A porous carbon-silicon composite negative electrode material and preparation method thereof

By using porous carbon-coated silicon carbon-silicon composite negative electrode material in lithium-ion batteries, the problems of low energy density and silicon volume expansion of graphite-like materials are solved, achieving higher cycle life and fast charging capability, and reducing manufacturing costs. and security risks.

CN113707858BActive Publication Date: 2024-10-15BEIJING JIAJING INT TRADING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110967732.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-23
Publication Date
2024-10-15
Estimated Expiration
2041-08-23

AI Technical Summary

Technical Problem

The energy density of graphite anode materials in lithium-ion batteries is low, which limits the mileage of electric vehicles. Silicon as an alternative material has volume expansion problems, which affects cycle life and safety performance, and the carbon coating method has high manufacturing costs and safety risks. .

Method used

Using porous carbon-coated silicon carbon-silicon composite negative electrode material, a honeycomb porous carbon layer is prepared by using phenolic compounds, formaldehyde and surfactants to control the thickness and pore size of the carbon layer, reduce the volume expansion during silicon lithiation, and improve the battery cycle life and fast charging capabilities.

Benefits of technology

It reduces the number of activation cycles of carbon-silicon composite materials, reduces manufacturing costs, improves the fast charging capability and cycle life of the battery, and ensures the safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113707858B_ABST
    Figure CN113707858B_ABST
Patent Text Reader

Abstract

The present invention discloses a porous carbon-silicon composite negative electrode material, the core of which is ≤5 micron silicon particles or silicon-graphene composites, and the outer layer is a porous carbon layer; the porous carbon layer is made of phenolic compounds, formaldehyde and surfactants, and the mass of carbon accounts for 5% to 80% of the total mass of the material; the thickness of the porous carbon layer is 10 to 5000nm, and the diameter of the porous carbon layer pores is 2 to 100nm; and the preparation method thereof is disclosed. The carbon layer coated with the porous carbon-silicon composite negative electrode material of the present application limits the volume expansion during silicon lithiation and improves the cycle life of the battery; the nanopores in the carbon layer are channels for lithium ions to enter and exit the composite material, ensuring the rapid entry and exit of lithium ions, achieving reaction kinetic equilibrium, reducing the number of activation cycles required for the carbon-silicon composite material, reducing manufacturing costs, and improving the rapid charging capability of the battery; the disclosed preparation method has an easy-to-control process and low cost, and is suitable for large-scale batch production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion rechargeable battery materials, and in particular to a porous carbon-silicon composite negative electrode material and a preparation method thereof. Background Art

[0002] Currently, the negative electrode materials of lithium-ion batteries used by global lithium-ion battery manufacturers are mainly graphite materials. However, with the rapid development and widespread use of electric vehicles, the problem of low energy of electric vehicle batteries has become increasingly prominent. The low energy density of graphite negative electrodes has become one of the bottlenecks restricting the mileage of electric vehicles.

[0003] Among all potential high-energy negative electrode materials, silicon has long been considered the most likely negative electrode material to replace graphite. Compared with graphite, the theoretical gram capacity of silicon is 4200 mAh per gram, which is about ten times that of graphite (theoretical gram capacity of 372 mAh per gram). The theoretical energy density of batteries with silicon as negative electrodes is 15% higher than that of graphite. However, silicon also has its technical difficulties as a negative electrode material for lithium-ion batteries. When silicon reacts with lithium, the volume of silicon increases, and the volume of fully lithiated silicon is 130% of the volume of pure silicon. The huge change in the volume of silicon before and after lithiation, on the one hand, destroys the stability of the SEI (solid-liquid interface) on the silicon surface, reduces the cycle life and safety performance of the battery, and on the other hand, causes changes in the volume and shape of the battery, which may cause damage to the equipment.

[0004] Carbon coating is a conventional method to improve the cycle life and safety performance of silicon negative electrodes. Although the specific capacity of carbon-coated silicon (silicon-carbon composite material) is reduced, the cycle life is greatly improved. Obviously, this improvement depends on the thickness and structure of the surface carbon coating layer: if the carbon coating layer is too thin, the carbon coating is incomplete, the capacity of the silicon-carbon composite negative electrode decays quickly, the battery cycle life is too short, and there is no commercial advantage; if the carbon coating layer is too thick, it is difficult for lithium ions to pass through the thick carbon layer, and the silicon-carbon composite negative electrode requires multiple charge and discharge cycles to achieve stability, which increases the manufacturing cost and the potential safety issues of the battery. Due to these technical difficulties, silicon or silicon-carbon composite materials have not yet been widely used in lithium-ion batteries. Summary of the invention

[0005] To solve the above problems, the present invention provides a porous carbon-coated silicon carbon-silicon composite negative electrode material and a preparation method. The obtained carbon-silicon composite negative electrode material can reduce the number of activation cycles required for the carbon-silicon composite material, reduce manufacturing costs, and improve the battery's rapid charging capability.

[0006] To achieve the above purpose, the technical solution of the present invention is as follows:

[0007] A porous carbon-silicon composite negative electrode material, wherein the inner core of the porous carbon-silicon composite negative electrode material is ≤5 micron silicon particles or silicon-graphene composites, and the outer layer is a porous carbon layer; the porous carbon layer is made of phenol compounds, formaldehyde and surfactants, and the mass of carbon accounts for 5% to 80% of the total mass of the material; the thickness of the porous carbon layer is 10 to 5000 nm, and the diameter of the pores of the porous carbon layer is 2 to 100 nm.

[0008] The porous carbon-silicon composite negative electrode material has a honeycomb-shaped porous carbon layer, and the mass of carbon accounts for 5% to 30% of the total mass of the material; the thickness of the porous carbon layer is 100 to 500 nm, and the diameter of the pores in the porous carbon layer is 10 to 50 nm.

[0009] The preparation method of the porous carbon-silicon composite negative electrode material comprises the following steps:

[0010] S1 Preparation of carbon-silicon composite:

[0011] The phenol compound and the surfactant are dissolved in a solvent, formaldehyde and a catalyst are added and mixed, silicon particles or a silicon-graphene composite are added after stirring, stirring is continued for 12 hours, the clear liquid is filtered off, the colloid is washed 5 times, and vacuum dried to obtain a carbon-silicon composite;

[0012] S2 Preparation of porous carbon-silicon composite negative electrode material:

[0013] The dried carbon-silicon composite solid obtained in S1 was thermally cracked at 450-750°C for 5-10 hours, naturally cooled to room temperature, and a black porous carbon-silicon composite negative electrode material was obtained, which was ball-milled to a particle size of 5-15 μm.

[0014] The above-mentioned method for preparing porous carbon-silicon composite negative electrode material, S1 said phenol compound is phenol, hydroquinone or pyroglucin; the surfactant is a long-chain hydrocarbon quaternary ammonium salt positive ion surfactant, a hydrocarbon sodium sulfate negative ion surfactant, a sulfonic acid anion surfactant, a non-ionic ether polymer surfactant, a polar polymer copolymer or a grafted polymer; the solvent is a 10% to 30% ethanol aqueous solution; the catalyst is concentrated hydrochloric acid or a strong base; the added amounts of the phenol compound, formaldehyde, solvent, surfactant and catalyst are designed and calculated according to the requirements of the porous carbon diameter and the carbon layer thickness.

[0015] In the above-mentioned method for preparing porous carbon-silicon composite negative electrode materials, the surfactant is cetyltrimethylammonium bromide, sodium dodecyl sulfate, polyether surfactant F127, polyoxyethylene-polyoxypropylene nonionic polymer surfactant, polyethylene glycol octylphenyl ether Triton X-100 or polyoxyethylene-21 stearyl alcohol ether Brij721; the strong base is NaOH or KOH. Different structural additives have different molecular weights and molecular structures, and the diameter of the carbon layer pores can be accurately controlled by selecting the type of surfactant.

[0016] In the aforementioned method for preparing the porous carbon-silicon composite negative electrode material, the diameter of the silicon particles or silicon-graphene composite in S1 is 50-200 nanometers.

[0017] In the above-mentioned method for preparing the porous carbon-silicon composite negative electrode material, the vacuum drying in S1 is at 80°C.

[0018] The aforementioned method for preparing the porous carbon-silicon composite negative electrode material, the thermal cracking method described in S2 is: the quartz tube is first filled with nitrogen to exhaust, and then replaced with a hydrogen / argon mixed gas with a volume ratio of 5% / 95%, and thermally cracked at 750°C for 5 hours.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention discloses a porous carbon-coated silicon carbon-silicon composite negative electrode material and a preparation method thereof. The core of the carbon-silicon composite negative electrode material is silicon particles or silicon-graphene composites, the outer layer is honeycomb porous carbon, and the outer shell porous carbon completely covers the core, and has the advantages of: a) the coated carbon layer limits the volume expansion of silicon during lithiation, thereby improving the cycle life of the battery; b) the nanopores in the carbon layer are channels for lithium ions to enter and exit the composite material, ensuring the rapid entry and exit of lithium ions, achieving reaction kinetic equilibrium, reducing the number of activation cycles required for the carbon-silicon composite material, and reaching the designed capacity of the battery faster than the negative electrode materials prepared by other methods, reducing the manufacturing cost, and improving the fast charging capability of the battery. The preparation method of the present invention can design and accurately control the thickness of the carbon layer and the diameter and distribution state of the pores on the carbon layer according to the required battery performance, while the carbon layer thickness obtained by other porous carbon layer preparation methods is insufficient, and the diameter and distribution of the carbon layer pores are disordered and uncontrollable; and the preparation method of the present invention is simple, the process parameter requirements are flexible, and it is easy to realize industrial production, reducing the cost of material manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a scanning electron microscope image of the porous carbon-silicon composite negative electrode material of the present invention;

[0022] Figure 2 The invention discloses the electrochemical performance of the porous carbon-silicon composite negative electrode material after being made into a negative electrode of a battery. DETAILED DESCRIPTION

[0023] Embodiment 1 of the present invention: A porous carbon-silicon composite negative electrode material:

[0024] The inner core of the porous carbon-silicon composite negative electrode material is 100nm silicon particles, and the outer layer is a honeycomb porous carbon layer; the porous carbon layer is made of phloroglucinol, formaldehyde and surfactant cetyltrimethylammonium bromide, and the mass of carbon accounts for 10% of the total mass of the material; the thickness of the honeycomb porous carbon layer is 100nm, and the diameter of the pores of the porous carbon layer is 2nm.

[0025] Example 2: A porous carbon-silicon composite negative electrode material:

[0026] The inner core of the porous carbon-silicon composite negative electrode material is a 20nm silicon-graphene composite, and the outer layer is a porous carbon layer; the porous carbon layer is made of hydroquinone, formaldehyde and sodium dodecyl sulfate negative ion surfactant, and the mass of carbon accounts for 50% of the total mass of the material; the thickness of the porous carbon layer is 200nm, and the diameter of the porous carbon layer pores is 2nm.

[0027] Example 3: A porous carbon-silicon composite negative electrode material:

[0028] The inner core of the porous carbon-silicon composite negative electrode material is 5-micron silicon particles, and the outer layer is a porous carbon layer; the porous carbon layer is made of phloroglucinol, formaldehyde and surfactant PEO-PPO diblock copolymer, and the mass of carbon accounts for 10% of the total mass of the material; the thickness of the porous carbon layer is 100nm, and the diameter of the pores of the porous carbon layer is 10nm.

[0029] Example 4: A porous carbon-silicon composite negative electrode material:

[0030] The inner core of the porous carbon-silicon composite negative electrode material is a silicon-graphene composite, and the outer layer is a porous carbon layer; the porous carbon layer is made of phloroglucinol, formaldehyde and polyether surfactant F127, and the mass of carbon accounts for 50% of the total mass of the material; the thickness of the porous carbon layer is 50nm, and the diameter of the pores of the porous carbon layer is 20nm.

[0031] Example 5: A porous carbon-silicon composite negative electrode material:

[0032] The inner core of the porous carbon-silicon composite negative electrode material is silicon particles, and the outer layer is a honeycomb porous carbon layer; the porous carbon layer is made of phloroglucinol, formaldehyde and polyoxyethylene-21 stearyl ether Brij721, and the mass of carbon accounts for 5% of the total mass of the material; the thickness of the porous carbon layer is 1000nm, and the diameter of the pores of the porous carbon layer is 50nm.

[0033] Example 6: A porous carbon-silicon composite negative electrode material:

[0034] The inner core of the porous carbon-silicon composite negative electrode material is silicon particles, and the outer layer is a honeycomb porous carbon layer; the porous carbon layer is made of phenol, formaldehyde and polyethylene glycol octylphenyl ether Triton X-100, and the mass of carbon accounts for 60% of the total mass of the material; the thickness of the porous carbon layer is 3000nm, and the diameter of the pores of the porous carbon layer is 90nm.

[0035] Example 7: Preparation method of the porous carbon-silicon composite negative electrode material described in Example 1:

[0036] 2.7 g of phloroglucinol and 6 g of cetyltrimethylammonium bromide were dissolved in a 20% ethanol aqueous solution at room temperature with stirring, and then 4.0 g of formaldehyde and 0.6 g of concentrated hydrochloric acid were added, and the mixture was stirred for 1 h. 20 g of silicon powder with a diameter of 100 nanometers was added, and the mixture was stirred for 12 h; the clear liquid was filtered off, and the obtained colloidal mixture was rinsed with a 95% ethanol aqueous solution for 5 times, and vacuum dried in an oven at 80°C; the dried solid was loaded into a muffle furnace quartz tube, first filled with nitrogen to exhaust, and then replaced with a hydrogen / argon mixed gas (5% / 95%), and heated to 650°C for 5 hours; the heating was stopped, and the mixture was naturally cooled to room temperature to obtain a black porous carbon-silicon composite negative electrode material solid, which was ball-milled to a particle size of 5 to 15 μm for storage.

[0037] Example 8: Preparation method of the porous carbon-silicon composite negative electrode material described in Example 2:

[0038] 8 grams of hydroquinone and 9 grams of sodium dodecyl sulfate were dissolved in a 15% ethanol aqueous solution at room temperature under stirring, and then 10 grams of formaldehyde and 0.4 grams of concentrated hydrochloric acid were added, and the mixture was stirred for 1 hour. 15 grams of a 20nm diameter silicon-graphene composite was added, and the mixture was stirred for 12 hours; the clear liquid was filtered off, and the obtained colloidal mixture was rinsed 5 times and vacuum dried in an oven at 80°C; the dried solid was loaded into a muffle furnace quartz tube, first filled with nitrogen to exhaust, and then replaced with a hydrogen / argon mixed gas (5% / 95%), and heated to 450°C for 5 hours; the heating was stopped, and the mixture was naturally cooled to room temperature to obtain a black porous carbon-silicon composite negative electrode material solid, which was ball-milled to a particle size of 5 to 15 μm for storage.

[0039] Example 9: Preparation method of the porous carbon-silicon composite negative electrode material described in Example 3:

[0040] 2.7 g of phloroglucinol and 3.5 g of PEO-PPO diblock copolymer were dissolved in a 25% ethanol aqueous solution under stirring at room temperature, and then 4.0 g of formaldehyde and 1 g of 10% NaOH were added and stirred for 1 h, 10 g of 5-micron silicon powder was added, and the mixture was stirred for 12 h; the clear liquid was filtered off, and the obtained colloidal mixture was washed with a water / ethanol mixed solution for 5 times and vacuum dried in an oven at 80°C; the dried solid was first filled with nitrogen to exhaust in a container, and then replaced with a hydrogen / argon mixed gas (5% / 95%), and heated to 700°C for 5 hours; the heating was stopped and naturally cooled to room temperature to obtain a black porous carbon-silicon composite negative electrode material solid, which was ball-milled to a particle size of 5 to 15 μm for storage.

[0041] Example 10: Preparation method of the porous carbon-silicon composite negative electrode material described in Example 4:

[0042] 7 g of phloroglucinol and 8.5 g of F127 were dissolved in a 30% ethanol aqueous solution at room temperature with stirring, and then 8.8 g of formaldehyde and 2 g of 10% KOH were added and stirred for 1 h, and 15 g of a 20 nm diameter silicon-graphene composite was added, and the mixture was stirred for 12 h; the clear liquid was filtered off, and the obtained colloidal mixture was rinsed 5 times with a 95% ethanol aqueous solution and vacuum dried in an oven at 80°C; the dried solid was first filled with nitrogen to exhaust in a container, and then replaced with a hydrogen / argon mixed gas (5% / 95%), and heated to 700°C for 5 hours; the heating was stopped, and the mixture was naturally cooled to room temperature to obtain a black porous carbon-silicon composite negative electrode material solid, which was ball-milled to a particle size of 5 to 15 μm for storage.

[0043] Experimental example:

[0044] Application of the porous carbon-silicon composite negative electrode material obtained in Examples 1-6:

[0045] 0.35 g of sodium carboxymethyl cellulose was dissolved in 15 ml of deionized water by mechanical stirring, and then 0.9 g of porous silicon-carbon composite material and 0.5 g of Super P-Li carbon black were added. After 2 hours, 10 ml of deionized water was added, and stirring was continued for 3 hours. Then, 0.3 g of styrene-butadiene latex (50% concentration) was added and stirred for 2 hours; the prepared mixture was poured on a 12-micron thick copper foil, coated with a scraper, and then heated to evaporate the water to obtain a negative electrode sheet; the negative electrode sheet was vacuum dried in a vacuum oven at 80°C for 12 hours.

[0046] Gram Capacity Test:

[0047] The obtained porous carbon-silicon composite negative electrode sheet was made into a 2032 button battery and the gram capacity of the battery was tested. The porous carbon-silicon composite negative electrode sheet was used as the positive electrode, the 250-micron-thick lithium sheet was used as the negative electrode, and the electrolyte was: 1.0M LiPF6, ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (the volume ratio of EC and EMC was 2:3). The battery charge and discharge rate was 0.1C, the discharge (lithiation) cut-off voltage was 0.01 volts, and the charge (delithiation) cut-off voltage was 1.5 volts.

[0048] The test results of the 2032 button battery capacity in grams are as follows Figure 2 As shown. The battery capacity is high, reaching 800mAh / g, and has good stability, with small changes in the numerical curve; the battery capacity does not decay after 140 cycles; it quickly reaches a steady state at the beginning of charging, and reaches the maximum battery capacity in about 10 cycles; the battery reaction kinetics is stable, and the battery activation cycle is quickly reached, meeting the designed capacity requirements.

Claims

1. A porous carbon-silicon composite negative electrode material, characterized in that: The core of the porous carbon-silicon composite negative electrode material is ≤5 micron silicon particles or silicon-graphene composites, and the outer layer is a porous carbon layer; the porous carbon layer is made of phenolic compounds, formaldehyde and surfactants, and the mass of the porous carbon layer accounts for 5% to 30% of the total mass of the material; the thickness of the porous carbon layer is 100 to 500 nm, and the diameter of the porous carbon layer pores is 10 to 50 nm; the porous carbon layer is honeycomb-shaped; the porous carbon-silicon composite negative electrode material is prepared according to the following method: S1 Preparation of carbon-silicon composite: The phenol compound and the surfactant are dissolved in a solvent, formaldehyde and a catalyst are added and mixed, silicon particles or silicon-graphene composites are added after stirring, stirring is continued for 12 hours, the clear liquid is filtered off, the colloid is washed 5 times, and vacuum dried to obtain a carbon-silicon composite; the surfactant is a long-chain hydrocarbon quaternary ammonium salt cationic surfactant, a hydrocarbon sodium sulfate anionic surfactant, a nonionic ether polymer surfactant, a polar polymer copolymer or a grafted polymer; the solvent is a 10% to 30% ethanol solution; S2 Preparation of porous carbon-silicon composite negative electrode material: The dried carbon-silicon composite solid obtained in S1 was thermally cracked at 450-750°C for 5-10 hours, naturally cooled to room temperature, and a black porous carbon-silicon composite negative electrode material was obtained, which was ball-milled to a particle size of 5-15 μm.

2. The method for preparing the porous carbon-silicon composite negative electrode material according to claim 1, characterized in that: Here are the steps: S1 Preparation of carbon-silicon composite: The phenol compound and the surfactant are dissolved in a solvent, formaldehyde and a catalyst are added and mixed, silicon particles or silicon-graphene composites are added after stirring, stirring is continued for 12 hours, the clear liquid is filtered off, the colloid is washed 5 times, and vacuum dried to obtain a carbon-silicon composite; the surfactant is a long-chain hydrocarbon quaternary ammonium salt cationic surfactant, a hydrocarbon sodium sulfate anionic surfactant, a nonionic ether polymer surfactant, a polar polymer copolymer or a grafted polymer; the solvent is a 10% to 30% ethanol solution; S2 Preparation of porous carbon-silicon composite negative electrode material: The dried carbon-silicon composite solid obtained in S1 was thermally cracked at 450-750°C for 5-10 hours, naturally cooled to room temperature, and a black porous carbon-silicon composite negative electrode material was obtained, which was ball-milled to a particle size of 5-15 μm.

3. The method for preparing the porous carbon-silicon composite negative electrode material according to claim 2, characterized in that: S1: the phenol compound is phenol, hydroquinone or phloroglucinol; the catalyst is concentrated hydrochloric acid or a strong base.

4. The method for preparing the porous carbon-silicon composite negative electrode material according to claim 3, characterized in that: The surfactant is cetyltrimethylammonium bromide, sodium dodecyl sulfate, polyether surfactant F127, polyoxyethylene-polyoxypropylene nonionic polymer surfactant, polyethylene glycol octylphenyl ether Triton X-100 or polyoxyethylene-21 stearyl alcohol ether Brij721; the strong base is NaOH or KOH.

5. The method for preparing the porous carbon-silicon composite negative electrode material according to claim 2, characterized in that: S1 The silicon particles or silicon-graphene composites have a diameter of 50-200 nanometers.

6. The method for preparing the porous carbon-silicon composite negative electrode material according to claim 2, characterized in that: The vacuum drying in S1 is 80°C.

7. The method for preparing the porous carbon-silicon composite negative electrode material according to claim 2, characterized in that: The thermal cracking method described in S2 is: nitrogen is first filled into the quartz tube to exhaust, and then replaced with a hydrogen / argon mixed gas with a volume ratio of 5% / 95%, and thermally cracked at 750°C for 5 hours.