Ceramic Heater
By using AlN ceramic substrate and optimized high and low resistance layer structure in the ceramic heater, the problem of peeling off of the silicon nitride ceramic insulating layer during repeated heating and cooling processes is solved, achieving long-term prevention of leakage current and high-precision temperature control.
Patent Information
- Application Number
- CN202080021382.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-18
- Filing Date
- 2020-03-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-03-04
AI Technical Summary
During the repeated heating and cooling process of existing ceramic heaters, the low thermal expansion rate of the silicon nitride ceramic insulating layer may cause it to peel off, making it impossible to prevent leakage current between the plasma generation electrode and the heater electrode for a long time.
An AlN ceramic matrix is used, and an AlN ceramic high-resistance layer and a low-resistance layer are set between the plasma generation electrode and the heater electrode. The high-resistance layer contains Si, Mg and Ti, has high volume resistivity, and is thermally conductive with the low-resistance layer. The rate is similar to avoid interlayer delamination, and the resistivity and thermal conductivity are improved by optimizing the content of Ti and Mg.
It achieves long-term prevention of leakage current between the plasma generation electrode and the heater electrode, ensures high-precision temperature control and heat uniformity, and avoids peeling of the insulation layer.
Smart Images

Figure CN113632589B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a ceramic heater. Background Art
[0002] For a long time, a plasma CVD process has sometimes been used in semiconductor manufacturing processes. In the plasma CVD process, a chip is placed on a chip mounting surface of a ceramic heater. A plasma generating electrode and a heater electrode are buried in the ceramic substrate of the ceramic heater. On the other hand, an upper electrode is arranged in the space above the chip. Moreover, if a high-frequency voltage is applied between the upper electrode and the plasma generating electrode, plasma is generated between these electrodes, and a thin film is deposited on the chip using the plasma. For such a ceramic heater, there is the following problem: if the leakage current of the high-frequency voltage applied to the plasma generating electrode is transmitted to the heater electrode, the power supply to the heater electrode cannot be controlled. In view of this, in patent document 1, a scheme is proposed to provide a high-resistance insulating layer (leakage current prevention layer) between the plasma generating electrode and the heater electrode. In addition, as an example, a scheme is proposed in which the ceramic substrate itself is formed of aluminum nitride ceramics, and as an insulating layer, a scheme is formed of silicon nitride ceramics having a resistance value greater than that of aluminum nitride.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 3602908 Summary of the invention
[0006] Problems to be solved by the invention
[0007] However, since the thermal expansion coefficient of silicon nitride ceramics is only about 60% of that of aluminum nitride ceramics, there is a possibility that the insulating layer will peel off during the repeated heating and cooling of the ceramic heater.
[0008] The present invention has been made to solve such a problem, and a main object of the present invention is to prevent leakage current between the plasma generating electrode and the heater electrode for a long period of time.
[0009] Solutions to Solve Problems
[0010] The ceramic heater of the present invention is a ceramic heater in which a plasma generating electrode and a heater electrode are buried in an AlN ceramic substrate having a wafer mounting surface in a separated state from a side close to the wafer mounting surface.
[0011] The AlN ceramic substrate has:
[0012] an AlN ceramic high resistance layer provided between the plasma generating electrode and the heater electrode, and
[0013] The AlN ceramic low resistance layer other than the high resistance layer,
[0014] The high resistance layer and the low resistance layer both contain Si, Mg and Ti,
[0015] The high resistance layer has a larger content of Mg and Ti than the low resistance layer and has a higher volume resistivity.
[0016] In the ceramic heater, the AlN ceramic substrate has an AlN ceramic high resistance layer arranged between the plasma generating electrode and the heater electrode and an AlN ceramic low resistance layer other than the high resistance layer. The high resistance layer and the low resistance layer both contain Si, Mg and Ti. Compared with the low resistance layer, the high resistance layer has a higher content of Mg and Ti and a higher volume resistivity. Therefore, the high resistance layer prevents leakage current from flowing between the plasma generating electrode and the heater electrode. The high resistance layer contains more Mg and Ti so that the volume resistivity is higher than that of the low resistance layer. In addition, the high resistance layer and the low resistance layer constituting the AlN ceramic substrate are basically AlN ceramics, so there is no large difference in thermal expansion coefficient. Therefore, even if the ceramic heater is repeatedly heated and cooled, it is difficult to peel off between the high resistance layer and the low resistance layer. Therefore, according to the ceramic heater, leakage current between the plasma generating electrode and the heater electrode can be prevented for a long time.
[0017] In the ceramic heater of the present invention, it is preferred that the high resistance layer contain less Si than the low resistance layer.
[0018] In the ceramic heater of the present invention, the low resistance layer is preferably an AlN ceramic layer containing 10 mass ppm or more and 50 mass ppm or less of Ti, and the high resistance layer is preferably an AlN ceramic layer containing 1000 mass ppm or more and 1500 mass ppm or less of Ti. In this way, the volume resistivity of the high resistance layer can be made higher than the volume resistivity of the low resistance layer, and the thermal conductivity of the high resistance layer can be made equal to the thermal conductivity of the low resistance layer.
[0019] In the ceramic heater of the present invention, the low resistance layer is preferably an AlN ceramic layer containing 90 mass ppm to 180 mass ppm of Mg, and the high resistance layer is preferably an AlN ceramic layer containing 200 mass ppm to 400 mass ppm of Mg.
[0020] In the ceramic heater of the present invention, the volume resistivity of the high resistance layer is preferably 1.2 times or more of the volume resistivity of the low resistance layer. This makes it easier to prevent leakage current between the plasma generation electrode and the heater electrode.
[0021] In the ceramic heater of the present invention, the thermal conductivity of the high resistance layer is preferably 90% or more of the thermal conductivity of the low resistance layer. In this way, since the thermal conductivity of the high resistance layer is relatively high, the thermal uniformity of the wafer becomes good.
[0022] In the ceramic heater of the present invention, it is preferred that the AlN ceramic substrate has a three-layer structure in which the low resistance layer, the high resistance layer and the low resistance layer are sequentially stacked, and the thickness of the high resistance layer is less than the sum of the thicknesses of the two low resistance layers. Generally, ceramics tend to have a lower thermal conductivity when the volume resistivity is high, but if such a structure is adopted, the thermal conductivity can be made relatively high as a whole, and the thermal uniformity of the chip becomes good. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a cross-sectional view schematically showing the structure of the plasma processing apparatus 10 .
[0024] Figure 2 yes Figure 1 An enlarged view of the part within the circle indicated by the single-dot dash line in FIG.
[0025] Figure 3 It is an enlarged view of the circled portion of another embodiment.
[0026] Figure 4 It is an enlarged view of the circled portion of another embodiment. DETAILED DESCRIPTION
[0027] Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings. Figure 1 is a cross-sectional view showing a schematic structure of the plasma processing device 10. Figure 2 yes Figure 1 An enlarged view of the part within the circle indicated by the single-dot dash line in FIG.
[0028] like Figure 1 As shown, the plasma processing apparatus 10 includes a chamber 12 , a shower head 20 , and a wafer mounting device 30 .
[0029] The chamber 12 is a box-shaped container made of aluminum alloy or the like. The chamber 12 has a circular hole 14 at the approximate center of the bottom surface. In addition, the chamber 12 has an exhaust pipe 16 at the bottom surface. The exhaust pipe 16 is provided with a pressure regulating valve, a vacuum pump, etc. (not shown) in the middle, and can adjust the interior of the chamber 12 to a desired pressure. The top of the chamber 12 is open.
[0030] The shower head 20 is installed in a manner to close the opening of the top of the chamber 12. An insulating member 22 is provided between the opening edge of the top of the chamber 12 and the shower head 20. The interior of the chamber 12 whose opening is closed by the shower head 20 is configured to be airtight. The shower head 20 sprays the gas introduced from the gas introduction pipe 24 toward the wafer W placed on the ceramic heater 31 from the plurality of gas injection holes 26. The shower head 20 is connected to an RF power supply 60 for plasma generation. Therefore, the shower head 20 functions as an electrode for plasma generation. The frequency of the RF power supply 60 is preferably 13 MHz or 27 MHz, for example.
[0031] The wafer mounting device 30 includes a ceramic heater 31 and a hollow shaft 38 .
[0032] In the ceramic heater 31 , an RF electrode 33 for plasma generation and a heater electrode 34 are embedded in a disk-shaped AlN ceramic base 32 having a wafer mounting surface 32 a in order to be separated from each other from the side close to the wafer mounting surface 32 a .
[0033] like Figure 2As shown, the AlN ceramic substrate 32 includes an AlN ceramic high resistance layer 321 disposed between the RF electrode 33 and the heater electrode 34 and AlN ceramic low resistance layers 322 and 323 other than the high resistance layer 321. The high resistance layer 321 and the low resistance layers 322 and 323 all contain Si, Mg and Ti. Here, the AlN ceramic substrate 32 is a three-layer structure in which the low resistance layer 322, the high resistance layer 321 and the low resistance layer 323 are sequentially stacked, and the thickness of the high resistance layer 321 is less than the total thickness of the two low resistance layers 322 and 323. The high resistance layer 321 has a higher content of Mg and Ti than the low resistance layers 322 and 323, and has a higher volume resistivity. The high resistance layer 321 has a higher content of Ti than the low resistance layers 322 and 323, so it looks black in appearance. The high resistance layer 321 preferably has a lower content of Si than the low resistance layers 322 and 323. The low resistance layers 322 and 323 are preferably AlN ceramic layers containing 10 mass ppm or more and 50 mass ppm or less of Ti, and the high resistance layer 321 is preferably an AlN ceramic layer containing 1000 mass ppm or more and 1500 mass ppm or less of Ti. The low resistance layers 322 and 323 are AlN ceramic layers containing 90 mass ppm or more and 180 mass ppm or less of Mg, and the high resistance layer 321 is preferably an AlN ceramic layer containing 200 mass ppm or more and 400 mass ppm or less of Mg. In addition, the volume resistivity of the high resistance layer 321 is preferably 1.2 times or more of the volume resistivity of the low resistance layers 322 and 323, and the thermal conductivity of the high resistance layer 321 is preferably 90% or more of the thermal conductivity of the low resistance layers 322 and 323. The thermal expansion coefficient α1 of the high resistance layer 321 is preferably equal to the thermal expansion coefficient α2 of the low resistance layers 322 and 323 (for example, within the range of α2±10%, preferably within the range of α2±5%).
[0034] The RF electrode 33 is in a grid shape, plate shape or film shape, and is made of, for example, a material mainly composed of a single substance or a compound (such as carbide) of W, Mo, Ti, Si or Ni, a material obtained by combining them, or a mixed material of them and a ceramic raw material used for the ceramic substrate 32. The RF electrode 33 is connected to an RF power source 60 for plasma generation via a power supply rod 35 inserted from the surface (back surface) of the ceramic substrate 32 opposite to the wafer mounting surface 32a.
[0035] The heater electrode 34 is in a coil shape or a belt shape, and is made of, for example, a material having W, Mo, Ti, Si, Ni as a single substance or a compound (carbide, etc.) as a main component, a material obtained by combining them, or a mixed material of them and a ceramic raw material used for the ceramic base 32. The heater electrode 34 is wired from one end 34a to the other end 34b in a one-stroke manner so as to cover the entire wafer mounting surface 32a. Power supply rods 36 and 37 are connected to one end 34a and the other end 34b of the heater electrode 34, respectively. A heater power supply 62 is connected between the two power supply rods 36 and 37. When the heater power supply 62 supplies power, the heater electrode 34 heats the wafer W adsorbed and held on the wafer mounting surface 32a.
[0036] The hollow shaft 38 is made of AlN like the ceramic substrate 32, and flanges 38a and 38b are provided around the openings at both ends. The hollow shaft 38 is bonded to the back of the ceramic substrate 32 via the flange 38a at one end by diffusion bonding or TCB (Thermal compression bonding). TCB refers to a well-known method of sandwiching a metal bonding material between two parts of the bonding object, heating to a temperature below the solidus temperature of the metal bonding material, and press-bonding the two parts in this state. It should be noted that if the operating temperature is low, the hollow shaft 38 can also be bonded to the back of the ceramic substrate 32 via an organic bonding layer. In addition, the hollow shaft 38 is airtightly installed around the circular hole 14 provided on the bottom surface of the chamber 12 via the flange 38b at the other end. Therefore, the interior of the hollow shaft 38 and the interior of the chamber 12 are completely isolated. A rod holder 39 is installed on the back of the flange 38b of the hollow shaft 38. The rod holder 39 fixes the power supply rods 35 , 36 , and 37 penetrating therethrough by a clamping mechanism (not shown).
[0037] Next, a manufacturing example of the plasma processing device 10 is described. Here, a manufacturing example of the wafer loading device 30 is described. It should be noted that this manufacturing example applies well-known technology, so only the outline is described. First, a forming mold with a flat cylindrical space is prepared. A raw material for a low resistance layer that becomes a low resistance layer when fired is put into the forming mold and spreads it. Next, an RF electrode 33 is arranged on it, and the raw material for the low resistance layer is further put in and spreads it on the RF electrode 33. Next, a raw material for a high resistance layer that becomes a high resistance layer when fired is put in and spreads it, and is temporarily formed into a disc shape. Next, a heater electrode 34 is arranged on the raw material for the high resistance layer, and the raw material for the low resistance layer is further put in and spreads it on the heater electrode 34, and is formed into a disc shape again. The obtained disc-shaped molded body is fired to obtain a ceramic heater 31. The firing can be pressure firing (for example, hot pressing firing) or normal pressure firing. Next, the surface of the ceramic heater 31 opposite to the wafer mounting surface 32a is cut to form holes for connecting the power supply rods 35, 36, and 37. After the cut ceramic heater 31 is joined to a separately manufactured hollow shaft 38, the power supply rod 35 is connected to the RF electrode 33, and the power supply rods 36 and 37 are connected to one end 34a and the other end 34b of the heater electrode 34, thereby obtaining the wafer mounting device 30.
[0038] Next, an example of using the plasma processing device 10 is described. Figure 1 As shown, a plasma processing device 10 is arranged in a chamber 12, and a wafer W is placed on a wafer placement surface 32a. Then, a reaction gas is supplied from a shower head 20, and a reaction gas atmosphere of a predetermined pressure (e.g., tens to hundreds of Pa) is set in the chamber 12. In this state, a high-frequency power is supplied from an RF power supply 60 to between the shower head 20 and an RF electrode 33 embedded in a ceramic substrate 32. Thus, plasma is generated between parallel plate electrodes formed by the shower head 20 and the RF electrode 33. CVD film formation or etching is performed on the wafer W using this plasma. In addition, the temperature of the wafer W is obtained based on the detection signal of a thermocouple not shown in the figure, and the voltage of the heater power supply 62 applied to the heater electrode 34 is controlled so that the temperature becomes a set temperature (e.g., 350° C. or 300° C.).
[0039] In the ceramic heater 31 described in detail above, the high resistance layer 321 prevents leakage current from flowing between the RF electrode 33 and the heater electrode 34. The high resistance layer 321 contains more Ti so that the volume resistivity is higher than that of the low resistance layers 322 and 323. When the Ti content of the AlN ceramic is too much, the volume resistivity becomes low, but if the Ti content is appropriate, there is a tendency for the volume resistivity to become high. This property is utilized in the present embodiment. In addition, the high resistance layer 321 and the low resistance layers 322 and 323 constituting the AlN ceramic substrate 32 are basically AlN ceramics, so there is no large difference in thermal expansion coefficient. Therefore, even if the ceramic heater 31 is repeatedly heated and cooled, it is difficult to peel off between the high resistance layer 321 and the low resistance layers 322 and 323. Therefore, according to the ceramic heater 31, leakage current between the RF electrode 33 and the heater electrode 34 can be prevented for a long time.
[0040] In addition, an RF electric field is induced around the RF electrode 33 due to the temporal change of the RF magnetic field generated by the RF current flowing in the RF electrode 33. The high resistance layer 321 prevents the RF electric field from coupling with the heater electrode 34. Therefore, it is possible to fully prevent the influence of RF noise on the heater circuit including the heater electrode 34. As a result, the temperature of the heater electrode 34 can be controlled with high accuracy.
[0041] The high resistance layer 321 preferably has a lower Si content than the low resistance layers 322 and 323. In this way, as shown in the measurement data of the experimental example described later, even if the Ti content is high, it can be made high resistance. The low resistance layers 322 and 323 are AlN ceramic layers containing 30 mass ppm or more and 120 mass ppm or less of Si, and the high resistance layer 321 is an AlN ceramic layer containing 20 mass ppm or more and 100 mass ppm or less of Si. The low resistance layers 322 and 323 preferably have a higher Si content than the high resistance layer 321.
[0042] It is preferred that the low resistance layers 322 and 323 are AlN ceramic layers containing 10 mass ppm or more and 50 mass ppm or less of Ti, and the high resistance layer 321 is an AlN ceramic layer containing 1000 mass ppm or more and 1500 mass ppm or less of Ti. In this way, the volume resistivity of the high resistance layer 321 can be made higher than the volume resistivity of the low resistance layers 322 and 323, and the thermal conductivity of the high resistance layer 321 can be made equal to the thermal conductivity of the low resistance layers 322 and 323.
[0043] It is preferred that the low resistance layers 322 and 323 are AlN ceramic layers containing Mg in an amount of 90 mass ppm or more and 180 mass ppm or less, and the high resistance layer 321 is an AlN ceramic layer containing Mg in an amount of 200 mass ppm or more and 400 mass ppm or less. In this way, as shown in the measurement data of the experimental example described later, even if the Ti content is high, high resistance can be achieved.
[0044] In addition, the volume resistivity of the high resistance layer 321 is preferably 1.2 times or more the volume resistivity of the low resistance layers 322 and 323. This makes it easier to prevent leakage current between the RF electrode 33 and the heater electrode 34.
[0045] The thermal conductivity of the high resistance layer 321 is preferably 90% or more of the thermal conductivity of the low resistance layers 322 and 323. Thus, the thermal conductivity of the high resistance layer 321 is relatively high, so that the thermal uniformity of the wafer W is improved.
[0046] Furthermore, the AlN ceramic substrate 32 has a three-layer structure in which a low resistance layer 322, a high resistance layer 321, and a low resistance layer 323 are sequentially stacked, and the thickness of the high resistance layer 321 is smaller than the sum of the thicknesses of the two low resistance layers 322 and 323. Generally, ceramics tend to have a lower thermal conductivity when the volume resistivity is high, but by adopting such a structure, the thermal conductivity can be made relatively high as a whole, and the thermal uniformity of the wafer W becomes good.
[0047] It should be noted that, needless to say, the present invention is not limited to the above-mentioned embodiments, and can be implemented in various forms as long as it belongs to the technical scope of the present invention.
[0048] For example, in the above-mentioned embodiment, the high resistance layer 321 is arranged below the lower surface of the RF electrode 33 and in contact with the upper surface of the heater electrode 34, but the present invention is not particularly limited thereto. Figure 3 As shown, the high resistance layer 321 may be arranged in contact with the lower surface of the RF electrode 33 and the upper surface of the heater electrode 34. Alternatively, at least one of the RF electrode 33 and the heater electrode 34 may be buried in the high resistance layer 321. Figure 4 FIG. 4 shows an example in which the heater electrode 34 is buried in the high resistance layer 321. Figure 3 and Figure 4 In the embodiment, the same reference numerals are used for the same components as those in the above embodiment. In any case, the same effects as those in the above embodiment can be obtained.
[0049] In the above-described embodiment, the wafer mounting surface 32 a may be divided into a plurality of regions, and the heater electrode 34 may be arranged in each region.
[0050] In the above-mentioned embodiment, an electrostatic electrode may be built in the AlN ceramic base 32 so that the wafer W is electrostatically attracted to the wafer mounting surface 32 a .
[0051] Example
[0052] Four types of ceramic heaters 31 (experimental examples 1 to 4) were manufactured according to the manufacturing example of the ceramic heater 31 described in the above embodiment, and the Ti content and characteristics of each AlN ceramic substrate 32 were evaluated. The results are shown in Table 1. The contents of Si, Mg and Ti were determined by ICP emission spectrometry (ICP-AES). The volume resistivity is a value measured at room temperature and is determined in accordance with JIS-C2141. The thermal conductivity is a value measured at room temperature and is determined in accordance with JIS-R1611. The thermal expansion coefficient is a value from room temperature to 1000°C and is determined in accordance with JIS-R1618.
[0053] [Table 1]
[0054]
[0055] In Experimental Examples 1 to 4, the high resistance layer 321 and the low resistance layers 322 and 323 all contain Si, Mg, and Ti. The high resistance layer 321 has a higher content of Mg and Ti than the low resistance layers 322 and 323, a higher volume resistivity, and a lower content of Si. Regarding the thermal expansion coefficient, in Experimental Examples 1 to 4, the high resistance layer 321 and the low resistance layers 322 and 323 are almost the same. Regarding the volume resistivity, in Experimental Examples 1 to 4, the high resistance layer 321 is higher than the low resistance layers 322 and 323. In Experimental Examples 1 and 2, the volume resistivity of the high resistance layer 321 is about 4 times the volume resistivity of the low resistance layers 322 and 323, and the thermal conductivity of the high resistance layer 321 is about 93% of the thermal conductivity of the low resistance layers 322 and 323. In Experimental Examples 3 and 4, the volume resistivity of the high resistance layer 321 is approximately 1.2 times that of the low resistance layers 322 and 323 , and the thermal conductivity of the high resistance layer 321 is approximately 96% of that of the low resistance layers 322 and 323 .
[0056] This application claims priority based on Japanese Patent Application No. 2019-049548 filed on March 18, 2019, the entire contents of which are incorporated herein by reference.
[0057] Industrial Applicability
[0058] The present invention can be used, for example, in semiconductor manufacturing processes.
[0059] Explanation of symbols
[0060] 10: plasma processing device, 12: chamber, 14: circular hole, 16: exhaust pipe, 20: nozzle, 22: insulating component, 24: gas introduction pipe, 26: gas injection hole, 30: chip loading device, 31: ceramic heater, 32: AlN ceramic substrate, 321: AlN ceramic high resistance layer, 322, 323: AlN ceramic low resistance layer, 32a: chip loading surface, 33: RF electrode, 34: heater electrode, 34a: one end, 34b: the other end, 35, 36, 37: power supply rod, 38: hollow shaft, 38a: flange, 38b: flange, 39: rod holder, 60: RF power supply, 62: heater power supply.
Claims
1. A ceramic heater, wherein a plasma generating electrode and a heater electrode are embedded in an AlN ceramic substrate having a wafer mounting surface in a separated state from a side close to the wafer mounting surface. The AlN ceramic substrate has: an AlN ceramic high resistance layer provided between the plasma generating electrode and the heater electrode, and The AlN ceramic low resistance layer other than the high resistance layer, The high resistance layer and the low resistance layer both contain Si, Mg and Ti, The high resistance layer has a higher content of Mg and Ti than the low resistance layer and has a higher volume resistivity. The AlN ceramic substrate has a three-layer structure in which the low resistance layer, the high resistance layer, and the low resistance layer are sequentially stacked, and the thickness of the high resistance layer is smaller than the total thickness of the two low resistance layers.
2. The ceramic heater according to claim 1, wherein The high resistance layer has a smaller Si content than the low resistance layer.
3. The ceramic heater according to claim 1 or 2, wherein: The low resistance layer is an AlN ceramic layer containing 10 mass ppm or more and 50 mass ppm or less of Ti, The high resistance layer is an AlN ceramic layer containing 1000 mass ppm or more and 1500 mass ppm or less of Ti.
4. The ceramic heater according to claim 1 or 2, wherein: The low resistance layer is an AlN ceramic layer containing 90 mass ppm or more and 180 mass ppm or less of Mg, The high resistance layer is an AlN ceramic layer containing 200 mass ppm or more and 400 mass ppm or less of Mg.
5. The ceramic heater according to claim 1 or 2, wherein: The volume resistivity of the high resistance layer is 1.2 times or more the volume resistivity of the low resistance layer.
6. The ceramic heater according to claim 1 or 2, wherein: The thermal conductivity of the high resistance layer is 90% or more of the thermal conductivity of the low resistance layer.
7. The ceramic heater according to claim 1 or 2, wherein: The low resistance layer is an AlN ceramic layer containing 30 mass ppm or more and 120 mass ppm or less of Si, The high resistance layer is an AlN ceramic layer containing 20 mass ppm or more and 100 mass ppm or less of Si.