Rework method of PCB board electroplating hard gold infiltration

Through detection and continuous treatment technology, nitrogen film and emery sandblasting is used to remove the gold layer of the gold seepage part. Combined with green oil treatment, the short circuit problem caused by loosening of the gold seepage dry film during the electroplating of PCB board is solved, which significantly reduces the Scrap rate and improve productivity and economic benefits.

CN113630974BActive Publication Date: 2024-11-22GUANGZHOU MEADVILLE ELECTRONICS
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202110690711.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-22
Publication Date
2024-11-22
Estimated Expiration
2041-06-22

AI Technical Summary

Technical Problem

Existing PCB boards are prone to loosening of gold seepage dry film during electroplating, resulting in etching resistance problems, short circuits and high scrap rate, especially in small-pitch positions that cannot be manually repaired, resulting in economic losses.

Method used

The gold layer in the gold seepage area is removed through the detection and continuous treatment method through nitrogen film and emery sandblasting technology, combined with green oil treatment to prevent gold seepage, and replacing the hard gold when necessary to ensure the quality of the circuit board.

Benefits of technology

It effectively reduces the scrap rate of PCB boards, improves production efficiency and economic benefits, and reduces repair time and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113630974B_ABST
    Figure CN113630974B_ABST
Patent Text Reader

Abstract

The invention discloses a rework method for electroplating hard gold and gold infiltration of a PCB board. The method comprises the following steps: processing a PCB inner sheet material of a required size, and after the processes of film pasting, exposure, etching, and film stripping, making a required circuit pattern on the PCB inner sheet material, bonding and curing the hot melt plastic with the inner copper surface and copper foil; pasting, exposure, and development, electroplating hard gold, and film stripping, inspecting whether gold infiltration occurs in the part to be etched, applying film with a nitrogen sheet, setting the gold infiltration part as the film window opening part, and setting the non-gold infiltration part as the film non-window opening part; printing the required solder mask on the PCB board surface and the hole, and performing green oil treatment, and performing development treatment after the green oil; spraying corundum on the film window opening part to remove the gold in the gold infiltration part. The repair of electroplating gold infiltration is carried out by using the detection and continuous treatment method, which solves the problem of high scrap rate of circuit boards, saves costs, and improves economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of circuit boards, and in particular to a reworking method for electroplating hard gold and gold infiltration of a PCB board. Background Art

[0002] At present, with the trend of miniaturization of electronic equipment, the size of electronic components is getting smaller and smaller, and the arrangement density is getting higher and higher. Printed circuit boards, also known as printed circuit boards, are providers of electrical connections for electronic components. In order to increase the area that can be wired, multilayer boards use more single-sided or double-sided wiring boards. A printed circuit board with one double-sided inner layer and two single-sided outer layers or two double-sided inner layers and two single-sided outer layers, alternately connected by a positioning system and insulating adhesive materials, and the conductive patterns are interconnected according to the design requirements, becomes a four-layer or six-layer printed circuit board, also known as a multilayer printed circuit board.

[0003] However, the existing PCB boards have the following defects during production:

[0004] During the production process of ordinary high-layer one-time pressed hard gold PCB boards, the water-gold dry film of the PCB boards after water-gold electroplating will loosen before or during the hard gold electroplating process. During the hard gold electroplating process, gold seepage will occur (the position of the gold seepage needs to be etched), and the thin gold layer at the gold seepage position cannot react with the etching solution of the film stripping etching process, resulting in corrosion resistance problems during the film stripping etching process (the part that needs to be etched is not etched), which will eventually cause the PCB board to short-circuit. The outer layer AOI can only be repaired, and the repair process is slow. In addition, the gold seepage short circuit at the position with a small spacing cannot be repaired manually, which eventually leads to the scrapping of the PCB board and a high scrap rate. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, one of the purposes of the present invention is to provide a rework method for electroplating hard gold and gold infiltration of a PCB board, which can solve the problem of high scrap rate.

[0006] One of the purposes of the present invention is achieved by the following technical solution:

[0007] A rework method for electroplating hard gold infiltration on a PCB board comprises the following steps:

[0008] Prefabrication process steps: Process the inner layer of PCB with the required size, make the required circuit pattern on the inner layer of PCB after the process of laminating, exposure, etching and film stripping, and bond and solidify the hot melt plastic with the inner copper surface and copper foil;

[0009] Finishing process steps: remove the part of the board edge where the glue solidifies during the lamination process to make the board edge neat and smooth, punch holes and realize subsequent inter-layer signal interconnection, and deposit and plate copper on the holes and board surface;

[0010] The first outer layer processing steps: film lamination, exposure, development, revealing the required pattern on the PCB board, and thickening the copper, nickel and gold in the hole and on the PCB board surface to the required degree;

[0011] Secondary outer layer processing steps: secondary film lamination, exposure, and development to reveal the required pattern on the PCB board;

[0012] Electroplating hard gold steps: Use chemical methods to electroplate the hard gold thickness required by the customer in the electroplating hard gold pattern area;

[0013] Film stripping step: remove the dry film on the board surface during primary and secondary outer processing to expose the area to be etched;

[0014] Electroplating inspection steps: Check whether gold seepage occurs in the area to be etched. If so, proceed to the next step;

[0015] Abnormal board processing steps: Use nitrogen film to apply film, set the gold-infiltrated part as the film window part, and set the non-gold-infiltrated part as the film non-window part; print the required solder mask on the PCB board surface and in the hole, and perform green oil and exposure treatment, and then perform development treatment after exposure;

[0016] Sandblasting steps: Spray corundum onto the film window opening to remove the gold from the gold-infiltrated area.

[0017] Furthermore, after the secondary outer layer processing step and before the hard gold electroplating step, an outer layer detection step is provided: check whether the dry film attached by the primary outer layer processing is loose, if so, remove the film of the abnormal PCB board, use nitrogen sheet to apply film, set the hard gold graphic part of the PCB board as the film window part, set the non-hard gold graphic part as the film non-window part, print the solder mask required by the customer on the PCB board surface and the hole and develop it, and re-electroplate hard gold to the required thickness; if not, perform the hard gold electroplating step.

[0018] Abnormal panel processing steps

[0019] Furthermore, in the prefabrication process step: the hot melt plastic PP is bonded to the inner copper surface and the copper foil and solidified.

[0020] Furthermore, in the finishing step, after drilling, debris on the board surface is removed and the copper surface is roughened.

[0021] Furthermore, the method further comprises a step of removing green oil: removing green oil on the surface of the plate by using a NaOH solution.

[0022] Furthermore, the method also includes a film stripping and etching step: using a chemical method to remove the dry film on the board surface, removing excess copper on the board surface and retaining the required circuits.

[0023] Furthermore, it also includes an outer layer inspection step: using an automatic optical inspection device to check the quality of the board surface, if the quality does not meet the requirements, marking it.

[0024] Furthermore, the method also includes a marking step: printing a required mark on the board surface.

[0025] Furthermore, in the sandblasting step, the green oil on the surface is solidified and pre-dried before sandblasting.

[0026] Furthermore, if gold penetration is found after the electroplated hard gold film is stripped, in the sandblasting step, the pre-drying temperature is set to 150° C. and the pre-drying time is set to 15 minutes.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] Check if the dry film attached by the outer layer processing is loose, use nitrogen film to apply film, set the graphic part without loose dry film as the film without window opening part, and set the graphic part with loose dry film as the film with window opening part; in the film with window opening part, remove the dry film of the entire board surface of the abnormal board, print the required solder mask on the PCB board surface and the hole and perform green oil treatment, and then perform development treatment after green oil; spray diamond sand on the film with window opening part to remove the gold in the gold infiltration part. The method of detection and continuous treatment is used to repair the electroplating gold infiltration, which solves the problem of high scrap rate of circuit boards, saves costs and improves economic benefits.

[0029] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a flow chart of a preferred embodiment of the rework method of PCB board electroplating hard gold infiltration. DETAILED DESCRIPTION

[0031] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.

[0032] It should be noted that when a component is referred to as being "fixed to" another component, it may be directly on the other component or there may also be a component centered. When a component is considered to be "connected to" another component, it may be directly connected to the other component or there may also be a component centered. When a component is considered to be "set on" another component, it may be directly set on the other component or there may also be a component centered. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0034] See also Figure 1 A rework method for electroplating hard gold on a PCB board comprises the following steps:

[0035] Prefabrication process steps: Process the inner layer of PCB with the required size, make the required circuit pattern on the inner layer of PCB after the process of laminating, exposure, etching and film stripping, and bond and solidify the hot melt plastic with the inner copper surface and copper foil;

[0036] Preferably, in the prefabrication step: the hot melt plastic PP is bonded to the inner copper surface and the copper foil and solidified.

[0037] Finishing process steps: remove the part of the board edge where the glue solidifies during the lamination process to make the board edge neat and smooth, punch holes and realize subsequent inter-layer signal interconnection, and deposit and plate copper on the holes and board surface;

[0038] Preferably, in the finishing step, after punching, debris on the board surface is removed and the copper surface is roughened.

[0039] The first outer layer processing steps: film lamination, exposure, development, revealing the required pattern on the PCB board, and thickening the copper, nickel and gold in the hole and on the PCB board surface to the required degree;

[0040] Secondary outer layer processing steps: secondary film lamination, exposure, and development to reveal the required pattern on the PCB board;

[0041] Electroplating hard gold steps: Use chemical methods to electroplate the hard gold thickness required by the customer in the electroplating hard gold pattern area;

[0042] Film stripping step: remove the dry film on the board surface during primary and secondary outer processing to expose the area to be etched;

[0043] Electroplating inspection steps: Check whether gold seepage occurs in the area to be etched. If so, proceed to the next step;

[0044] Abnormal board processing steps: Use nitrogen film to apply film, set the gold-infiltrated part as the film window part, and set the non-gold-infiltrated part as the film non-window part; print the required solder mask on the PCB board surface and in the hole and perform green oil and exposure treatment, and then perform development treatment after exposure; Abnormal board processing steps

[0045] Sandblasting step: Spray corundum onto the film window opening to remove the gold from the gold-infiltrated area. The gold-infiltrated electroplating repair is carried out by using the detection and continuous processing method, which solves the problem of high scrap rate of circuit boards, saves costs and improves economic benefits.

[0046] Preferably, if gold seepage is found after the electroplated hard gold film is removed, in the sandblasting step, the green oil on the surface is solidified and pre-dried before sandblasting. The pre-drying temperature is set to 150° C. and the pre-drying time is set to 15 minutes.

[0047] Specifically, if the problem of hard gold electroplating seepage is found before hard gold electroplating, the principle is explained as follows: the hard gold electroplating or water gold electroplating process will plate copper, nickel, and water gold on some positions of the PCB, and this position will have a height difference with the non-water gold electroplating position. In the case of liquid, the fluidity of green oil is stronger than that of dry film. Even if there is a height difference between the water gold plated position and the non-water gold plated position of the PCB after water gold electroplating, the gap between the electroplated position and the non-electroplated position can be well combined with green oil and filled. The green oil after pre-drying has a stronger bonding force with the non-water gold position, so there will be no gold seepage in the PCB board during the process of hard gold electroplating rework.

[0048] Specifically, if the problem of hard gold infiltration is found after hard gold electroplating, the principle is as follows: green oil has strong fluidity in liquid state, and it can be well combined and filled with the hard gold layer and the water gold electroplating layer. The green oil has stronger bonding force after pre-drying, so during the sandblasting process of the gold-infiltrated PCB board, the green oil will protect the underlying hard gold layer / water gold electroplating layer. Sandblasting uses a physical method, and the diamond sand rubs against the gold layer at the gold-infiltrated position to remove the gold at the gold-infiltrated position, and finally achieve the purpose of rework.

[0049] Green oil removal step: Use NaOH solution to remove the green oil on the surface of the plate.

[0050] Stripping and etching steps: Use chemical methods to remove the dry film on the board surface, remove excess copper on the board surface and retain the required circuits.

[0051] Outer layer inspection steps: Use automatic optical inspection equipment to check the quality of the board surface. If the quality does not meet the requirements, mark it.

[0052] Marking steps: Print the required logo on the board.

[0053] Preferably, after the secondary outer layer processing step and before the hard gold electroplating step, an outer layer inspection step is provided: check whether the dry film attached by the primary outer layer processing is loose, if so, use nitrogen sheet to apply film, set the hard gold graphic part of the PCB board as the film window part, set the non-hard gold graphic part as the film non-window part, print the solder mask required by the customer on the PCB board surface and the hole and develop it, and re-electroplate hard gold to the required thickness; if not, perform the hard gold electroplating step.

[0054] Specifically, if gold seepage occurs, the method of the present application can be used to solve the problem before or after hard gold electroplating; if gold seepage does not occur, the main production process of multi-layer one-time pressed hard gold PCB board is as follows:

[0055] Cutting step: Cut the large-sized PCB inner layer sheet into the required small PCB inner layer sheets;

[0056] Inner IDF step: After the film lamination, exposure, etching, and film stripping processes, the circuit pattern required by the customer is made on the inner layer of the PCB board;

[0057] Inner layer AOI step: Use optical principles to check inner layer graphic board defects;

[0058] Pressing step: hot-melting the solid PP, bonding the hot-melt PP to the inner copper surface and copper foil and finally solidifying it to achieve subsequent inter-layer signal insulation and interconnection;

[0059] Trimming step: remove the part of the board edge where the glue has solidified during the lamination process to make the board edge neat and smooth;

[0060] Drilling step: Drill the holes required by the customer to achieve subsequent inter-layer signal interconnection;

[0061] Deburring steps: remove debris from the board surface and roughen the copper surface;

[0062] Copper deposition step: Use chemical methods to deposit a thin layer of copper in the hole and on the board surface to achieve conduction;

[0063] Board plating steps: Use chemical methods to plate a thin layer of copper in the holes and on the board surface to play a conductive role and prepare for the subsequent "water-gold electroplating copper" process;

[0064] Outer IDF1 step: After the film lamination, exposure and development processes, the graphics required by the customer are exposed on the PCB board;

[0065] Water-gold plating steps: thicken the copper inside the hole and on the PCB surface, and plate nickel and thin gold to meet the copper thickness, nickel thickness, and thin gold thickness required by customers;

[0066] Outer IDF2 step: After the film lamination, exposure and development process, the electroplated hard gold pattern required by the customer is exposed on the PCB board;

[0067] Electroplating hard gold steps: through chemical methods, electroplating the hard gold thickness required by the customer in the electroplating hard gold pattern area;

[0068] Stripping step: Use chemical methods to remove the dry film on the board surface to prepare for subsequent etching. Etching step: Remove excess copper on the board surface to retain the circuit required by the customer;

[0069] Outer layer AOI step: Use optical principles to check the quality of the PCB surface;

[0070] Green oil step: print the solder mask required by the customer on the PCB board surface and inside the hole;

[0071] Character step: Print the logo required by the customer on the PCB surface to facilitate the subsequent installation of PCB components.

[0072] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A rework method for electroplating hard gold infiltration of a PCB board, characterized in that: The following steps are involved: Prefabrication process steps: Process the inner layer of PCB with the required size, make the required circuit pattern on the inner layer of PCB after the process of laminating, exposure, etching and film stripping, and bond and solidify the hot melt plastic with the inner copper surface and copper foil; Finishing process steps: remove the part of the board edge where the glue solidifies during the lamination process to make the board edge neat and smooth, punch holes and realize subsequent inter-layer signal interconnection, and deposit and plate copper on the holes and board surface; The first outer layer processing steps: film lamination, exposure, development, revealing the required pattern on the PCB board, and thickening the copper, nickel and gold in the hole and on the PCB board surface to the required degree; Secondary outer layer processing steps: secondary film lamination, exposure, and development to reveal the required pattern on the PCB board; Electroplating hard gold steps: Use chemical methods to electroplate the hard gold thickness required by the customer in the electroplating hard gold pattern area; Film stripping step: remove the dry film on the board surface during primary and secondary outer processing to expose the area to be etched; Electroplating inspection steps: Check whether gold seepage occurs in the area to be etched. If so, proceed to the next step; Abnormal board processing steps: Use nitrogen film to apply film, set the gold-infiltrated part as the film window part, and set the non-gold-infiltrated part as the film non-window part; print the required solder mask on the PCB board surface and in the hole, and perform green oil and exposure treatment, and then perform development treatment after exposure; Sandblasting steps: Spray corundum onto the film window opening to remove the gold from the gold-infiltrated area. Before sandblasting, solidify the green oil on the surface and perform pre-drying. The pre-drying temperature is set to 150°C and the pre-drying time is set to 15 minutes.

2. The reworking method of PCB board electroplating hard gold infiltration as claimed in claim 1, characterized in that: After the secondary outer layer processing step and before the hard gold electroplating step, an outer layer detection step is provided: check whether the dry film attached by the primary outer layer processing is loose, if so, remove the film of the abnormal PCB board, use nitrogen sheet to apply film, set the hard gold graphic part of the PCB board as the film window part, set the non-hard gold graphic part as the film non-window part, print the solder mask required by the customer on the board surface and the hole of the PCB board and develop it, and re-electroplate hard gold to the required thickness; if not, perform the hard gold electroplating step.

3. The reworking method of PCB board electroplating hard gold infiltration as claimed in claim 2, characterized in that: In the prefabrication process, the hot melt plastic PP is bonded to the inner copper surface and the copper foil and then cured.

4. The reworking method of PCB board electroplating hard gold infiltration as claimed in claim 1, characterized in that: In the finishing process, after drilling, impurities on the board surface are removed and the copper surface is roughened.

5. The reworking method of PCB board electroplating hard gold infiltration as claimed in claim 1, characterized in that: The method also includes a step of removing green oil: using a NaOH solution to remove the green oil on the surface of the plate.

6. The reworking method of PCB board electroplating hard gold infiltration as claimed in claim 5, characterized in that: It also includes a stripping and etching step: using chemical methods to remove the dry film on the board surface, remove excess copper on the board surface and retain the required circuits.

7. The reworking method of PCB board electroplating hard gold infiltration as claimed in claim 1, characterized in that: It also includes an outer layer inspection step: using an automatic optical inspection device to check the quality of the board surface. If the quality does not meet the requirements, it will be marked.

8. The reworking method of PCB board electroplating hard gold infiltration as claimed in claim 7, characterized in that: The method also includes a marking step: printing a desired mark on the board surface.

Citation Information

Patent Citations

  • Novel production method of board deep-recess line

    CN102006728A

  • Making method of outer layer patterns of local gold-plating printed plate

    CN103179795A

  • Manufacturing method of generalized silver circuit board

    CN104619133A

  • Surface processing technology for circuit board

    CN110035618A

  • Method and apparatus for attaching an electrical component to a circuit

    GB1077224A