Semiconductor device and method for manufacturing the same
By preparing an epitaxial layer on the substrate of a semiconductor device and using plasma bombardment to form a rough surface, the problem of high ohmic contact resistance of existing semiconductor devices is solved, lower ohmic contact resistance is achieved, and device performance is improved.
Patent Information
- Application Number
- CN202110848584.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-07-27
AI Technical Summary
Existing semiconductor devices have large ohmic contact resistance, which affects their performance.
Prepare an epitaxial layer on the substrate, including a barrier layer on one side away from the substrate, and bombard the ohmic contact area with plasma to form a rough surface to increase the roughness of the ohmic contact area, and then prepare an ohmic contact electrode in the ohmic contact area to make It forms ohmic contact with the barrier layer.
Achieving low-ohmic contact resistance of semiconductor devices improves their performance.
Smart Images

Figure CN113594044B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the technical field of semiconductor devices, and in particular, to a semiconductor device and a method for manufacturing the same. Background Art
[0002] The third generation of semiconductor materials, namely wide bandgap semiconductor (WBGS) semiconductor materials, were developed after the first generation of silicon, germanium and the second generation of gallium arsenide, indium phosphide, etc. Among the third generation of semiconductor materials, gallium nitride (GaN) has superior properties such as wide bandgap, direct bandgap, high breakdown electric field, low dielectric constant, high electron saturation drift velocity, strong radiation resistance and good chemical stability, becoming the key semiconductor material for manufacturing a new generation of microelectronic devices and circuits after germanium, silicon and gallium arsenide. In particular, it has unique advantages in high temperature, high power, high frequency and radiation-resistant electronic devices and full wavelength and short wavelength optoelectronic devices. It is an ideal material for realizing high temperature, high power, high frequency and radiation-resistant, full wavelength optoelectronic devices. It is a key basic material for the continued development of high-tech such as microelectronics, power electronics, optoelectronics, and pillar industries such as national defense industry, information industry, electromechanical industry and energy industry after entering the 21st century.
[0003] Ohmic contact resistance is an important parameter that characterizes the performance of semiconductor devices. In existing semiconductor devices, the ohmic contact resistance is relatively large, which affects the performance of semiconductor devices. Summary of the invention
[0004] In view of this, an embodiment of the present invention provides a semiconductor device and a method for manufacturing the same, to achieve low ohmic contact resistance.
[0005] An embodiment of the present invention provides a method for manufacturing a semiconductor device, comprising:
[0006] providing a substrate;
[0007] Preparing an epitaxial layer on one side of the substrate, wherein the epitaxial layer includes a barrier layer away from one side of the substrate, and the barrier layer includes an ohmic contact region;
[0008] The ohmic contact region is bombarded with plasma to form a rough surface in the ohmic contact region; the rough surface includes at least a first position and a second position, and the first position and the second position have different heights along a first direction; the first direction is perpendicular to the plane where the substrate is located;
[0009] Prepare an ohmic contact electrode in the ohmic contact region, wherein the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region;
[0010] Optionally, bombarding the ohmic contact region with plasma to form a rough surface in the ohmic contact region comprises:
[0011] bombarding the ohmic contact region with at least one of hydrogen plasma, inert gas plasma, fluorine-based plasma, and chlorine-based plasma to form a rough surface in the ohmic contact region;
[0012] Optionally, along the first direction, a height difference h between the first position and the second position satisfies 10 nm ≤ h ≤ 30 nm;
[0013] Optionally, preparing an ohmic contact electrode in the ohmic contact region includes:
[0014] A deposition or sputtering process is used to prepare a stacked multilayer ohmic contact electrode in the ohmic contact area.
[0015] Optionally, the multilayer ohmic contact electrode includes a titanium metal layer, an aluminum metal layer, a nickel metal layer and a titanium nitride metal layer stacked in sequence;
[0016] Wherein, along the first direction, the thickness d1 of the titanium metal layer satisfies 2nm≤d1≤500nm;
[0017] The thickness d2 of the aluminum metal layer satisfies 2nm≤d2≤500nm;
[0018] The thickness d3 of the nickel metal layer satisfies 2nm≤d3≤500nm;
[0019] The thickness d4 of the titanium nitride metal layer satisfies 2nm≤d4≤500nm;
[0020] Optionally, after the ohmic contact electrode is prepared in the ohmic contact region, the method further comprises:
[0021] Performing high temperature thermal annealing on the ohmic contact electrode;
[0022] Optionally, before bombarding the ohmic contact region with plasma, the method further comprises:
[0023] The barrier layer is etched in the ohmic contact region by using an inductively coupled plasma etching process or a reactive ion etching process; along the first direction, the etching depth is less than the thickness of the barrier layer;
[0024] Optionally, the ohmic contact electrode includes a source and a drain;
[0025] After the ohmic contact electrode is prepared in the ohmic contact area, the method further comprises:
[0026] Forming a gate dielectric layer on a side of the barrier layer away from the substrate;
[0027] A gate is prepared on a side of the gate dielectric layer away from the substrate, wherein the gate forms a Schottky contact with the barrier layer;
[0028] Optionally, before bombarding the ohmic contact region with plasma, the method further comprises:
[0029] The epitaxial layer is etched by an inductively coupled plasma etching process to form an active region of the semiconductor device in the epitaxial layer.
[0030] In a second aspect, an embodiment of the present invention provides a semiconductor device, wherein the semiconductor device is obtained by the method for preparing a semiconductor device according to any embodiment of the present invention, and the semiconductor device comprises:
[0031] substrate;
[0032] An epitaxial layer located on one side of the substrate, the epitaxial layer comprising a barrier layer away from one side of the substrate, the barrier layer comprising an ohmic contact region;
[0033] The surface of the ohmic contact area is a rough surface; the rough surface includes at least a first position and a second position, and along a first direction, the first position and the second position have different heights; the first direction is perpendicular to the plane where the substrate is located;
[0034] An ohmic contact electrode is located in the ohmic contact region, and the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region.
[0035] The technical solution provided by the embodiment of the present invention is to prepare an epitaxial layer on a substrate, wherein the epitaxial layer includes a barrier layer on a side away from the substrate, and use plasma to bombard an ohmic contact region in the barrier layer to form a rough surface, that is, the rough surface includes a first position and a second position with different heights, and then prepare an ohmic contact electrode in the ohmic contact region to form an ohmic contact with the barrier layer. The ohmic contact region is bombarded with plasma, so that the ohmic region has a higher level of roughness, so that the semiconductor device has an ohmic contact with a lower resistance, thereby ensuring the improvement of the performance of the semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0037] Figure 1 A flow chart of a method for preparing a first semiconductor device provided by an embodiment of the present invention;
[0038] Figure 2 A flow chart of a method for preparing a second semiconductor device provided by an embodiment of the present invention;
[0039] Figure 3 A flow chart of a method for preparing a third semiconductor device provided by an embodiment of the present invention;
[0040] Figure 4 A flow chart of a fourth method for preparing a semiconductor device provided by an embodiment of the present invention;
[0041] Figure 5 A flow chart of a method for preparing a fifth semiconductor device provided by an embodiment of the present invention;
[0042] Figure 6 A flow chart of a sixth method for preparing a semiconductor device provided by an embodiment of the present invention;
[0043] Figure 7 to Figure 13 The embodiment of the present invention provides Figure 6 Schematic diagram of the preparation structure of the corresponding semiconductor device. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be fully described below in combination with the drawings in the embodiments of the present invention through specific implementation methods. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work fall within the protection scope of the present invention.
[0045] Figure 1 FIG. 1 is a flow chart of a method for preparing a first semiconductor device according to an embodiment of the present invention. Figure 1 As shown, the specific steps include the following:
[0046] S101. Provide a substrate.
[0047] The substrate is a clean single crystal wafer used to grow an epitaxial layer, and may be, for example, silicon carbide (SiC), sapphire or silicon (Si). The embodiment of the present invention does not limit the type of substrate.
[0048] S102, preparing an epitaxial layer on one side of the substrate, wherein the epitaxial layer includes a barrier layer away from the side of the substrate, and the barrier layer includes an ohmic contact region.
[0049] The epitaxial layer is a heteroepitaxial layer of a semiconductor device, that is, grown on a substrate, and may be a GaN-based epitaxial layer, for example.
[0050] The barrier layer refers to the blocking layer formed by the diffusion of electrons and holes. The potential difference on both sides is called the barrier. For example, when using aluminum gallium nitride / gallium nitride (AlGaN / GaN) heterostructure, the barrier layer is mainly AlGaN.
[0051] The ohmic contact region refers to the region where the semiconductor and the metal form contact. In order to ensure the effective operation of the device, the contact resistance of the ohmic contact region should be as small as possible.
[0052] S103, bombarding the ohmic contact area with plasma to form a rough surface in the ohmic contact area.
[0053] The rough surface includes at least a first position and a second position, and along a first direction, the first position and the second position have different heights; the first direction is perpendicular to the plane where the substrate is located.
[0054] Plasma bombardment is an etching technology, that is, using high-energy ion beams to bombard materials. Since the high-energy ion bombardment process will cause damage to the material surface, plasma etching can be combined with the use of highly chemically active atoms or ions in the plasma to react chemically with the material. The specific etching method is not limited in the embodiment of the present invention, for example, it can be reactive ion etching, inductively coupled plasma etching or electron cyclotron resonance plasma etching.
[0055] Specifically, plasma bombardment is used to form concave-convex areas with different heights in the ohmic contact area, that is, a rough surface. That is, the rough surface includes positions with different heights, such as a first position and a second position, and the first position and the second position have different heights along the direction perpendicular to the plane where the substrate is located. That is, the surface roughness of the ohmic contact area is increased by plasma bombardment of the ohmic contact area, so that the ohmic contact electrode prepared in the ohmic contact area subsequently forms a more comprehensive contact with the barrier layer.
[0056] Furthermore, the first position and the second position may be the highest point and the lowest point on the rough surface, or may be other two positions with different heights, which is not limited in the embodiment of the present invention.
[0057] S104, preparing an ohmic contact electrode in the ohmic contact region, wherein the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region.
[0058] Specifically, the ohmic contact electrode forms an ohmic contact with the barrier layer, and applying a voltage to the ohmic contact electrode controls the output current characteristics.
[0059] It should be noted that the semiconductor device in the embodiment of the present invention may include a triode structure or a diode structure, which is not limited in the embodiment of the present invention.
[0060] For example, when the semiconductor device includes a triode structure, the ohmic contact electrode can be the source and drain of the semiconductor device. For example, when the source or drain includes metal Ti and the barrier layer includes AlGaN, the surface roughness of the ohmic contact area can be increased by bombarding the ohmic contact area with high-energy plasma, so that the metal Ti and the N element in the underlying AlGaN barrier layer can be more comprehensively combined to generate a TiN alloy product, which can reduce the metal barrier and achieve a lower ohmic contact resistance.
[0061] In summary, the technical solution provided by the embodiment of the present invention is to prepare an epitaxial layer on a substrate, wherein the epitaxial layer includes a barrier layer on one side away from the substrate, and use plasma to bombard the ohmic contact area in the barrier layer to form a rough surface, that is, the rough surface includes a first position and a second position with different heights, and then prepare an ohmic contact electrode in the ohmic contact area to form an ohmic contact with the barrier layer. The ohmic contact area is bombarded with plasma, so that the ohmic area has a higher level of roughness, so that the semiconductor device has an ohmic contact with a lower resistance, thereby ensuring the improvement of the performance of the semiconductor device.
[0062] Optionally, the ohmic contact region is bombarded with plasma to form a rough surface in the ohmic contact region, including: bombarding the ohmic contact region with at least one of hydrogen plasma, inert gas plasma, fluorine-based plasma and chlorine-based plasma to form a rough surface in the ohmic contact region.
[0063] The fluorine-based plasma refers to a plasma containing fluorine, such as carbon tetrafluoride, etc. Similarly, the chlorine-based plasma refers to a plasma containing chlorine, such as boron trichloride, etc.
[0064] Specifically, bombarding the ohmic contact area with hydrogen plasma, inert gas plasma, fluorine-based plasma or chlorine-based plasma can form a rough surface in the ohmic contact area, thereby increasing the contact area of the ohmic contact area, and the metal in the ohmic contact area is more comprehensively combined with the N element in the AlGaN barrier layer, and the resulting alloy product can have a lower ohmic contact resistance.
[0065] Optionally, along the first direction, a height difference h between the first position and the second position satisfies 10 nm≤h≤30 nm.
[0066] Specifically, along the first direction perpendicular to the plane of the substrate, the height difference h between the first position and the second position satisfies the condition of being greater than or equal to 10 nm and less than or equal to 30 nm, thereby ensuring that the roughness of the ohmic contact area is moderate, which will not affect the surface quality of the ohmic contact area and can ensure sufficient contact area to effectively reduce the ohmic contact resistance.
[0067] Optionally, preparing an ohmic contact electrode in the ohmic contact region includes: adopting a deposition or sputtering process to prepare a stacked layer of ohmic contact electrodes in the ohmic contact region.
[0068] Deposition refers to metal deposition on the ohmic contact region to form an ohmic contact electrode, and sputtering refers to plasma bombardment on the ohmic contact region to form an ohmic contact electrode. For example, the deposition process may adopt an electron beam evaporation method.
[0069] Specifically, the ohmic contact electrode can be formed by stacking multiple metal films in sequence. Different metal film layers, number of layers and thickness of metal film layers have different effects on the ohmic contact resistance and the surface morphology of the ohmic contact area. By setting up multiple ohmic contact electrodes, the contact resistance between the ohmic contact electrode and the barrier layer can be further reduced. Furthermore, the multi-layer ohmic contact electrode obtained by depositing stacked metal layers in the ohmic contact area by a deposition or sputtering process can ensure that the surface of the ohmic contact electrode is flat and smooth, there are no metal spikes and it has good ohmic characteristics.
[0070] Optionally, the multilayer ohmic contact electrode includes a titanium metal layer, an aluminum metal layer, a nickel metal layer and a titanium nitride metal layer stacked in sequence; wherein, along the first direction, the thickness d1 of the titanium metal layer satisfies 2nm≤d1≤500nm; the thickness d2 of the aluminum metal layer satisfies 2nm≤d2≤500nm; the thickness d3 of the nickel metal layer satisfies 2nm≤d3≤500nm; and the thickness d4 of the titanium nitride metal layer satisfies 2nm≤d4≤500nm.
[0071] Specifically, a titanium (Ti) metal layer, an aluminum (Al) metal layer, a nickel (Ni) metal layer and a titanium nitride (TiN) metal layer are sequentially stacked along a first direction away from a side of the substrate, that is, the titanium (Ti) metal layer is located on a side close to the barrier layer. Further, the thicknesses d1, d2, d3 and d4 of the different metal layers are respectively greater than 2nm and less than 500nm, for example, preferably d1 is 23nm, d2 is 90nm, d3 is 60nm, and d4 is 60nm, so as to ensure that the Ti element in the metal layer is sufficient to combine with the N element in the AlGaN barrier layer to produce an alloy product TiN, thereby achieving a lower ohmic contact resistance.
[0072] Figure 2 A flow chart of a method for preparing a second semiconductor device provided by an embodiment of the present invention, such as Figure 2 As shown, the specific steps include:
[0073] S201, providing a substrate.
[0074] S202, preparing an epitaxial layer on one side of the substrate, wherein the epitaxial layer includes a barrier layer away from the side of the substrate, and the barrier layer includes an ohmic contact region.
[0075] S203, bombarding the ohmic contact region with plasma to form a rough surface in the ohmic contact region.
[0076] S204, preparing an ohmic contact electrode in the ohmic contact region, wherein the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region.
[0077] S205, performing high temperature thermal annealing treatment on the ohmic contact electrode.
[0078] Specifically, the specific implementation method of high-temperature thermal annealing is not limited in the embodiment of the present invention. For example, it can be implemented in a rapid thermal annealing machine or a rapid thermal processing machine. The rapid thermal annealing can be performed in an N2 atmosphere, and the temperature can be set to 700°C to 950°C and the time can be 20s to 50s.
[0079] In this embodiment, after preparing an ohmic contact electrode in the ohmic contact region, the ohmic contact electrode is subjected to high-temperature thermal annealing to form an ohmic contact, so that the dopant in the barrier layer in the ohmic contact region and the metal in the ohmic electrode can fully contact and react, which can shorten the process time and reduce the ohmic contact resistance.
[0080] Figure 3 A flow chart of a method for preparing a third semiconductor device provided by an embodiment of the present invention, such as Figure 3 As shown, the specific steps include:
[0081] S301, providing a substrate.
[0082] S302 , preparing an epitaxial layer on one side of the substrate, wherein the epitaxial layer includes a barrier layer away from the side of the substrate, and the barrier layer includes an ohmic contact region.
[0083] S303 , etching the barrier layer in the ohmic contact region by using an inductively coupled plasma etching process or a reactive ion etching process; along the first direction, the etching depth is less than the thickness of the barrier layer.
[0084] Among them, the inductively coupled plasma etching process refers to the generation of plasma through the inductively coupled mode excited by the radio frequency power supply, and the reactive ion etching process refers to the plasma generated by gas discharge with a large number of chemically active gas ions. The barrier layer at the ohmic contact area is etched by the inductively coupled plasma etching process or the reactive ion etching process, and the etching depth is less than the thickness of the barrier layer. For example, if the etching depth is 2nm to 280nm, the thickness of the barrier layer must be greater than 280nm. In this way, the ohmic contact area is ensured to be within the barrier layer, and the metal layer Ti on the ohmic contact electrode can produce TiN alloy products with the N element in the AlGaN barrier layer, thereby reducing the ohmic contact resistance.
[0085] S304, bombarding the ohmic contact region with plasma to form a rough surface in the ohmic contact region.
[0086] S305 , preparing an ohmic contact electrode in the ohmic contact region, wherein the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region.
[0087] In this embodiment, the barrier layer at the ohmic contact area is etched by an inductively coupled plasma etching process or a reactive ion etching process, and the etching depth is less than the thickness of the barrier layer, thereby ensuring that the ohmic electrode in the ohmic contact area reacts with the barrier layer and that the generated compound can effectively reduce the ohmic contact resistance.
[0088] Figure 4 A flow chart of a fourth method for preparing a semiconductor device provided by an embodiment of the present invention, such as Figure 4 As shown, the specific steps include:
[0089] S401, providing a substrate.
[0090] S402 , preparing an epitaxial layer on one side of the substrate, wherein the epitaxial layer includes a barrier layer away from the side of the substrate, and the barrier layer includes an ohmic contact region.
[0091] S403, bombarding the ohmic contact region with plasma to form a rough surface in the ohmic contact region.
[0092] S404, preparing an ohmic contact electrode in the ohmic contact region, wherein the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region.
[0093] S405 , preparing a gate dielectric layer on a side of the barrier layer away from the substrate; preparing a gate on a side of the gate dielectric layer away from the substrate, the gate and the barrier layer forming a Schottky contact.
[0094] The gate dielectric layer is an oxide dielectric, which may be aluminum oxide, silicon oxide, aluminum nitride, hafnium oxide, silicon oxynitride, etc. The specific preparation process is not limited in the embodiment of the present invention, and may be generated by, for example, film growth technology, specifically, atomic layer deposition (ALD), low pressure chemical vapor deposition (LPCVD) or plasma enhanced chemical vapor deposition (PECVD).
[0095] Schottky contact is another case of metal-semiconductor contact. Unlike ohmic contact, there is an obvious potential barrier at the contact surface. When metal and semiconductor contact to form a Schottky barrier, electrons can only flow from the semiconductor to the metal due to the barrier, but cannot be transferred from the metal side to the semiconductor side. Therefore, the Schottky barrier has a unidirectional conduction rectification characteristic, which is not available in ohmic contact.
[0096] Specifically, the semiconductor device includes a source, a drain and a gate, wherein the ohmic contact electrode includes a source and a drain, and after the ohmic contact electrode is prepared in the ohmic contact region, a gate dielectric layer is prepared on the side of the barrier layer away from the substrate, and then a gate is prepared on the side of the gate dielectric layer away from the substrate, so that the gate and the barrier layer form a Schottky contact. It should be noted that the preparation process of the gate can use deposition or sputtering technology to deposit a stacked metal in the gate region, and the nickel metal layer and the titanium nitride metal layer can be sequentially in the direction away from the gate dielectric layer. The thickness of the different metal layers is greater than 2nm and less than 500nm, respectively. For example, it is preferred that the thickness of the nickel metal layer is 60nm and the thickness of the titanium nitride metal layer is 60nm. Since the gate is the switch control source of the entire device, the concentration of channel electrons in the heterojunction is controlled by applying different voltages to the gate, and then the device is well controlled. In order to prevent the semiconductor from generating current to the metal side, the barrier height of the gate Schottky contact can be appropriately increased, so as to effectively avoid the reverse leakage current of the Schottky and increase the breakdown voltage.
[0097] In this embodiment, after the ohmic contact electrode is formed in the ohmic contact region, a gate dielectric layer is formed on the side of the barrier layer away from the substrate, and then a gate is formed on the side of the gate dielectric layer away from the substrate, so that the gate and the barrier layer form a Schottky contact. The semiconductor device can be used as a switching device in various occasions when it has a complete source, drain and gate, wherein the gate is the switch control source of the entire device, and different voltages are applied to the gate to control the device.
[0098] Figure 5 A flow chart of a method for preparing a fifth semiconductor device provided by an embodiment of the present invention, such as Figure 5 As shown, the specific steps include:
[0099] S501 , providing a substrate.
[0100] S502 , preparing an epitaxial layer on one side of the substrate, wherein the epitaxial layer includes a barrier layer away from the side of the substrate, and the barrier layer includes an ohmic contact region.
[0101] S503 , etching the epitaxial layer using an inductively coupled plasma etching process to form an active region of the semiconductor device in the epitaxial layer.
[0102] The active area refers to the area covered by the source, drain and conductive channel of the semiconductor device.
[0103] Specifically, the epitaxial layer is etched using an inductively coupled plasma etching process, and the area outside the active region of the semiconductor device is etched to a certain depth, for example, along the first direction, the etching depth is 300nm to 2um.
[0104] S504, bombarding the ohmic contact region with plasma to form a rough surface in the ohmic contact region.
[0105] S505 , preparing an ohmic contact electrode in the ohmic contact region, wherein the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region.
[0106] In this embodiment, an inductively coupled plasma etching process is used to etch the epitaxial layer to form the active area of the semiconductor device. In this way, the two-dimensional electron gas channels originally existing in these positions are cut off, so that the high electron mobility transistor devices on the active area are electrically isolated, thereby ensuring that the devices will not affect each other when electrical testing is performed.
[0107] Based on the above embodiments, the following is a detailed description of the method for preparing a semiconductor device based on the actual preparation process. Specifically, Figure 6 A flow chart of a sixth method for preparing a semiconductor device provided by an embodiment of the present invention, such as Figure 6 As shown, the specific implementation process mainly includes the following steps:
[0108] S601, providing a substrate.
[0109] like Figure 7 As shown, the substrate 101 of the semiconductor device may be a Si substrate.
[0110] S602 , preparing an epitaxial layer on one side of the substrate, wherein the epitaxial layer includes a barrier layer away from the side of the substrate, and the barrier layer includes an ohmic contact region.
[0111] like Figure 8 As shown, the epitaxial layer 102 further includes a buffer layer 105 and a channel layer 104, which are stacked in sequence in a direction away from the substrate 101, wherein the buffer layer 105 and the channel layer 104 may be GaN, and the barrier layer 103 may be AlGaN.
[0112] S603 , etching the epitaxial layer using an inductively coupled plasma etching process to form an active region of the semiconductor device in the epitaxial layer.
[0113] like Fig. 9As shown, the buffer layer 105, the channel layer 104 and the barrier layer 103 are etched by inductively coupled plasma, and the etching depth along the first direction Y is 300nm-2um.
[0114] S604 , etching the barrier layer in the ohmic contact region by using an inductively coupled plasma etching process or a reactive ion etching process; along the first direction, the etching depth is less than the thickness of the barrier layer.
[0115] like Fig.10 As shown, the barrier layer 103 is etched in the ohmic contact region 106 by using an inductively coupled plasma etching process or a reactive ion etching process, and the etching depth along the first direction Y is 2 nm to 280 nm.
[0116] S605 , bombarding the ohmic contact region with plasma to form a rough surface in the ohmic contact region.
[0117] like Fig.11 As shown, the ohmic contact region 106 is bombarded with hydrogen plasma, inert gas plasma, fluorine-based plasma or chlorine-based plasma to form a rough surface. Along the first direction Y, the height difference between the first position 1061 and the second position 1062 is 10nm to 30nm.
[0118] S606 , preparing an ohmic contact electrode in the ohmic contact region, wherein the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region.
[0119] like Fig.12 As shown, a deposition or sputtering process is used to prepare a multilayer ohmic contact electrode 1063 in a stacked manner in the ohmic contact area 106, and a titanium metal layer 10634, an aluminum metal layer 10633, a nickel metal layer 10632 and a titanium nitride metal layer 10631 are stacked in sequence along a direction away from the side of the substrate 101. Along the first direction Y, the thickness d1 of the titanium metal layer 10634 satisfies 2nm≤d1≤500nm; the thickness d2 of the aluminum metal layer 10633 satisfies 2nm≤d2≤500nm; the thickness d3 of the nickel metal layer 10632 satisfies 2nm≤d3≤500nm; and the thickness d4 of the titanium nitride metal layer 10631 satisfies 2nm≤d4≤500nm.
[0120] S607 , performing high temperature thermal annealing treatment on the ohmic contact electrode.
[0121] Continue to refer Fig.12 As shown, a rapid thermal annealing machine or a rapid thermal processing machine is used to perform high-temperature thermal annealing on the ohmic contact electrode 1063, and the temperature is set to 700° C. to 950° C. and the time is 20s to 50s.
[0122] S608, preparing a gate dielectric layer on the side of the barrier layer away from the substrate; preparing a gate on the side of the gate dielectric layer away from the substrate, the gate and the barrier layer forming a Schottky contact.
[0123] like Fig.13 As shown, a gate dielectric layer 107 is prepared on a side of the barrier layer 103 away from the substrate 101, and a gate 108 is prepared on a side of the gate dielectric layer 107 away from the substrate 101. The preparation process of the gate 108 can use a deposition or sputtering technology to deposit a stacked metal in the gate area, and a nickel metal layer and a titanium nitride metal layer can be stacked in sequence along the direction away from the side of the gate dielectric layer 107. The thickness of the different metal layers meets the requirements of being greater than 2nm and less than 500nm, so that the gate 107 forms a Schottky contact with the barrier layer 103.
[0124] In this embodiment, an epitaxial layer is prepared on a substrate, including a barrier layer, a channel layer and a buffer layer, and an inductively coupled plasma is used to etch the epitaxial layer to form an active region, and then the ohmic contact region in the barrier layer is etched with inductively coupled plasma to make the etching depth less than the thickness of the barrier layer, and then the ohmic contact region is bombarded with plasma to form a rough surface with different heights at the first position and the second position, and then a multilayer ohmic contact electrode is prepared in the ohmic contact region to form an ohmic contact with the barrier layer, and the ohmic contact electrode is subjected to high-temperature thermal annealing, and then a gate dielectric layer and a gate are prepared on the side away from the substrate. In this way, the complete preparation of the semiconductor device is achieved, ensuring that the semiconductor device has a lower ohmic contact resistance, and improving the performance of the semiconductor device.
[0125] Based on the same inventive concept, an embodiment of the present invention further provides a semiconductor device, which is specifically obtained by the method for preparing the semiconductor device in any of the above embodiments, and further reference is made to Fig.13 As shown, the semiconductor device includes: a substrate 101; an epitaxial layer 102 located on one side of the substrate, the epitaxial layer 102 includes a barrier layer 103 away from the side of the substrate 101, and the barrier layer 103 includes an ohmic contact area 106; the surface of the ohmic contact area 106 is a rough surface; the rough surface at least includes a first position 1061 and a second position 1062, and along a first direction Y, the first position 1061 and the second position 1062 have different heights; the first direction Y is perpendicular to the plane where the substrate 101 is located; an ohmic contact electrode 1063 located in the ohmic contact area 106, and the ohmic contact electrode 1063 forms an ohmic contact with the barrier layer 103 in the ohmic contact area 106.
[0126] The epitaxial layer 102 at least includes a barrier layer 103, a channel layer 104 and a buffer layer 105, which are stacked in sequence in a direction away from the substrate 101. The barrier layer 103 includes an ohmic contact region 106, the surface of which is a rough surface, including a first position 1061 and a second position 1062, and when observed along a first direction Y perpendicular to the plane where the substrate 101 is located, the first position 1061 and the second position 1062 have different heights, and an ohmic contact electrode 1063 of the ohmic contact region 106 forms an ohmic contact with the barrier layer 103, so that the contact area is increased by setting the surface of the ohmic contact region 106 to be a rough surface, thereby achieving low ohmic contact.
[0127] A semiconductor device provided by an embodiment of the present invention can be obtained by a method for preparing a semiconductor device provided by any embodiment of the present invention, by arranging an epitaxial layer on a substrate, a barrier layer being provided on the side of the epitaxial layer away from the substrate, the barrier layer including an ohmic contact region, the surface of the ohmic contact region being a rough surface including a first position and a second position with different heights, an ohmic contact electrode in the ohmic contact region forms an ohmic contact with the barrier layer, thereby increasing the contact area between the ohmic electrode in the ohmic contact region and the barrier layer, thereby achieving low ohmic contact.
[0128] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and the features of the various embodiments of the present invention may be partially or completely coupled or combined with each other, and may cooperate with each other in various ways and be technically driven. It is possible for those skilled in the art to make various obvious changes, readjustments, combinations and substitutions without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A method for preparing a semiconductor device, characterized in that: include: providing a substrate; Preparing an epitaxial layer on one side of the substrate, wherein the epitaxial layer includes a barrier layer away from one side of the substrate, and the barrier layer includes an ohmic contact region; The ohmic contact region is bombarded with plasma to form a rough surface in the ohmic contact region; the rough surface includes at least a first position and a second position, and the first position and the second position have different heights along a first direction; the first direction is perpendicular to the plane where the substrate is located; Prepare an ohmic contact electrode in the ohmic contact region, wherein the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region; Wherein, the barrier layer comprises AlGaN, and the ohmic contact electrode comprises metal Ti; Before bombarding the ohmic contact region with plasma, the method further comprises: The barrier layer is etched in the ohmic contact region by using an inductively coupled plasma etching process or a reactive ion etching process; along the first direction, the etching depth is less than the thickness of the barrier layer; Before bombarding the ohmic contact region with plasma, the method further comprises: The epitaxial layer is etched by an inductively coupled plasma etching process to form an active region of the semiconductor device in the epitaxial layer.
2. The preparation method according to claim 1, characterized in that: Bombarding the ohmic contact region with plasma to form a rough surface in the ohmic contact region comprises: The ohmic contact region is bombarded with at least one of hydrogen plasma, inert gas plasma, fluorine-based plasma, and chlorine-based plasma to form a rough surface on the ohmic contact region.
3. The preparation method according to claim 1, characterized in that: Along the first direction, a height difference h between the first position and the second position satisfies 10 nm≤h≤30 nm.
4. The preparation method according to claim 1, characterized in that: The ohmic contact electrode is prepared in the ohmic contact region, comprising: A deposition or sputtering process is used to prepare a stacked multilayer ohmic contact electrode in the ohmic contact area.
5. The preparation method according to claim 4, characterized in that: The multilayer ohmic contact electrode comprises a titanium metal layer, an aluminum metal layer, a nickel metal layer and a titanium nitride metal layer stacked in sequence; Wherein, along the first direction, the thickness d1 of the titanium metal layer satisfies 2nm≤d1≤500nm; The thickness d2 of the aluminum metal layer satisfies 2nm≤d2≤500nm; The thickness d3 of the nickel metal layer satisfies 2nm≤d3≤500nm; The thickness d4 of the titanium nitride metal layer satisfies 2nm≤d4≤500nm.
6. The preparation method according to claim 1, characterized in that: After the ohmic contact electrode is prepared in the ohmic contact area, the method further comprises: The ohmic contact electrode is subjected to high temperature thermal annealing treatment.
7. The preparation method according to claim 1, characterized in that: The ohmic contact electrode includes a source electrode and a drain electrode; After the ohmic contact electrode is prepared in the ohmic contact area, the method further comprises: Forming a gate dielectric layer on a side of the barrier layer away from the substrate; A gate is formed on a side of the gate dielectric layer away from the substrate, and the gate forms a Schottky contact with the barrier layer.
8. A semiconductor device, characterized in that: Prepared by the preparation method according to any one of claims 1 to 7; the semiconductor device comprises: substrate; An epitaxial layer located on one side of the substrate, the epitaxial layer includes a barrier layer away from the side of the substrate, the barrier layer includes an ohmic contact region; the surface of the ohmic contact region is a rough surface; the rough surface includes at least a first position and a second position, and along a first direction, the first position and the second position have different heights; the first direction is perpendicular to the plane where the substrate is located; An ohmic contact electrode is located in the ohmic contact region, and the ohmic contact electrode forms an ohmic contact with the barrier layer in the ohmic contact region.