Method for preparing various calcium sulfate powders from industrial by-product gypsum and calcium sulfate powder

By dissolving industrial by-product gypsum in an acid solution and mixing it with concentrated sulfuric acid, combining pH adjustment and additive treatment, high-whiteness and low-impact calcium sulfate powder is prepared, which solves the problem of resource utilization of industrial by-product gypsum. The protection of the environment and efficient utilization of resources have been achieved.

CN113603128BActive Publication Date: 2024-11-22NEI MENG GU JIN HUI XI KUANG YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111048817.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-08
Publication Date
2024-11-22
Estimated Expiration
2041-09-08

AI Technical Summary

Technical Problem

Due to the high impurity content of industrial by-product gypsum, it cannot be directly used, resulting in environmental pollution and waste of resources. How to effectively deal with and resource utilization has become an urgent problem.

Method used

By dissolving industrial by-product gypsum in an acid solution, filtration and mixing it with concentrated sulfuric acid, adjusting the pH value, and using alkaline additives and calcium alkaline substances to adjust the solution, calcium sulfate powder with different micromorphic and phases was prepared. , and the acidic filtrate produced is processed to extract chlorophyllium minerals to achieve efficient utilization of resources.

Benefits of technology

It realizes low-cost and efficient utilization of industrial by-product gypsum, reduces the harm to the environment, and the prepared calcium sulfate powder has high whiteness and few impurities, and does not require a high-pressure hydrothermal kettle. It has a simple process and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113603128B_ABST
    Figure CN113603128B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing various calcium sulfate powders from industrial by-product gypsum and calcium sulfate powders, the method comprising: dissolving industrial by-product gypsum in an acid solution to obtain a crude calcium sulfate acid solution, filtering to obtain a refined calcium sulfate acid solution; adding concentrated sulfuric acid or concentrated sulfuric acid and ethanol solution to obtain a first calcium sulfate dihydrate suspension or a calcium sulfate hemihydrate suspension; filtering the first calcium sulfate dihydrate suspension to obtain a first filter cake and a first filtrate, filtering the calcium sulfate hemihydrate suspension to obtain a second filter cake and a second filtrate; adjusting the pH of the first filtrate and the second filtrate to obtain a jarosite mineral suspension; filtering to obtain a third filter cake and a third filtrate; adjusting the pH of the third filtrate to obtain a second calcium sulfate dihydrate suspension; filtering the second calcium sulfate dihydrate suspension to obtain a fourth filter cake and a fourth filtrate. The preparation method of the present invention has a wide range of raw material sources, a simple process and mild conditions, and the obtained calcium sulfate powder has high whiteness and purity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste treatment and resource utilization, and in particular to a method for preparing various calcium sulfate powders from industrial by-product gypsum and the calcium sulfate powder. Background Art

[0002] As industrial waste discharged from industrial production, my country produces a huge amount of industrial by-product gypsum. The storage of industrial by-product gypsum not only occupies a large amount of land and increases the production costs of enterprises, but also causes environmental pollution. During the stacking process, the evaporation of water in the industrial by-product gypsum makes the surrounding air acidic, and the soluble impurities such as phosphorus, fluorine, and sulfur in the industrial by-product gypsum seep into the ground with surface water, causing the phosphorus, fluorine, and sulfur content of groundwater to exceed the standard. The pollution of soil, atmosphere, and water systems by industrial by-product gypsum not only reduces the yield and quality of crops, but also affects the health of local residents. It has caused many local cases of fluorosis, dental fluorosis, etc., and the losses caused are immeasurable. Under the requirements of environmental protection, how to effectively deal with the large amount of accumulated industrial by-product gypsum has become an imminent issue in my country and even in the world.

[0003] The main component of industrial by-product gypsum is CaSO4·2H2O (i.e. calcium sulfate dihydrate). By using industrial by-product gypsum as raw material or admixture and modifying it to eliminate the influence of impurities on its performance, it can replace natural gypsum to produce gypsum building materials.

[0004] In summary, industrial by-product gypsum contains a lot of impurities and cannot be used directly. It is very meaningful to use simple and effective process conditions to treat the by-product gypsum and turn it into a useful and high-value material. Summary of the invention

[0005] The object of the present invention is to solve at least one of the above-mentioned deficiencies in the prior art. For example, one of the objects of the present invention is to provide a method for preparing a variety of calcium sulfate powders, which has a wide source of raw material industrial by-product gypsum, low cost, can reduce the harm of industrial by-product gypsum to the environment, and realize high value-added utilization of low value-added resources. For another example, one of the other objects of the present invention is to provide a calcium sulfate powder with high whiteness, high purity, small product size, and can be used directly without grinding.

[0006] In order to achieve the above object, one aspect of the present invention provides a method for preparing a variety of calcium sulfate powders from industrial by-product gypsum, the method comprising the following steps:

[0007] Dissolving industrial by-product gypsum in an acid solution to obtain a crude calcium sulfate acid solution;

[0008] filtering the crude calcium sulfate acidic solution to obtain a refined calcium sulfate acidic solution;

[0009] The purified calcium sulfate acid solution is mixed with concentrated sulfuric acid to obtain a first calcium sulfate dihydrate suspension; the first calcium sulfate dihydrate suspension is filtered to obtain a first filter cake and a first filtrate, and the first filter cake is washed and dried to obtain a first calcium sulfate dihydrate powder;

[0010] or after mixing the refined calcium sulfate acid solution with concentrated sulfuric acid, adding anhydrous ethanol to obtain a hemihydrate calcium sulfate suspension; filtering the hemihydrate calcium sulfate suspension to obtain a second filter cake and a second filtrate, washing the second filter cake and drying to obtain hemihydrate calcium sulfate powder;

[0011] Using an alkaline auxiliary agent to adjust the pH of the first filtrate and the second filtrate to obtain a yellow jarosite mineral suspension;

[0012] The jarosite mineral suspension is filtered to obtain a third filter cake and a third filtrate, and the third filter cake is washed and dried to obtain a crude jarosite mineral powder;

[0013] Using a calcic alkaline substance to adjust the pH of the third filtrate to obtain a grayish white second calcium sulfate dihydrate suspension;

[0014] The second calcium sulfate dihydrate suspension is filtered to obtain a fourth filter cake and a fourth filtrate, and the third filter cake is dried to obtain a second calcium sulfate dihydrate powder.

[0015] In an exemplary embodiment of an aspect of the present invention, the alkaline auxiliary agent adjusts the pH of the first filtrate and the second filtrate to 1.5-3, and the calcic alkaline substance adjusts the pH of the third filtrate to 6.5-7.5.

[0016] In an exemplary embodiment of an aspect of the present invention, the jarosite mineral suspension may be yellow, and the second calcium sulfate dihydrate suspension may be off-white.

[0017] In an exemplary embodiment of an aspect of the present invention, the jarosite-based mineral may include at least one of sodium jarosite, yellow potassium jarosite or yellow ammonium jarosite.

[0018] In an exemplary embodiment of one aspect of the present invention, the concentration of the acid solution may be 1 to 3 mol / L, the temperature of dissolving the industrial by-product gypsum in the acid solution may be 70 to 100° C., and the dissolution time may be 1 to 4 hours;

[0019] The refined calcium sulfate acid solution can be mixed with concentrated sulfuric acid and reacted at 80-100° C. for 1-6 hours;

[0020] The refined calcium sulfate acid solution can be mixed with concentrated sulfuric acid and reacted at 80-100° C. for 1-6 hours, and then anhydrous ethanol is added and reacted at 80-100° C. for 1-6 hours.

[0021] In an exemplary embodiment of one aspect of the present invention, the industrial by-product gypsum and the acid solution can be dissolved in a mass volume ratio of 1:4 to 1:12 kg / L, and the acid solution can include one or more of hydrochloric acid, nitric acid, citric acid, acetic acid, and phosphoric acid solution.

[0022] In an exemplary embodiment of an aspect of the present invention, the alkaline auxiliary agent may include one or more of sodium hydroxide, potassium hydroxide and ammonium hydroxide, and the alkaline calcium material may include one or more of limestone, quicklime, slaked lime and carbide slag.

[0023] In an exemplary embodiment of one aspect of the present invention, the volume ratio of the refined calcium sulfate acidic solution to concentrated sulfuric acid may be 1:1 to 100:1 L / L, and the volume ratio of the refined calcium sulfate acidic solution to anhydrous ethanol may be 1:1 to 20:1 L / L.

[0024] Another aspect of the present invention provides a calcium sulfate powder, which can be prepared by any of the methods described above, and the calcium sulfate powder may include one or more of a first calcium sulfate dihydrate powder, a second calcium sulfate dihydrate powder, and a calcium sulfate hemihydrate powder.

[0025] In an exemplary embodiment of another aspect of the present invention, the microscopic morphology of the first calcium sulfate dihydrate powder may be flaky, and the flake diameter may be 5 to 60 μm; the microscopic morphology of the calcium sulfate hemihydrate powder may include flakes and plates, the flake diameter of the flake micromorphology may be 5 to 40 μm, the crystal length of the plate-like micromorphology may be 5 to 40 μm, and the thickness may be 0.5 to 2 μm; the microscopic morphology of the second calcium sulfate dihydrate powder may be fibrous, the length may be 50 to 600 μm, and the diameter may be 5 to 15 μm.

[0026] Compared with the prior art, the beneficial effects of the present invention may include at least one of the following:

[0027] (1) The preparation method of the present invention uses industrial by-product gypsum as raw material, which has a wide source of raw materials and low cost, belongs to the category of solid waste utilization and resource utilization, realizes high value-added utilization of low value-added resources, can reduce the harm of industrial by-product gypsum to the environment, and has important ecological protection and sustainable development significance for resource protection and conservation;

[0028] (2) Compared with other calcium sulfate preparation methods, the preparation method of the present invention does not add a crystal form control agent, and uses less auxiliary agents;

[0029] (3) The preparation method of the present invention does not require a high-pressure hydrothermal autoclave, has a simple process, mild conditions, low cost, short production cycle, easy process control, and easy to scale up, thus facilitating industrial production;

[0030] (4) The preparation method of the present invention can prepare calcium sulfate with two physical phases and different microscopic morphologies at different stages;

[0031] (5) The preparation method of the present invention dissolves calcium sulfate in industrial by-product gypsum into a solution through the action of an acid, and then adjusts the temperature and water activity to crystallize calcium sulfate using the common ion effect of sulfate (a two-step dissolution-crystallization method). The various calcium sulfate powders prepared by the method of the present invention have a whiteness of up to 99%, a low impurity content, and a small product size. The product is a powder and can be used directly without grinding.

[0032] (6) The preparation method of the present invention not only obtains calcium sulfate powders of different appearances and different phases, but also treats the acidic filtrate generated in the preparation process, and extracts the valuable components therein by adjusting the pH value, thereby synthesizing crude jarosite minerals (mainly sodium jarosite, yellow potassium jarosite or yellow ammonium jarosite). BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A process flow diagram showing an exemplary embodiment of the method of the present invention;

[0034] Figure 2 An optical microscope image at 100 times magnification of the original sample of titanium gypsum used in the examples of the present invention is shown;

[0035] Figure 3 The XRD pattern of the original sample of titanium gypsum used in the examples of the present invention is shown;

[0036] Figure 4 A 400-fold optical microscope image of the product A1 obtained in Example 1 of the present invention is shown;

[0037] Figure 5 The XRD pattern of the product A1 obtained in Example 1 of the present invention is shown;

[0038] Figure 6 A 40x optical microscope image of the product A2 obtained in Example 1 of the present invention is shown;

[0039] Figure 7 The 100-fold optical microscope image of the product B1 obtained in Example 2 of the present invention is shown;

[0040] Figure 8 The XRD pattern of the product B1 obtained in Example 2 of the present invention is shown;

[0041] Fig. 9 A 1000 optical microscope image of the product B2 obtained in Example 2 of the present invention is shown;

[0042] Fig.10An optical microscope image at 200 times magnification of the product C1 obtained in Example 3 of the present invention is shown;

[0043] Fig.11 The XRD pattern of the product C1 obtained in Example 3 of the present invention is shown;

[0044] Fig.12 An optical microscope image at 100 times magnification of the product C2 obtained in Example 3 of the present invention is shown. Description of the drawings:

[0046] The ordinate of the XRD spectrum in the accompanying drawings represents intensity (Intensity), and the unit is au (arbitrary unit). DETAILED DESCRIPTION

[0047] Hereinafter, the method for preparing various calcium sulfate powders from industrial by-product gypsum of the present invention and the calcium sulfate powder will be described in detail in conjunction with exemplary embodiments. Herein, "first", "second", "third", "fourth", etc. are only for the convenience of description and distinction, and cannot be understood as indicating or implying relative importance or having a strict order.

[0048] Exemplary Embodiment 1

[0049] like Figure 1 As shown, a method for preparing various calcium sulfate powders from industrial by-product gypsum provided in this exemplary embodiment can be achieved by the following steps:

[0050] S1, obtain crude calcium sulfate acidic solution

[0051] Specifically, industrial by-product gypsum is dissolved in an acid solution to obtain a crude calcium sulfate acid solution. Here, the industrial by-product gypsum and the acid solution are dissolved in a mass volume ratio of 1:4 to 1:12 kg / L, that is, 1 kg of industrial by-product gypsum is dissolved in 4 to 12 L of acid solution. The concentration of the acid solution is 1 to 3 mol / L, where the concentration of the acid solution refers to the hydrogen ions [H + ] The acid solution includes one or more of hydrochloric acid, nitric acid, citric acid, acetic acid, and phosphoric acid solution.

[0052] The industrial by-product gypsum is dissolved in the acid solution at a temperature of 70 to 100°C (with additional stirring) for 1 to 4 hours, so that the industrial by-product gypsum can be dissolved in the acid solution to the greatest extent. Preferably, the industrial by-product gypsum is dissolved in the acid solution at a temperature of 75 to 85°C for 1.5 to 2.5 hours.

[0053] In addition, the industrial by-product gypsum raw material can be dried and ground at 35°C to 55°C, and passed through a 100-200 mesh sieve to obtain the industrial by-product gypsum powder, and then the industrial by-product gypsum powder can be dissolved in an acid solution. Drying, grinding, sieving, and then dissolving the industrial by-product gypsum raw material in an acid solution can, on the one hand, play a role in homogenization and reduce the error caused by the unevenness of the raw material; on the other hand, the raw material is fully in contact with the acid solution, and the reaction is more complete.

[0054] The industrial by-product gypsum raw material in the present invention may include one or more of desulfurized gypsum, titanium gypsum, phosphogypsum, fluorinated gypsum, boric gypsum, citric acid gypsum, ceramic waste mold gypsum, waste gypsum board, tartaric acid gypsum, lactic acid gypsum, and mirabilite gypsum.

[0055] S2, filter to obtain refined calcium sulfate acid solution

[0056] Specifically, the crude calcium sulfate acidic solution obtained in step S1 is filtered to obtain a refined calcium sulfate acidic solution and a filter residue. The filter residue is mainly composed of calcium sulfate dihydrate, which contains other impurities of different types. Alkaline calcium substances (such as limestone powder, which will be described in detail below) are added to neutralize the filter residue, which can be used as a building material.

[0057] S31, mixed with concentrated sulfuric acid to obtain calcium sulfate dihydrate suspension

[0058] Specifically, the refined calcium sulfate acid solution obtained in step S2 is mixed with concentrated sulfuric acid to obtain a calcium sulfate dihydrate suspension. Here, the volume ratio of the refined calcium sulfate acid solution and the concentrated sulfuric acid is 1:1 to 100:1 L / L, that is, 1 L of concentrated sulfuric acid needs to be added to every 1 to 100 L of the refined calcium sulfate acid solution. The concentration of the concentrated sulfuric acid can be 18.4 mol / L.

[0059] The reaction temperature after mixing the refined calcium sulfate acidic solution with concentrated sulfuric acid is 80-100° C. (additional stirring may be performed) and the reaction time is 1-6 hours, which can accelerate the chemical reaction between the mutually soluble components (specifically the precipitation of calcium sulfate dihydrate) to obtain the first calcium sulfate dihydrate suspension. Preferably, the temperature for mixing the refined calcium sulfate acidic solution with concentrated sulfuric acid can be 75-85° C., and the mixing time can be 1-2.5 hours.

[0060] S41, obtaining the first calcium sulfate dihydrate powder

[0061] Specifically, the calcium sulfate dihydrate suspension obtained in step S31 is filtered to obtain a first filter cake and a first filtrate. The first filter cake is washed and dried to obtain a first calcium sulfate dihydrate powder. Here, the first filter cake can be washed with water above 95°C, and then washed once with ethanol to terminate the reaction and prevent hydration. After the first filter cake is washed, it can be dried naturally or at 35°C to 55°C to obtain a first calcium sulfate dihydrate powder. It should be noted that the microscopic morphology of the first calcium sulfate dihydrate powder obtained can be flaky, and the flake diameter can be 5 to 60 μm.

[0062] S5. Obtain the second calcium sulfate dihydrate powder

[0063] Specifically, the pH of the first filtrate obtained in step S41 is adjusted by an alkaline auxiliary agent to obtain a yellow suspension; the yellow suspension is filtered to obtain a third filter cake and a third filtrate, and the third filter cake is washed, dried, and ground to obtain a crude yellow jarosite mineral (mainly yellow sodium jarosite, yellow jarosite or yellow ammonium jarosite) powder; here, the pH of the first filtrate is adjusted to 1.5-3.0 by an alkaline auxiliary agent, so that the iron ions in the first filtrate are precipitated into a crude yellow jarosite mineral (mainly yellow sodium jarosite, yellow jarosite or yellow ammonium jarosite) (the synthesis process of yellow sodium jarosite, yellow jarosite and yellow ammonium jarosite is shown in formula (1)-(3)), and filtered to remove. The pH can be adjusted by one or more of sodium hydroxide, potassium hydroxide and ammonium hydroxide. Preferably, the pH value of the first filtrate can be adjusted to 1.5-3.0 by an alkaline auxiliary agent.

[0064] Yellow sodium ferroaluminate:

[0065] 3Fe 3+ +Na + +2SO4 2- +6H2O→Na[Fe3(SO4)2(OH)6]+6H + (1)

[0066] Potassium ferroalum:

[0067] 3Fe 3+ +K + +2SO4 2- +6H2O→K[Fe3(SO4)2(OH)6]+6H + (2)

[0068] Yellow ammonium iron alum:

[0069] 3Fe 3+ +NH4 + +2SO4 2- +6H2O→NH4[Fe3(SO4)2(OH)6]+6H + (3)

[0070] In addition, in this embodiment, a calcareous alkaline substance can be added to the third filtrate obtained in step S51 to adjust the pH value to 6.5-7.5, and obtain an off-white suspension containing calcium sulfate dihydrate; the obtained off-white suspension containing calcium sulfate dihydrate filtrate is filtered to obtain a fourth filter cake and a fourth filtrate; the fourth filter cake is dried to obtain a second calcium sulfate dihydrate powder, and the pH value of the third filtrate is about 6.5-7.5, which can be used as an acid solution for dissolving industrial by-product gypsum in the dilution step S1, so that acid solutions of different concentrations can be obtained according to process requirements for production. In the present invention, the calcareous alkaline substance may include one or more of limestone, quicklime, slaked lime, and carbide slag. It should be noted that the microscopic morphology of the second calcium sulfate dihydrate powder can be fibrous, with a length of 50-600 μm and a diameter of 5-15 μm.

[0071] Exemplary Embodiment 2

[0072] like Figure 1 As shown, a method for preparing various calcium sulfate powders from industrial by-product gypsum provided in this exemplary embodiment can be achieved by the following steps:

[0073] Step S1 and step S2 may be the same as step S1 and step S2 in the above exemplary embodiment 1, and will not be described in detail here.

[0074] S32, add concentrated sulfuric acid and anhydrous ethanol to obtain a hemihydrate calcium sulfate suspension

[0075] Specifically, the refined calcium sulfate acidic solution obtained in step S2 is mixed with concentrated sulfuric acid, and then anhydrous ethanol is added to obtain a hemihydrate calcium sulfate suspension. Here, the volume ratio of the refined calcium sulfate acidic solution mixed with concentrated sulfuric acid is 1:1-100:1L / L, and the volume ratio of the refined calcium sulfate acidic solution mixed with anhydrous ethanol is 1:1-20:1L / L. In other words, 1L of concentrated sulfuric acid needs to be added to every 1-100L of refined calcium sulfate acidic solution, and 1L of anhydrous ethanol needs to be added to every 1-20L of refined calcium sulfate acidic solution. The concentration of concentrated sulfuric acid can be 18.4mol / L.

[0076] After the concentrated sulfuric acid and the refined calcium sulfate acid solution are mixed, the mixture is reacted at 80-100° C. for 1-6 hours (stirring may be added), and then anhydrous ethanol is added to react at 80-100° C. for 1-6 hours (stirring may be added) to accelerate the chemical reaction between the mutually soluble components (specifically the precipitation of calcium sulfate hemihydrate) to obtain a calcium sulfate hemihydrate suspension.

[0077] S42, obtain calcium sulfate hemihydrate powder

[0078] Specifically, the hemihydrate calcium sulfate suspension obtained in step S32 is filtered to obtain a second filter cake and a second filtrate. The second filter cake is washed and dried to obtain hemihydrate calcium sulfate powder. Here, the second filter cake can be washed with water above 95°C, and then washed once with ethanol to terminate the reaction and prevent hydration. After the second filter cake is washed, it can be dried naturally or at 35°C to 55°C to obtain hemihydrate calcium sulfate powder. It should be noted that the microscopic morphology of the obtained hemihydrate calcium sulfate powder may include flakes and plates, the diameter of the flake microscopic morphology may be 5 to 40 μm, the crystal length of the plate-like microscopic morphology may be 5 to 40 μm, and the thickness may be 0.5 to 2 μm.

[0079] The treatment of the second filtrate is as described in step S5 in exemplary embodiment 1, and will not be described in detail here.

[0080] The technical solution of the present invention is further illustrated below through detailed examples. The original titanium gypsum used in the following Examples 1 and 3 is khaki in color, blocky, and has a whiteness of 9.8%. The chemical composition of the original titanium gypsum is shown in Table 1. The results show that the main chemical components of the titanium gypsum include 33.58% SO3, 31.70% CaO, 10.63% TFe2O3, and also contain a small amount of Al2O3, MgO, TiO2, SiO2, etc. The loss on ignition is 18.38%, and the loss on ignition is mainly caused by the loss of water of gypsum and hydrated oxides of iron during the roasting process of the titanium gypsum. From the chemical composition analysis of the original titanium gypsum, it can be seen that the original titanium gypsum has a relatively complex composition and a high impurity content, especially the Fe2O3 content is as high as 10.63%, and the trivalent iron compound is red, which limits the resource utilization of titanium gypsum. Figure 2 As shown in the figure, the main phase in titanium gypsum is calcium sulfate dihydrate. The microscopic morphology of titanium gypsum is as follows: Figure 3 as shown in .

[0081] Table 1 Chemical composition analysis of titanium gypsum original sample (wB / %)

[0082]

[0083] The original sample of phosphogypsum used in the following Example 2 is gray, powdery, and has a whiteness of 30%. The chemical composition of the original sample of phosphogypsum is shown in Table 2. The results show that the main chemical components of phosphogypsum include 39.36% SO3, 29.60% CaO, 5.03% SiO2, 1.85% Al2O3, 1.60% P2O5, and a small amount of TFe2O3, F, etc. The ignition loss is 20.74%, which is mainly caused by the loss of water of gypsum and iron hydrate oxides during the roasting process of titanium gypsum. There are many types of impurities in phosphogypsum, and the iron content is less than that of titanium gypsum.

[0084] Table 2 Chemical composition analysis of phosphogypsum original sample (wB / %)

[0085]

[0086] Example 1

[0087] The specific preparation method of this example is as follows:

[0088] 100 mL of 3 mol / L hydrochloric acid aqueous solution was measured and placed in a 250 mL conical flask, 10 g of titanium gypsum was weighed and mixed with the hydrochloric acid solution, and placed in a water bath at 80°C for reaction for 120 min. After the reaction was completed, the mixture was filtered to obtain about 100 mL of filtrate 1 and filter residue 1. The filter residue 1 was washed with water until neutral, and then added with limestone powder for neutralization and used as a building material.

[0089] Add 5 mL of concentrated sulfuric acid to the filtrate 1, react at 80°C for 120 min, and filter while hot to obtain filter cake 2 and filtrate 2. Wash the filter cake 2 with water above 95°C until it is neutral, and then wash it once with ethanol to terminate the reaction and prevent hydration. Dry it at 45±10°C to obtain product A1.

[0090] Sodium hydroxide was added to the filtrate 2 to adjust the pH value of the filtrate to 1.8, so that the components in the filtrate 2 reacted to form yellow sodium ferroalcohol precipitate. Filtrate 3 and filter cake 3 (i.e., crude yellow sodium ferroalcohol 1) were obtained by filtration.

[0091] CaO was continuously added to the filtrate 3 to make the pH value of the filtrate 3 reach about 6.5 to 7.5, and the product A2 was obtained after filtering and drying.

[0092] Microscope image of product A1 Figure 4 As shown in the figure, the XRD pattern of product A1 is as follows Figure 5 As shown in Figure 4 and Figure 5 It can be seen that the main phase is CaSO4·2H2O, the crystal morphology of product A1 is flaky, the maximum diameter of the flake can reach 60μm, the crystal surface is smooth, the edge is clear, the crystallinity of calcium sulfate dihydrate powder is high, 94.83%, and the whiteness measured by whiteness analyzer is 99.2%. The chemical composition analysis of product A1 is shown in Table 3. The main chemical components include 44.1% SO3 and 37.9% CaO, and other small amounts of impurities. The ignition loss is 17.8%, which is mainly caused by the loss of water of gypsum and iron hydrate oxides during the roasting process of titanium gypsum. Compared with the original chemical composition of titanium gypsum, the impurity content in product A1 obtained by treatment is significantly reduced.

[0093] Table 3 Chemical composition analysis of product A1 (wB / %)

[0094]

[0095] The crude yellow sodium ferroaluminate 1 obtained has a light yellow powder appearance. The microscopic image of product A2 is as follows Figure 6As shown in the figure, it can be seen that the crystal morphology of product A2 is fibrous, the maximum aspect ratio is 40, and the whiteness is 86.5% as measured by a whiteness analyzer.

[0096] Example 2

[0097] The specific preparation method of this example is as follows:

[0098] 100 mL of 1 mol / L nitric acid aqueous solution was measured and placed in a 250 mL conical flask. 10 g of phosphogypsum was weighed and mixed with the hydrochloric acid solution, and placed in a water bath at 80°C for reaction for 120 min. After the reaction was completed, the mixture was filtered to obtain about 100 ml of filtrate 4 and filter residue 4. The filter residue 4 was washed with water until neutralized, and then added with limestone powder for neutralization and used as a building material.

[0099] Add 5 mL of concentrated sulfuric acid to the filtrate 4, react at 80°C for 120 min, and filter while hot to obtain filter cake 5 and filtrate 5. Wash the filter cake 5 with water above 95°C until it is neutral, and then wash it once with ethanol to terminate the reaction and prevent hydration. Dry it at 45±10°C to obtain product B1.

[0100] Sodium hydroxide is added to the filtrate 5 to adjust the pH value of the filtrate to 1.8, so that the components in the filtrate 5 react to form yellow sodium ferroalloy precipitate. Filtrate 6 and filter cake 6 (i.e., crude yellow sodium ferroalloy 2) are obtained by filtration. CaO is further added to the filtrate 6 to adjust the pH value of the filtrate 6 to about 6.5 to 7.5, and the product B2 is obtained after filtration and drying.

[0101] Microscope image of product B1 Figure 7 As shown in the table, the crystal morphology of product B1 is flaky and the size is about 10-20 μm. The chemical composition analysis of product B1 is shown in Table 4. The chemical composition analysis of product B1 is shown in Table 3. The main chemical components include 43.58% SO3 and 36.34% CaO, and also contain a small amount of SrO, SiO2, Al2O3. The loss on ignition is 20%, which is mainly caused by the loss of water in the gypsum during the roasting process of product B1. Compared with the original chemical composition of titanium gypsum, the impurity content in the product B1 obtained by treatment is significantly reduced. Figure 8 is the XRD diffraction pattern of product B1, Figure 8 It can be seen that the main phase of product B1 is CaSO4·2H2O, and the crystallinity is relatively high, which is 83%. The whiteness of product B1 is 98.6% as measured by a whiteness analyzer.

[0102] Table 4 Chemical composition analysis of product B1 (wB / %)

[0103]

[0104] The crude yellow sodium ferroalite 2 obtained has a light yellow powder appearance. Due to the low iron content in phosphogypsum, the amount of crude yellow sodium ferroalite 2 obtained is relatively small. The microscope image of product B2 is as follows Fig. 9 As shown, the crystal morphology of product B2 is fibrous, and the maximum aspect ratio is 60. The whiteness of product B2 is 86.6% as measured by a whiteness analyzer.

[0105] Example 3

[0106] The specific preparation method of this example is as follows:

[0107] 100 mL of 1.5 mol / L hydrochloric acid aqueous solution was measured and placed in a 250 mL conical flask. 10 g of titanium gypsum was weighed and mixed with the hydrochloric acid solution, and placed in a water bath at 80°C for reaction for 120 min. After the reaction was completed, the mixture was filtered to obtain about 100 ml of filtrate 7 and filter residue 7. The filter residue 7 was washed with water until neutralized, and then added with limestone powder for neutralization and used as a building material.

[0108] Add 5 mL of concentrated sulfuric acid to the filtrate 7, react at 80°C for 60 min, then add 20 mL of anhydrous ethanol to the reaction system, react for another 60 min, and filter while hot to obtain filter cake 8 and filtrate 8. Wash filter cake 8 with water above 95°C until neutral, then wash once with ethanol to terminate the reaction and prevent hydration. Dry at 45±10°C to obtain product C1.

[0109] Potassium hydroxide is added to the filtrate 8 to adjust the pH value of the filtrate to 2, so that the components in the filtrate 8 react to form jarosite precipitate, and the filtrate 9 and filter cake 9 (i.e. crude jarosite) are obtained by filtration.

[0110] CaO is continuously added to the filtrate 9 to make the pH value of the filtrate 9 reach about 6.5 to 7.5, and the product C2 is obtained after filtering and drying.

[0111] Microscope image of product C1 Fig.10 As shown in Figure 1, the crystal morphology of product C1 is mostly flake-shaped, with a small part being plate-shaped. The maximum diameter of the flake crystal is 40 μm, the length of the plate crystal is 5 to 40 μm, and the thickness is 0.5 to 2 μm. The XRD spectrum of product C1 is shown in Figure 1. Fig.11As shown in , the physical phase of product C1 is mainly CaSO4·0.5H2O. Analysis of the XRD diffraction pattern shows that the crystallinity of product C1 is 98.17%, and no peaks of other substances are found, indicating that the purity of calcium sulfate hemihydrate in the obtained product C1 is relatively high. Table 4 is the chemical composition analysis of product C1. From Table 5, it can be seen that the main chemical components of product C1 include 51.72% SO3 and 40.90% CaO, containing a small amount of SrO, SiO2, Fe2O3, Cl, and MgO. The loss on ignition is 6.43%, which is mainly caused by the loss of water of calcium sulfate hemihydrate and hydrated oxide of iron during the roasting process of product C1. From the chemical composition analysis of product C1, it can be seen that product C1 has less impurities. The whiteness of product C1 is 97.6% as measured by a whiteness analyzer.

[0112] Table 5 Chemical composition analysis of product C1 (wB / %)

[0113]

[0114] The appearance of the crude yellow jarosite obtained is light yellow. The microscopic image of product C2 is as follows Fig.12 As shown in , the crystal morphology of product C2 is fibrous, and the aspect ratio can reach 120. The whiteness is 86.3 as measured by a whiteness analyzer.

[0115] In summary, the present invention can prepare a variety of calcium sulfate powders using industrial by-product gypsum, and its beneficial effects may include at least one of the following:

[0116] (1) Using industrial by-product gypsum as raw material to realize the utilization of low-grade resources and solid waste;

[0117] (2) The preparation method of the present invention does not add a crystal form control agent, and uses less auxiliary agents;

[0118] (3) Calcium sulfate with different phases and microscopic morphologies can be obtained at different stages through the two-step dissolution-crystallization method;

[0119] (4) The solution after filtration in this method can be reused multiple times or recycled, which can reduce process costs;

[0120] (5) This method uses a step-by-step precipitation method to synthesize crude jarosite minerals from the difficult-to-treat iron in titanium gypsum by using the acidic filtrate produced during the preparation of various calcium sulfate powders, thereby achieving the purpose of extracting valuable components therein. The treated filtrate is nearly neutral and can be recycled.

[0121] (6) The various calcium sulfate powders prepared by the method described in the present invention have a whiteness of up to 99% and a low impurity content.

[0122] Although the present invention has been described above in conjunction with the exemplary embodiments and the accompanying drawings, it should be apparent to those skilled in the art that various modifications may be made to the above-described embodiments without departing from the spirit and scope of the claims.

Claims

1. A method for preparing various calcium sulfate powders from industrial by-product gypsum, It is characterized in that The method comprises the following steps: Dissolving industrial by-product gypsum in an acid solution to obtain a crude calcium sulfate acid solution; filtering the crude calcium sulfate acidic solution to obtain a refined calcium sulfate acidic solution; The refined calcium sulfate acid solution is mixed with concentrated sulfuric acid to obtain a first calcium sulfate dihydrate suspension; the first calcium sulfate dihydrate suspension is filtered to obtain a first filter cake and a first filtrate, and the first filter cake is washed and dried to obtain a first calcium sulfate dihydrate powder; the first calcium sulfate dihydrate powder has a flaky morphology with a flake diameter of 5 to 60 μm; or after mixing the refined calcium sulfate acid solution with concentrated sulfuric acid, adding anhydrous ethanol to obtain a hemihydrate calcium sulfate suspension; filtering the hemihydrate calcium sulfate suspension to obtain a second filter cake and a second filtrate, washing the second filter cake and drying to obtain hemihydrate calcium sulfate powder; the microscopic morphology of the hemihydrate calcium sulfate powder includes flake and plate, the flake microscopic morphology has a flake diameter of 5 to 40 μm, and the plate microscopic morphology has a crystal length of 5 to 40 μm and a thickness of 0.5 to 2 μm; Using an alkaline auxiliary agent to adjust the pH of the first filtrate or the second filtrate to obtain a yellow jarosite mineral suspension; The jarosite mineral suspension is filtered to obtain a third filter cake and a third filtrate, and the third filter cake is washed and dried to obtain a crude jarosite mineral powder; the jarosite mineral includes at least one of yellow sodium jarosite, yellow potassium jarosite or yellow ammonium jarosite; Using a calcic alkaline substance to adjust the pH of the third filtrate to obtain a grayish white second calcium sulfate dihydrate suspension; The second calcium sulfate dihydrate suspension is filtered to obtain a fourth filter cake and a fourth filtrate, and the fourth filter cake is dried to obtain a second calcium sulfate dihydrate powder; the second calcium sulfate dihydrate powder has a fibrous morphology, a length of 50 to 600 μm, and a diameter of 5 to 15 μm; The alkaline auxiliary agent adjusts the pH of the first filtrate or the second filtrate to 1.5-3; The concentration of the acid solution is 1-3 mol / L, the temperature for dissolving the industrial by-product gypsum in the acid solution is 70-100°C, and the dissolution time is 1-4 hours; the industrial by-product gypsum and the acid solution are dissolved in a mass volume ratio of 1:4-1:12 kg / L; The refined calcium sulfate acid solution is mixed with concentrated sulfuric acid and reacted at 80-100° C. for 1-6 hours, and then anhydrous ethanol is added and reacted at 80-100° C. for 1-6 hours; The volume ratio of the refined calcium sulfate acidic solution to concentrated sulfuric acid is 1:1 to 100:1 L / L, and the volume ratio of the refined calcium sulfate acidic solution to anhydrous ethanol is 1:1 to 20:1 L / L; The acid solution includes one or more of hydrochloric acid, nitric acid, citric acid, acetic acid, and phosphoric acid solution; The alkaline auxiliary agent includes one or more of sodium hydroxide, potassium hydroxide and ammonium hydroxide.

2. The method for preparing various calcium sulfate powders from industrial by-product gypsum according to claim 1, It is characterized in that The calcic alkaline substance adjusts the pH of the third filtrate to 6.5-7.

5.

3. The method for preparing various calcium sulfate powders from industrial by-product gypsum according to claim 1, It is characterized in that The jarosite mineral suspension is yellow.

4. The method for preparing various calcium sulfate powders from industrial by-product gypsum according to claim 1, It is characterized in that The calcareous alkaline substance includes one or more of limestone, quicklime, slaked lime and carbide slag.