Adhesive composition, adhesive layer, and adhesive sheet
By using oligomers of vinyl monomers with pigment structures on the side chains and (meth)acrylic polymers, the dispersion and exudation of the adhesive tape during coloring are solved, and good adhesion is achieved. and corrosion resistance.
Patent Information
- Application Number
- CN202080024968.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-03-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-03-23
AI Technical Summary
Existing adhesive tapes are prone to agglomerates when coloring, with poor dispersion and pigment components that may exudate, affecting the adhesive properties and corrosiveness.
Using oligomers obtained from vinyl monomers with pigment structure on the side chain as the basis of the binder composition, combining (meth)acrylic polymers, avoiding the use of high acid resins and dispersants to ensure dispersion and adhesion.
It is achieved without using high acid value resins and dispersants, and the good dispersion and adhesion of the adhesive composition is avoided while the seepage of pigment components is avoided, and the adhesion performance and corrosion resistance are improved.
Smart Images

Figure CN113646401B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive composition, an adhesive layer, and an adhesive sheet. Background Art
[0002] Conventionally, transparent adhesive tapes are preferably used to facilitate the position control during processing, lamination, etc. On the other hand, colored adhesive tapes are also used for the purpose of changing the design, improving the design and visibility, etc.
[0003] Pigments and dyes are often used in the coloring of adhesive tapes. For example, Patent Document 1 discloses that in an adhesive composition containing an acrylic polymer, a phenolic resin, an epoxy resin and a colorant, and containing 10 parts by weight or less of the colorant relative to 100 parts by weight of the acrylic polymer, a pigment or dye is preferably used as the colorant.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-013946 Summary of the invention
[0007] Problems to be solved by the invention
[0008] However, when a pigment or dye is used to color an adhesive tape, aggregates may be generated in the adhesive composition, and good dispersibility cannot be obtained without using a dispersant.
[0009] In addition, there is a problem that the coloring component bleeds out from the adhesive composition and remains on the adherend after the adhesive tape is peeled off.
[0010] In addition, depending on the type of pigment or dye, the adhesive property may also be deteriorated. In addition, in order to improve the dispersibility of the pigment, a resin with a high acid value is sometimes used, which may cause corrosion of metal adherends such as iron, stainless steel, and ITO.
[0011] Therefore, an object of the present invention is to provide a colored adhesive composition having good adhesive strength, good dispersibility even without using a resin or a dispersant having a high acid value, and no bleeding of a pigment component.
[0012] Means for solving problems
[0013] The inventors of the present application have conducted intensive studies to solve the above-mentioned problems and have found that the above-mentioned problems can be solved by using an oligomer obtained from a vinyl monomer having at least one dye structure in a side chain, thereby completing the present invention.
[0014] One embodiment of the present invention relates to an adhesive composition, characterized in that it is an adhesive composition comprising a base polymer and at least one oligomer, wherein the oligomer is an oligomer obtained by polymerizing a monomer composition, and the monomer composition at least comprises a vinyl monomer having at least one pigment structure on a side chain.
[0015] In one embodiment of the present invention, in the pressure-sensitive adhesive composition, the base polymer is preferably a (meth)acrylic polymer.
[0016] In one embodiment of the present invention, in the pressure-sensitive adhesive composition, the oligomer is preferably a (meth)acrylic oligomer.
[0017] In one embodiment of the present invention, in the adhesive composition, the (meth)acrylic oligomer may be a homopolymer of a (meth)acrylic monomer having at least one pigment structure in a side chain.
[0018] In one embodiment of the present invention, in the adhesive composition, the (meth)acrylic oligomer may be a copolymer of a (meth)acrylic monomer having at least one pigment structure in a side chain and an alkyl (meth)acrylate.
[0019] In one embodiment of the present invention, in the pressure-sensitive adhesive composition, the weight average molecular weight of the oligomer is preferably 1,000 to 50,000.
[0020] One embodiment of the present invention relates to a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition described above.
[0021] One embodiment of the present invention relates to a pressure-sensitive adhesive sheet including the pressure-sensitive adhesive layer described above.
[0022] In one embodiment of the present invention, the pressure-sensitive adhesive sheet may include the pressure-sensitive adhesive layer on a transparent film.
[0023] Effects of the Invention
[0024] According to one embodiment of the present invention, a colored adhesive composition can be provided which has good adhesive strength, good dispersibility even without using a resin or a dispersant having a high acid value, and does not cause bleeding of a pigment component. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] [ Figure 1 ] Figure 1 This is an example of a schematic cross-sectional view of a pressure-sensitive adhesive layer according to an embodiment of the present invention.
[0026] [ Figure 2 ] Figure 2This is an example of a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to an embodiment of the present invention.
[0027] [ Figure 3 ] Figure 3 This is an example of a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to an embodiment of the present invention. DETAILED DESCRIPTION
[0028] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention is not limited to the embodiments described below.
[0029] In the present specification, "A to B" indicating a range means "A or more and B or less". In the present specification, "mass %" is considered to be synonymous with "weight %", and "mass parts" is considered to be synonymous with "weight parts".
[0030] [Adhesive composition]
[0031] An adhesive composition according to one embodiment of the present invention is characterized in that it is an adhesive composition comprising a base polymer and at least one oligomer, wherein the oligomer is obtained by polymerizing the following monomer composition, wherein the monomer composition at least comprises a vinyl monomer having at least one pigment structure in a side chain.
[0032] The adhesive composition uses an oligomer obtained by polymerizing a vinyl monomer having a pigment structure in a side chain as a pigment, so the dispersibility is good even without using a high acid value resin or a dispersant, and the pigment component does not bleed out.
[0033] Hereinafter, each component contained in the said adhesive composition is demonstrated in detail.
[0034] <Base polymer>
[0035] In the adhesive composition according to one embodiment of the present invention, the base polymer constituting the adhesive composition is not particularly limited, and a known polymer used in adhesives can be used.
[0036] For example, (meth) acrylic acid polymers, rubber polymers, vinyl alkyl ether polymers, silicone polymers, polyester polymers, polyamide polymers, urethane polymers, fluorine polymers, and epoxy polymers can be cited. Among them, from the viewpoint that the coloring brought by the pigment becomes significant, (meth) acrylic acid polymers with high transparency are more preferably used. It should be noted that the polymer can be used alone or in combination of two or more.
[0037] In addition, a (meth)acrylic acid-based polymer means an acrylic acid-based polymer and / or a methacrylic acid-based polymer, and (meth) in the present invention has the same meaning.
[0038] Hereinafter, although the description will be mainly based on an embodiment in which the pressure-sensitive adhesive composition according to one embodiment of the present invention contains a (meth)acrylic polymer as a base polymer, the present invention is not limited to this embodiment.
[0039] The adhesive composition according to one embodiment of the present invention may include a (meth)acrylic polymer as a base polymer. Typically, the adhesive composition may be a (meth)acrylic adhesive composition having a (meth)acrylic polymer as a main component. The (meth)acrylic adhesive composition has excellent transparency.
[0040] As an adhesive composition according to one embodiment of the present invention, for example, it is preferred that the (meth)acrylic polymer is composed of the following monomer components as a base polymer, wherein the monomer components contain 40% by mass or more of an alkyl (meth)acrylate having a linear or branched alkyl group with a carbon number of 1 or more and 20 or less at the ester terminal. Hereinafter, the alkyl (meth)acrylate having an alkyl group with a carbon number of X or more and Y or less at the ester terminal is sometimes referred to as “alkyl (meth)acrylate C X-Y Alkyl esters".
[0041] In order to easily obtain a balance of properties, in the entire monomer components of the (meth)acrylic acid-based polymer according to one embodiment, (meth)acrylic acid C 1-20 The proportion of the alkyl ester is appropriately higher than 50% by mass, and may be, for example, 55% by mass or higher, 60% by mass or higher, or 70% by mass or higher.
[0042] For the same reason, among the monomer components, (meth)acrylic acid C 1-20 The proportion of the alkyl ester may be, for example, 99.9% by mass or less, 99.5% by mass or less, or 99% by mass or less.
[0043] In another embodiment, the (meth)acrylic acid C in the (meth)acrylic acid-based polymer 1-20 The proportion of the alkyl ester in the total monomer component can be, for example, 98% by mass or less. From the viewpoint of improving the cohesiveness of the adhesive layer, it can be 95% by mass or less, 85% by mass or less (for example, less than 80% by mass), 70% by mass or less, or 60% by mass or less.
[0044] As (meth)acrylic acid C 1-20Specific non-limiting examples of the alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and tert-butyl (meth)acrylate. Nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.
[0045] Among these, it is preferred to use at least (meth)acrylic acid C 4-20 Alkyl esters, more preferably at least (meth) acrylic acid C 4-18 Alkyl esters. For example, it is preferred that the (meth)acrylic adhesive contains one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) as the monomer component, and it is particularly preferred that the (meth)acrylic adhesive contains at least BA.
[0046] As the (meth)acrylic acid C that can be preferably used 4-20 Other examples of the alkyl ester include isononyl acrylate, n-butyl methacrylate (BMA), 2-ethylhexyl methacrylate (2EHMA), and isostearyl acrylate (iSTA).
[0047] In some embodiments, the monomer components constituting the (meth)acrylic acid-based polymer may contain (meth)acrylic acid C in a ratio of 40% by mass or more. 4-18 Alkyl ester. (Meth) acrylic acid C 4-18 The proportion of the alkyl ester in the monomer component may be, for example, 50% by mass or more, 60% by mass or more, or 65% by mass or more. The (meth)acrylic acid C may be contained in a proportion greater than or equal to any of the above lower limits. 6-18 The monomer component of the alkyl ester.
[0048] In addition, from the viewpoint of improving the cohesiveness of the pressure-sensitive adhesive layer, (meth)acrylic acid C 4-18The proportion of the alkyl ester in the monomer component is usually 99.5% by mass or less, and can be 95% by mass or less, 85% by mass or less, or 75% by mass or less. The (meth)acrylic acid C may be contained in a proportion below any of the above upper limits. 6-18 The monomer component of the alkyl ester.
[0049] The monomer components constituting the (meth)acrylic polymer may include an alkyl (meth)acrylate and, if necessary, other monomers (copolymerizable monomers) copolymerizable with the alkyl (meth)acrylate.
[0050] As the copolymerizable monomer, a monomer having a polar group (for example, a carboxyl group, a hydroxyl group, a ring containing a nitrogen atom, etc.) or a monomer having a high glass transition temperature (for example, 10° C. or higher) of a homopolymer can be preferably used.
[0051] The monomer having a polar group can contribute to the introduction of crosslinking points into the (meth)acrylic polymer or to the improvement of the cohesive force of the adhesive. The copolymerizable monomers can be used alone or in combination of two or more.
[0052] Specific non-limiting examples of the copolymerizable monomer include the following monomers.
[0053] Monomers containing a carboxyl group include, for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.
[0054] Monomers containing anhydride groups: for example, maleic anhydride and itaconic anhydride.
[0055] Monomers containing hydroxyl groups: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate.
[0056] Monomers containing sulfonic acid groups or phosphoric acid groups: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, (meth)acrylate sulfopropyl ester, (meth)acryloyloxynaphthalenesulfonic acid, and 2-hydroxyethylacryloyl phosphate.
[0057] Epoxy group-containing monomers: For example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl glycidyl (meth)acrylate ether, allyl glycidyl ether, and glycidyl (meth)acrylate ether.
[0058] Monomers containing a cyano group: for example, acrylonitrile and methacrylonitrile.
[0059] Isocyanate group-containing monomer: for example, 2-isocyanateethyl (meth)acrylate, etc.
[0060] Monomers containing amide groups: for example, (meth)acrylamide; N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N,N-di(n-butyl) (meth)acrylamide, N,N-di(tert-butyl) (meth)acrylamide and the like N,N-dialkyl (meth)acrylamide; N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, N-n-butyl (meth)acrylamide and the like N-alkyl (meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinyl acetamide; Monomers having hydroxyl groups and amide groups, for example, N-(2-hydroxyethyl) (meth)acrylamide, The monomers include N-hydroxyalkyl (meth)acrylamide, N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, and N-(4-hydroxybutyl) (meth)acrylamide; monomers having an alkoxy group and an amide group, for example, N-alkoxyalkyl (meth)acrylamide, such as N-methoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; and N,N-dimethylaminopropyl (meth)acrylamide, and N-(meth)acryloyl morpholine.
[0061] Monomers containing amino groups include, for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and tert-butylaminoethyl (meth)acrylate.
[0062] Monomers having an epoxy group: for example, glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.
[0063] Monomers having a ring containing a nitrogen atom: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, and N-vinylpyridazine (for example, lactams such as N-vinyl-2-caprolactam) and the like.
[0064] Monomers having a succinimide skeleton include, for example, N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyhexamethylenesuccinimide.
[0065] Maleimides: for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide.
[0066] Itaconimides: for example, N-methyl itaconimide, N-ethyl itaconimide, N-butyl itaconimide, N-octyl itaconimide, N-2-ethylhexyl itaconimide, N-cyclohexyl itaconimide, and N-lauryl itaconimide.
[0067] Aminoalkyl (meth)acrylates: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate, and the like.
[0068] Alkoxy group-containing monomers: for example, alkoxyalkyl (meth)acrylates (alkoxyalkyl (meth)acrylates) such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; and alkoxyalkyl (meth)acrylates (e.g., alkoxypolyalkylene glycol (meth)acrylate) such as methoxyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate.
[0069] Monomers containing alkoxysilyl groups: for example, (meth)acrylates containing alkoxysilyl groups such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and vinyl compounds containing alkoxysilyl groups such as vinyltrimethoxysilane and vinyltriethoxysilane.
[0070] Vinyl esters: for example, vinyl acetate and vinyl propionate.
[0071] Vinyl ethers: For example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether.
[0072] Aromatic vinyl compounds: for example, styrene, α-methylstyrene, and vinyltoluene.
[0073] Olefins: for example, ethylene, butadiene, isoprene, and isobutylene.
[0074] (Meth)acrylates having an alicyclic hydrocarbon group: for example, (meth)acrylates having an alicyclic hydrocarbon group such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentyl (meth)acrylate, and adamantyl (meth)acrylate.
[0075] (Meth)acrylates having an aromatic hydrocarbon group: for example, (meth)acrylates having an aromatic hydrocarbon group such as phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, and benzyl (meth)acrylate.
[0076] In addition, (meth)acrylates containing heterocycles such as tetrahydrofurfuryl (meth)acrylate, (meth)acrylates containing halogen atoms such as (meth)acrylates containing vinyl chloride and fluorine atoms, (meth)acrylates containing silicon atoms such as silicone (meth)acrylate, and (meth)acrylates obtained from terpene compound derivative alcohols, etc.
[0077] When using such a copolymerizable monomer, its usage amount is not particularly limited, and it is usually appropriate to be 0.01 mass % or more of the overall monomer component. From the viewpoint of better exerting the use effect of the copolymerizable monomer, the usage amount of the copolymerizable monomer can be 0.1 mass % or more of the overall monomer component, and can be 0.5 mass % or more.
[0078] In addition, from the viewpoint of easily obtaining a balance in adhesive properties, the amount of the copolymerizable monomer used is usually appropriately 50% by mass or less, and preferably 40% by mass or less, based on the total monomer components.
[0079] In some embodiments, the monomer component constituting the (meth)acrylic polymer may include a monomer having a nitrogen atom. This can increase the cohesive force of the adhesive and satisfactorily improve the peeling force after a period of time.
[0080] A preferred example of the monomer having a nitrogen atom is a monomer having a ring containing a nitrogen atom. The monomer having a ring containing a nitrogen atom can be the monomers exemplified above, for example, N-vinyl cyclic amide represented by the following general formula (1).
[0081] [Chemical formula 1]
[0082]
[0083] Here, in the general formula (1), R 1 is a divalent organic group, specifically -(CH2) n -. n is an integer of 2 to 7 (preferably 2, 3 or 4). Among them, N-vinyl-2-pyrrolidone can be preferably used. Another preferred example of the monomer having a nitrogen atom is (meth)acrylamide.
[0084] The amount of the monomer having a nitrogen atom (preferably a monomer having a ring containing a nitrogen atom) used is not particularly limited, and may be, for example, 1% by mass or more, 3% by mass or more, 5% by mass or more, or 7% by mass or more of the total monomer component.
[0085] In one embodiment, the amount of the monomer having a nitrogen atom used may be 10% by mass or more, 15% by mass or more, or 20% by mass or more of the total monomer components.
[0086] The amount of the monomer having a nitrogen atom to be used is, for example, appropriately 40% by mass or less, and may be 35% by mass or less, 30% by mass or less, or 25% by mass or less of the total monomer components.
[0087] In another embodiment, the amount of the monomer having a nitrogen atom to be used may be, for example, 20% by mass or less, or 15% by mass or less, based on the total monomer components.
[0088] In some embodiments, the monomer components constituting the (meth)acrylic polymer may include a hydroxyl-containing monomer. By using a hydroxyl-containing monomer, the cohesive force of the adhesive and the degree of crosslinking (eg, crosslinking by an isocyanate crosslinking agent) can be appropriately adjusted.
[0089] The amount of hydroxyl-containing monomers used is not particularly limited, and may be, for example, 0.01% by mass or more, 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 5% by mass or more, or 10% by mass or more of the total monomer components.
[0090] In addition, from the perspective of suppressing the water absorption of the adhesive layer, in some embodiments, the amount of the hydroxyl-containing monomer used is appropriately 40% by mass or less of the total monomer component, for example, it can be 30% by mass or less, it can be 25% by mass or less, or it can be 20% by mass or less.
[0091] In another embodiment, the amount of the hydroxyl group-containing monomer used may be, for example, 15% by mass or less, 10% by mass or less, or 5% by mass or less of the total monomer components.
[0092] In the pressure-sensitive adhesive composition according to one embodiment of the present invention, the monomer component of the (meth)acrylic polymer may or may not contain the alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate exemplified above.
[0093] In one embodiment of the technology involved in the present embodiment, in the monomer components of the (meth)acrylic polymer, the ratio of alkoxyalkyl (meth)acrylate is less than 20% by mass, and the ratio of alkoxypolyalkylene glycol (meth)acrylate is less than 20% by mass. As a result, the adhesive layer can be easily formed into a sheet without gelation and other problems. By adopting the above monomer composition, the solid content concentration of the monomer mixture can be maintained within a specified range and the desired high molecular weight body (for example, a weight average molecular weight (Mw) of more than 30×10 4 , typically Mw is 40×10 4 above).
[0094] The proportion of the alkoxyalkyl (meth)acrylate in the above-mentioned monomer component is preferably less than 10% by mass, more preferably less than 3% by mass, and further preferably less than 1% by mass. In a particularly preferred embodiment, the above-mentioned monomer component does not substantially contain alkoxyalkyl (meth)acrylate (content 0 to 0.3% by mass).
[0095] Similarly, the proportion of alkoxypolyalkylene glycol (meth)acrylate in the above-mentioned monomer component is preferably less than 10% by mass, more preferably less than 3% by mass, and further preferably less than 1% by mass. In a particularly preferred embodiment, the above-mentioned monomer component does not substantially contain alkoxypolyalkylene glycol (meth)acrylate (content 0 to 0.3% by mass).
[0096] From the viewpoint of suppressing gelation, the total proportion of alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate in the monomer components of the (meth)acrylic polymer according to a preferred embodiment is limited to less than 20% by mass.
[0097] The total proportion of the alkoxyalkyl (meth)acrylate and the alkoxypolyalkylene glycol (meth)acrylate is more preferably less than 10% by mass, further preferably less than 3% by mass, and particularly preferably less than 1% by mass. In one embodiment, the monomer component does not substantially contain alkoxyalkyl (meth)acrylate and alkoxypolyalkylene glycol (meth)acrylate (content 0 to 0.3% by mass).
[0098] Similarly, the monomer component of the (meth)acrylic polymer involved in this embodiment may contain an alkoxy-containing monomer at a ratio of less than 20% by mass, or may not contain it. The amount of the alkoxy-containing monomer in the above-mentioned monomer component is preferably less than 10% by mass, more preferably less than 3% by mass, and further preferably less than 1% by mass. In a particularly preferred embodiment, the above-mentioned monomer component does not substantially contain an alkoxy-containing monomer (content 0 to 0.3% by mass).
[0099] In some embodiments, the proportion of carboxyl-containing monomers in the monomer components of the (meth)acrylic polymer can be, for example, 2% by mass or less, 1% by mass or less, or 0.5% by mass or less (e.g., less than 0.1% by mass). Carboxyl-containing monomers may also be substantially not used as monomer components of the (meth)acrylic polymer. Here, substantially not using carboxyl-containing monomers means at least not intentionally using carboxyl-containing monomers.
[0100] The (meth)acrylic polymer having such a composition is likely to be a polymer having high water resistance reliability and can also be a polymer having metal corrosion resistance to an adherend containing metal.
[0101] In addition, in a preferred embodiment, the proportion of hydrophilic monomers in the monomer components of the (meth)acrylic polymer is limited. Here, the "hydrophilic monomer" in this specification refers to a carboxyl group-containing monomer, an anhydride group-containing monomer, a hydroxyl group-containing monomer, a nitrogen atom-containing monomer (typically, an amide group-containing monomer such as (meth)acrylamide, and a nitrogen atom-containing ring monomer such as N-vinyl-2-pyrrolidone) and an alkoxy group-containing monomer (typically, an alkoxyalkyl (meth)acrylate and an alkoxypolyalkylene glycol (meth)acrylate).
[0102] In this embodiment, the ratio of the hydrophilic monomer in the monomer components of the (meth)acrylic polymer is preferably 32% by mass or less, for example, 30% by mass or less, or 28% by mass or less.
[0103] Although not particularly limited, the ratio of the hydrophilic monomer in the monomer components of the (meth)acrylic polymer may be 1% by mass or more, 10% by mass or more, or 20% by mass or more.
[0104] In some embodiments, the monomer component constituting the (meth)acrylic polymer may include an alicyclic hydrocarbon group-containing (meth)acrylate, which can improve the cohesive force of the pressure-sensitive adhesive and improve the peeling force after a certain period of time.
[0105] As the (meth)acrylate containing alicyclic hydrocarbon group, the substances exemplified above can be used, for example, cyclohexyl acrylate and isobornyl acrylate can be preferably used. The amount of (meth)acrylate containing alicyclic hydrocarbon group is not particularly limited, for example, it can be 1% by mass or more, 3% by mass or more, or 5% by mass or more of the total monomer component.
[0106] In one embodiment, the amount of the alicyclic hydrocarbon group-containing (meth)acrylate used may be 10% by mass or more, and may be 15% by mass or more, based on the total monomer components.
[0107] The upper limit of the amount of the alicyclic hydrocarbon group-containing (meth)acrylate used is appropriately 40 mass % or less, for example, 30 mass % or less, or 25 mass % or less (eg, 15 mass % or less, further 10 mass % or less).
[0108] The composition of the monomer components constituting the (meth)acrylic polymer can be set so that the glass transition temperature Tg determined by the Fox equation based on the composition of the monomer components is -75°C or higher and 10°C or lower.
[0109] In some embodiments, from the viewpoints of cohesion, impact resistance, etc., the Tg is suitably 0°C or lower, preferably -10°C or lower, and may be -20°C or lower or -30°C or lower.
[0110] The Tg may be, for example, -60°C or higher, -50°C or higher, -45°C or higher, or -40°C or higher.
[0111] Here, the FOX formula is a relationship formula of Tg of a copolymer and glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each monomer constituting the copolymer, as shown below.
[0112] 1 / Tg=Σ(Wi / Tgi)
[0113] It should be noted that, in the above Fox formula, Tg represents the glass transition temperature of the copolymer (unit: K), Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio based on weight), and Tgi represents the glass transition temperature of the homopolymer of monomer i (unit: K).
[0114] As the glass transition temperature of the homopolymer used for calculating Tg, the value described in the known document is used. For example, regarding the monomers listed below, the following values are used as the glass transition temperature of the homopolymer of the monomer.
[0115]
[0116]
[0117] Regarding the glass transition temperature of homopolymers of monomers other than those exemplified above, the values described in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989) were used. When a plurality of values were described in the document, the highest value was adopted.
[0118] For monomers whose homopolymer glass transition temperatures are not described in the above-mentioned Polymer Handbook, values obtained by the following measurement method are used (see Japanese Patent Application Laid-Open No. 2007-51271).
[0119] Specifically, 100 parts by mass of monomer, 0.2 parts by mass of azobisisobutyronitrile and 200 parts by mass of ethyl acetate as a polymerization solvent were added to a reactor equipped with a thermometer, a stirrer, a nitrogen inlet pipe and a reflux condenser, and stirred for 1 hour while nitrogen was circulated. After removing oxygen from the polymerization system in this way, the temperature was raised to 63°C and reacted for 10 hours. Then, it was cooled to room temperature to obtain a homopolymer solution having a solid content concentration of 33% by mass. Then, the homopolymer solution was cast on a release liner and dried to prepare a test sample (sheet-shaped homopolymer) having a thickness of about 2 mm. The test sample was punched into a disc with a diameter of 7.9 mm, sandwiched with parallel plates, and a viscoelasticity tester (ARES, manufactured by TA Instruments) was used to apply a shear strain with a frequency of 1 Hz. At the same time, the viscoelasticity was measured in a shear mode at a temperature range of -70 to 150°C at a heating rate of 5°C / minute, and the peak temperature of tanδ was used as the Tg of the homopolymer.
[0120] The (meth)acrylic acid-based polymer according to the present embodiment is not particularly limited, but preferably has an SP value of 23.0 (MJ / m 3 ) 1 / 2 The above SP value is more preferably 21.0 (MJ / m 3 ) 1 / 2 Below (e.g. 20.0(MJ / m 3 ) 1 / 2 the following).
[0121] The lower limit of the SP value is not particularly limited, but is, for example, 10.0 (MJ / m 3 )1 / 2 Above, 15.0 (MJ / m 3 ) 1 / 2 The above is appropriate, preferably 18.0 (MJ / m 3 ) 1 / 2 above.
[0122] It should be noted that the SP value of a (meth)acrylic polymer can be calculated according to the method of Fedors [see "Polymer Process and Technology (POLYMER ENG. & SCI.)", Vol. 14, No. 2 (1974), pp. 148-154], that is, the formula: SP value δ = (ΣΔe / ΣΔv) 1 / 2 to calculate.
[0123] (In the above formula, Δe is the evaporation energy Δe of each atom or atomic group at 25°C, and Δv is the molar volume of each atom or atomic group at the same temperature.)
[0124] The (meth)acrylic polymer having the above-mentioned SP value can be obtained by appropriately determining the monomer composition based on the technical common sense of those skilled in the art.
[0125] The pressure-sensitive adhesive composition contains the monomer components having the above-mentioned composition in the form of a polymer, an unpolymer (that is, a form in which the polymerizable functional group has not reacted), or a mixture thereof.
[0126] The above-mentioned adhesive composition can be in the following various forms: a water-dispersible adhesive composition in which the adhesive (adhesive component) is dispersed in water; a solvent-type adhesive composition in which the adhesive is contained in an organic solvent; an active energy ray-curable adhesive composition prepared by curing the adhesive by active energy rays such as ultraviolet rays and radiation; and a hot-melt adhesive composition that forms an adhesive when applied in a heated molten state and cooled to near room temperature, etc.
[0127] The adhesive composition according to a preferred embodiment is a solvent-based adhesive composition or a solvent-free adhesive composition. The solvent-free adhesive composition includes an active energy ray-curable adhesive composition and a hot melt adhesive composition.
[0128] When the polymerization is carried out, a known or customary thermal polymerization initiator or photopolymerization initiator may be used according to the polymerization method, polymerization mode, etc. Such polymerization initiators may be used alone or in combination of two or more.
[0129] The thermal polymerization initiator is not particularly limited, and for example, an azo polymerization initiator, a peroxide initiator, a redox initiator based on a combination of a peroxide and a reducing agent, and a substituted ethane initiator can be used.
[0130] More specifically, examples include azo initiators such as 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylpropionamidine) disulfate, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis(N,N'-dimethyleneisobutyramidine), and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate; persulfates such as potassium persulfate and ammonium persulfate; peroxide initiators such as benzoyl peroxide, tert-butyl hydroperoxide, and hydrogen peroxide; substituted ethane initiators such as phenyl-substituted ethane; redox initiators such as a combination of a persulfate and sodium bisulfite, a combination of a peroxide and sodium ascorbate; and the like, but the present invention is not limited to these. In addition, thermal polymerization can be suitably performed at a temperature of, for example, 20 to 100° C. (typically 40 to 80° C.).
[0131] The photopolymerization initiator is not particularly limited, and for example, ketal photopolymerization initiators, acetophenone photopolymerization initiators, benzoin ether photopolymerization initiators, acylphosphine oxide photopolymerization initiators, α-ketol photopolymerization initiators, aromatic sulfonyl chloride photopolymerization initiators, photoactive oxime photopolymerization initiators, benzoin photopolymerization initiators, benzyl photopolymerization initiators, benzophenone photopolymerization initiators, and thioxanthone photopolymerization initiators can be used.
[0132] The amount of such a thermal polymerization initiator or photopolymerization initiator used can be a normal amount used in accordance with the polymerization method, polymerization mode, etc., and is not particularly limited. For example, 0.001 to 5 parts by mass (typically 0.01 to 2 parts by mass, for example 0.01 to 1 part by mass) of polymerization initiator can be used relative to 100 parts by mass of the monomer to be polymerized.
[0133] In the above polymerization, various conventionally known chain transfer agents (which may also be considered as molecular weight modifiers or polymerization degree modifiers) may be used as necessary.
[0134] As the chain transfer agent, mercaptans such as n-dodecyl mercaptan, tert-dodecyl mercaptan, thioglycolic acid, and α-thioglycerol can be used. Alternatively, a chain transfer agent not containing a sulfur atom (non-sulfur chain transfer agent) can be used.
[0135] Specific examples of non-sulfur chain transfer agents include: anilines such as N,N-dimethylaniline and N,N-diethylaniline; terpenes such as α-pinene and terpinolene; styrenes such as α-methylstyrene and α-methylstyrene dimer; compounds having a benzylidene group such as dibenzylideneacetone, cinnamyl alcohol, and cinnamaldehyde; hydroquinones such as hydroquinone and dihydroxynaphthalene; quinones such as benzoquinone and naphthoquinone; olefins such as 2,3-dimethyl-2-butene and 1,5-cyclooctadiene; alcohols such as phenol, benzyl alcohol, and allyl alcohol; benzyl hydrogens such as diphenylbenzene and triphenylbenzene; and the like.
[0136] The chain transfer agent may be used alone or in combination of two or more.
[0137] When a chain transfer agent is used, the amount used may be, for example, 0.01 to 1 part by mass based on 100 parts by mass of the monomer component. The technique according to the present embodiment can be suitably implemented even in an embodiment in which a chain transfer agent is not used.
[0138] The molecular weight of the (meth)acrylic acid polymer obtained by appropriately adopting the above-mentioned various polymerization methods is not particularly limited and can be set within an appropriate range according to the required performance. The weight average molecular weight (Mw) of the (meth)acrylic acid polymer is generally 10×10 4 Above (e.g. 20×10 4 From the perspective of achieving both cohesive force and adhesive force in a well-balanced manner, more than 30 × 10 4 is appropriate.
[0139] From the viewpoint of obtaining good adhesive reliability even in a high temperature environment, the (meth)acrylic polymer according to one embodiment preferably has a 4 Above (typically 50×10 4 Above, for example, 55×10 4 According to a preferred embodiment of the technology involved in this embodiment, gelation can be suppressed by designing the monomer composition, so that a high molecular weight body in the above range can be obtained with good productivity by setting an appropriate solid content concentration.
[0140] The upper limit of the Mw of the (meth)acrylic acid-based polymer is usually 500×10 4 Below (for example, 150×10 4 The above Mw can be 75×10 4 the following.
[0141] Here, Mw refers to a value converted to standard polystyrene using gel permeation chromatography (GPC). As a GPC device, for example, a model name "HLC-8320GPC" (column: TSKgel GMH-H (S), manufactured by Tosoh Corporation) can be used. The same is true in the embodiments described later. The above Mw can be the Mw of the (meth) acrylic polymer in either the adhesive composition or the adhesive layer.
[0142] The adhesive composition of some embodiments may be an active energy ray-curable adhesive composition. Examples of the active energy rays include ultraviolet rays, visible rays, infrared rays, α rays, β rays, γ rays, electron rays, neutron rays, and radiation such as X-rays, and examples include energy rays having energy that can cause chemical reactions such as polymerization reactions, crosslinking reactions, and decomposition of initiators.
[0143] A preferred example of an active energy ray-curable adhesive composition is a photocurable adhesive composition. A photocurable adhesive composition has the following advantages: even a thick adhesive layer can be easily formed. Among them, an ultraviolet-curable adhesive composition is preferred.
[0144] Typically, the photocurable adhesive composition contains at least a portion of the monomer components of the composition in the form of a polymer (it may be a portion of the monomer types or a portion of the amount).
[0145] The polymerization method for forming the above-mentioned polymer is not particularly limited, and various polymerization methods known in the past can be appropriately used. For example, thermal polymerization such as solution polymerization, emulsion polymerization, and bulk polymerization (typically, carried out in the presence of a thermal polymerization initiator); photopolymerization by irradiation with light such as ultraviolet rays (typically, carried out in the presence of a photopolymerization initiator); radiation polymerization by irradiation with radiation such as β rays and γ rays; etc. Among them, photopolymerization is preferred.
[0146] A preferred embodiment of the photocurable adhesive composition includes a partial polymer of a monomer component. Such a partial polymer is typically a mixture of a polymer derived from a monomer component and an unreacted monomer, and preferably presents a slurry (viscous liquid). Hereinafter, the partial polymer of this property is sometimes referred to as "monomer slurry" or simply "slurry".
[0147] The polymerization method when making the monomer component partially polymerized is not particularly limited, and various polymerization methods such as those mentioned above can be appropriately selected and used. From the viewpoint of efficiency and simplicity, photopolymerization can be preferably adopted. According to photopolymerization, the polymerization conversion rate (monomer conversion) of the monomer component can be easily controlled by polymerization conditions such as the irradiation amount of light (amount of light).
[0148] The polymerization conversion rate of the monomer mixture in the above-mentioned partial polymer is not particularly limited. The above-mentioned polymerization conversion rate can be, for example, 70% by mass or less, preferably 60% by mass or less. From the viewpoints of ease of preparation and coating properties of the adhesive composition containing the above-mentioned partial polymer, it is usually appropriate for the above-mentioned polymerization conversion rate to be 50% by mass or less, preferably 40% by mass or less (for example, 35% by mass or less).
[0149] The lower limit of the polymerization conversion rate is not particularly limited, but is typically 1% by mass or more, and usually 5% by mass or more is appropriate.
[0150] The adhesive composition containing a partial polymer of monomer components can be obtained, for example, by partially polymerizing a monomer mixture containing all monomer components used for preparing the adhesive composition by an appropriate polymerization method (eg, photopolymerization).
[0151] In addition, the adhesive composition comprising a partial polymer of a monomer component may be a mixture of a partial polymer or a complete polymer of a monomer mixture comprising a part of a monomer component (which is a monomer component used in the preparation of the adhesive composition) and a mixture of the remaining monomer component or a partial polymer thereof. It should be noted that in this specification, the so-called "complete polymer" refers to a polymerization conversion rate exceeding 95% by mass.
[0152] <Oligomer>
[0153] The adhesive composition related to one embodiment of the present invention may include at least one oligomer. The oligomer in one embodiment of the present invention is obtained by polymerizing a monomer composition containing at least one vinyl monomer having at least one pigment structure on the side chain. That is, the oligomer contains at least one vinyl monomer having at least one pigment structure on the side chain as a monomer unit.
[0154] The adhesive composition according to one embodiment of the present invention uses an oligomer including a vinyl monomer having a pigment structure in a side chain as a pigment component, thereby avoiding the problems of poor dispersibility and pigment bleeding when using pigments and dyes.
[0155] As the vinyl monomer having at least one pigment structure on the side chain, there can be mentioned (meth) acrylic monomers, aromatic vinyl monomers, aliphatic hydrocarbon monomers, etc. From the viewpoint of good compatibility with the (meth) acrylic base polymer and maintaining transparency, preferably (meth) acrylic monomers can be mentioned.
[0156] There are no particular restrictions on the (meth)acrylic acid monomer. For example, the various (meth)acrylic acid C 1-20Alkyl esters; the above-mentioned various alicyclic hydrocarbon group-containing (meth)acrylates; the above-mentioned various aromatic hydrocarbon group-containing (meth)acrylates; (meth)acrylate monomers such as (meth)acrylates obtained from terpene compound derivative alcohols. These can be used alone or in combination of two or more.
[0157] The aromatic vinyl monomer is not particularly limited, and examples thereof include styrene monomers such as styrene, chlorostyrene, chloromethylstyrene, and α-methylstyrene. These monomers may be used alone or in combination of two or more.
[0158] The aliphatic hydrocarbon monomer is not particularly limited, and examples thereof include olefin monomers and diene monomers, and these may be used alone or in combination of two or more.
[0159] As oligomer in one embodiment of the present invention, other monomers except the vinyl monomer with at least one pigment structure on the above-mentioned side chain can be included.As this monomer, there is no particular restriction as mentioned above.For example, (methyl) acrylic acid monomer, aromatic vinyl monomer and aliphatic hydrocarbon monomer etc. can be enumerated.
[0160] In the oligomer according to one embodiment of the present invention, the vinyl monomer having at least one dye structure in the side chain is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the oligomer.
[0161] From the viewpoint of compatibility with the base polymer, the amount is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 70 parts by mass or less.
[0162] As the oligomer in one embodiment of the present invention, a (meth)acrylic oligomer is preferred.
[0163] The (meth)acrylic oligomer may be a homopolymer of a (meth)acrylic monomer having at least one pigment structure in a side chain.
[0164] In addition, the (meth)acrylic oligomer may be a copolymer of a "vinyl monomer having at least one pigment structure on a side chain" and a "monomer other than the vinyl monomer having at least one pigment structure on a side chain". In this case, the monomer corresponding to the (meth)acrylic monomer is preferably 50% by mass or more of the total amount of the "vinyl monomer having at least one pigment structure on a side chain" and the "monomer other than the vinyl monomer having at least one pigment structure on a side chain". More preferably, it is 70% by mass or more, and even more preferably, 80% by mass or more.
[0165] The above-mentioned "monomer other than a vinyl monomer having at least one colorant structure in a side chain" is preferably a "(meth)acrylic monomer having no colorant structure in a side chain", and more preferably a "(meth)acrylic acid alkyl ester having no colorant structure in a side chain".
[0166] When the (meth)acrylic oligomer is a copolymer of a "vinyl monomer having at least one pigment structure on the side chain" and a "monomer other than the vinyl monomer having at least one pigment structure on the side chain", a preferred combination is a combination of a "(meth)acrylic monomer having at least one pigment structure on the side chain" and a "(meth)acrylic monomer not having a pigment structure on the side chain". A more preferred combination is a combination of a "(meth)acrylic monomer having at least one pigment structure on the side chain" and an "alkyl (meth)acrylate not having a pigment structure on the side chain".
[0167] The (meth)acrylic monomer and the (meth)acrylic acid alkyl ester mentioned above can be used.
[0168] In addition, from the viewpoint of improving adhesion, the (meth)acrylic oligomer preferably contains as a monomer unit a (meth)acrylic monomer having a relatively bulky structure, such as (meth)acrylic acid alkyl esters having a branched alkyl group such as isobutyl (meth)acrylate and tert-butyl (meth)acrylate, (meth)acrylic acid esters containing an alicyclic hydrocarbon group, and (meth)acrylic acid esters containing an aromatic hydrocarbon group.
[0169] In addition, when ultraviolet rays are used when synthesizing (meth)acrylic oligomers or preparing adhesive layers, monomers having a saturated hydrocarbon group at the ester terminal are preferred from the perspective of being less likely to cause polymerization inhibition. For example, (meth)acrylic acid alkyl esters having a branched alkyl group and (meth)acrylic acid esters containing a saturated alicyclic hydrocarbon group can be preferably used.
[0170] As a monomer component constituting the (meth)acrylic oligomer, in addition to the above-mentioned (meth)acrylic monomer, a monomer having a functional group may be used as necessary.
[0171] Examples of monomers containing functional groups include: monomers having a heterocyclic ring containing a nitrogen atom, such as N-vinyl-2-pyrrolidone and N-acryloylmorpholine; monomers containing an amino group, such as N,N-dimethylaminoethyl (meth)acrylate; monomers containing an amide group, such as N,N-diethyl (meth)acrylamide; monomers containing a carboxyl group, such as AA and MAA; and monomers containing a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate.
[0172] The above-mentioned monomer containing a functional group can be used alone or in combination of two or more. When a monomer containing a functional group is used, the proportion of the monomer containing a functional group in the total monomer components constituting the (meth) acrylic acid oligomer can be, for example, 1% by mass or more, 2% by mass or more, or 3% by mass or more. In addition, the proportion of the above-mentioned monomer containing a functional group can be, for example, 15% by mass or less, 10% by mass or less, or 7% by mass or less.
[0173] The pigment structure of the oligomer in one embodiment of the present invention in one molecule can be the same pigment structure or different pigment structures. It should be noted that in one embodiment of the present invention, the so-called different pigment structures include not only pigment structures with different pigment skeletons, but also pigment structures with the same pigment skeleton but different types of substituents bonded to the pigment skeleton.
[0174] It should be noted that, in one embodiment of the present invention, the pigment structure refers to a structure derived from a pigment compound, and for example, a structure obtained by removing one or more arbitrary atoms possessed by the pigment compound.
[0175] The type of pigment structure is not particularly limited and can be appropriately selected according to the purpose. The pigment structure can be a structure from a pigment compound having absorption in the visible light region (preferably a wavelength of 400 to 700 nm, more preferably a scope of 400 to 650 nm). In addition, it can be a structure from a pigment compound having absorption in the infrared region (preferably a compound having a maximum absorption wavelength in the scope of 700 to 1200 nm).
[0176] Among them, a structure derived from a pigment compound having absorption in the visible light region is preferred.
[0177] Examples of the pigment structure include a triarylmethane pigment structure, a xanthene pigment structure, an anthraquinone pigment structure, a cyanine pigment structure, a squarylium pigment structure, a quinophthalone pigment structure, a phthalocyanine pigment structure, a subphthalocyanine pigment structure, an azo pigment structure, a pyrazolotriazole pigment structure, a dipyrromethene pigment structure, an isoindoline pigment structure, a thiazole pigment structure, a benzimidazolone pigment structure, a pyrene pigment structure, a pyrrolopyrrole pigment structure, a pyrrolopyrrole dione pigment structure, a diimmonium pigment structure, a naphthalocyanine pigment structure, a rylene pigment structure, a dibenzofuranone pigment structure, a merocyanine pigment structure, a crotonium pigment structure, and an oxonol pigment structure.
[0178] Among them, a triarylmethane dye structure, a xanthene dye structure, and a cyanine dye structure are preferred.
[0179] The vinyl monomer in one embodiment of the present invention may have at least one of the above-mentioned pigment structures in a side chain.
[0180] The oligomer in one embodiment of the present invention can be formed by polymerizing a monomer composition containing at least a vinyl monomer having at least one pigment structure on the side chain. The polymerization method and polymerization mode are not particularly limited, and various polymerization methods known in the past (for example, solution polymerization, emulsion polymerization, bulk polymerization, photopolymerization, and radiation polymerization, etc.) can be used in an appropriate manner.
[0181] The types of polymerization initiators (e.g., azo polymerization initiators) that can be used as needed are generally as exemplified for the synthesis of (meth)acrylic polymers. The amount of polymerization initiators and the amount of chain transfer agents (e.g., mercaptans such as n-dodecyl mercaptan (NDM)) that can be used optionally are appropriately set based on common technical knowledge to obtain a desired molecular weight, and thus detailed descriptions thereof are omitted.
[0182] From the viewpoint of compatibility with the base polymer, the weight average molecular weight (Mw) of the oligomer in one embodiment of the present invention is preferably 1,000 to 50,000. The weight average molecular weight (Mw) is more preferably 2,000 or more, and further preferably 3,000 or more. In addition, the weight average molecular weight (Mw) is more preferably 25,000 or less, and further preferably 10,000 or less.
[0183] The weight average molecular weight (Mw) herein refers to a value converted to standard polystyrene using gel permeation chromatography (GPC). As a GPC device, for example, a machine model "HLC-8320GPC" (column: TSKgel GMH-H (S), manufactured by Tosoh Corporation) can be used. The same is true in the embodiments described later. The above-mentioned Mw can be the Mw of an oligomer in either the adhesive composition or the adhesive layer.
[0184] In addition, from the viewpoint of good compatibility, the combination of the base polymer and the oligomer in one embodiment of the present invention is preferably a combination of a (meth)acrylic polymer and a (meth)acrylic oligomer.
[0185] The pressure-sensitive adhesive composition according to one embodiment of the present invention preferably contains 0.01 parts by mass or more of the oligomer, more preferably 1 part by mass or more, and even more preferably 5 parts by mass or more, based on 100 parts by mass of the base polymer, from the viewpoint of colorability.
[0186] From the viewpoint of the influence on physical properties such as adhesive strength, the content of the oligomer is usually appropriately 100 parts by mass or less, preferably 90 parts by mass or less, and more preferably 80 parts by mass or less.
[0187] (Other ingredients)
[0188] The adhesive composition to which one embodiment of the present invention relates may include various additives commonly used in the field of adhesive compositions such as tackifier resins (e.g., rosin-based, petroleum-based, terpene-based, phenol-based, and ketone-based tackifier resins), viscosity modifiers (e.g., thickeners), leveling agents, plasticizers, fillers, stabilizers, preservatives, and anti-aging agents as other optional components as needed within the scope of not hindering the effect of the present invention. Regarding such various additives, conventionally known substances may be used, and since no special features are given to the present invention, detailed description is omitted.
[0189] It should be noted that the technology involved in this embodiment can exert good adhesive force without using the above-mentioned tackifier resin. Therefore, the content of the above-mentioned tackifier resin in the adhesive composition can be less than 10 parts by mass, and further can be less than 5 parts by mass relative to 100 parts by mass of the base polymer.
[0190] The content of the tackifier resin may be less than 1 part by mass (eg, less than 0.5 part by mass), or less than 0.1 part by mass (0 part by mass or more and less than 0.1 part by mass), and the adhesive composition may not contain the tackifier resin.
[0191] In the pressure-sensitive adhesive composition according to one embodiment of the present invention, from the viewpoint of improving transparency and achieving remarkable coloration with a pigment, it is preferred that the amount of components other than the base polymer in the pressure-sensitive adhesive composition be limited.
[0192] In the technology according to this aspect, the amount of components other than the base polymer in the PSA composition is usually 30% by mass or less, preferably 15% by mass or less, and preferably 12% by mass or less (eg, 10% by mass or less).
[0193] The amount of components other than the base polymer in the adhesive composition of one embodiment can be 5% by mass or less, can be 3% by mass or less, can be 1.5% by mass or less (e.g., 1% by mass or less). Such a composition in which the amount of components other than the base polymer is limited can be preferably used in the adhesive composition of this embodiment.
[0194] <Adhesive layer>
[0195] The pressure-sensitive adhesive layer according to one embodiment of the present invention is formed from the above-mentioned pressure-sensitive adhesive composition. Figure 1 A schematic cross-sectional view showing a configuration example of the adhesive layer 11 is shown.
[0196] The above-mentioned adhesive layer can be a cured layer of an adhesive composition. That is, the adhesive layer can be formed in the following manner: after the adhesive composition is imparted (e.g., applied) to an appropriate surface, a curing treatment is appropriately implemented. In the case of carrying out two or more curing treatments (drying, crosslinking, and polymerization, etc.), they can be carried out simultaneously or in multiple stages.
[0197] In the adhesive composition using the partially polymerized product (polymer syrup) of the monomer components, a final copolymerization reaction is typically performed as the above-mentioned curing treatment. That is, the partially polymerized product is subjected to a further copolymerization reaction to form a fully polymerized product.
[0198] For example, in the case of a light-curable adhesive composition, light irradiation is performed, and curing treatment such as crosslinking and drying may be performed as necessary.
[0199] For example, when the photocurable adhesive composition needs to be dried (for example, in the case of a photocurable adhesive composition in the form of a partial polymer of a monomer component dissolved in an organic solvent), the composition may be dried and then photocured.
[0200] In the adhesive composition using a complete polymer, typically, as the above-mentioned curing treatment, drying (heat drying), crosslinking and other treatments are carried out as needed. In the case of a solvent-based adhesive composition that is imparted with photocurability (photocrosslinkability) by the addition of a multifunctional monomer, photocuring can be performed after drying the composition.
[0201] Here, the term "after drying the composition" means after the drying of the adhesive sheet described below is applied to an adherend. The adhesive sheet described below can be used by applying the adhesive sheet to the adherend using a method including the step of photocuring the adhesive sheet after applying the adhesive sheet to the adherend.
[0202] The adhesive layer of a multilayer structure of two or more layers can be produced by laminating preformed adhesive layers. Alternatively, an adhesive composition can be applied on a preformed first adhesive layer and the adhesive composition can be cured to form a second adhesive layer.
[0203] When the adhesive layer of the adhesive sheet described below used in a pasting manner by being attached to an adherend and then photocured has a multilayer structure, the adhesive layer to be photocured may be a partial layer (e.g., one layer) or all layers included in the multilayer structure.
[0204] The adhesive composition can be applied using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, or a spray coater.
[0205] In the case of a PSA sheet having a substrate as described below, as a method for providing a PSA layer on the substrate, a direct method of directly applying a PSA composition to the substrate to form the PSA layer or a transfer method of transferring the PSA layer formed on the release surface to the substrate can be used.
[0206] The thickness of the adhesive layer is not particularly limited, and may be, for example, 3 μm to 2000 μm.
[0207] From the perspective of step tracking and adhesion to the adherend, in some embodiments, the thickness of the adhesive layer can be, for example, 5 μm or more, 10 μm or more is appropriate, preferably 20 μm or more, and more preferably 30 μm or more. The thickness of the adhesive layer can be 50 μm or more, can exceed 50 μm, can be 70 μm or more, can be 100 μm or more, and can be 120 μm or more.
[0208] In addition, from the perspective of preventing the occurrence of slurry residue due to cohesive failure of the adhesive layer, in some embodiments, the thickness of the adhesive layer can be, for example, 1000 μm or less, 700 μm or less, 500 μm or less, 300 μm or less, 200 μm or less, or 170 μm or less. As for the technology involved in this embodiment, it can also be appropriately implemented in the form of the adhesive sheet described later with a thickness of the adhesive layer of 130 μm or less, 90 μm or less, 60 μm or less (for example, 40 μm or less).
[0209] In a PSA sheet having a multilayer structure of two or more PSA layers described below, the thickness of the PSA layer refers to the thickness from the adhesive surface to be attached to an adherend to the surface opposite to the adhesive surface.
[0210] <Adhesive Sheet>
[0211] The adhesive sheet involved in one embodiment of the present invention has the above-mentioned adhesive layer. The adhesive sheet of one embodiment of the present invention can be an adhesive sheet with a substrate in the form of an adhesive layer on one or both sides of a sheet-like substrate (support), or an adhesive sheet without a substrate in the form of an adhesive layer being retained on a release sheet. The concept of the so-called adhesive sheet here may include items such as adhesive tapes, adhesive labels, and adhesive films.
[0212] It should be noted that, typically, the adhesive layer is continuously formed, but is not limited to this form, for example, it can also be an adhesive layer forming regular or irregular patterns such as dot-shaped and striped. In addition, the adhesive sheet of one embodiment of the present invention can be in a roll or in a single sheet. Alternatively, it can also be an adhesive sheet further processed into a form of various shapes.
[0213] (Base material)
[0214] The PSA sheet according to some embodiments may be in the form of a PSA sheet with a substrate (the PSA sheet includes a substrate bonded to the other back surface of the PSA layer). Figure 2 A schematic cross-sectional view showing a configuration example in which a pressure-sensitive adhesive layer is formed on one surface of a substrate in a pressure-sensitive adhesive sheet according to one embodiment of the present invention.
[0215] Figure 2 The adhesive sheet 1 shown includes a substrate 21 and an adhesive layer 11 formed on one surface of the substrate. Figure 3 A schematic cross-sectional view showing a configuration example in which adhesive layers are formed on both surfaces of a substrate 21 . Figure 3 The illustrated pressure-sensitive adhesive sheet 2 includes a substrate 21 , and a first pressure-sensitive adhesive layer 11 and a second pressure-sensitive adhesive layer 12 formed on both surfaces of the substrate.
[0216] The material of the substrate is not particularly limited and can be appropriately selected depending on the intended use and form of use of the pressure-sensitive adhesive sheet, etc. A transparent film is preferred.
[0217] As non-limiting examples of the substrate that can be used, there can be mentioned: polyolefin films with polyolefins such as polypropylene and ethylene-propylene copolymer as the main component, polyester films with polyesters such as polyethylene terephthalate and polybutylene terephthalate as the main component, polyvinyl chloride films with polyvinyl chloride as the main component, and other plastic films; foam sheets formed by foams such as polyurethane foam, polyethylene foam, and polychloroprene foam; fabrics and nonwoven fabrics formed by various fibrous materials (which may be natural fibers such as hemp and cotton, synthetic fibers such as polyester and vinylon, and semi-synthetic fibers such as acetate, etc.) alone or in a blend; Japanese paper, high-quality paper, kraft paper, crepe paper, and other paper; aluminum foil, copper foil, and other metal foils; etc. The substrate may be a composite of these.
[0218] Examples of such a composite structure substrate include a substrate having a structure in which a metal foil and the above-mentioned plastic film are laminated, and a plastic sheet reinforced with inorganic fibers such as glass cloth.
[0219] As the substrate of the adhesive sheet involved in one embodiment of the present invention, various films (hereinafter also referred to as support films) can be preferably used. The support film can be a porous film such as a foam film, a non-woven fabric sheet, etc., or a non-porous film, or a film having a structure of a porous layer and a non-porous layer stacked.
[0220] In some aspects, as the support film, a film including a resin film capable of independently maintaining a shape (self-supporting or independent) as a base film can be preferably used.
[0221] The so-called "resin film" herein is a non-porous structure, and typically refers to a resin film that does not contain bubbles (non-porous) in substance. Therefore, the above-mentioned resin film is a concept distinguished from foam film and non-woven fabric. The above-mentioned resin film can be a single-layer structure, or a multi-layer structure (e.g., a three-layer structure) of more than two layers.
[0222] As the resin material constituting the resin film, for example, polyester, polyolefin, polycycloolefin derived from a monomer having an aliphatic ring structure such as a norbornene structure, nylon 6, nylon 66, and partially aromatic polyamides such as polyamide (PA), polyimide (PI), polyamideimide (PAI), polyetheretherketone (PEEK), polyethersulfone (PES), polyphenylene sulfide (PPS), polycarbonate (PC), polyurethane (PU), ethylene-vinyl acetate copolymer (EVA), polystyrene, polyvinyl chloride, polyvinylidene chloride, and polytetrafluoroethylene (PTFE) and other fluororesins, acrylic resins such as polymethyl methacrylate, cellulose polymers such as cellulose diacetate and cellulose triacetate, vinyl butyral polymers, acrylate polymers, polyoxymethylene polymers, and epoxy polymers can be used.
[0223] The resin film may be formed using a resin material containing one type of such resin alone or a resin material obtained by blending two or more types of such resin. The resin film may be unstretched or stretched (eg, uniaxially stretched or biaxially stretched).
[0224] Preferred examples of the resin material constituting the resin film include polyester resins, PPS resins, and polyolefin resins. Here, the so-called polyester resin refers to a resin containing polyester at a ratio exceeding 50% by mass. Similarly, PPS resin refers to a resin containing PPS at a ratio exceeding 50% by mass, and polyolefin resin refers to a resin containing polyolefin at a ratio exceeding 50% by mass.
[0225] As the polyester resin, typically, a polyester resin containing a polyester obtained by polycondensation of a dicarboxylic acid and a diol as a main component can be used. Specific examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polybutylene naphthalate.
[0226] As the polyolefin resin, one polyolefin may be used alone or two or more polyolefins may be used in combination. The polyolefin may be, for example, a homopolymer of α-olefin, a copolymer of two or more α-olefins, or a copolymer of one or more α-olefins and other vinyl monomers.
[0227] Specific examples include polyethylene (PE), polypropylene (PP), poly-1-butene, poly-4-methyl-1-pentene, and ethylene-propylene copolymers such as ethylene propylene rubber (EPR), ethylene-propylene-butene copolymers, ethylene-butene copolymers, ethylene-vinyl alcohol copolymers, and ethylene-ethyl acrylate copolymers. Any of low-density (LD) polyolefins and high-density (HD) polyolefins can be used.
[0228] Examples of polyolefin resin films include unstretched polypropylene (CPP) films, biaxially stretched polypropylene (OPP) films, low-density polyethylene (LDPE) films, linear low-density polyethylene (LLDPE) films, medium-density polyethylene (MDPE) films, high-density polyethylene (HDPE) films, polyethylene (PE) films obtained by blending two or more polyethylene (PE), and PP / PE blended films obtained by blending polypropylene (PP) and polyethylene (PE).
[0229] Specific examples of the resin film that can be preferably used as the substrate include a PET film, a PEN film, a PPS film, a PEEK film, a CPP film, and an OPP film.
[0230] From the viewpoint of strength, preferred examples include PET film, PEN film, PPS film, and PEEK film. From the viewpoint of availability, dimensional stability, and optical properties, preferred examples include PET film.
[0231] The resin film may be mixed with known additives such as light stabilizers, antioxidants, antistatic agents, colorants (dyes, pigments, etc.), fillers, slip agents, and anti-blocking agents as needed. The amount of the additives is not particularly limited and can be appropriately set according to the purpose of the adhesive sheet.
[0232] The method for producing the resin film is not particularly limited, and for example, conventionally known general resin film forming methods such as extrusion molding, inflation molding, T-die casting, and calendar roll molding can be appropriately adopted.
[0233] The substrate may be substantially composed of such a resin film. Alternatively, the substrate may include an auxiliary layer in addition to the resin film.
[0234] Examples of the auxiliary layer include an optical property adjustment layer (e.g., an antireflection layer), a printed layer for imparting a desired appearance to the substrate or adhesive sheet, a laminate layer, an antistatic layer, a primer layer, and a surface treatment layer such as a peeling layer. In addition, the substrate may be an optical component described below.
[0235] The thickness of the substrate is not particularly limited and can be selected according to the purpose of use of the adhesive sheet, the mode of use, etc. The thickness of the substrate can be, for example, 1000 μm or less, 500 μm or less, 100 μm or less, 70 μm or less, 50 μm or less, 25 μm or less, 10 μm or less, or 5 μm or less.
[0236] When the thickness of the substrate is small, there is a tendency that the softness of the adhesive sheet and the ability to follow the surface shape of the adherend are improved. In addition, from the perspectives of operability and processability, the thickness of the substrate can be, for example, 2 μm or more, more than 5 μm or more than 10 μm. In some embodiments, the thickness of the substrate can be, for example, 20 μm or more, more than 35 μm or more, or more than 55 μm.
[0237] The surface of the substrate to be bonded to the adhesive layer may be subjected to conventionally known surface treatments such as corona discharge treatment, plasma treatment, ultraviolet irradiation treatment, acid treatment, alkali treatment, application of a primer, and antistatic treatment, as required.
[0238] Such surface treatment may be a treatment for improving the adhesion between the substrate and the adhesive layer, in other words, the anchoring property of the adhesive layer to the substrate. The composition of the primer is not particularly limited and may be appropriately selected from known ones.
[0239] The thickness of the primer layer is not particularly limited, but is usually appropriately 0.01 μm to 1 μm, preferably 0.1 μm to 1 μm.
[0240] The surface of the substrate opposite to the side bonded to the pressure-sensitive adhesive layer (hereinafter also referred to as the back side) may be subjected to conventionally known surface treatments such as release treatment, treatment to improve adhesion or tackiness, and antistatic treatment, as required.
[0241] For example, by treating the back side of the substrate with a release agent, the unwinding force of the adhesive sheet wound into a roll can be reduced. As the release agent, silicone-based release agents, long-chain alkyl-based release agents, olefin-based release agents, fluorine-based release agents, fatty acid amide-based release agents, molybdenum sulfide, and silica powder can be used.
[0242] (Release liner)
[0243] In the pressure-sensitive adhesive sheet according to one embodiment of the present invention, the pressure-sensitive adhesive layer may be protected by a release liner (separator, release film) until use.
[0244] As the release liner, conventional release paper or the like can be used without particular limitation. For example, a substrate having a release treatment layer, a low-adhesive substrate formed of a fluorine-based polymer, a low-adhesive substrate formed of a nonpolar polymer, etc. can be used.
[0245] Examples of the substrate having a release treatment layer include plastic films and paper that have been surface-treated with a release treatment agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide-based release treatment agent.
[0246] Examples of the fluorine-based polymer of the low-adhesive substrate include polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinyl fluoride, polyvinylidene fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, and chlorofluoroethylene-vinylidene fluoride copolymer.
[0247] As the non-polar polymer of the low adhesive substrate formed by the non-polar polymer, for example, olefin resins (for example, polyethylene, polypropylene, etc.) can be cited. It should be noted that the release liner can be formed by a known or conventional method. In addition, the thickness of the release liner is not particularly limited.
[0248] In the technology involved in this embodiment, the haze value of the adhesive sheet is appropriately 10% or less, and can be 5% or less (for example, 3% or less). The above haze value is preferably 1.0% or less. Considering that the appearance changes significantly when discolored or colored in one embodiment of the present invention, such an adhesive sheet with high transparency is preferred.
[0249] The haze value of the PSA sheet may be less than 1.0%, less than 0.7%, or less than 0.5% (eg, 0 to 0.5%). These haze values related to the PSA sheet can also be well applied to the haze values of the PSA layer in the technology according to this embodiment.
[0250] The "haze value" here refers to the ratio of diffuse transmitted light to total transmitted light when the object to be measured is irradiated with visible light. It is also called haze value. The haze value can be expressed by the following formula.
[0251] Th[%]=Td / Tt×100
[0252] In the above formula, Th is the haze value [%], Td is the scattered light transmittance, and Tt is the total light transmittance. The haze value can be measured by the method described in the examples described below. The haze value can be adjusted by selecting the composition and thickness of the adhesive layer, for example.
[0253] The technology according to this aspect can be preferably used in, for example, electronic parts, optical parts, and building parts.
[0254] Example
[0255] Hereinafter, embodiments of the present invention will be described in detail using examples.
[0256] <Preparation of Adhesive Composition>
[0257] [Preparation of adhesive solution]
[0258] (Binder solution A1)
[0259] Into a reaction container equipped with a condenser, a nitrogen inlet pipe, a thermometer and a stirring device, 97 parts by mass of n-butyl acrylate (BA), 2 parts by mass of acrylic acid (AA), 1 part by mass of 4-hydroxybutyl acrylate (4HBA) as monomer components, and 122 parts by mass of ethyl acetate as a polymerization solvent were added, and 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator was added, and solution polymerization was carried out under a nitrogen atmosphere, thereby obtaining an adhesive solution A1 containing a (meth)acrylic polymer with a Mw of 700,000.
[0260] (Binder solution A2)
[0261] Binder solution A2 having a Mw of 650,000 was prepared in the same manner as in the preparation of binder solution A1 except that the monomer components were 95 parts by mass of n-butyl acrylate (BA), 5 parts by mass of acrylic acid (AA), and 0 parts by mass of 4-hydroxybutyl acrylate (4HBA).
[0262] (Binder solution A3)
[0263] Binder solution A3 having a Mw of 600,000 was prepared in the same manner as in the preparation of binder solution A1 except that the monomer components were 95 parts by mass of n-butyl acrylate (BA), 0 parts by mass of acrylic acid (AA), and 5 parts by mass of 4-hydroxybutyl acrylate (4HBA).
[0264] The formulations of the above-mentioned adhesive solutions are summarized in Table 1 below.
[0265] [Table 1]
[0266] Table 1
[0267]
[0268] 〔Preparation of dye oligomer solution〕
[0269] (Dye oligomer solution B1)
[0270] Into a reaction container equipped with a condenser, a nitrogen inlet pipe, a thermometer and a stirring device, 90 parts by mass of n-butyl acrylate (BA) as a monomer component, 10 parts by mass of a blue polymerizable dye RDW-B01 (manufactured by Fuji Film and Wako Pure Chemical Industries, Ltd.) which is a vinyl monomer having a pigment structure on the side chain, 5 parts by mass of n-dodecyl mercaptan (NDM) as a chain transfer agent, and 122 parts by mass of ethyl acetate as a polymerization solvent were added, and 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a thermal polymerization initiator was added, and solution polymerization was carried out under a nitrogen atmosphere, thereby obtaining a dye oligomer solution B1 containing a (meth)acrylic blue dye oligomer having a Mw of 5,000.
[0271] (Dye oligomer solution B2)
[0272] A dye oligomer solution B2 having a Mw of 5,000 was obtained in the same manner as in the preparation of the dye oligomer B1 except that 10 parts by mass of RDW-Y02 (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) which is a yellow polymerizable dye was used.
[0273] (Dye oligomer solution B3)
[0274] A dye oligomer solution B3 having a Mw of 1,300 was obtained in the same manner as in the preparation of the dye oligomer B1 except that the amount of n-dodecyl mercaptan (NDM) used was 20 parts by mass based on 100 parts by mass of the above monomer components.
[0275] (Dye oligomer solution B4)
[0276] A dye oligomer solution B4 having a Mw of 48,000 was obtained in the same manner as in the preparation of the dye oligomer B1 except that the amount of n-dodecyl mercaptan (NDM) used was 0.1 parts by mass based on 100 parts by mass of the above monomer components.
[0277] (Dye oligomer solution B5)
[0278] A dye oligomer solution B5 having a Mw of 600 was obtained in the same manner as in the preparation of the dye oligomer B1 except that the amount of n-dodecyl mercaptan (NDM) used was 30 parts by mass based on 100 parts by mass of the above monomer components.
[0279] (Dye oligomer solution B6)
[0280] A dye oligomer solution B6 having a Mw of 120,000 was obtained in the same manner as in the preparation of the dye oligomer B1 except that the amount of n-dodecyl mercaptan (NDM) used was 0.02 parts by mass based on 100 parts by mass of the above monomer components.
[0281] The formulations of the dye oligomer solutions are summarized in Table 2 below.
[0282] [Table 2]
[0283] Table 2
[0284]
[0285] [Preparation of adhesive composition]
[0286] (Adhesive composition C1)
[0287] To the PSA solution A1 obtained above, 1 part by mass of the dye oligomer solution B1 and 0.8 parts by mass of an isocyanate crosslinking agent Coronate L (manufactured by Tosoh) were added and uniformly mixed to prepare a PSA composition C1.
[0288] (Adhesive composition C2)
[0289] PSA composition C2 was prepared in the same manner as in the preparation of PSA composition C1 except that the amount of dye oligomer solution B1 used was 5 parts by mass.
[0290] (Adhesive composition C3)
[0291] Binder composition C3 was prepared in the same manner as in preparation of binder composition C2, except that binder solution A2 was used and 0.08 parts by mass of Tetrad C (manufactured by Mitsubishi Gas Chemical) was used instead of 0.8 parts by mass of Coronate L.
[0292] (Adhesive composition C4)
[0293] Adhesive composition C4 was prepared in the same manner as in the preparation of Adhesive composition C2, except that Adhesive solution A3 was used as the Adhesive solution.
[0294] (Adhesive composition C5)
[0295] Adhesive composition C5 was prepared in the same manner as in the preparation of Adhesive composition C2, except that the dye oligomer solution B1 was used in an amount of 2.5 parts by mass and B2 was used in an amount of 2.5 parts by mass.
[0296] (Adhesive composition C6)
[0297] Adhesive composition C6 was prepared in the same manner as in the preparation of adhesive composition C2, except that 2.5 parts by mass of dye oligomer solution B1 was used, 2.5 parts by mass of organic pigment Pigment Blue 15 (manufactured by Tokyo Chemical Industry) and 0.5 parts by mass of dispersant Ajisper PB821 (manufactured by Ajinomoto Fine-Techno) were added.
[0298] (Adhesive composition C7)
[0299] Adhesive composition C7 was prepared in the same manner as in the preparation of Adhesive composition C2, except that the dye oligomer solution used was the dye oligomer solution B3.
[0300] (Adhesive composition C8)
[0301] Adhesive composition C8 was prepared in the same manner as in the preparation of Adhesive composition C2, except that the dye oligomer solution used was the dye oligomer solution B4.
[0302] (Adhesive composition C9)
[0303] Adhesive composition C9 was prepared in the same manner as in the preparation of Adhesive composition C2, except that the dye oligomer solution used was the dye oligomer solution B5.
[0304] (Adhesive composition C10)
[0305] Adhesive composition C10 was prepared in the same manner as in the preparation of Adhesive composition C2, except that the dye oligomer solution used was the dye oligomer solution B6.
[0306] (Adhesive composition C11)
[0307] An adhesive composition C11 was prepared in the same manner as in the preparation of the adhesive composition C1, except that 1 part by mass of the organic pigment Pigment Blue 15 was used instead of the dye oligomer solution B1.
[0308] (Adhesive composition C12)
[0309] Adhesive composition C12 was prepared in the same manner as in the preparation of adhesive composition C11 except that the organic pigments were changed to 2.5 parts by mass of Pigment Blue 15 and 2.5 parts by mass of Pigment Yellow 74 (manufactured by Oakwood Products, Inc.).
[0310] (Adhesive composition C13)
[0311] PSA composition C13 was prepared in the same manner as in the preparation of PSA composition C1 except that the dye oligomer solution B1 was not used.
[0312] (Adhesive composition C14)
[0313] PSA composition C14 was prepared in the same manner as in the preparation of PSA composition C11 except that 0.5 parts by mass of the dispersant Ajisper PB821 (manufactured by Ajinomoto Fine-Techno) was added.
[0314] (Adhesive composition C15)
[0315] PSA composition C15 was prepared in the same manner as in the preparation of PSA composition C14 except that the amount of organic pigment Pigment Blue 15 used was 5 parts by mass.
[0316] (Adhesive composition C16)
[0317] Binder composition C16 was prepared in the same manner as in the preparation of binder composition C15, except that binder solution A3 was used, 0.08 parts of Tetrad C (manufactured by Mitsubishi Gas Chemical) was used instead of 0.8 parts by mass of Coronate L, and no dispersant was used.
[0318] <Preparation of adhesive sheets>
[0319] (Example 1)
[0320] The adhesive composition C1 was applied to a release film R1 (Mitsubishi Plastics Co., Ltd., MRF#38) with a thickness of 38 μm, which was a release surface on one side of the polyester film, and dried at 135° C. for 2 minutes to form an adhesive layer with a thickness of 30 μm. A polyethylene terephthalate (PET) film with a thickness of 75 μm and subjected to corona treatment was attached to the adhesive layer, thereby obtaining an adhesive sheet 1 in which a PET film (support), an adhesive layer, and a release film R1 were sequentially laminated.
[0321] (Examples 2 to 10)
[0322] PSA sheets 2 to 10 were prepared in the same manner as in Example 1 except that PSA compositions C2 to C10 were used respectively in place of PSA composition C1.
[0323] (Comparative Examples 1 and 2)
[0324] PSA sheets 11 and 12 were prepared in the same manner as in Example 1 except that PSA compositions C11 and C12 were used, respectively, instead of PSA composition C1.
[0325] (Reference Examples 1 to 4)
[0326] PSA sheets 13 to 16 according to the respective examples were prepared in the same manner as in Example 1 except that PSA compositions C13 to C16 were used, respectively, instead of PSA composition C1.
[0327] <Evaluation of dispersibility>
[0328] The dispersibility of the dye oligomer or known organic pigment in the PSA sheets 1 to 16 prepared above was evaluated based on the degree of existence of aggregates as described below.
[0329] ○ (good dispersibility): No visually recognizable aggregates were observed in the 10 cm×10 cm test piece
[0330] △ (slightly good dispersibility): Less than 10 visually recognizable aggregates were observed in a 10 cm × 10 cm test piece.
[0331] × (poor dispersibility): 10 or more visually recognizable aggregates were observed in a 10 cm × 10 cm test piece.
[0332] The results are shown in Table 3. In Table 3, “-” means that the evaluation was not performed.
[0333] <Evaluation of exudation>
[0334] The exudation properties of the adhesive sheets 1 to 16 prepared above were evaluated by the extent to which the pigment component remained on the adherend after peeling, as described below. It should be noted that the residual area of the pigment component in the following evaluation was obtained by setting the specific gravity of the adhesive layer to 1.17 g / cm 3 The weight change of the adhesive sheet before and after peeling was measured.
[0335] ○ (Good exudation): No residual pigment component was observed on the 2.5 cm × 7 cm peeled surface
[0336] △ (slightly good exudation): Residual pigment components were observed in less than 10% of the area on the 2.5 cm × 7 cm peeled surface.
[0337] × (poor bleeding): Residue of the pigment component was observed in 10% or more of the area on the 2.5 cm × 7 cm peeled surface
[0338] The results are shown in Table 3. In Table 3, “-” means that the evaluation was not performed.
[0339] <Measurement of Adhesive Strength>
[0340] The adhesive strength of the PSA sheets 1 to 16 prepared above was measured.
[0341] For the measurement of adhesive strength, each of the PSA sheets 1 to 16 was cut into a piece having a width of 25 mm and a length of 10 cm, and the release liner was peeled off.
[0342] Next, a 2 kg roller was reciprocated once to pressure-bond and affix each pressure-sensitive adhesive sheet to an acrylic glass.
[0343] The force when peeling was measured using a tensile tester (AUTOGRAPH AGS-X, manufactured by Shimadzu Corporation) at a peeling angle of 180 degrees and a peeling speed of 300 mm / min, and the result was defined as the adhesive force (N / 25 mm).
[0344] The results are shown in Table 3. In Table 3, “-” means that the measurement was not performed.
[0345] [Table 3]
[0346]
[0347] The adhesive sheets of Examples 1 to 10 containing dye oligomers had good dispersibility and exudation properties. Among them, Examples 1 to 8 in which the weight average molecular weight (Mw) of the dye oligomer was 1,000 to 50,000 had particularly good dispersibility and exudation properties. In addition, the adhesive sheet of Example 6, although containing a pigment, also contained a dispersant, and thus obtained good results.
[0348] On the other hand, since the PSA sheets of Comparative Examples 1 and 2 contained a pigment instead of a dye oligomer, both dispersibility and bleeding properties were poor.
[0349] It should be noted that, in the case of the adhesive sheets of Reference Examples 2 and 3, a dispersant was added to the adhesive composition of Comparative Example 1. Therefore, although the dispersibility and exudation properties of the adhesive sheet of Comparative Example 1 were both poor, the dispersibility and exudation properties of the adhesive sheets of Reference Examples 2 and 3 were both good. In addition, in the case of the adhesive sheet of Reference Example 4, since an adhesive solution containing a polymer having a high acid value was used, both the dispersibility and exudation properties were good.
[0350] In the above, various embodiments are described with reference to the accompanying drawings, but it goes without saying that the present invention is not limited to these examples. It can be understood by those skilled in the art that various variations or modifications can be thought of within the scope of the claims, which are of course also within the technical scope of the present invention. In addition, the various constituent elements in the above embodiments can be arbitrarily combined within the scope of the invention.
[0351] It should be noted that the present application is based on a Japanese patent application (Japanese Patent Application No. 2019-065069) filed on March 28, 2019, the contents of which are incorporated herein by reference.
[0352] Description of Reference Numerals
[0353] 1, 2 Adhesive sheet
[0354] 11, 12 Adhesive layer
[0355] 21. Substrate
Claims
1. An adhesive composition, characterized in that The invention relates to an adhesive composition comprising a base polymer and at least one oligomer, wherein the oligomer is obtained by polymerizing a monomer composition, wherein the monomer composition at least comprises a vinyl monomer having at least one pigment structure on a side chain and an alkyl (meth)acrylate having no pigment structure on a side chain. The weight average molecular weight of the oligomer is 1,000-50,000.
2. The adhesive composition according to claim 1, wherein The base polymer is a (meth)acrylic polymer.
3. The adhesive composition according to claim 1 or 2, wherein The oligomer is a (meth)acrylic oligomer. 4 . An adhesive layer formed from the adhesive composition according to claim 1 . 5 . A pressure-sensitive adhesive sheet comprising the pressure-sensitive adhesive layer according to claim 4 . The pressure-sensitive adhesive sheet according to claim 5 , comprising the pressure-sensitive adhesive layer on a transparent film.
Citation Information
Patent Citations
Adhesive composition, pressure sensitive adhesive double coated tape, adhesion method and portable electronic device
JP2007051271A
Adhesive composition and adhesive sheet
JP2015013946A
Colored acrylic adhesive and marking film
CN101688090A
Colored photosensitive resin composition, pattern forming method, color filter and manufacture thereof and display device
CN102236255A
Acrylic pressure-sensitive adhesive composition and acrylic pressure-sensitive adhesive tape
CN102822296A