Preparation method of low temperature resistant lithium ion battery

By arranging nanocarbon heating films and temperature adjustment systems on lithium-ion battery sheets, the problem of shortened life of lithium-ion batteries under low temperature conditions is solved, and battery performance improvement and cost savings are achieved.

CN113594551BInactive Publication Date: 2024-10-29XINJIANG HUAPU ENERGY TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202110821468.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-20
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The service life of lithium-ion batteries is shortened under low temperature conditions, especially in cold areas, resulting in reduced battery performance and increased replacement costs.

Method used

A nanocarbon heating film is set on the lithium-ion battery sheet to increase the battery temperature through preheating treatment, and a temperature adjustment system is set up in the battery inner shell to ensure that the battery maintains a suitable temperature under low temperature conditions.

Benefits of technology

Extends the service life of lithium-ion batteries, improves battery performance, and avoids performance degradation and replacement costs caused by low temperatures.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a method for preparing a low-temperature resistant lithium-ion battery, which comprises the following steps: placing an electrolyte membrane between a positive electrode sheet and a negative electrode sheet, and obtaining a combined battery sheet through a single sheet pressing process; coating an insulating protective layer on the upper and lower surfaces of the combined battery sheet, and then evenly placing at least three first temperature sensors on the upper surface and bonding a layer of nano-carbon heating film, and rolling up from one end after a secondary sheet pressing process to obtain a battery core; placing the battery core in a prefabricated battery inner shell, connecting a heating switch from both ends of the nano-carbon heating film, and the heating switch is electrically connected to the first temperature sensor; placing at least two battery inner shells equipped with battery cores side by side in a battery outer shell to obtain a finished low-temperature resistant lithium-ion battery. The present invention is provided with a nano-carbon heating film on the battery sheet, which can preheat the battery in advance under low temperature conditions, so that the battery is charged and discharged after the temperature is increased, thereby improving its service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium ion batteries, and in particular relates to a method for preparing a low-temperature resistant lithium ion battery. Background Art

[0002] With the large-scale promotion and use of new energy vehicles, their shortcomings of poor low-temperature resistance have gradually been exposed, affecting and restricting their service life and geographical range. In cold seasons, especially in the Northeast, the service life of lithium-ion batteries will be significantly shortened after several years. For consumers, replacing new batteries is also a considerable expense. Summary of the invention

[0003] An object of the present invention is to provide a method for preparing a low-temperature resistant lithium-ion battery and to provide at least the advantages to be described below.

[0004] Another object of the present invention is to provide a method for preparing a low-temperature resistant lithium-ion battery. A nanocarbon heating film is arranged on the battery cell, which can preheat the battery under low temperature conditions, so that charging and discharging can be carried out after the temperature is increased, thereby improving its service life.

[0005] The technical solution of the present invention is as follows:

[0006] A method for preparing a low-temperature resistant lithium-ion battery comprises the following steps:

[0007] Taking the pre-prepared electrolyte membrane, positive electrode sheet and negative electrode sheet, cutting them into strips of the same size, placing the electrolyte membrane between the positive electrode sheet and the negative electrode sheet, and performing a sheet pressing process to obtain a combined battery sheet;

[0008] An insulating protective layer is coated on the upper and lower surfaces of the combined battery cell, at least three first temperature sensors are evenly placed on the upper surface, and then a nano-carbon heating film is bonded thereto, and after a secondary sheeting process, the battery cell is rolled up from one end to obtain a battery core;

[0009] The battery core is placed in a prefabricated battery inner shell, a heating switch is connected from both ends of the nano-carbon heating film, and the heating switch is electrically connected to the first temperature sensor;

[0010] At least two battery inner shells containing battery cells are placed side by side in a battery outer shell, and the battery cells in two adjacent battery inner shells are connected in series through a wire to obtain a low-temperature resistant lithium-ion battery product.

[0011] Preferably, in the method for preparing the low-temperature resistant lithium-ion battery, the one-time tableting process comprises:

[0012] Preheat the adhesive, keep the temperature at 53-61°C, place the negative electrode sheet and apply the adhesive on its upper surface, place the electrolyte membrane, perform primary pressing for 14-17 minutes, and then let it stand until the temperature drops to 42°C;

[0013] After the adhesive is applied to the surface, the positive electrode sheet is placed and the secondary pressing is performed for 35-42 minutes.

[0014] Preferably, in the method for preparing the low-temperature resistant lithium-ion battery, the secondary tableting process comprises:

[0015] In the first stage, the pressing temperature is 68-80°C and the pressing time is 3-5 minutes;

[0016] In the second stage, the pressing temperature is 100-110°C and the pressing time is 8-11 minutes;

[0017] The third stage, the pressing temperature is 94-102℃, and the pressing time is 2-4min;

[0018] The fourth stage is to keep warm until the rolling is completed, the temperature is 55-59℃.

[0019] Preferably, in the method for preparing the low-temperature resistant lithium-ion battery,

[0020] The battery inner shell includes an insulating layer, a temperature regulating layer and an outer protective layer from the inside to the outside;

[0021] A second temperature sensor is arranged on the inner side of the insulating layer;

[0022] The temperature regulating layer is provided with a temperature regulating water pipe, and the temperature regulating water pipe is connected to a water tank through a circulation pipeline;

[0023] The circulation pipeline includes a refrigeration pipeline and a heating pipeline connected in parallel, on which a refrigerator and a heater electrically connected to the second temperature sensor are respectively arranged, and the refrigerator and the heater are not turned on at the same time;

[0024] The circulation pipeline is also provided with a circulation pump.

[0025] Preferably, in the method for preparing the low-temperature resistant lithium-ion battery, a plurality of battery inner shell accommodating grooves are provided in the battery outer shell, and a buffer shock absorbing device is provided in the battery inner shell accommodating groove.

[0026] The beneficial effects of the present invention are:

[0027] (1) A nanocarbon heating film is provided on the battery cell, which can preheat the battery under low temperature conditions, so that the battery can be charged and discharged after the temperature rises, thereby increasing its service life;

[0028] (2) During the primary pressing process, the adhesive is preheated, and then primary pressing and secondary pressing are performed respectively, so that the positive electrode sheet, the negative electrode sheet and the electrolyte membrane are pressed tightly without bubbles, and the battery performance is good;

[0029] (3) The secondary pressing process includes four stages, which ensures a good bonding effect between the nanocarbon heating film and the battery cell, thereby ensuring its heating effect;

[0030] (4) The battery inner shell is provided with a temperature regulating layer, and the refrigerator or heater is selected to be turned on according to the temperature detected by the second temperature sensor to keep the battery warm and prevent the battery from overheating or overcooling.

[0031] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION

[0032] The present invention is described in further detail below so that those skilled in the art can implement it according to the description.

[0033] It should be understood that terms such as “having”, “including” and “comprising” used herein do not specify the existence or addition of one or more other elements or combinations thereof.

[0034] The present invention provides a method for preparing a low-temperature resistant lithium-ion battery, which comprises the following steps:

[0035] Taking the pre-prepared electrolyte membrane, positive electrode sheet and negative electrode sheet, cutting them into strips of the same size, placing the electrolyte membrane between the positive electrode sheet and the negative electrode sheet, and performing a sheet pressing process to obtain a combined battery sheet;

[0036] An insulating protective layer is coated on the upper and lower surfaces of the combined battery cell, at least three first temperature sensors are evenly placed on the upper surface, and then a nano-carbon heating film is bonded thereto, and after a secondary sheeting process, the battery cell is rolled up from one end to obtain a battery core;

[0037] The battery core is placed in a prefabricated battery inner shell, a heating switch is connected from both ends of the nano-carbon heating film, and the heating switch is electrically connected to the first temperature sensor;

[0038] At least two battery inner shells containing battery cells are placed side by side in a battery outer shell, and the battery cells in two adjacent battery inner shells are connected in series through a wire to obtain a low-temperature resistant lithium-ion battery product.

[0039] There is no need to explain the production of the electrolyte membrane, the positive electrode sheet, and the negative electrode sheet here. Those skilled in the art can select finished products or produce them by themselves according to their needs.

[0040] In one embodiment of the method for preparing the low-temperature resistant lithium-ion battery provided by the present invention, the one-time tableting process comprises:

[0041] Preheat the adhesive, keep the temperature at 53-61°C, place the negative electrode sheet and apply the adhesive on its upper surface, place the electrolyte membrane, perform primary pressing for 14-17 minutes, and then let it stand until the temperature drops to 42°C;

[0042] After the adhesive is applied to the surface, the positive electrode sheet is placed and the secondary pressing is performed for 35-42 minutes.

[0043] In one embodiment of the method for preparing the low-temperature resistant lithium-ion battery provided by the present invention, the secondary tableting process comprises:

[0044] In the first stage, the pressing temperature is 68-80°C and the pressing time is 3-5 minutes;

[0045] In the second stage, the pressing temperature is 100-110°C and the pressing time is 8-11 minutes;

[0046] The third stage, the pressing temperature is 94-102℃, and the pressing time is 2-4min;

[0047] The fourth stage is to keep warm until the rolling is completed, the temperature is 55-59℃.

[0048] In one embodiment of the method for preparing the low-temperature resistant lithium-ion battery provided by the present invention,

[0049] The battery inner shell includes an insulating layer, a temperature regulating layer and an outer protective layer from the inside to the outside;

[0050] A second temperature sensor is arranged on the inner side of the insulating layer;

[0051] The temperature regulating layer is provided with a temperature regulating water pipe, and the temperature regulating water pipe is connected to a water tank through a circulation pipeline;

[0052] The circulation pipeline includes a refrigeration pipeline and a heating pipeline connected in parallel, on which a refrigerator and a heater electrically connected to the second temperature sensor are respectively arranged, and the refrigerator and the heater are not turned on at the same time;

[0053] The circulation pipeline is also provided with a circulation pump.

[0054] In one embodiment of the method for preparing the low-temperature resistant lithium-ion battery provided by the present invention, a plurality of battery inner shell accommodating grooves are arranged in the battery outer shell, and a buffer shock absorbing device is arranged in the battery inner shell accommodating groove.

[0055] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. Preparation method of low temperature resistant lithium ion battery, It is characterized in that The following steps are involved: Taking the pre-prepared electrolyte membrane, positive electrode sheet and negative electrode sheet, cutting them into strips of the same size, placing the electrolyte membrane between the positive electrode sheet and the negative electrode sheet, and performing a sheet pressing process to obtain a combined battery sheet; An insulating protective layer is coated on the upper and lower surfaces of the combined battery cell, at least three first temperature sensors are evenly placed on the upper surface, and then a nano-carbon heating film is bonded thereto, and after a secondary sheeting process, the battery cell is rolled up from one end to obtain a battery core; The battery core is placed in a prefabricated battery inner shell, a heating switch is connected from both ends of the nano-carbon heating film, and the heating switch is electrically connected to the first temperature sensor; Placing at least two battery inner shells containing battery cells side by side in a battery outer shell, and connecting the battery cells in two adjacent battery inner shells in series through a wire to obtain a low-temperature resistant lithium-ion battery product; in ; The one-time tableting process comprises: Preheat the adhesive, keep the temperature at 53-61°C, place the negative electrode sheet and apply the adhesive on its upper surface, place the electrolyte membrane, perform primary pressing for 14-17 minutes, and then let it stand until the temperature drops to 42°C; After the adhesive is applied to the surface, the positive electrode sheet is placed and the secondary pressing is performed for 35-42 minutes; The secondary tableting process comprises: In the first stage, the pressing temperature is 68-80°C and the pressing time is 3-5 minutes; In the second stage, the pressing temperature is 100-110°C and the pressing time is 8-11 minutes; The third stage, the pressing temperature is 94-102℃, and the pressing time is 2-4min; The fourth stage is to keep warm until the rolling is completed, the temperature is 55-59℃.

2. The method for preparing a low-temperature resistant lithium-ion battery according to claim 1, It is characterized in that The battery inner shell includes an insulating layer, a temperature regulating layer and an outer protective layer from the inside to the outside; A second temperature sensor is arranged on the inner side of the insulating layer; The temperature regulating layer is provided with a temperature regulating water pipe, and the temperature regulating water pipe is connected to a water tank through a circulation pipeline; The circulation pipeline includes a refrigeration pipeline and a heating pipeline connected in parallel, on which a refrigerator and a heater electrically connected to the second temperature sensor are respectively arranged, and the refrigerator and the heater are not turned on at the same time; The circulation pipeline is also provided with a circulation pump.

3. The method for preparing a low-temperature resistant lithium-ion battery according to claim 1, It is characterized in that A plurality of battery inner shell accommodating grooves are arranged in the battery outer shell, and a buffer shock absorbing device is arranged in the battery inner shell accommodating groove.

Citation Information

Patent Citations

  • Pure electric vehicle power battery cooling and heating device with liquid cooling plate

    CN103943913A

  • Binder for lithium ion battery compound pole piece, preparation method for binder, compound pole piece, battery core, and lithium ion battery

    CN105304907A

  • Nano carbon crystal heating battery

    CN106532189A

  • Low-temperature battery with active and passive dual protection

    CN111725588A