As a result, the exposure reflected light R can effectively expose the portion of the photoresist layer 24 (for example, the dry film resist layer 24a) directly below the foreign matter F. In this way, the formation of the unexposed portion of the photoresist layer 24 caused by the foreign matter F can be effectively prevented (refer to Figure 5 (iii)), suppressing the formation of unnecessary holes H caused by development (refer to Figure 5 (iv)). It is believed that in this way, it is difficult for the circuit to have problems such as short circuits and convex portions. On the other hand, when the surface of the chemical plating layer 22 has a rough concave-convex shape, it can be said that the etching property of the chemical plating layer 22 is easily reduced. In this regard, it can be considered that by forming the thickness of the chemical plating layer 22 to be as thin as less than 1.0μm, and setting the arithmetic mean waviness Wa of the surface of the chemical plating layer 22 to less than 0.25μm, and setting the kurtosis Sku to more than 2.0μm, it is possible to ensure good etching property of the chemical plating layer 22 and improve fine circuit formation.
[0056] From the above viewpoints, the arithmetic mean waviness Wa of the surface of the chemical plating layer 22 is 0.10 μm to 0.25 μm, preferably 0.20 μm to 0.25 μm. The kurtosis Sku of the surface of the chemical plating layer 22 is 2.0 to 3.5, preferably 3.0 to 3.5.
[0057] The void volume Vvv of the valley portion on the surface of the chemical plating layer 22 is preferably 0.010 μm 3 / μm 2 Above and 0.028μm 3 / μm 2 Below, more preferably 0.017 μm 3 / μm 2 Above and 0.025μm 3 / μm 2 As a result, the valleys on the surface of the chemical plating layer 22 become shallower, and as a result, diffuse reflection of the exposure incident light I is more likely to occur, and the light intensity of the exposure reflected light R can be further maintained at a high state.
[0058] The chemical plating layer 22 having the above-mentioned unique surface parameters can be formed by performing chemical plating with a thickness of less than 1.0 μm on the rough surface 20a of the insulating substrate 20. As described above, it can be said that the surface shape of the chemical plating layer 22 roughly reflects the surface shape of the rough surface 20a of the insulating substrate 20. And, the rough surface 20a can be preferably formed by transferring the surface shape of the surface-treated copper foil 10 having the surface parameters described in (a) above to the insulating substrate 20, for example.
[0059] The thickness of the chemical plating layer 22 is less than 1.0 μm, preferably 0.3 μm or more and less than 1.0 μm. With such a thickness, the etching amount during wiring pattern formation can be reduced, and it is very suitable for forming a fine circuit.
[0060] (c) Photoresist layer stacking
[0061] like Figure 1 As shown in (c), a photoresist layer 24 is laminated on the surface of the chemical plating layer 22. The lamination speed when laminating the photoresist layer 24 is not particularly limited, and is typically 1.0 m / min or more and 2.0 m / min or less. The photoresist layer 24 can use a known material commonly used in the manufacture of printed circuit boards. The photoresist layer 24 can be either negative or positive, and can be either a film type or a liquid type. Preferably, the photoresist layer 24 includes a dry film resist layer 24a. In addition, the photoresist layer 24 is preferably a photosensitive film, such as a photosensitive dry film. Figure 1As shown in (c), the photoresist layer 24 may further be laminated with a support film 24b such as a polyethylene terephthalate (PET) film on the dry film resist layer 24a as a photosensitive layer. The thickness of the photoresist layer 24 or the dry film resist layer 24a is preferably 2 μm or more and 35 μm or less, and more preferably 5 μm or more and 24 μm or less.
[0062] (d) Formation of resist pattern
[0063] like Figure 2 As shown in (d), the photoresist layer 24 is exposed and developed to form a resist pattern 26. The exposure and development can be carried out according to the known methods and conditions commonly used in the manufacture of printed circuit boards, and are not particularly limited. For example, as an exposure method, in addition to a mask exposure method using a negative or positive mask pattern, a direct drawing exposure method such as a laser direct imaging (Laser Direct Imaging, LDI) exposure method and a digital light processing (Digital Light Processing, DLP) exposure method can be used. The exposure amount during exposure is preferably 5mJ / cm 2 Above and 150mJ / cm 2 As follows. On the other hand, as a developing method, both wet developing and dry developing are possible. In the case of wet developing, the developer used may be a developer such as sodium carbonate, sodium hydroxide, or an amine aqueous solution. It should be noted that when the photoresist layer 24 includes a support film 24b, it is preferred that the development be performed after removing the support film 24b.
[0064] (e) Formation of electroplating layer
[0065] Electroplating (for example, copper electroplating) is performed on the chemical plating layer 22 via the resist pattern 26. Figure 2 As shown in (e), a plating layer 28 can be formed between the resist patterns 26. The electroplating can be performed by various pattern plating methods and conditions commonly used in the manufacture of printed circuit boards, such as copper sulfate plating solutions and copper pyrophosphate plating solutions, and is not particularly limited.
[0066] (f) Stripping of resist pattern
[0067] In this process, the resist pattern 26 is peeled off. As a result, Figure 2 As shown in (f), the electroplating layer 28 remains in the form of a wiring pattern, and the unnecessary portion of the chemical plating layer 22 that does not form a wiring pattern is exposed. The stripping of the resist pattern 26 can be carried out using a sodium hydroxide aqueous solution, an amine solution / an aqueous solution thereof, etc., and in accordance with various stripping methods and conditions commonly used in printed circuit boards, without particular limitation.
[0068] (g) Formation of wiring pattern
[0069] The unnecessary part of the chemical plating layer 22 exposed by the peeling of the resist pattern 26 (i.e., the part where the wiring pattern is not formed) is removed by etching to form the wiring pattern 30. The etching of the unnecessary part of the chemical plating layer 22 can be carried out, for example, using an etching solution of sulfuric acid-hydrogen peroxide system, and according to the etching method and conditions commonly used in the manufacture of printed circuit boards, and is not particularly limited. The thickness of the wiring pattern 30 (i.e., the circuit height) is preferably 2 μm or more and 30 μm or less. The wiring pitch of the wiring pattern 30 is preferably in the range of 10 μm (e.g., line / space = 5 μm / 5 μm) to 20 μm (e.g., line / space = 10 μm / 10 μm). By forming a circuit on the chemical plating layer 22 having the surface parameters specified above and a thickness of less than 1.0 μm, such a highly fine wiring pattern can be formed. In addition, the wiring pattern with a wiring pitch within the above range can be said to be prone to problems of pattern defects such as short circuits and the occurrence of convex portions, but as mentioned above, this problem can be effectively eliminated by the method of the present invention.
[0070] As required, an insulating layer and an nth wiring pattern (n is an integer greater than 2) can also be alternately formed on the wiring pattern 30 to form a multilayer wiring board. For each wiring pattern constituting the multilayer wiring board, the wiring pattern 30 can be used as the first wiring pattern, and is successively referred to as the second wiring pattern, the third wiring pattern, ..., the nth wiring pattern. The successive stacking structure consisting of the first wiring pattern, the nth wiring pattern and the insulating layer is usually referred to as a build-up layer or a build-up wiring layer. For the method of forming the build-up layer after the second wiring pattern, the method is not particularly limited. In addition to the above-mentioned SAP method, a modified semi-additive method (MSAP method), a full additive method, a subtractive method, etc. can be used. In addition, bumps for mounting such as solder resists and pillars can also be formed on the wiring pattern on the outermost surface of the build-up layer as required. In short, the known method used in the conventional printed circuit board can be appropriately added and carried out without special restrictions.
[0071] Example
[0072] The present invention is further specifically described by the following examples.
[0073] Examples 1 to 6
[0074] Six types of surface-treated copper foils were prepared, and the surface shape was transferred to an insulating substrate using the surface-treated copper foils. The rough surface of the obtained insulating substrate was subjected to chemical plating to produce a laminate for evaluation, and various evaluations were performed as follows.
[0075] (1) Preparation of surface treated copper foil
[0076] Six types of surface-treated copper foils 10 were prepared, each of which had a treated surface 10a having the parameters shown in Table 1 on at least one side. Some of these surface-treated copper foils 10 were commercially available, and the others were separately produced based on a known method. The measurement / calculation method of each parameter at the treated surface 10a of the prepared surface-treated copper foil 10 is as follows.
[0077] (Arithmetic mean waviness Wa)
[0078] The arithmetic mean waviness Wa of the copper foil surface was measured using a laser microscope (VK-X200 manufactured by Keyence Co., Ltd.) with a 150x objective lens at a magnification of 3000x, slope correction, optical correction, no cutoff, and an evaluation length of 64.124 μm in accordance with JIS B0601-2001.
[0079] (Maximum height Sz and valley void volume Vvv)
[0080] A laser microscope (Keyence Co., Ltd., VK-X200) was used with a 150x objective lens, a magnification of 3000x, waviness removal (intensity 5), no optical correction, cutoffs based on S filters (0.25 μm) and L filters (0.025 mm), and an evaluation area of 6811.801 μm. 2 The maximum height Sz of the copper foil surface and the void volume Vvv of the valley were measured according to ISO25178.
[0081] (2) Preparation of evaluation laminate
[0082] After laminating two prepregs (Mitsubishi Gas Chemical Co., Ltd., GHPL-830NSF, thickness 100 μm), Figure 3 As shown, the surface treated copper foil 10 prepared in (1) is laminated on the insulating substrate 20' in such a manner as to contact the treated surface 10a, and the pressing temperature is 220°C, the pressing time is 90 minutes, and the pressing pressure is 40 kgf / cm 2 The copper-clad laminate 12 was obtained by pressing under the conditions of . The surface-treated copper foil 10 of the copper-clad laminate 12 was completely removed by a sulfuric acid-hydrogen peroxide-based etching solution to obtain an insulating substrate 20 having a rough surface 20a to which the surface shape of the treated surface 10a was transferred. For the insulating substrate 20, chemical copper plating was performed using a chemical copper plating solution (manufactured by Uemura Industry Co., Ltd., THRU-CUP PEA) to form a chemical plating layer 22 with a thickness of 0.7 μm on the rough surface 20a side. In this way, a laminate before laminating a photoresist layer in the SAP method (hereinafter referred to as an evaluation laminate) was obtained.
[0083] (3) Measurement of surface profile of evaluation laminate
[0084] The various parameters on the surface of the electroless plating layer 22 side of the evaluation laminate obtained above were measured as follows.
[0085] (Arithmetic mean waviness Wa)
[0086] Using a laser microscope (VK-X200 manufactured by KEYENCE Co., Ltd.), a 150x objective lens, a magnification of 3000x, slope correction, noise removal based on DCL / BCL, no cutoff, and an evaluation length of 64.124 μm, the arithmetic mean waviness Wa of the side surface of the chemical plating layer 22 of the evaluation stack was measured in accordance with JIS B0601-2001.
[0087] (kurtosis Sku and valley void volume Vvv)
[0088] A laser microscope (Keyence Co., Ltd., VK-X200) was used with a 150x objective lens, a magnification of 3000x, waviness removal (intensity 5), no noise removal by DCL / BCL, cutoff by S filter (0.25 μm) and L filter (0.025 mm), and an evaluation area of 6811.801 μm. 2 The kurtosis Sku of the side surface of the chemical plating layer 22 of the evaluation stack and the void volume Vvv of the valley portion were measured in accordance with ISO25178 under the conditions of .
[0089] (4) Evaluation of evaluation laminate
[0090] The evaluation of various properties of the evaluation laminate obtained above was performed as follows.
[0091] <Dust detection number>
[0092] The dust detection number was evaluated as follows. First, a negative photoresist layer 24 (RY-5319 manufactured by Hitachi Chemical Co., Ltd.) having a thickness of 19 μm was laminated on the surface of the chemical plating layer 22 side of the evaluation laminate obtained above at a lamination speed of 1.5 m / min. Figure 6 As shown in (i), a glass mask 25 is stacked on the surface of the photoresist layer 24. It should be noted that on the glass mask 25, a circular shading portion B (diameter 6μm, 7μm, 8μm or 9μm, 200 each) assumed to be foreign matter such as dust is provided at the center of each area divided into 100μm×100μm. Therefore, light will pass through the portion of the glass mask 25 where the shading portion B is not provided, and on the other hand, light will not pass through the portion of the glass mask 25 where the shading portion B is provided. The evaluation laminated body after the glass mask 25 is stacked is exposed (70mJ / cm 2) and developed to form a resist pattern 26. The surface of the resist pattern 26 side of the evaluation laminate after development was observed under a condition of 50 times magnification using a digital microscope (DSX510 manufactured by Olympus Corporation). Figure 6 As shown in (ii), the number of holes H formed on the anti-etching pattern 26 is counted as the number of dust detections. The results are shown in Table 1. It should be noted that the greater the number of dust detections (i.e., the better the resolution), the higher the risk of unnecessary electroplating at a location where a circuit should not be formed, and the more likely it is that a pattern defect will occur.
[0093] <Circuit Formability>
[0094] The circuit formation properties were evaluated as follows. Figure 1 As shown, a negative photoresist layer 24 (UFG-155 manufactured by Asahi Kasei Corporation) with a thickness of 15 μm was laminated on the surface of the chemical plating layer 22 of the evaluation laminate obtained above at a lamination speed of 1.5 m / min, and then a mask with a line / space (L / S) of 9 μm / 6 μm was laminated on the photoresist layer 24 so that the target circuit width would be 7 μm. Figure 2 As shown in the figure, the evaluation laminated body after mask lamination was exposed (70 mJ / cm 2 ) and development to form a resist pattern 26. For the evaluation laminate after the formation of the resist pattern 26, copper electroplating is performed under known conditions to form an electroplated layer 28 between the resist patterns 26. For the evaluation laminate after the formation of the electroplated layer 28, the resist pattern 26 is peeled off, and the unnecessary part of the chemical plating layer 22 exposed thereby is removed by etching using a sulfuric acid-hydrogen peroxide etching solution to form a wiring pattern 30 with a circuit height of 11μm. Regarding the etching amount at this time, the etching rate of the chemical plating layer 22 is measured in advance, and the etching is performed under the condition of further etching by about 0.3μm than the so-called appropriate etching (about 0.7μm), so-called over-etching. The circuit width of the wiring pattern 30 obtained in this way is observed by SEM at a magnification of 5000 times. The circuit width is determined by measuring the length of 10 places at intervals of 1μm for the circuit top width of the wiring pattern 30 in one SEM field of view, and calculating their average value. The circuit width obtained is evaluated according to the following criteria. The results are shown in Table 1.
[0095] -Evaluation A: 6.6μm or more
[0096] -Evaluation B: 5.6 μm or more and less than 6.6 μm
[0097] -Evaluation C: 4.6μm or more and less than 5.6μm
[0098] - Rating D: less than 4.6μm
[0099] [Table 1]
[0100] Table 1
[0101]
[0102] * indicates a comparative example.
Claims
1. A method for manufacturing a printed circuit board, comprising the following steps: (a) a step of preparing an insulating substrate having a rough surface; (b) a step of performing chemical plating on the rough surface of the insulating substrate to form a chemical plating layer having a thickness of less than 1.0 μm, wherein the chemical plating layer has a surface having an arithmetic mean waviness Wa of 0.10 μm or more and 0.25 μm or less as measured in accordance with JIS B0601-2001 and a kurtosis Sku of 2.0 or more and 3.5 or less as measured in accordance with ISO25178; (c) a step of laminating a photoresist layer on the surface of the chemically plated layer; (d) exposing and developing the photoresist layer to form a resist pattern; (e) a step of electroplating the chemical plating layer through the resist pattern; (f) a step of peeling off the resist pattern; and (g) a step of removing unnecessary portions of the chemical plating layer exposed by peeling off the resist pattern by etching to form a wiring pattern, The step (a) comprises: (a-1) preparing a surface-treated copper foil having a treated surface having an arithmetic mean waviness Wa of 0.20 μm or more and 0.35 μm or less as measured in accordance with JIS B0601-2001 and a maximum height Sz of 3.0 μm or more and 4.0 μm or less as measured in accordance with ISO25178, (a-2) laminating an insulating base material on the treated surface of the surface-treated copper foil, transferring the surface shape of the treated surface to the surface of the insulating base material, and then, (a-3) The surface-treated copper foil is removed by etching to obtain the insulating base material having the rough surface.
2. The method according to claim 1, wherein: The arithmetic mean waviness Wa of the surface of the chemical plating layer is greater than or equal to 0.20 μm and less than or equal to 0.25 μm.
3. The method according to claim 1 or 2, wherein: The kurtosis Sku of the surface of the chemical plating layer is greater than or equal to 3.0 and less than or equal to 3.
5.
4. The method according to claim 1 or 2, wherein: The thickness of the chemical plating layer is greater than or equal to 0.3 μm and less than 1.0 μm.
5. The method according to claim 1 or 2, wherein: The photoresist layer includes a dry film resist layer.
6. The method according to claim 5, wherein: The dry film resist layer has a thickness of 2 μm or more and 35 μm or less.
7. The method according to claim 1 or 2, wherein: The wiring pattern has a thickness of 2 μm or more and 30 μm or less.
Citation Information
Patent Citations
Roughened copper foil, copper foil provided with carrier, copper-clad laminated sheet, and printed wiring board
WO2016158775A1
Roughened copper foil, carrier-attached copper foil, copper clad laminate, and printed wiring board
WO2018211951A1
Manufacturing method for printed wiring board
CN101965106A
Manufacturing method of wiring board
JP2012033642A