Alkyl chain modified covalent organic framework membrane, preparation method and application thereof

An alkyl chain-modified covalent organic framework membrane is prepared through interfacial polymerization or in-situ polymerization, and combined with polyethylene glycol and lithium bistriflate to form a high-performance solid electrolyte, which solves the problem of uneven composition and thermal problems of traditional materials. It solves the problem of poor stability and achieves high ion conductivity and battery cycle stability, significantly improving the performance of lithium-ion batteries.

CN113621118BActive Publication Date: 2024-10-29NANJING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110775539.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-08
Publication Date
2024-10-29
Estimated Expiration
2041-07-08

AI Technical Summary

Technical Problem

Traditional covalent organic framework powder materials have uneven composition and poor thermal stability when preparing solid electrolytes, resulting in unstable electrochemical performance of lithium-ion batteries, and the ion conductivity of existing alkyl chain modified materials is insufficient.

Method used

An alkyl chain-modified covalent organic framework film is prepared by interfacial polymerization or in-situ polymerization on the copper foil surface, and is mixed with polyethylene glycol and lithium bistriflate to form a high-performance solid electrolyte that enhances Li-ion conductivity and battery cycle stability.

Benefits of technology

Achieving high ion conductivity and good cycle performance, the ion conductivity of lithium-ion battery reaches 2.13×10-3S cm-1 at 120°C, and the battery cycle stability exceeds 20 cycles, significantly improving the safety and energy of the battery density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113621118B_ABST
    Figure CN113621118B_ABST
Patent Text Reader

Abstract

The invention discloses an alkyl chain-modified covalent organic framework membrane, a preparation method and an application thereof. The alkyl chain-modified covalent organic framework membrane is prepared by using an alkyl chain-modified amino compound and 1,3,5-triformylbenzene as raw materials, and can be prepared by interfacial polymerization or in-situ polymerization. The alkyl chain-modified covalent organic framework membrane of the invention has excellent flexibility and ultrathinness, and can be used as a solid electrolyte in a lithium battery to improve the lithium ion conductivity of the battery and the stability of the cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of covalent organic framework compounds and relates to an alkyl chain-modified covalent organic framework film, a preparation method and application of the film in a solid electrolyte. Background Art

[0002] Commercial lithium-ion batteries have a safety hazard of explosion due to the use of large amounts of flammable organic solvents. Solid electrolytes have high ionic conductivity and high safety, and can effectively inhibit the growth of lithium dendrites, thereby increasing the energy density of lithium-ion batteries, which has attracted extensive research. Traditional covalent organic framework powder materials are subsequently used to make solid electrolytes through powder tableting, which will lead to uneven composition and poor high-temperature stability. The effective ingredients are easily lost, causing battery failure and short circuits. How to produce covalent organic framework membrane-based electrolyte materials with stable electrochemical properties remains a challenge.

[0003] Covalent organic framework is a new type of long-range ordered polymer material formed by light elements (C, N, O, S) connected by covalent bonds. It has the characteristics of low weight density, permanent high porosity, large specific surface area, pre-designed structure and high stability. Covalent organic framework membrane material has more superior performance and has potential application prospects in catalysis, batteries, ion conduction, gas storage, compound separation and other aspects.

[0004] Rationally designing COFs membrane materials modified with alkyl chains, using the framework characteristics of COFs and the easy processing of membrane materials to improve the overall structural stability of solid electrolyte materials, and using modified alkyl segments to facilitate the formation of membranes, new solid electrolyte materials with stable structural, thermodynamic and electrochemical properties can be obtained. However, in terms of covalent organic frameworks, there are few reports on the application of solid electrolytes based on covalent organic framework membrane materials, and the conductivity is not particularly ideal. Reference 1 uses a covalent organic framework (Li2O3) modified with polyethylene oxide chains impregnated with ionic liquids. + @TPB-BMTP-COF) polyelectrolyte, but the material is in powder form, and the powder cannot conduct ions well. Its ion conductivity is only 5.49×10 -4 S cm -1 (J.Am.Chem.Soc.2018,140,7429-7432). Document 2 combines polyethylene glycol (PEG) into a covalent organic framework to accelerate Li+ conduction, but the material is a powder rather than a uniform film structure, and has poor cycle stability in solid electrolyte applications (Am.Chem.Soc.2019,141,1923-1927.). Summary of the invention

[0005] The object of the present invention is to provide an alkyl chain-modified covalent organic framework membrane, a preparation method and application thereof in solid electrolytes.

[0006] The alkyl chain-modified covalent organic framework membrane (COF-C-2) of the present invention is a hexagonal topological structure synthesized by connecting three aldehydes in 1,3,5-triformylbenzene and two amine groups of an alkyl chain-modified amino compound ([C-2,2-NHNH2]) to form a -C=N-NH covalent bond, and its structural formula is as follows:

[0007]

[0008] The structural formula of the alkyl chain modified amino compound of the present invention is as follows:

[0009]

[0010] The structural formula of 1,3,5-triformylbenzene of the present invention is as follows:

[0011]

[0012] The present invention also provides a method for preparing the above-mentioned alkyl chain-modified covalent organic framework membrane, which adopts an interfacial polymerization method and comprises the following steps:

[0013] 1,3,5-triformylbenzene is dissolved in dichloromethane to form an organic phase solution, and an alkyl chain-modified amino compound is dissolved in an acetic acid aqueous solution to form an aqueous phase solution. The aqueous phase solution is added dropwise to the organic phase solution at a molar ratio of 1,3,5-triformylbenzene to the alkyl chain-modified amino compound of 2:3. After sealing, a film-forming reaction is carried out at the interface of the two phases at room temperature. After the reaction is completed, the film is washed and dried to obtain an alkyl chain-modified covalent organic framework membrane.

[0014] Preferably, in the organic phase solution, the concentration of 1,3,5-triformylbenzene is 0.01 to 0.3 mol / L.

[0015] Preferably, in the aqueous solution, the concentration of the alkyl chain-modified amino compound is 0.01 to 0.3 mol / L.

[0016] Preferably, the concentration of acetic acid in the aqueous acetic acid solution is 3 to 9 mol / L, more preferably 6 mol / L.

[0017] Preferably, the volume ratio of the organic phase solution to the aqueous phase solution is 1:1 to 1:10.

[0018] Preferably, the washing method is to use dichloromethane, ethanol and acetone in sequence, and the total washing time is 12 to 18 hours.

[0019] Preferably, the drying temperature is 45-50° C. and the drying time is 40-48 hours.

[0020] Furthermore, the present invention provides another method for preparing an alkyl chain-modified covalent organic framework film by in-situ polymerization on the surface of a copper foil, comprising the following steps:

[0021] First, 1,3,5-triformylbenzene is ultrasonically dissolved in a mixed solvent composed of 1,3-dioxolane and ethylene glycol dimethyl ether, and an alkyl chain-modified amino compound is ultrasonically dissolved in triethylene glycol dimethyl ether. Then, according to a molar ratio of 1,3,5-triformylbenzene to the alkyl chain-modified amino compound of 2:3, the two solutions are mixed, and acetic acid aqueous solution is added, and ultrasonication is continued until the mixture is uniform. At room temperature, the mixed solution is slowly dripped onto a copper foil, allowed to stand, and in-situ polymerization is performed to obtain an alkyl chain-modified covalent organic framework membrane.

[0022] Preferably, the concentration of the acetic acid aqueous solution is 2 to 6 mol / L.

[0023] Preferably, the volume ratio of 1,3-dioxolane to ethylene glycol dimethyl ether is 3:1 to 1:3.

[0024] Preferably, the volume ratio of the mixed solution of 1,3-dioxolane and ethylene glycol dimethyl ether to triethylene glycol dimethyl ether is 1:1.

[0025] The present invention provides a solid electrolyte based on the above alkyl chain-modified covalent organic framework film.

[0026] The alkyl chain modified covalent organic framework membrane solid electrolyte of the present invention is prepared by mixing the vacuum dried alkyl chain modified covalent organic framework membrane with a mixture of polyethylene glycol (PEG) and lithium bistrifluoromethanesulfonyl imide (LiTFSI), and letting the mixture stand for 24 hours.

[0027] Furthermore, the present invention provides the use of the above-mentioned alkyl chain modified covalent organic framework membrane solid electrolyte in a battery.

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] (1) The present invention realizes the rapid and easy preparation of the covalent organic framework membrane by interfacial polymerization or by in situ polymerization on the surface of copper foil, and modifies the alkyl side chains in the pores of the covalent organic framework, which not only improves the mechanical strength and structural stability of the covalent organic framework membrane, but also can well lock the lithium salt and polyethylene glycol injected into the structure, greatly enhancing its lithium ion conductivity and the stability of lithium battery cycling.

[0030] (2) The alkyl chain-modified covalent organic framework membrane of the present invention, as an electrolyte, exhibits high ion conductivity and excellent ion conductivity. The ion conductivity at 120°C can reach 2.13×10 -3 S cm -1 , an order of magnitude higher.

[0031] (3) The solid-state lithium battery constructed with an alkyl chain-modified covalent organic framework membrane solid electrolyte of the present invention has good cycling performance. For example, the all-solid-state battery of LiFePO4 / COF-C-2-Li / Li battery with COF-C-2-Li as the solid electrolyte can stably cycle for more than 20 cycles. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 XRD of (a) COF-C-2 film prepared in Example 1, (b) COF-C-2 powder, (c) C-2,2-NHNH2 and (d) 1,3,5-triformylbenzene;

[0033] Figure 2 Infrared images of (a) COF-C-2 film prepared in Example 1, (b) C-2,2-NHNH2 and (c) 1,3,5-triformylbenzene;

[0034] Figure 3 The actual pictures of the covalent organic framework membrane obtained by interfacial polymerization at different acetic acid concentrations;

[0035] Figure 4 XRD of covalent organic framework films obtained by interfacial polymerization under different acetic acid concentrations;

[0036] Figure 5 Figure 1 is a nitrogen absorption and desorption diagram of the COF-C-2 membrane prepared in Example 1;

[0037] Figure 6 This is an electronic scanning image of the COF-C-2 film prepared in Example 1;

[0038] Figure 7 This is a performance test diagram of ion conduction of the covalent organic framework membrane of COF-C-2-Li prepared in Example 1 at 60-120°C;

[0039] Figure 8 This is a performance test diagram of ion conduction of the covalent organic framework membrane of COF-C-2-Li prepared in Example 1 at 60-120°C;

[0040] Fig. 9 The charge and discharge curves of an all-solid-state battery of a LiFePO4 / LiFePO4 / COF-C-2-Li / Li battery using COF-C-2-Li / LiFePO4 prepared in Example 1 as a solid electrolyte;

[0041] Fig.10 The cycle specific capacity diagram of the all-solid-state battery of LiFePO4 / LiFePO4 / COF-C-2-Li / Li battery using COF-C-2-Li / LiFePO4 prepared in Example 1 as the solid electrolyte;

[0042] Fig.11 This is a cycle efficiency diagram of a LiFePO4 / LiFePO4 / COF-C-2-Li / Li battery using COF-C-2-Li / LiFePO4 prepared in Example 1 as a solid electrolyte. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below through embodiments and in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0044] The C-2,2-NHNH2 of the present invention can be purchased commercially or prepared by itself. The specific synthesis route is as follows:

[0045]

[0046] The specific steps are as follows:

[0047] (1) Compound 1c: 1 mmol of compound 1a, 3 mmol of compound 1b and 1 mmol of K2CO3 were added to 30 ml of N,N-dimethylformamide (DMF), and reacted at 65°C for 48 hours under a protective atmosphere of N2. After the reaction, the mixture was extracted with dichloromethane, washed with saturated brine, dried over anhydrous sodium sulfate, and the solvent was removed by spin drying. The mixture was separated by column chromatography using a developing solvent to obtain compound 1c;

[0048] (2) C-1,1-NHNH2: Compound 1c and hydrazine hydrate were added to 15 ml of ethanol solution, reacted for 12 hours, and directly filtered after freezing. The white solid was washed with petroleum ether solvent for multiple times to obtain C-2,2-NHNH2.

[0049] Example 1

[0050] 1. Alkyl chain modified covalent organic framework membrane (COF-C-2) is an organic framework structure formed by Schiff base reaction of 1,3,5-triformylbenzene and C-2,2-NHNH2. Its structure is shown below:

[0051]

[0052] The structure of C-2,2-NHNH2 is shown below:

[0053]

[0054] 2. Preparation of COF-C-2

[0055] (1) Synthesized by interfacial polymerization, the specific steps are as follows:

[0056] 0.1 mmol 1,3,5-triformylbenzene was weighed and dissolved in dichloromethane to form an organic phase solution, 0.15 mmol C-2,2-NHNH2 was weighed and dissolved in 6 mol / L acetic acid aqueous solution to form an aqueous phase solution, and the aqueous phase solution was gradually added dropwise to the top of the organic phase solution. After sealing, the two-phase interface film-forming reaction was carried out at room temperature for 40 to 48 hours. After the reaction was completed, the alkyl chain-modified covalent organic framework membrane COF-C-2 was obtained by washing and drying. The synthesis route is as follows:

[0057]

[0058] (2) Synthesized by in-situ polymerization on the copper foil surface, the specific steps are as follows:

[0059] Weigh 4.3 mg of the amino-containing monomer alkyl chain modified amino compound (C-2,2-NHNH2), add it to a 5 mL glass tube, and add 5 mL of a mixed solution of 1,3-dioxolane and ethylene glycol dimethyl ether (volume ratio 1:1). Weigh 2.8 mg of the aldehyde-containing monomer 1,3,5-triformylbenzene, add it to a 5 mL glass tube, and add 5 mL of triethylene glycol dimethyl ether. Ultrasound is used to dissolve the two monomers in the solvent respectively, mix them, and then 0.1 mL of 3 mol / L acetic acid aqueous solution is added to the mixed solution. Finally, the mixed solution is dripped onto the copper foil and left to stand for 24 hours to form a powdered COF-C-2 material. The synthesis route is as follows:

[0060]

[0061] 3. The dried alkyl chain-modified covalent organic framework membrane was mixed with the already mixed mixture of polyethylene glycol (PEG) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) at 90°C and allowed to stand for 24 hours to prepare a solid electrolyte. The entire infusion process was carried out in an argon-filled glove box. The button cell was assembled with the infused covalent organic framework membrane and its ion conduction curve was measured at 60-120°C.

[0062] (1) Assembly of button batteries. The specific method is as follows:

[0063] LiFePO4 is used as the positive electrode material, the above-mentioned alkyl chain-modified covalent organic framework membrane perfused with polyethylene glycol (PEG) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) is used as the solid electrolyte, and the lithium sheet is used as the negative electrode sheet. The battery is assembled in the vacuum glove box in the following order: the negative electrode shell faces up, the reed, the gasket, the lithium sheet, the solid electrolyte, the positive electrode sheet (face down), and finally the positive electrode shell is buckled. The battery is sealed in the glove box, put into the sample bag and taken out. Note: The gasket, positive electrode sheet, diaphragm and lithium sheet should be placed in the middle as much as possible, and plastic tweezers should be used during the operation.

[0064] (2) The battery performance test method is as follows:

[0065] (a) The battery cycle test uses the LANDct V7.3 battery test system. The specific test process is as follows: Place the battery in a 25°C constant temperature box, use a special button battery fixture to fix the battery according to the positive and negative poles, and set the static duration to 12 hours; discharge at a constant current of 565.2μA for 2 hours; charge at a constant current of 565.2μA until the voltage reaches 1V; cycle 20 times to end the test.

[0066] (b) The ion conduction test was performed using a Biological SF-200 portable workstation: the electrolyte was inserted between two stainless steel electrodes and assembled into a button cell, which was performed in a glove box. After controlling the equilibrium temperature from 60 to 120 °C, the test frequency was 7 MHz-0.1 Hz and the amplitude voltage was 10 mV.

[0067] Example 2

[0068] This embodiment is basically the same as embodiment 1, the only difference being that the acetic acid concentration of the acetic acid aqueous solution used is 3 mol / L, specifically:

[0069] 0.1mmol 1,3,5-triformylbenzene was weighed and dissolved in dichloromethane to form an organic phase solution, 0.15mmol C-2,2-NHNH2 was weighed and dissolved in 3mol / L acetic acid aqueous solution to form an aqueous phase solution, the aqueous phase solution was gradually added to the top of the organic phase solution, sealed, and the two-phase interface film-forming reaction was carried out at room temperature for 40 to 48 hours. After the reaction was completed, the alkyl chain-modified covalent organic framework film was washed and dried to obtain a uniform and complete film with high crystallinity.

[0070] Example 3

[0071] This embodiment is basically the same as embodiment 1, the only difference being that the acetic acid concentration of the acetic acid aqueous solution used is 9 mol / L, specifically:

[0072] 0.1mmol 1,3,5-triformylbenzene was weighed and dissolved in dichloromethane to form an organic phase solution, 0.15mmol C-2,2-NHNH2 was weighed and dissolved in 9mol / L acetic acid aqueous solution to form an aqueous phase solution, the aqueous phase solution was gradually added to the top of the organic phase solution, sealed, and the two-phase interface film-forming reaction was carried out at room temperature for 40 to 48 hours. After the reaction was completed, the alkyl chain-modified covalent organic framework film was washed and dried to obtain a uniform and complete film with high crystallinity.

[0073] Comparative Example 1

[0074] This comparative example is basically the same as Example 1, except that the acetic acid concentration of the acetic acid aqueous solution used is 1 mol / L, specifically:

[0075] 0.1mmol 1,3,5-triformylbenzene was weighed and dissolved in dichloromethane to form an organic phase solution, 0.15mmol C-2,2-NHNH2 was weighed and dissolved in 1mol / L acetic acid aqueous solution to form an aqueous phase solution, and the aqueous phase solution was gradually added to the top of the organic phase solution. After sealing, the two-phase interface film-forming reaction was carried out at room temperature for 40 to 48 hours. After the reaction was completed, the alkyl chain-modified covalent organic framework film was washed and dried. Due to the low acetic acid concentration, the film formation speed was slow, the integrity of the film was poor, and the crystallinity was low.

[0076] Comparative Example 2

[0077] This comparative example is basically the same as Example 1, except that the acetic acid concentration of the acetic acid aqueous solution used is 10 mol / L, specifically:

[0078] 0.1mmol 1,3,5-triformylbenzene was weighed and dissolved in dichloromethane to form an organic phase solution, 0.15mmol C-2,2-NHNH2 was weighed and dissolved in 10mol / L acetic acid aqueous solution to form an aqueous phase solution, and the aqueous phase solution was gradually added to the top of the organic phase solution. After sealing, the two-phase interface film-forming reaction was carried out at room temperature for 40 to 48 hours. After the reaction was completed, the alkyl chain-modified covalent organic framework film was washed and dried. Due to the high acetic acid concentration, the film formation speed was fast, resulting in uneven and incomplete films with low crystallinity.

[0079] Figure 1 XRD patterns of (a) COF-C-2 film, (b) COF-C-2 powder, (c) C-2,2-NHNH2 and (d) 1,3,5-triformylbenzene. XRD patterns of COF-C-2 films prepared by two synthesis methods Figure 1 The results show that the alkyl chain-modified covalent organic framework COF-C-2 membrane was successfully synthesized.

[0080] Figure 2The infrared images of (a) COF-C-2 film, (b) C-2,2-NHNH2 and (c) 1,3,5-triformylbenzene. The infrared images of COF-C-2 films prepared by the two synthesis methods are shown in Figure 1. Figure 1 It can be seen that the COF-C-2 film has a peak at 1226 cm -1 and 1675cm -1 The infrared absorption peak of can confirm the formation of C=N bond.

[0081] Figure 3 Actual pictures of covalent organic framework membranes prepared under different acetic acid concentrations: (a) 1 mol / L (b) 3 mol / L (c) 6 mol / L (d) 9 mol / L (e) 10 mol / L.

[0082] Figure 4 XRD patterns of covalent organic framework films prepared under different acetic acid concentrations: (a) 1 mol / L (b) 3 mol / L (c) 6 mol / L (d) 9 mol / L (e) 10 mol / L.

[0083] Figure 5 The nitrogen adsorption diagram of COF-C-2 membrane is shown in Figure 2. The nitrogen adsorption of COF-C-2 membranes prepared by two synthesis methods is shown in Figure 2. Figure 1 This indicates that the covalent organic framework membrane has abundant specific surface area and void distribution, which is extremely beneficial to the conduction of lithium ions.

[0084] Figure 6 This is an electron scanning image of the COF-C-2 membrane. It can be seen that the entire membrane is uniform and dense and has a large number of alkyl chain-modified COF voids, which is extremely beneficial to the conduction of lithium ions.

[0085] Figure 7 The COF-C-2 membrane was infused with polyethylene glycol (PEG) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and assembled into a button battery. (a) 60℃ (b) 80℃ (c) 100℃ (d) 120℃ tested its complete test diagram of ion conductivity performance at 60-120℃.

[0086] Figure 8 The membrane of COF-C-2 was assembled into a button cell after being coated with polyethylene glycol (PEG) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI). The local magnified image of the ion conductivity at 60-120℃ was tested at (a) 60℃ (b) 80℃ (c) 100℃ (d) 120℃. The maximum value at 120℃ was 2.13×10 -3 S cm -1 .

[0087] Fig. 9The charge and discharge curve of the solid-state lithium-ion battery with COF-C-2-Li / LiFePO4 membrane shows that this battery can be stably cycled for more than 20 times.

[0088] Fig.10 This is the cycle specific capacity diagram of the COF-C-2-Li / LiFePO4 solid-state lithium-ion battery. It can be seen that after more than 20 cycles, the battery specific capacity still remains above 160mAh / g, indicating good cycle stability.

[0089] Fig.11 This is the cycle efficiency diagram of the solid-state lithium-ion battery of COF-C-2-Li / LiFePO4. It can be seen that after more than 20 cycles, the battery efficiency still remains above 95%, indicating good cycle stability.

Claims

1. Solid electrolytes based on alkyl chain-modified covalent organic framework membranes, It is characterized in that The alkyl chain-modified covalent organic framework membrane is prepared by mixing the vacuum-dried alkyl chain-modified covalent organic framework membrane with a mixture of polyethylene glycol and lithium bis(trifluoromethanesulfonyl)imide and standing for 24 hours. The structural formula of the alkyl chain-modified covalent organic framework membrane is as follows: , Prepared by the following steps: Dissolving 1,3,5-triformylbenzene in dichloromethane to form an organic phase solution, dissolving an alkyl chain-modified amino compound in an acetic acid aqueous solution to form an aqueous phase solution, wherein the concentration of acetic acid in the acetic acid aqueous solution is 3-9 mol / L, and the molar ratio of 1,3,5-triformylbenzene to the alkyl chain-modified amino compound is 2:3, and the aqueous phase solution is added dropwise to the organic phase solution, after sealing, undergoing a two-phase interface film-forming reaction at room temperature, and after the reaction is completed, washing and drying to obtain an alkyl chain-modified covalent organic framework membrane; Alternatively, 1,3,5-triformylbenzene is first ultrasonically dissolved in a mixed solvent consisting of 1,3-dioxolane and ethylene glycol dimethyl ether, and the alkyl chain-modified amino compound is ultrasonically dissolved in triethylene glycol dimethyl ether. Then, according to the molar ratio of 1,3,5-triformylbenzene to the alkyl chain-modified amino compound being 2:3, the two solutions are mixed and then an acetic acid aqueous solution is added, the concentration of the acetic acid aqueous solution is 2-6 mol / L, and ultrasonication is continued until the mixture is uniform. At room temperature, the mixed solution is slowly dripped onto a copper foil, allowed to stand, and in-situ polymerization is performed to obtain an alkyl chain-modified covalent organic framework membrane.

2. The solid electrolyte according to claim 1, It is characterized in that In the organic phase solution, the concentration of 1,3,5-triformylbenzene is 0.01-0.3 mol / L; in the aqueous phase solution, the concentration of the alkyl chain-modified amino compound is 0.01-0.3 mol / L; and the volume ratio of the organic phase solution to the aqueous phase solution is 1:1-1:

10.

3. The solid electrolyte according to claim 1, It is characterized in that The washing method is to use dichloromethane, ethanol and acetone in sequence, and the total washing time is 12~18h; the drying temperature is 45~50℃, and the drying time is 40~48h.

4. The solid electrolyte according to claim 1, It is characterized in that The volume ratio of 1,3-dioxolane to ethylene glycol dimethyl ether is 3:1-1:3, and the volume ratio of the mixed solution of 1,3-dioxolane and ethylene glycol dimethyl ether to triethylene glycol dimethyl ether is 1:

1.

5. Use of the solid electrolyte according to claim 1 in a battery.

Citation Information

Patent Citations

  • Full-solid-state electrolyte material, preparation method and application thereof

    CN109904519A

  • Method of preparing covalent organic frame material film through quantitative layer-by-layer self-assembly

    CN110698710A