Method for forming semiconductor structure
By forming a sacrificial layer with a specific mask structure on the surface of the layer to be etched of the semiconductor structure and etching and removing it, the poor performance problem caused by the short channel effect is solved, and the graphics accuracy and device performance are improved.
Patent Information
- Application Number
- CN202010450009.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-05-25
AI Technical Summary
The existing semiconductor structures have short-channel effects during the manufacturing process, resulting in poor device performance, especially the difficulty of fin manufacturing in the manufacturing of fin field effect transistors, which affects the electrical performance of the device.
By forming a sacrificial layer with a first opening on the surface of the layer to be etched and forming a first mask structure therein, the edge of the surface is higher than the center, the sacrificial layer is etched to remove its material, using an anisotropic reaction Methods such as ion etching process and chemical mechanical planarization process to improve the pattern accuracy of the mask structure.
The graphics accuracy and performance of the semiconductor structure are improved, the process window of the mask structure is increased, the graphics accuracy and transmission accuracy of the subsequent mask structure are improved, and the overall performance of the semiconductor device is improved.
Smart Images

Figure CN113725083B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of semiconductor manufacturing, and in particular to a method for forming a semiconductor structure. Background Art
[0002] With the high integration of semiconductor devices, the channel length of Metal-Oxide-Semiconductor Field-Effect Transistor (MOSFET) is constantly shortening, and a series of effects that can be ignored in the MOSFET long channel model have become more and more significant, and even become the dominant factor affecting device performance. This phenomenon is collectively referred to as the short channel effect. The short channel effect will deteriorate the electrical performance of the device, such as causing a decrease in gate threshold voltage, increased power consumption, and a decrease in signal-to-noise ratio.
[0003] In order to overcome the short channel effect, a three-dimensional device structure of a fin field effect transistor is proposed. The fin field effect transistor is a transistor with a fin-shaped channel structure. The fin field effect transistor uses several surfaces of a thin fin as a channel, thereby preventing the short channel effect in traditional transistors and increasing the operating current. In the manufacturing process of the fin field effect transistor, the manufacturing of the fin is a very important part.
[0004] However, the performance of existing semiconductor structures is still poor. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for forming a semiconductor structure to improve the performance of the semiconductor structure.
[0006] In order to solve the above technical problems, the technical solution of the present invention provides a method for forming a semiconductor structure, including: providing a layer to be etched; forming a sacrificial layer on the surface of the layer to be etched, the sacrificial layer having a first opening; forming a first mask structure in the first opening, the edge of the surface of the first mask structure being higher than the center of the surface; etching the sacrificial layer until the sacrificial layer is removed.
[0007] Optionally, a height difference between an edge of the surface of the first mask structure and a center of the surface ranges from 20 angstroms to 100 angstroms.
[0008] Optionally, the surface of the first mask structure is a curved surface.
[0009] Optionally, an obtuse angle is formed between the sidewall surface of the first opening and the surface of the layer to be etched at the bottom of the first opening, and a top dimension of the first opening is larger than a bottom dimension.
[0010] Optionally, an obtuse angle between a side wall surface of the first opening and a surface of the to-be-etched layer at the bottom of the first opening ranges from 91° to 100°.
[0011] Optionally, the etching process for removing the sacrificial layer includes: an anisotropic reactive ion etching process.
[0012] Optionally, in the anisotropic reactive ion etching process, an etching selectivity ratio of the material of the sacrificial layer to the material of the first mask structure is greater than 5:1.
[0013] Optionally, process parameters of the anisotropic reactive ion etching process include: a bias power range of 800 watts to 4000 watts.
[0014] Optionally, the process parameters of the anisotropic reactive ion etching process also include: the etching gas includes C x F y , C x H y F z , C x H y , NF3, H2, Cl2, HBr, Ar and He; the source RF power is 200 W to 1000 W; the flow range of the etching gas is 70 standard ml / min to 500 standard ml / min; the pressure range is 4 mTorr to 50 mTorr.
[0015] Optionally, the method for forming the first mask structure includes: forming a first mask material layer in the first opening and on the surface of the sacrificial layer; and etching back the first mask material layer until the surface of the sacrificial layer is exposed.
[0016] Optionally, the process of etching back the first mask material layer includes: a chemical mechanical planarization process, a reactive ion etching process or a gaseous wet etching process.
[0017] Optionally, the process of etching back the first mask material layer is a chemical mechanical planarization process, and the process parameters of the chemical mechanical planarization process include: a pressure range of the polishing liquid is 2 pounds per square inch to 20 pounds per square inch.
[0018] Optionally, the process of etching back the first mask material layer is a reactive ion etching process, and the process parameters of the reactive ion etching process include: the gas used includes C X H Y F Z , wherein X:Z is less than or equal to 3:1; and the pressure range is 50 mTorr to 200 mTorr.
[0019] Optionally, the process of etching back the first mask material layer is a gaseous wet etching process, and the process parameters of the gaseous wet etching process include: the etchant used includes one or more of NF3, NH3, N2 and H2.
[0020] Optionally, the method for forming the sacrificial layer includes: forming a sacrificial material layer on the surface of the layer to be etched; forming a second mask structure on the surface of the sacrificial material layer, the second mask structure exposing a portion of the surface of the sacrificial material layer; using the second mask structure as a mask, etching the sacrificial material layer until the surface of the layer to be etched is exposed.
[0021] Optionally, the etching process for etching the sacrificial material layer includes a reactive ion etching process.
[0022] Optionally, the material of the second mask includes: amorphous carbon, low temperature oxide or photoresist.
[0023] Optionally, the material of the first mask structure includes: amorphous silicon, silicon nitride, silicon oxide or amorphous carbon.
[0024] Optionally, the material of the sacrificial layer includes: a dielectric material or a metal material.
[0025] Optionally, the material of the sacrificial layer includes silicon oxide, silicon nitride, silicon, titanium oxide, titanium nitride or tungsten carbide.
[0026] Optionally, the first mask structure has a first projection on the layer to be etched, a width of the first projection is less than 20 nanometers, and a length of the first projection is less than 60 nanometers.
[0027] Optionally, the method further includes: forming a plurality of mutually discrete third mask structures on the surface of the layer to be etched, and at least one of the third mask structures spans across the first mask structure.
[0028] Optionally, the method for forming several of the third mask structures includes: forming a third mask material layer on the surface of the layer to be etched and the surface of the first mask structure; forming several separate fourth mask structures on the surface of the third mask material layer; and etching the third mask material layer using the fourth mask structure as a mask until the surface of the layer to be etched is exposed.
[0029] Optionally, the process of forming the fourth mask structure includes a self-aligned multiple patterning process.
[0030] Optionally, it also includes: before forming the sacrificial layer, forming a fifth mask material layer on the surface of the layer to be etched; using several of the third mask structures and the first mask structure as masks, etching the fifth mask material layer until the surface of the layer to be etched is exposed to form a fifth mask structure.
[0031] Optionally, the method further includes: etching the layer to be etched using the fifth mask structure as a mask to form an interconnect opening in the layer to be etched; and forming an interconnect structure in the interconnect opening.
[0032] Optionally, the method further includes: etching the layer to be etched using the plurality of the third mask structures and the first mask structure as masks to form interconnect openings in the layer to be etched; and forming an interconnect structure in the interconnect openings.
[0033] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0034] In the method for forming a semiconductor structure provided by the technical solution of the present invention, since the first mask structure is formed in the first opening, and the edge of the surface of the first mask structure is higher than the center of the surface, the material of the first mask structure at the edge of the pattern is increased, thereby increasing the material of the edge of the pattern at the top of the first mask structure. Since the material of the edge of the pattern at the top of the first mask structure is increased, and after the first mask structure is formed, the sacrificial layer is etched until the sacrificial layer is removed, the verticality of the side wall of the first mask structure can be increased by the loss of the increased material of the first mask structure during the etching process of the sacrificial layer, thereby improving the pattern accuracy of the first mask structure. By improving the pattern accuracy of the first mask structure, on the one hand, the process window of the photolithography process when other mask structures are subsequently formed on the first mask structure can be increased, thereby improving the pattern accuracy of the other mask structures, so that the pattern accuracy of the other mask structures is improved; on the other hand, when the pattern is transferred downward using the first mask structure as a mask, the accuracy of the transferred pattern of the first mask structure can be improved. In summary, the pattern accuracy of the semiconductor structure is improved, thereby improving the performance of the semiconductor structure.
[0035] Furthermore, since there is an obtuse angle between the side wall surface of the first opening and the surface of the layer to be etched at the bottom of the first opening, and the top size of the first opening is larger than the bottom size, the first mask structure subsequently formed in the first opening can increase the top size to increase the material at the top of the first mask structure, thereby being more conducive to improving the verticality of the side wall surface of the first mask structure to improve the performance of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figures 1 to 3 It is a schematic cross-sectional structure diagram of each step of a method for forming a semiconductor structure;
[0037] Figures 4 to 17 It is a structural schematic diagram of each step of the method for forming a semiconductor structure in an embodiment of the present invention. DETAILED DESCRIPTION
[0038] As described in the background art, the performance of the semiconductor structure is still relatively poor. Now, an analysis and description will be given in conjunction with a specific embodiment.
[0039] It should be noted that the “surface” in this specification is used to describe the relative position relationship in space and is not limited to direct contact.
[0040] Figures 1 to 3 The invention is a schematic cross-sectional structure diagram of each step of a method for forming a semiconductor structure.
[0041] Please refer to Figure 1 , providing a layer to be etched 10, wherein the layer to be etched 10 includes a plurality of invalid areas B and an effective area A surrounding the plurality of invalid areas B; forming a first mask material layer 20 on the surfaces of the effective areas A and the invalid areas B; forming a cutting blocking material layer 30 on the surface of the first mask material layer 20; forming a second mask material layer 40 on the surface of the cutting blocking material layer 30; forming a first anti-reflection layer 41 on the surface of the second mask material layer 40; and forming a first photoresist layer 50 on the surface of the anti-reflection layer 41 in the invalid area B.
[0042] Please refer to Figure 2 , using the first photoresist layer 50 as a mask, etching the first anti-reflection layer 41 and the second mask material layer 40 until the surface of the cutting mask material layer 30 is exposed to form a second mask layer (not shown); using the second mask layer as a mask, etching the cutting material layer 30 until the surface of the first mask material layer 20 is exposed to form a cutting blocking structure 31; forming a third mask material layer 60 on the exposed surface of the cutting blocking structure 31 and the first mask material layer 20; forming a second anti-reflection layer 61 on the surface of the third mask material layer 60; and forming a plurality of separate second photoresist structures 70 on the surface of the second anti-reflection layer 61.
[0043] Please refer to Figure 3 , using the second photoresist structure 70 as a mask, etching the second anti-reflection layer 61 and the third mask material layer 60 until the surface of the first mask material layer 20 is exposed to form a third mask layer (not shown); using the third mask layer and the cutting blocking structure 31 as masks, etching the first mask material layer 20 until the surface of the layer to be etched 10 is exposed to form a first mask layer 21; using the first mask layer 21 as a mask, etching the layer to be etched 10 until an interconnect opening (not shown) is formed in the effective area, and forming an interconnect structure (not shown) in the interconnect opening.
[0044] However, in the above method, due to the limitation of the exposure and development process, on the one hand, the sidewall of the formed first photoresist layer 50 is inclined, so that in the process of transferring the pattern of the first photoresist layer 50 to the cutting barrier material layer 30, the material of the lower layer is easily over-etched, resulting in the formed cutting barrier structure 31 being easily an island-type structure with inclined sidewalls, resulting in poor pattern accuracy of the cutting barrier structure 31. On the other hand, when etching the cutting barrier material layer 30, not only the top of the cutting barrier material layer 30 is etched for a longer time than the bottom, but also, due to the distribution of etching gas, the etching rate of the top of the cutting barrier material layer 30 is also greater than the etching rate of the bottom, thus aggravating the inclination of the sidewall of the cutting barrier structure 31.
[0045] Since the sidewall of the cutting barrier structure 31 is severely inclined, when the first mask material layer 20 is etched using the cutting barrier structure 31 and the third mask layer as masks, the first mask material layer 20 is easily over-etched at the edge of the cutting barrier structure 31 pattern, so that the first mask structure 21 formed is lost at the edge of the cutting barrier structure 31 pattern (e.g., Figure 4 As shown in the groove 22), the formed interconnect structure cannot be disconnected in the ineffective area B.
[0046] In summary, since the sidewall of the cutting blocking structure 31 is severely tilted, the pattern accuracy of the cutting blocking structure 31 is poor, and the accuracy of the pattern transmitted by the cutting blocking structure 31 is also poor. Therefore, the pattern accuracy of the formed semiconductor structure is poor, resulting in poor performance of the semiconductor structure.
[0047] In order to solve the technical problem, an embodiment of the present invention provides a method for forming a semiconductor structure, by forming a sacrificial layer on the surface of the effective area, wherein the sacrificial layer in the invalid area has a first opening; forming a first mask structure in the first opening, wherein the edge of the surface of the first mask structure is higher than the center of the surface; etching the sacrificial layer until the sacrificial layer is removed, thereby improving the verticality of the side wall surface of the first mask structure, thereby improving the performance of the semiconductor structure.
[0048] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0049] Figures 4 to 17 It is a structural schematic diagram of each step of the method for forming a semiconductor structure in an embodiment of the present invention.
[0050] Please refer to Figure 4 and Figure 5 , Figure 4 is along Figure 5 Schematic diagram of the structure in the middle direction Y, Figure 5 yes Figure 4A schematic diagram of the cross-sectional structure along the direction X-X1 is provided, providing a layer 100 to be etched; forming a fifth mask material layer 200 on the surface of the layer 100 to be etched; forming a sacrificial material layer 300 on the surface of the fifth mask material layer 200; forming a second mask structure 400 on the surface of the sacrificial material layer 300, and exposing a portion of the surface of the sacrificial material layer 300.
[0051] In this embodiment, the layer to be etched 100 includes a substrate 110 and a dielectric layer 120 located on the surface of the substrate 110 .
[0052] The substrate 110 is made of semiconductor material.
[0053] In this embodiment, the material of the substrate 110 is single crystal silicon.
[0054] In other embodiments, the material of the substrate includes silicon carbide, silicon germanium, a multinary semiconductor material composed of group III-V elements, silicon on insulator (SOI) or germanium on insulator (GOI), etc. Among them, the multinary semiconductor material composed of group III-V elements includes InP, GaAs, GaP, InAs, InSb, InGaAs or InGaAsP, etc.
[0055] In other embodiments, the layer to be etched further includes an etching stop layer located between the substrate and the dielectric layer.
[0056] In this embodiment, the material of the dielectric layer 120 includes oxide.
[0057] The fifth mask material layer 200 is used to provide material for subsequently forming a fifth mask structure.
[0058] In other embodiments, the fifth mask material layer is not formed, and the fifth mask structure is not formed subsequently.
[0059] In this embodiment, the process of forming the fifth mask material layer 200 includes a chemical vapor deposition process or an atomic layer deposition process.
[0060] The sacrificial material layer 300 is used to provide material for subsequently forming a sacrificial layer.
[0061] The material of the sacrificial material layer 300 includes: a dielectric material or a metal material. Accordingly, the material of the sacrificial layer includes: a dielectric material or a metal material.
[0062] In this embodiment, the material of the sacrificial material layer 300 includes silicon oxide, silicon nitride, silicon, titanium oxide, titanium nitride or tungsten carbide (tungsten doped carbon / tungsten implanted carbon).
[0063] Accordingly, in this embodiment, the material of the sacrificial layer includes: silicon oxide, silicon nitride, silicon, titanium oxide, titanium nitride or tungsten carbide.
[0064] In this embodiment, the process of forming the sacrificial material layer 300 includes: a spin coating process or a deposition process, and the deposition process is, for example, a chemical vapor deposition process or an atomic layer deposition process.
[0065] In this embodiment, the material of the second mask structure 400 includes amorphous carbon or low temperature oxide.
[0066] In this embodiment, the method for forming the second mask structure 400 includes: forming a second mask material layer (not shown) on the surface of the sacrificial material layer 300; forming a second anti-reflection layer (not shown) on the surface of the second mask material layer; forming a second photoresist layer (not shown) on the surface of the second anti-reflection layer, the second photoresist layer exposing a portion of the surface of the second anti-reflection layer; using the second photoresist layer as a mask, etching the second anti-reflection layer and the second mask material layer until the surface of the sacrificial material layer 300 is exposed.
[0067] The second mask material layer is helpful to improve the stability of the second photoresist layer during the pattern transfer process.
[0068] The second anti-reflection layer is helpful to improve the anti-reflection effect when forming the second photoresist layer, thereby improving the pattern accuracy of the second mask structure 400 .
[0069] In this embodiment, the second anti-reflection layer includes: a thin silicon anti-reflection layer (Si-ARC), an organic bottom anti-reflection layer (organic BARC), a dielectric anti-reflection layer (DARC), or a combination of an organic bottom anti-reflection layer and a dielectric anti-reflection layer.
[0070] In other embodiments, the second anti-reflection layer is not formed.
[0071] In other embodiments, the material of the second mask material layer is photoresist and does not include a second photoresist layer, so that the second mask structure is directly formed through an exposure and development process.
[0072] In this embodiment, the second photoresist layer and the second anti-reflection layer are removed after the second mask structure 400 is formed.
[0073] In other embodiments, after the sacrificial layer is subsequently formed, the second photoresist layer and the second anti-reflection layer are removed.
[0074] Please Figure 5 Based on reference Figure 6The sacrificial material layer 300 is etched using the second mask structure 400 as a mask until the surface of the layer to be etched 100 is exposed, so as to form a sacrificial layer 310 on the surface of the layer to be etched 100, wherein the sacrificial layer 310 has a first opening 301.
[0075] In this embodiment, the first opening 301 exposes a portion of the surface of the to-be-etched layer 100 .
[0076] It should be noted that, in the present embodiment, since the fifth mask material layer 200 is formed on the surface of the layer to be etched 100 before the sacrificial material layer 300 is formed, etching the sacrificial material layer 300 using the second mask structure 400 as a mask until the surface of the layer to be etched 100 is exposed means that etching the sacrificial material layer 300 using the second mask structure 400 as a mask until the surface of the fifth mask material layer 200 is exposed; and, the first opening 301 exposing a portion of the surface of the layer to be etched 100 means that the first opening 301 exposes the surface of the fifth mask material layer 200.
[0077] The first opening 301 is used to provide space and position limitation for subsequently forming a first mask structure in the first opening 301 .
[0078] In this embodiment, an obtuse angle α is formed between the sidewall surface of the first opening 301 and the surface of the to-be-etched layer 100 at the bottom of the first opening 301, and the top size of the first opening 301 is larger than the bottom size. Therefore, a structure in which the sidewall surface of the first opening 301 is inclined from the top to the bottom toward the inside of the first opening 301 can be formed.
[0079] In this embodiment, the obtuse angle α between the sidewall surface of the first opening 301 and the surface of the to-be-etched layer 100 at the bottom of the first opening 301 ranges from 91° to 100°.
[0080] In this embodiment, the process of etching the sacrificial material layer 300 includes: a reactive ion etching process.
[0081] In this embodiment, the process parameters of the reactive ion etching process include: a ratio of source power to bias power ranging from 1:1 to 1:4.
[0082] On the one hand, by adjusting the source power and the bias power, the obtuse angle α can be adjusted. On the other hand, by making the ratio of the source power to the bias power range from 1:1 to 1:4, it is more conducive to making the obtuse angle α range from 91° to 100°.
[0083] In this embodiment, after the sacrificial layer 310 is formed, the second mask structure 400 is removed.
[0084] Please refer to Figure 7 , a first mask structure 330 is formed in the first opening 301 , and the edge of the surface of the first mask structure 330 is higher than the center of the surface.
[0085] Since the first mask structure 330 is formed in the first opening 301, and the edge of the surface of the first mask structure 330 is higher than the center of the surface, the material of the first mask structure 330 at the edge of the pattern is increased, thereby increasing the material of the edge of the pattern at the top of the first mask structure 330. Since the material of the edge of the pattern at the top of the first mask structure 330 is increased, and the sacrificial layer 310 is subsequently etched until the sacrificial layer 310 is removed after the first mask structure 330 is formed, the material of the increased first mask structure 330 is lost during the etching process during the etching of the sacrificial layer 310, that is, the balance between the increased material of the first mask structure 330 and the loss can improve the verticality of the sidewall surface of the first mask structure 330, thereby improving the pattern accuracy of the first mask structure 330.
[0086] By improving the pattern accuracy of the first mask structure 330, on the one hand, the process window of the photolithography process when other mask structures are subsequently formed on the first mask structure 330 can be increased, thereby improving the pattern accuracy of the other mask structures, so that the pattern accuracy transmitted by the other mask structures is improved; on the other hand, when the pattern is transmitted downward using the first mask structure 330 as a mask, the accuracy of the pattern transmitted by the first mask structure 330 can be improved. In summary, the pattern accuracy of the semiconductor structure is improved, thereby improving the performance of the semiconductor structure.
[0087] In this embodiment, a height difference Q1 between the edge of the surface of the first mask structure 330 and the center of the surface ranges from 20 angstroms to 100 angstroms.
[0088] If the height difference Q1 is too small, less material is added to the edge of the pattern at the top of the first mask structure 330, resulting in that in the subsequent etching process for removing the sacrificial layer 310, the loss of the edge of the pattern at the top of the first mask structure 330 during the etching process is greater than the increased material, which is not conducive to improving the verticality of the side wall surface of the first mask structure 330. If the height difference Q1 is too large, more material is added to the edge of the pattern at the top of the first mask structure 330, resulting in that in the subsequent etching process for removing the sacrificial layer 310, the loss of the edge of the pattern at the top of the first mask structure 330 during the etching process is less than the increased material, which is also not conducive to improving the verticality of the side wall surface of the first mask structure 330. Therefore, by selecting a suitable height difference Q1, that is, when the height difference Q1 ranges from 20 angstroms to 100 angstroms, it is possible to better balance the material added to the edge of the pattern at the top of the first mask structure 330 and the material loss at the edge of the pattern at the top of the first mask structure 330 during the etching process, thereby facilitating improving the verticality of the sidewall surface of the first mask structure 330 after removing the sacrificial layer 310.
[0089] In this embodiment, the surface of the first mask structure 330 is a curved surface.
[0090] In other embodiments, a surface at an edge of a pattern on the top of the first mask structure is flat, and a surface near the center of the top of the first mask structure is concave.
[0091] In this embodiment, the material of the first mask structure 330 is different from the material of the sacrificial layer 310 .
[0092] Therefore, by flexibly selecting the material of the sacrificial layer 310 and the material of the first mask structure 330, in the subsequent etching process of removing the sacrificial layer 310, the loss of the first mask structure caused by the etching process can be controlled, so as to better achieve a balance between the increased first mask structure 330 material and the loss. Therefore, after removing the sacrificial layer 310, the verticality of the side wall of the first mask structure 330 is further increased, so as to better improve the performance of the semiconductor structure.
[0093] In this embodiment, the material of the first mask structure 330 includes: amorphous silicon, silicon nitride, silicon oxide or amorphous carbon.
[0094] In this embodiment, the method for forming the first mask structure 330 includes: forming a first mask material layer (not shown) in the first opening 301 and on the surface of the sacrificial layer 310; and etching back the first mask material layer until the surface of the sacrificial layer 310 is exposed.
[0095] Since the first mask structure 330 is formed through the first opening 301, an obtuse angle α is present between the side wall of the first mask structure 330 and the surface of the layer to be etched 100 at the bottom of the first opening 301, and the top size is larger than the bottom size, that is, the side wall of the first mask structure 330 is inclined from the top to the bottom toward the inside of the first opening 301, thereby increasing the size of the top of the first mask structure 330 and increasing the material of the top of the first mask structure 330.
[0096] Since in the subsequent etching process for removing the sacrificial layer 310, the etchant of the etching process contacts the top of the first mask structure 330 longer than the bottom of the first mask structure 330, therefore, by increasing the material on the top of the first mask structure 330, it is possible to better balance the increased material of the first mask structure 330 and the loss of the first mask structure 330 caused by the etching process, thereby being more conducive to improving the verticality of the side wall of the first mask structure 330 after removing the sacrificial layer 310, so as to improve the performance of the semiconductor structure.
[0097] In this embodiment, since the obtuse angle α between the side wall surface of the first opening 301 and the surface of the layer to be etched 100 at the bottom of the first opening 301 ranges from 91° to 100°, the obtuse angle α between the side wall surface of the first mask structure 330 and the surface of the layer to be etched 100 at the bottom of the first opening 301 ranges from 91° to 100°.
[0098] If the obtuse angle α is too small, it is not conducive to increasing the material on the top of the first mask structure 330, and thus, it is not conducive to better balancing the increased material of the first mask structure 330 and the loss of the first mask structure 330 during the etching process, resulting in a disadvantage in better improving the verticality of the sidewall surface of the first mask structure 330. If the obtuse angle α is too large, the etching process cannot completely consume the increased material of the first mask structure 330, and it is not conducive to improving the verticality of the sidewall surface of the first mask structure 330. Therefore, when the obtuse angle α is within a suitable range, that is, when the obtuse angle α is 91° to 100°, it is possible to better balance the increased material of the first mask structure 330 and the loss of the first mask structure 330 during the etching process, so that after the subsequent removal of the sacrificial layer 310, the verticality of the sidewall surface of the first mask structure 330 can be better improved.
[0099] In this embodiment, the process of forming the first mask material layer includes a spin coating process, an epitaxial growth process or a deposition process, and the deposition process is, for example, a chemical vapor deposition process or an atomic layer deposition process.
[0100] The process of etching back the first mask material layer includes: a chemical mechanical planarization process, a reactive ion etching process or a gaseous wet etching process.
[0101] In this embodiment, the process of etching back the first mask material layer is a reactive ion etching process, and the process parameters of the reactive ion etching process include: the gas used includes C X H Y F Z , wherein X:Z is less than or equal to 3:1; and the pressure range is 50 mTorr to 200 mTorr.
[0102] On the one hand, using C X H Y F Z It is beneficial to make the height difference Q between the edge and the center of the surface of the first mask structure 330. Moreover, by adjusting the ratio of X:Z, the height difference Q between the edge and the center of the surface of the first mask structure 330 can be adjusted. Therefore, by making X:Z less than or equal to 3:1, it is more beneficial to make the height difference Q within a suitable range.
[0103] On the other hand, by adjusting the pressure, the height difference Q between the edge and the center of the surface of the first mask structure 330 can also be adjusted. Therefore, by making the pressure range from 50 mTorr to 200 mTorr, it is more conducive to making the height difference Q within an appropriate range.
[0104] In other embodiments, the process of etching back the first mask material layer is a chemical mechanical planarization process or a gaseous wet etching process.
[0105] The process parameters of the chemical mechanical planarization process include: the pressure range of the polishing liquid is 2 pounds per square inch to 20 pounds per square inch.
[0106] By adjusting the pressure range of the polishing liquid, the height difference Q between the edge of the surface of the first mask structure 330 and the center of the surface can be adjusted. Therefore, by making the pressure range of the polishing liquid 2 pounds per square inch to 20 pounds per square inch, it can be more conducive to making the height difference Q within an appropriate range.
[0107] The process parameters of the gaseous wet etching process include: the etchant used includes one or more of NF3, NH3, N2 and H2. Therefore, the etchant used makes it easier to form a structure in which the edge of the surface of the first mask structure 330 is higher than the center of the surface.
[0108] Please refer to Figure 8 and Fig. 9 , Figure 8 is along Fig. 9 Schematic diagram of the structure in the middle direction Y, Fig. 9 yes Figure 8 The schematic diagram of the cross-sectional structure along the direction X-X1 is shown in FIG. 3 , wherein the sacrificial layer 310 is etched until the sacrificial layer 310 is removed.
[0109] In this embodiment, the etching process for removing the sacrificial layer 310 includes: an anisotropic reactive ion etching process.
[0110] In this embodiment, the anisotropic reactive ion etching process has an etching selectivity ratio of greater than 5:1 for the material of the sacrificial layer 310 and the material of the first mask structure 330. Therefore, through a larger etching selectivity, the sacrificial layer 310 can be removed and the material of the increased first mask structure 330 can be consumed, while at the same time, the damage to the first mask structure 330 after the increased material of the first mask structure 330 is consumed can be reduced, so as to facilitate the formation of the first mask structure 330 with a higher sidewall verticality.
[0111] In this embodiment, the process parameters of the anisotropic reactive ion etching process include: a bias power range of 800 W to 4000 W. Thus, through a higher bias power, the angle between the reactive ions of the reactive ion etching process and the normal direction of the surface of the layer to be etched 100 is smaller, that is, the movement direction of the reactive ions is more perpendicular to the surface of the layer to be etched 100, so that while removing the sacrificial layer 310, the portion of the first mask structure 330 that is inclined relative to the normal direction can be better consumed, thereby facilitating further improving the verticality of the side wall of the first mask structure 330.
[0112] In this embodiment, the process parameters of the anisotropic reactive ion etching process also include: the etching gas includes C x F y , C x H y F z , C x H y , NF3, H2, Cl2, HBr, Ar and He; the source RF power is 200 W to 1000 W; the flow range of the etching gas is 70 standard ml / min to 500 standard ml / min; the pressure range is 4 mTorr to 50 mTorr.
[0113] In this embodiment, the first mask structure 330 has a first projection on the surface of the to-be-etched layer 100, the width W of the first projection is less than 20 nanometers, and the length L of the first projection is less than 60 nanometers. Therefore, by forming the first mask structure 330 with a smaller critical dimension, it is beneficial to improve the integration of the semiconductor structure.
[0114] Subsequently, in this embodiment, a plurality of mutually discrete third mask structures are formed on the surface of the to-be-etched layer 100, and at least one of the third mask structures spans the first mask structure 330. For a specific process of forming the third mask structure, please refer to Figures 10 to 13 .
[0115] Please refer to Fig.10 and Fig.11 , Fig.10 is along Fig.11 Schematic diagram of the structure in the middle direction Y, Fig.11 yes Fig.10 The schematic cross-sectional structure diagram along the direction X-X1 shows that a third mask material layer 500 is formed on the surface of the layer to be etched 100 and the surface of the first mask structure 330; and a plurality of fourth mask structures 510 separated from each other are formed on the surface of the third mask material layer 500.
[0116] The third mask material layer 500, on the one hand, is used to provide material for the subsequent formation of the third mask layer. On the other hand, the third mask material layer 500 can improve the surface flatness of the semiconductor structure, thereby facilitating the improvement of the graphic accuracy of the fourth mask structure 510. Moreover, the third mask material layer 500 can also improve the stability of the fourth mask structure 510 during the graphic transfer process.
[0117] In this embodiment, the process of forming the third mask material layer 500 includes a spin coating process or a deposition process, and the deposition process is, for example, a chemical vapor deposition process or an atomic layer deposition process.
[0118] In this embodiment, the material of the fourth mask structure 510 includes photoresist.
[0119] In this embodiment, before forming the fourth mask structure 510 , a first anti-reflection layer 520 is formed on the surface of the third mask material layer 500 .
[0120] The first anti-reflection layer 520 is helpful to improve the anti-reflection effect when forming the fourth mask structure 510 , thereby improving the pattern accuracy of the fourth mask structure 510 .
[0121] In this embodiment, the first anti-reflection layer 520 includes: a thin silicon anti-reflection layer (Si-ARC), an organic bottom anti-reflection layer (organic BARC), a dielectric anti-reflection layer (DARC), or a combination of an organic bottom anti-reflection layer and a dielectric anti-reflection layer.
[0122] In other embodiments, the first anti-reflection layer is not formed.
[0123] In other embodiments, the process of forming the fourth mask structure includes a self-aligned multi-patterning process.
[0124] Please refer to Fig.12 and Fig.13 , Fig.12 is along Fig.13 Schematic diagram of the structure in the middle direction Y, Fig.13 yes Fig.12 The schematic diagram of the cross-sectional structure along the direction X-X1 shows that the third mask material layer 500 is etched with the fourth mask structure 510 as a mask until the surface of the layer to be etched 100 is exposed, and a plurality of mutually discrete third mask structures 540 are formed on the surface of the layer to be etched 100, and at least one of the third mask structures 540 spans across the first mask structure 330.
[0125] It should be noted that, in this example, since the fifth mask material layer 200 is formed on the surface of the layer to be etched 100 before the sacrificial material layer 300 is formed, using the fourth mask structure 510 as a mask to etch the third mask material layer 500 until the surface of the layer to be etched 100 is exposed means using the fourth mask structure 510 as a mask to etch the third mask material layer 500 until the surface of the fifth mask material layer 200 is exposed.
[0126] In this embodiment, the process of etching the third mask material layer 500 includes a dry etching process or a wet etching process.
[0127] In this embodiment, after the third mask structure 540 is formed, the fourth mask structure 510 is removed.
[0128] Please refer to Fig.14 and Fig.15 , Fig.14 is along Fig.15 Schematic diagram of the structure in the middle direction Y, Fig.15 yes Fig.14 The schematic diagram of the cross-sectional structure along the direction X-X1 shows that the fifth mask material layer 200 is etched using the third mask structures 540 and the first mask structures 330 as masks until the surface of the layer to be etched 100 is exposed to form a fifth mask structure 210.
[0129] The fifth mask structure 210 is used to subsequently form interconnect openings in the dielectric layer 120 .
[0130] In this embodiment, since the verticality of the side wall surface of the first mask structure 330 is improved, the over-etching of the fifth mask structure 210 during the formation of the third mask structure 540 is reduced, and the accuracy of transferring the pattern of the first mask structure 330 to the fifth mask structure 210 is improved, thereby reducing the probability of the subsequently formed interconnect structure not being separated by two short circuits, thereby improving the performance and reliability of the semiconductor structure.
[0131] In this embodiment, the process of etching the fifth mask material layer 200 includes a dry etching process or a wet etching process.
[0132] In this embodiment, after the fifth mask structure 210 is formed, the first mask structure 330 and the third mask structure 540 are removed.
[0133] Please refer to Fig.16 and Fig.17 , Fig.16 is along Fig.17 Schematic diagram of the structure in the middle direction Y, Fig.17 yes Fig.16 The schematic cross-sectional structure diagram along the direction X-X1 is shown in FIG. 1 , wherein the layer to be etched 100 is etched using the fifth mask structure 210 as a mask to form an interconnect opening 550 in the layer to be etched 100 .
[0134] Specifically, in this embodiment, the dielectric layer 120 of the layer to be etched 100 is etched using the fifth mask structure 210 as a mask until the surface of the substrate 110 is exposed, so as to form the interconnection opening 550 in the dielectric layer 120 .
[0135] In this embodiment, after the interconnection opening 550 is formed, an electrical interconnection structure (not shown) is formed in the interconnection opening 550 .
[0136] In other embodiments, since the fifth mask material layer is not formed and the fifth mask structure is not formed, the method for forming the semiconductor structure includes: etching the layer to be etched using the plurality of the third mask structures and the first mask structure as masks to form an interconnect opening in the layer to be etched; and forming an interconnect structure in the interconnect opening. Specifically, etching the dielectric layer of the layer to be etched using the plurality of the third mask structures and the first mask structure as masks until the substrate surface is exposed to form an interconnect opening in the dielectric layer; and forming an electrical interconnect structure in the interconnect opening.
[0137] In this embodiment, after forming the interconnect opening 550 and before forming the electrical interconnect structure, the fifth mask structure 210 is removed.
[0138] In other embodiments, the first mask structure is not limited to being used for forming interconnect openings, but can also be used for forming other semiconductor structures, for example, as a cutting blocking structure (block layer) for forming a fin structure.
[0139] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: Providing a layer to be etched; Forming a sacrificial layer on the surface of the layer to be etched, wherein the sacrificial layer has a first opening, and a sidewall surface of the first opening is inclined from the top to the bottom toward the inside of the first opening; forming a first mask structure in the first opening, wherein an edge of a surface of the first mask structure is higher than a center of the surface, and a sidewall surface of the first mask structure and a sidewall surface of the first opening have the same inclination; The sacrificial layer is etched until the sacrificial layer is removed.
2. The method for forming a semiconductor structure according to claim 1, wherein: The height difference between the edge of the surface of the first mask structure and the center of the surface ranges from 20 angstroms to 100 angstroms.
3. The method for forming a semiconductor structure according to claim 1, wherein: The surface of the first mask structure is a curved surface.
4. The method for forming a semiconductor structure according to claim 1, wherein: An obtuse angle is formed between the sidewall surface of the first opening and the surface of the to-be-etched layer at the bottom of the first opening, and the top size of the first opening is larger than the bottom size.
5. The method for forming a semiconductor structure according to claim 4, wherein: The obtuse angle between the side wall surface of the first opening and the surface of the to-be-etched layer at the bottom of the first opening ranges from 91° to 100°.
6. The method for forming a semiconductor structure according to claim 1, wherein: The etching process for removing the sacrificial layer includes: an anisotropic reactive ion etching process.
7. The method for forming a semiconductor structure according to claim 6, wherein: The anisotropic reactive ion etching process has an etching selectivity ratio of greater than 5:1 for the material of the sacrificial layer and the material of the first mask structure.
8. The method for forming a semiconductor structure according to claim 6, wherein: The process parameters of the anisotropic reactive ion etching process include: a bias power range of 800 watts to 4000 watts.
9. The method for forming a semiconductor structure according to claim 8, wherein: The process parameters of the anisotropic reactive ion etching process also include: the etching gas includes C x F y , C x H y F z , C x H y , one or more of NF3, H2, Cl2, HBr, Ar and He; the source RF power is 200 W to 1000 W; the flow rate of the etching gas ranges from 70 standard ml / min to 500 standard ml / min; The pressure range is 4 mTorr to 50 mTorr.
10. The method for forming a semiconductor structure according to claim 1, wherein: The method for forming the first mask structure includes: forming a first mask material layer in the first opening and on the surface of the sacrificial layer; and etching back the first mask material layer until the surface of the sacrificial layer is exposed.
11. The method for forming a semiconductor structure according to claim 10, wherein: The process of etching back the first mask material layer includes: a chemical mechanical planarization process, a reactive ion etching process or a gaseous wet etching process.
12. The method for forming a semiconductor structure according to claim 11, wherein: The process of etching back the first mask material layer is a chemical mechanical planarization process, and the process parameters of the chemical mechanical planarization process include: the pressure range of the polishing liquid is 2 pounds per square inch to 20 pounds per square inch.
13. The method for forming a semiconductor structure according to claim 11, wherein: The process of etching back the first mask material layer is a reactive ion etching process, and the process parameters of the reactive ion etching process include: the gas used includes C X H Y F Z , wherein X:Z is less than or equal to 3:1; and the pressure range is 50 mTorr to 200 mTorr.
14. The method for forming a semiconductor structure according to claim 11, wherein: The process of etching back the first mask material layer is a gaseous wet etching process, and the process parameters of the gaseous wet etching process include: the etchant used includes one or more of NF3, NH3, N2 and H2.
15. The method for forming a semiconductor structure according to claim 1, wherein: The method for forming the sacrificial layer includes: forming a sacrificial material layer on the surface of the layer to be etched; forming a second mask structure on the surface of the sacrificial material layer, the second mask structure exposing a portion of the surface of the sacrificial material layer; using the second mask structure as a mask, etching the sacrificial material layer until the surface of the layer to be etched is exposed.
16. The method for forming a semiconductor structure according to claim 15, wherein: The etching process for etching the sacrificial material layer includes a reactive ion etching process.
17. The method for forming a semiconductor structure according to claim 15, wherein: The material of the second mask includes: amorphous carbon, low temperature oxide or photoresist.
18. The method for forming a semiconductor structure according to claim 1, wherein: The material of the first mask structure includes: amorphous silicon, silicon nitride, silicon oxide or amorphous carbon.
19. The method for forming a semiconductor structure according to claim 1, wherein: The material of the sacrificial layer includes: dielectric material or metal material.
20. The method for forming a semiconductor structure according to claim 19, wherein: The material of the sacrificial layer includes silicon oxide, silicon nitride, silicon, titanium oxide, titanium nitride or tungsten carbide.
21. The method for forming a semiconductor structure according to claim 1, wherein: The first mask structure has a first projection on the layer to be etched, a width of the first projection is less than 20 nanometers, and a length of the first projection is less than 60 nanometers.
22. The method for forming a semiconductor structure according to claim 1, wherein: Also includes: A plurality of mutually independent third mask structures are formed on the surface of the layer to be etched, and at least one of the third mask structures spans across the first mask structure.
23. The method for forming a semiconductor structure according to claim 22, wherein: The method for forming several of the third mask structures includes: forming a third mask material layer on the surface of the layer to be etched and the surface of the first mask structure; forming several mutually discrete fourth mask structures on the surface of the third mask material layer; and etching the third mask material layer using the fourth mask structure as a mask until the surface of the layer to be etched is exposed.
24. The method for forming a semiconductor structure according to claim 23, wherein: The process of forming the fourth mask structure includes a self-aligned multi-patterning process.
25. The method for forming a semiconductor structure according to claim 22, wherein: Also includes: Before forming the sacrificial layer, forming a fifth mask material layer on the surface of the layer to be etched; The fifth mask material layer is etched using the plurality of the third mask structures and the first mask structure as masks until the surface of the layer to be etched is exposed, so as to form a fifth mask structure.
26. The method for forming a semiconductor structure according to claim 25, wherein: Also includes: Using the fifth mask structure as a mask, etching the layer to be etched to form an interconnect opening in the layer to be etched; An interconnect structure is formed within the interconnect opening.
27. The method for forming a semiconductor structure according to claim 22, wherein: Also includes: Using the third mask structures and the first mask structure as masks, etching the layer to be etched to form interconnect openings in the layer to be etched; An interconnect structure is formed within the interconnect opening.