Semiconductor structure and method for forming the same
By forming a filled and exposed sacrificial layer in the first mask layer of the semiconductor structure, the flatness problem caused by the opening of the hard mask layer is solved, and the dimensional accuracy of the semiconductor structure is improved.
Patent Information
- Application Number
- CN202010486143.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-06-01
AI Technical Summary
The dimensional accuracy of the existing semiconductor structure is not high, mainly due to the existence of the first opening of the hard mask layer, the surface flatness of the subsequent film layer is not high, which affects the lithography process.
A filled and exposed sacrificial layer is formed in the first opening of the first mask layer, thereby increasing the flatness of the first mask layer, thereby improving the surface flatness of the second mask layer, thereby improving the photolithography process Dimensional accuracy.
By increasing the flatness of the first mask layer and the second mask layer, the dimensional accuracy of the subsequently formed semiconductor structure is significantly improved.
Smart Images

Figure CN113764260B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] In the process of forming semiconductor devices, it is often necessary to form different semiconductor structures in different areas of the substrate. In the prior art, a mask layer is usually formed on the surface of the substrate first, and a first opening is formed in a hard mask layer in one area, and a second opening is formed in a hard mask layer in another area, and the hard mask layer is further used as a mask to form different semiconductor structures.
[0003] However, the dimensional accuracy of semiconductor structures formed by existing processes needs to be improved. Summary of the invention
[0004] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the dimensional accuracy of the semiconductor structure.
[0005] To solve the above problems, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising:
[0006] A substrate is provided, wherein a first mask layer is formed on the surface of the substrate, and the first mask layer has a first opening; a sacrificial layer is formed to fill the first opening and expose the top surface of the first mask layer; and a second mask layer is formed on the first mask layer, and the second mask layer is used as an initial mask for forming a second opening in the first mask layer.
[0007] Accordingly, an embodiment of the present invention further provides a semiconductor structure, including:
[0008] A substrate, a first mask layer is disposed on the substrate, a first opening is formed in the first mask layer; a sacrificial layer is located in the first opening, the sacrificial layer fills the first opening; and a second mask layer is located on the first mask layer.
[0009] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0010] In the embodiment of the present invention, a sacrificial layer is formed in the first opening of the first mask layer to fill the first opening and expose the top surface of the first mask layer, so that the flatness of the surface of the first mask layer itself is improved, thereby correspondingly improving the surface flatness of the second mask layer formed on the first mask layer, thereby improving the dimensional accuracy of the subsequent photolithography process, and thus correspondingly improving the dimensional accuracy of the semiconductor structure formed subsequently. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figures 1 to 4It is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure;
[0012] Figures 5 to 14 It is a schematic structural diagram corresponding to each step of the method for forming a semiconductor structure according to an embodiment of the present invention;
[0013] Fig.15 It is a structural schematic diagram of an embodiment of a semiconductor structure according to an embodiment of the present invention. DETAILED DESCRIPTION
[0014] As described in the background art, the dimensional accuracy of semiconductor structures formed by existing processes needs to be improved.
[0015] refer to Figures 1 to 4 ,Now ,combined with a semiconductor structure formation process, ,analyzes the reasons why the dimensional accuracy of the semiconductor ,structure is low.
[0016] refer to Figure 1 , a hard mask layer 110 is formed on the semiconductor substrate 100 , wherein the hard mask layer has a first opening W1 .
[0017] refer to Figure 2 A hard mask covering layer 120 is formed on the hard mask layer 110, and the hard mask covering layer 120 completely covers the first opening W1; wherein the hard mask covering layer 120 can be, for example, a spin on carbon (SOC) layer. The SOC layer is formed by a spin coating process, and is used to improve the surface flatness of the hard mask covering layer, and provide a good interface state for the formation of subsequent film layers.
[0018] refer to Figure 3 , a photolithography mask layer 130 is formed on the hard mask cover layer 120; wherein the photolithography mask layer 130 has a mask pattern for forming a second opening, and the mask pattern is obtained by photolithography development.
[0019] refer to Figure 4 , using the photolithography mask layer 130 as a mask, the hard mask cap layer 120 and the hard mask layer 110 are sequentially etched to form a second opening W2 on the hard mask layer.
[0020] However, the inventors found that the dimensional accuracy of the semiconductor structure obtained by the above process flow is not high.
[0021] After further research, the inventors believe that, based on the existence of the first opening W1 of the hard mask layer, the layer structure (such as the hard mask covering layer 120 and the photolithography mask layer 130) subsequently formed on the hard mask layer 110, while covering the hard mask layer 110, also needs to fill the first opening W1 of the hard mask layer 110, thereby making the surface height of the film layer in the area with the first opening W1 lower than the film layer in other areas, resulting in the surface flatness of the film layer being low. In some areas where the first openings are distributed more frequently, the thickness deviation between the film layers can reach 30nm or even more, thereby affecting the subsequent photolithography process and reducing the dimensional accuracy of the subsequently formed semiconductor structure.
[0022] Based on this, an embodiment of the present invention provides a method for forming a semiconductor structure, including: providing a substrate, a first mask layer is formed on the surface of the substrate, and the first mask layer has a first opening; forming a sacrificial layer that fills the first opening and exposes the top surface of the first mask layer; forming a second mask layer on the first mask layer, and the second mask layer is used as an initial mask for forming a second opening in the first mask layer. By forming a sacrificial layer that fills the first opening and exposes the top surface of the first mask layer in the first opening, the flatness of the surface of the first mask layer in the embodiment of the present invention is improved, and then the surface flatness of the second mask layer formed on the first mask layer is correspondingly improved, so that the dimensional accuracy of the subsequent photolithography process is improved, and the dimensional accuracy of the semiconductor structure formed subsequently is also improved accordingly.
[0023] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0024] Figures 5 to 14 It is a schematic structural diagram corresponding to each step of the method for forming a semiconductor structure in an embodiment of the present invention.
[0025] refer to Figure 5 , a substrate 200 is provided, a first mask layer 210 is formed on the surface of the substrate 200, and the first mask layer 210 is provided with a first opening W21.
[0026] In this embodiment, the base 200 is used to provide a process basis for subsequent processes. The base 200 may include a substrate, or may include a substrate and active devices formed on the substrate.
[0027] The material of the substrate may be silicon. In other embodiments, the material of the substrate may also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be other types of substrates such as a silicon substrate on an insulator or a germanium substrate on an insulator. The active device is a semiconductor device disposed on the surface of the substrate, which may specifically be a transistor, a capacitor, a resistor, a diode, a photodiode, a fuse, etc., and is formed on the surface of the substrate by a corresponding semiconductor process.
[0028] The substrate 200 may further include a material layer to be processed, and the material layer to be processed is used to expose a portion of the material layer to be processed through the patterned first mask layer, so as to perform corresponding process treatment on the exposed material layer to be processed. Taking the method for forming a gate structure as an example, the functional material layer may be a gate material layer. In other embodiments, according to actual process conditions, the functional material layer may also be other types of material layers, such as an interlayer dielectric layer.
[0029] Optionally, the surface of the substrate 200 may be a plane, so that the surface of the first mask layer formed on the surface of the substrate 200 is a plane.
[0030] The first mask layer 210 is used to expose a portion of the material layer to be processed after patterning. In an embodiment of the present invention, the first mask layer 210 may be a hard mask layer, which may meet the requirements of accuracy and stability of pattern transfer under a smaller critical dimension.
[0031] It should be noted that, during the formation of a complex device structure, the first region of the first mask layer needs to be subjected to a first process, and the second region of the first mask layer needs to be subjected to a second process. Correspondingly, when patterning the first mask layer, it is necessary to open a first opening in the first region, perform the first process on the substrate region exposed by the first opening, and further cover the first opening in the first region, and open a second opening in the second region to perform the second process. The embodiment of the present invention mainly describes the process of covering the first opening after forming the first opening.
[0032] In this embodiment, the material of the first mask layer 210 (hard mask layer) can be silicon nitride. Silicon nitride has high hardness and density, which is conducive to improving the mask effect of the subsequent patterned hard mask layer. In addition, silicon nitride is a commonly used dielectric material in semiconductor processes and has high process compatibility. In other embodiments, the material of the hard mask layer can also be amorphous carbon. In other embodiments, the material of the first mask layer can also be selected from SiOC, SiOCH, SiC, SiCN, SiO 2 , SiN, SiON or one or more thereof.
[0033] refer to Figures 6 to 10 , forming a sacrificial layer filling the first opening and exposing a top surface of the first mask layer.
[0034] By forming a sacrificial layer that fills the first opening and exposes the top surface of the first mask layer, the flatness of the surface of the first mask layer in the present invention is improved, thereby improving the surface flatness of the second mask layer formed on the first mask layer, thereby improving the dimensional accuracy of the subsequent photolithography process, and thus improving the dimensional accuracy of the subsequently formed semiconductor structure.
[0035] In this embodiment, the sacrificial layer can completely fill the first opening, so that the top surface of the sacrificial layer is flush with the top surface of the first mask layer, or can slightly exceed the top surface of the first mask layer. This is because, when the subsequent film layer formation process is performed, the main factor affecting the surface flatness of the film layer is the depression of the underlying film layer. When there are many depressions, it is easy to cause thickness deviations in different areas of the film layer. When the underlying film layer has protrusions that exceed the underlying surface, it is easy to be completely covered by the subsequently formed film layer, thereby having little effect on the flatness of the subsequently formed film layer.
[0036] In other optional embodiments, the sacrificial layer may also partially fill the first opening. When the sacrificial layer partially fills the first opening, the height of the sacrificial layer in the first opening is greater than or equal to 70% of the depth of the first opening, thereby filling most of the space of the first opening, improving the flatness of the surface of the first mask layer, reducing the thickness deviation that may be produced in the subsequently formed second mask layer, and thereby improving the surface flatness of the second mask layer formed on the first mask layer.
[0037] There are multiple first openings, the area where the multiple first openings are located is the first area, and other areas outside the first area are the second area; forming a sacrificial layer in the first openings to fill the first openings can adopt the following process:
[0038] refer to Figure 6 , forming a sacrificial material layer 221 that completely covers the surface of the first mask layer 210, and the sacrificial material layer 221 completely fills the first opening W21, wherein the thickness of the sacrificial material layer on the top of the first mask layer 210 located in the first area 10A is less than the thickness of the sacrificial material layer on the top of the first mask layer 210 located in the second area 20A.
[0039] The sacrificial material layer 221 provides a basis for subsequently forming the sacrificial layer.
[0040] The material of the sacrificial material layer 221 is a material that can be modified in different regions, so that different treatments can be performed according to the characteristics of different regions. In this embodiment, the sacrificial material layer 221 can be a photosensitive material that has cross-linking or degradation characteristics under light, so that light treatment can be used to make the material in the first opening have different characteristics from the material outside the first opening, so that the material outside the first opening is removed according to the corresponding characteristics, thereby achieving filling of only the first opening.
[0041] Specifically, the sacrificial material layer 221 has a cross-linking property under light, and the corresponding material may be an epoxy and phenolic hydroxyl polymer; the sacrificial material layer has a degradation property under light, and the corresponding material may be a polyacrylate polymer.
[0042] The sacrificial material layer can be formed on the surface of the first mask layer by a spin coating process. Specifically, the sacrificial material is spin coated to form a sacrificial material layer that completely fills the first opening on the surface of the first mask layer, and the sacrificial material layer is solidified by baking and other processes. The thickness of the sacrificial material layer should not be too large or too small. If it is too large, it will easily increase the difficulty of the subsequent step of removing the sacrificial material layer, while if it is too small, the sacrificial material layer may not be completely filled. In an embodiment of the present invention, the thickness of the sacrificial material layer can be 100nm to 300nm.
[0043] Wherein, based on the multiple openings in the first region, during the film forming process, the thickness of the sacrificial material layer on top of the first mask layer 210 located in the first region 10A is less than the thickness of the sacrificial material layer on top of the first mask layer 210 located in the second region 20A.
[0044] In this embodiment, the formation of the sacrificial layer filling the first opening can also be achieved based on sacrificial material layers of different thicknesses in different regions. Specifically, based on the thickness of the sacrificial material layer on the top of the first mask layer 210 in the first region 10A being less than the thickness of the sacrificial material layer in the second region 20A, the sacrificial material layer of a preset thickness is removed by dry etching to expose the top surface of the first region 10A, and the etching degree is controlled at the same time, the sacrificial material layer located in the first opening is retained, and the remaining sacrificial material layer in the second region 20A is further removed in a subsequent step.
[0045] Specifically, refer to Figure 7-Figure 8 , modifying the sacrificial material layer so that an etching rate of the sacrificial material layer in the first region in the second etching process is smaller than an etching rate of the sacrificial material layer in the second region in the second etching process.
[0046] By modifying the sacrificial material layer, the sacrificial material layer in the first region and the sacrificial material layer in the second region have different properties, so that the material of the sacrificial material layer in the second region can be removed according to the corresponding properties, thereby achieving filling of the first opening in the first region only.
[0047] Correspondingly, a suitable modification process can be selected so that in the second etching process, the etching selectivity ratio of the sacrificial material layer in the second region to the sacrificial material layer in the first region is greater than or equal to 10:1, thereby achieving removal of the sacrificial material layer in the second region in the second etching process.
[0048] In an optional example, the sacrificial material layer has a cross-linking property under light irradiation, for example, the sacrificial material layer can be a polymer of epoxy and phenolic hydroxyl groups, so that the sacrificial material layer in the first region can be phototreated, so that the etching rate of the sacrificial material layer in the first region in the second etching process is less than the etching rate of the sacrificial material layer in the second region in the second etching process, so that the sacrificial material layer in the first opening is not easy to remove, and thus may not be removed in the subsequent second etching process. Correspondingly, the modification treatment can be phototreatment, and the corresponding modification treatment is performed based on the characteristics of the sacrificial material layer, specifically:
[0049] See also Figure 7 , the sacrificial material layer 221 of the first region 10A is subjected to light treatment.
[0050] Correspondingly, the sacrificial material layer may be exposed using photolithography technology. For example, ultraviolet light is used to illuminate the sacrificial material layer, wherein the wavelength of the ultraviolet light is 360 to 370 nm, for example, 365 nm, and the intensity is 2000 to 3000 mJ / cm 2 .
[0051] In another optional example, the sacrificial material layer has a degradation characteristic under light, for example, the sacrificial material layer can be a polyacrylate polymer, so that the sacrificial material layer in the second region can be phototreated, so that the etching rate of the sacrificial material layer in the first region in the second etching process is less than the etching rate of the sacrificial material layer in the second region in the second etching process, so that the sacrificial material layer in the first opening is not easy to remove, and thus may not be removed in the subsequent second etching process. Similarly, the modification treatment can be phototreatment, and the corresponding modification treatment is performed based on the characteristics of the sacrificial material layer, specifically:
[0052] See also Figure 8 , the sacrificial material layer 221 of the second region 20A is subjected to light treatment.
[0053] In this example, the sacrificial material layer can also be exposed using photolithography technology. For example, ultraviolet light is used to illuminate the sacrificial material layer, wherein the wavelength of the ultraviolet light is 360-370 nm, for example, 365 nm, and the intensity is 2000-3000 mJ / cm 2 .
[0054] refer to Fig. 9 , a first etching process is used to remove the sacrificial material layer 221 in the first region 10A until the top surface of the first mask layer 210 in the first region 10A is exposed.
[0055] The sacrificial material layer in the first area is removed by a first etching process until the top surface of the first mask layer in the first area is exposed, thereby retaining the sacrificial material layer in the first opening as a sacrificial layer.
[0056] In an embodiment of the present invention, a dry etching process with easily controllable etching thickness may be used as the first etching process, so that etching stops when the top surface of the first mask layer exposing the first region, avoiding etching of the sacrificial material layer in the first opening.
[0057] It should be noted that when performing the first etching process, the first etching process simultaneously thins the sacrificial material layer in the second region, thereby reducing the process cost of the subsequent second etching process. Correspondingly, in this step, a dry etching process is used to remove the sacrificial material layer of a preset thickness until the sacrificial material layer 221 remaining in the first region 10A is flush with the surface of the first mask layer 210, thereby retaining the sacrificial material layer filled in the first opening.
[0058] The process of removing the sacrificial material layer may adopt an etching process with anisotropic properties to achieve precise control of the etching thickness. In an embodiment of the present invention, the dry etching process is a plasma etching process, wherein the etching gas is H 2 , CO 2 , CH 4 , O 2 One or more of .
[0059] refer to Fig.10 , using the second etching process to remove the sacrificial material layer in the second region 20A until the top surface of the first mask layer 210 in the second region is exposed.
[0060] Among them, the second etching process is a process that matches the modification process, so that in the second etching process, the etching selectivity ratio of the modified sacrificial material layer in the second area to the sacrificial material layer in the first area is greater than or equal to 10:1.
[0061] Optionally, the second etching process may be a wet etching process, and when the sacrificial material layer has cross-linking properties under light, for example, when the sacrificial material layer is a polymer of epoxy and phenolic hydroxyl groups, the etching liquid used in the second etching process is chloroform or tetrahydrofuran. The second etching process may also be a stripping process, and correspondingly, chloroform or tetrahydrofuran is used as a stripping liquid to remove the sacrificial material layer.
[0062] After optically processing the sacrificial material layer in the first area, the sacrificial material layer in the first opening is difficult to remove. The sacrificial material layer in the second area on the surface of the first mask layer can be removed by further etching process (such as stripping process) compatible with the sacrificial material layer.
[0063] In other examples, the sacrificial material layer has degradation characteristics under light. For example, when the sacrificial material layer is a polyacrylate polymer, the etching solution used in the second etching process is propylene glycol methyl ether (PGME), wherein the second etching process can also be a stripping process, and correspondingly, propylene glycol methyl ether stripping solution is used to remove the sacrificial material layer.
[0064] After the sacrificial material layer in the second area is phototreated, the sacrificial material layer in the second area is relatively easy to remove, and further the sacrificial material layer in the second area on the surface of the first mask layer can be removed by a second etching process adapted to the sacrificial material layer after the phototreatment.
[0065] It should be noted that when removing the sacrificial material layer in the second area in this step, a small amount of residue may be generated. However, since the residue is easily covered by the layer structure and will not affect the surface flatness of the layer structure, the embodiment of the present invention will not be affected by the residue.
[0066] It should be noted that, in the embodiment of the present invention, the second etching process may be performed after the first etching process, or the first etching process may be performed after the second etching process, and the present invention does not make any specific limitation here.
[0067] In some specific examples, for example, if the viscosity of the sacrificial material layer is low in liquid state, the surface of the sacrificial material layer is a flat surface. Correspondingly, the sacrificial material layer of a preset thickness can be removed only until the sacrificial material layer remaining in the first opening is flush with the surface of the first mask layer. That is, the sacrificial material layer above the first mask layer in the first and second areas can be completely removed, leaving only the sacrificial material layer filled in the first opening.
[0068] Next, after forming a sacrificial layer filling the first opening and exposing the top surface of the first mask layer, referring to Fig.11 , forming a hard mask capping layer 230 covering the hard mask layer 210 (ie, the first mask layer).
[0069] The hard mask cap (HM cap) layer 230 is used to further improve the surface flatness of the hard mask layer 210, thereby providing a good interface state for the formation of subsequent film layers. The hard mask cap layer can be a spin on carbon (SOC) layer. The SOC layer is formed by a spin coating process, and the process cost is low; moreover, by using the SOC layer, the surface flatness of the hard mask layer can be significantly improved. In other embodiments, the material of the hard mask cap layer can also be silicon oxide.
[0070] Specifically, when the hard mask cover layer is a spin-on carbon layer, it can be formed by a spin coating process.
[0071] Next, refer to Fig.12 , an anti-reflective coating 240 covering the hard mask capping layer 230 is formed.
[0072] The anti-reflective coating 240 is used to reduce the reflection effect during exposure, thereby improving the transfer accuracy of the pattern. In this embodiment, the anti-reflective coating is a silicon anti-reflective coating (Si-ARC). The Si-ARC layer is beneficial to increasing the exposure depth of field (DOF) during the photolithography process and improving the exposure uniformity. Moreover, the Si-ARC layer is rich in silicon, which is beneficial to improving the hardness of the anti-reflective coating 240, thereby further improving the transfer accuracy of the pattern.
[0073] Next, refer to Fig.13 , forming a second mask layer 250 on the first mask layer 210 .
[0074] The second mask layer 250 is used as an initial mask for forming a second opening in the first mask layer 210 .
[0075] In this embodiment, the first mask layer 210 is a hard mask layer, and the second mask layer 250 is a photolithography mask layer. The corresponding material of the photolithography mask layer 250 may be photoresist. The photoresist may be a positive photoresist or a negative photoresist, which is not specifically limited in the present invention.
[0076] The second mask layer 250 is provided with a mask opening corresponding to the second opening, so that a second opening can be formed on the first mask layer 210 exposed by the mask opening of the second mask layer. The second opening can be located in the first region and / or the second region, and the present invention does not make any specific limitation here.
[0077] Specifically, the formation process of the second mask layer 250 may include: forming a second mask material layer on the anti-reflective coating 240, exposing and developing the second mask material layer to form the mask opening. The second mask material layer is a photoresist layer, which may be formed by spin coating and curing processes, and the exposure and development may be achieved using corresponding process parameters.
[0078] refer to Fig.14 After forming the second mask layer, the embodiment of the present invention further performs etching of the first mask layer. In the embodiment of the present invention, the first mask layer 210 is a hard mask layer. Correspondingly, the etching process of the hard mask layer may include:
[0079] Using the second mask layer as an initial mask, the anti-reflective coating 240, the hard mask cover layer 230 and the hard mask layer 210 are sequentially etched to form a second opening W22 on the hard mask layer 210; and the remaining photolithography mask layer, the hard mask cover layer and the anti-reflective coating are removed.
[0080] The etching process may be a plasma etching process, in which the anti-reflective coating 240, the hard mask cover layer 230 and the hard mask layer 210 are sequentially etched to form a second opening on the hard mask layer. Further, after the second opening is formed, the remaining photolithography mask layer, the hard mask cover layer and the anti-reflective coating are removed, so that in a subsequent process, the etched hard mask layer can be used as a mask to perform a subsequent process.
[0081] In an embodiment of the present invention, a sacrificial layer filling the first opening and exposing the top surface of the first mask layer is formed in the first opening of the first mask layer, so that the flatness of the surface of the first mask layer itself is improved, and then the surface flatness of the second mask layer formed on the first mask layer is correspondingly improved, so that the dimensional accuracy of the subsequent photolithography process is improved, and thus the dimensional accuracy of the subsequently formed semiconductor structure is also correspondingly improved.
[0082] The present invention also provides a semiconductor structure, referring to Fig.15 ,include:
[0083] A substrate 300 is provided with a first mask layer 310 , wherein a first opening W31 is formed in the first mask layer 310 ; a sacrificial layer 320 is located in the first opening W31 , wherein the sacrificial layer 320 fills the first opening W31 ; and a second mask layer 350 is located on the first mask layer 310 .
[0084] The material of the substrate may be silicon. In other embodiments, the material of the substrate may also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be other types of substrates such as a silicon substrate on an insulator or a germanium substrate on an insulator. The active device is a semiconductor device disposed on the surface of the substrate, which may specifically be a transistor, a capacitor, a resistor, a diode, a photodiode, a fuse, etc., and is formed on the surface of the substrate by a corresponding semiconductor process.
[0085] The substrate may further include a material layer to be processed, and the material layer to be processed is used to expose a portion of the material layer to be processed through the patterned first mask layer, so as to perform corresponding process treatment on the exposed material layer to be processed. Taking the method for forming a gate structure as an example, the functional material layer may be a gate material layer. In other embodiments, according to actual process conditions, the functional material layer may also be other types of material layers, such as an interlayer dielectric layer.
[0086] Optionally, the substrate surface may be a plane, so that the surface of the first mask layer formed on the substrate surface is a plane.
[0087] The first mask layer 310 is used to expose a portion of the material layer to be processed after patterning. In an embodiment of the present invention, the first mask layer 310 may be a hard mask layer, which may meet the requirements of accuracy and stability of pattern transfer under a smaller critical dimension.
[0088] In this embodiment, the material of the first mask layer 310 (hard mask layer) can be silicon nitride. Silicon nitride has high hardness and density, which is conducive to improving the mask effect of the subsequent patterned hard mask layer. In addition, silicon nitride is a commonly used dielectric material in semiconductor processes and has high process compatibility. In other embodiments, the material of the hard mask layer can also be amorphous carbon. In other embodiments, the material of the first mask layer 310 can also be selected from SiOC, SiOCH, SiC, SiCN, SiO 2 , SiN, SiON or one or more thereof.
[0089] In this embodiment, the sacrificial layer 320 located in the first opening W31 completely fills the first opening W31, so that the flatness of the surface of the first mask layer 310 in the present application is improved, and then the surface flatness of the second mask layer 350 formed on the first mask layer 310 is correspondingly improved, so that the dimensional accuracy of the subsequent photolithography process is improved, and the dimensional accuracy of the subsequently formed semiconductor structure is also correspondingly improved.
[0090] In other optional embodiments, the sacrificial layer may also partially fill the first opening. When the sacrificial layer partially fills the first opening, the height of the sacrificial layer in the first opening is greater than or equal to 70% of the depth of the first opening, thereby filling most of the space of the first opening, improving the flatness of the surface of the first mask layer, reducing the thickness deviation that may be produced in the subsequently formed second mask layer, and thereby improving the surface flatness of the second mask layer formed on the first mask layer.
[0091] Furthermore, the sacrificial layer 320 has a cross-linking property under light, or the sacrificial layer has a degradation property under light.
[0092] The material of the sacrificial material layer can be a photosensitive material with cross-linking or degradation characteristics under light, so that a photolithography process can be used to make the material inside the first opening have different properties from the material outside the first opening, so that the material outside the first opening is removed according to the corresponding characteristics, thereby achieving filling of only the first opening.
[0093] Specifically, the sacrificial material layer has a cross-linking property under light, and the corresponding material may be an epoxy and phenolic hydroxyl polymer; the sacrificial material layer has a degradation property under light, and the corresponding material may be a polyacrylate polymer.
[0094] The sacrificial material layer can be formed on the surface of the first mask layer by a spin coating process. Specifically, the sacrificial material is spin coated to form a sacrificial material layer that completely fills the first opening on the surface of the first mask layer, and the sacrificial material layer is solidified by baking and other processes. The thickness of the sacrificial material layer should not be too large or too small. If it is too large, it will easily increase the difficulty of the subsequent step of removing the sacrificial material layer, while if it is too small, the sacrificial material layer may not be completely filled. In an embodiment of the present invention, the thickness of the sacrificial material layer can be 100nm to 300nm.
[0095] The sacrificial material layer may be exposed using photolithography technology. For example, ultraviolet light is used to expose the sacrificial material layer, wherein the wavelength of the ultraviolet light is 360-370 nm, for example, 365 nm, and the intensity is 2000-3000 mJ / cm 2 .
[0096] Optionally, the first mask layer 310 is a hard mask layer, the second mask layer 350 is a photolithography mask layer, and a hard mask cover layer 330 covering the hard mask layer and an anti-reflective coating 340 covering the hard mask cover layer 330 are included between the first mask layer 310 and the second mask layer 350 .
[0097] The corresponding material of the photolithography mask layer may be photoresist, which may be positive photoresist or negative photoresist, and may be formed by spin coating and curing processes, which are not specifically limited in the present invention.
[0098] The second mask layer 350 is provided with a mask opening corresponding to the second opening W32 , so that a second opening can be formed on the first mask layer 310 exposed by the mask opening of the second mask layer 350 .
[0099] In an embodiment of the present invention, a sacrificial layer filling the first opening is provided in the first opening, so that the flatness of the surface of the first mask layer itself in the present application is improved, thereby making the surface flatness of the second mask layer formed on the first mask layer correspondingly improved, thereby improving the dimensional accuracy of the subsequent photolithography process, and thus improving the dimensional accuracy of the subsequently formed semiconductor structure accordingly.
[0100] The semiconductor structure can be formed by the formation method described in the above embodiment, or by other formation methods. For the specific description of the semiconductor structure described in this embodiment, reference can be made to the corresponding description in the above embodiment, and this embodiment will not be repeated here.
[0101] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, wherein a first mask layer is formed on a surface of the substrate, wherein the first mask layer is provided with a first opening, wherein there are a plurality of first openings, wherein an area where the plurality of first openings are located is a first area, and other areas outside the first area are second areas; The sacrificial layer filling the first opening and exposing the top surface of the first mask layer comprises: forming a sacrificial material layer completely covering the surface of the first mask layer, the sacrificial material layer completely filling the first opening, wherein the thickness of the sacrificial material layer at the top of the first mask layer in the first area is less than the thickness of the sacrificial material layer at the top of the first mask layer in the second area; performing a modification treatment on the sacrificial material layer so that the etching rate of the sacrificial material layer in the first area in the second etching process is less than the etching rate of the sacrificial material layer in the second area in the second etching process; after performing the modification treatment, using the first etching process to remove the sacrificial material layer in the first area until the top surface of the first mask layer in the first area is exposed; after performing the modification treatment, using the second etching process to remove the sacrificial material layer in the second area until the top surface of the first mask layer in the second area is exposed; A second mask layer is formed on the first mask layer, and the second mask layer is used as an initial mask for forming a second opening in the first mask layer.
2. The method for forming a semiconductor structure according to claim 1, wherein: The sacrificial layer completely fills the first opening or partially fills the first opening; when the sacrificial layer partially fills the first opening, the height of the sacrificial layer in the first opening is greater than or equal to 70% of the depth of the first opening.
3. The method for forming a semiconductor structure according to claim 1, wherein: The second etching process is performed after the first etching process; the first etching process simultaneously thins the sacrificial material layer in the second region, and in the second etching process, the etching selectivity ratio of the sacrificial material layer in the second region to the sacrificial material layer in the first region is greater than or equal to 10:
1.
4. The method for forming a semiconductor structure according to claim 3, wherein: The sacrificial material layer has cross-linking properties under light exposure; The modification process includes: performing phototreatment on the sacrificial material layer in the first region.
5. The method for forming a semiconductor structure according to claim 4, wherein: The sacrificial material layer is a polymer of epoxy and phenolic hydroxyl groups.
6. The method for forming a semiconductor structure according to claim 4, wherein: The second etching process is a wet etching process, and the etching solution used in the second etching process is chloroform or tetrahydrofuran.
7. The method for forming a semiconductor structure according to claim 3, wherein: The sacrificial material layer has a degradation characteristic under light exposure; The modification process includes: performing phototreatment on the sacrificial material layer in the second region.
8. The method for forming a semiconductor structure according to claim 7, wherein: The sacrificial material layer is a polyacrylate polymer.
9. The method for forming a semiconductor structure according to claim 7, wherein: The second etching process is a wet etching process, and the etching solution used in the second etching process is propylene glycol methyl ether.
10. The method for forming a semiconductor structure according to claim 4 or 7, characterized in that: The light treatment uses ultraviolet light.
11. The method for forming a semiconductor structure according to claim 10, wherein: The wavelength of the ultraviolet light is 360-370nm, and the intensity is 2000-3000mJ / cm 2 .
12. The method for forming a semiconductor structure according to claim 1, wherein: The first etching process is a dry etching process.
13. The method for forming a semiconductor structure according to claim 12, wherein: The dry etching process is a plasma etching process, wherein the etching gas is one or more of H2, CO2, CH4, and O2.
14. The method for forming a semiconductor structure according to claim 1, wherein: The first mask layer is a hard mask layer, the second mask layer is a photolithography mask layer, and after forming a sacrificial layer that fills the first opening and exposes the top surface of the first mask layer and before forming the second mask layer on the first mask layer, the method further includes: forming a hard mask capping layer covering the hard mask layer; An anti-reflective coating is formed covering the hard mask capping layer.
15. The method for forming a semiconductor structure according to claim 14, wherein: After forming the second mask layer on the first mask layer, the method further includes: Using the second mask layer as an initial mask, sequentially etching the hard mask cover layer, the anti-reflective coating layer and the hard mask layer to form a second opening on the hard mask layer; wherein the second opening is located in the first region and / or the second region; The remaining second mask layer, the hard mask cap layer and the anti-reflective coating are removed.
16. A semiconductor structure obtained by the method for forming a semiconductor structure according to any one of claims 1 to 14, characterized in that: include: A substrate, wherein a first mask layer is disposed on the substrate, and a first opening is formed in the first mask layer; a sacrificial layer located in the first opening, the sacrificial layer filling the first opening; A second mask layer is located on the first mask layer.
17. The semiconductor structure according to claim 16, wherein: The sacrificial layer has a cross-linking property under light irradiation, or the sacrificial layer has a degrading property under light irradiation.
18. The semiconductor structure according to claim 16, wherein: When the sacrificial layer has cross-linking properties under light, the sacrificial layer is a polymer of epoxy and phenolic hydroxyl groups; When the sacrificial layer has a degradation characteristic under light, the sacrificial layer is a polyacrylate polymer.
19. The semiconductor structure according to claim 16, wherein: The first mask layer is a hard mask layer, the second mask layer is a photolithography mask layer, and a hard mask cover layer covering the hard mask layer and an anti-reflective coating covering the hard mask cover layer are further included between the first mask layer and the second mask layer.