A porous film getter structure and preparation method thereof
By forming porous film getter structure and gold particle-assisted etching technology in high-vacuum MEMS devices, the problems of small deposition surface area and weak adhesion of film getter are solved, and higher suction performance and service life are achieved .
Patent Information
- Application Number
- CN202111091412.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-09-17
AI Technical Summary
In existing high-vacuum MEMS devices, the deposition surface area of the thin film getter is small, the side wall adhesion is weak, and it is easy to fall off, resulting in difficulty in maintaining the vacuum degree and short service life.
Using a porous film getter structure, by forming a groove structure on the wafer surface and setting a porous structure on its inner wall, gold particles assist in etching to form a uniformly distributed porous structure, and after high-temperature annealing, the film getter is evaporated to Increase the deposition area and adhesion.
It effectively increases the deposition area and adhesion of the film getter, avoids shedding, extends service life and maintains the stability of high vacuum.
Smart Images

Figure CN113772618B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs exclusively to the field of high vacuum MEMS device packaging, and in particular relates to a porous film getter structure and a preparation method thereof. Background Art
[0002] At present, the requirements for the internal vacuum degree and service life of devices in the field of high vacuum MEMS packaging are getting higher and higher. In particular, as electronic devices are becoming increasingly miniaturized, how to maintain high vacuum degree and service life in a limited space has become a technical difficulty. In today's electronic packaging field, the most common method of maintaining vacuum degree is to evaporate thin film getters inside electronic devices. The characteristics of thin film getters are to continuously absorb residual gas, infiltrated gas and residual adsorbed gas inside the cavity. This achieves the requirement of maintaining the internal vacuum degree of electronic devices.
[0003] The air absorption performance of thin film getters is mainly related to their deposition surface area and material properties. Under the condition that the material properties are not much different, increasing their deposition surface area becomes the most suitable method to improve their air absorption efficiency. At present, there is a related patent that increases the deposition area of the getter by preparing a vertical three-dimensional structure of bumps and grooves inside the cavity. First of all, the simple concave-convex structure designed by the patent has limited effect on the increase of the deposition area of the getter. In addition, the three-dimensional structure of bumps and grooves is weakly dense. The most critical thing is that the adhesion between the thin film getter deposited on the smooth side wall and the side wall is very weak. The weak adhesion between the film and the side wall can easily cause the thin film getter to fall off during the use of the device, polluting the inside of the device, causing the performance of the device's thermal sensitive unit to decline or even fail. In addition, the three-dimensional getter structure prepared in the related patent has no attached support structure and is prone to fracture and collapse. Therefore, the practicality of this patent is weak and difficult to use in actual production. In the prior art, there is a silicon processing technology for wafers that uses direct deposition of gold particles to form a porous structure. However, gold particles can only be directly deposited on a flat wafer substrate. Therefore, this process can basically only etch the surface of the wafer base, and the increase in the getter structure is still limited. In addition, the density of the directly deposited gold particles will form a very dense porous structure on the base surface. When the porous structure is too dense, the bottom porous structure is very easy to break and collapse. Therefore, the application of this technology is very limited. Summary of the invention
[0004] In view of the above problems existing in the prior art, the present invention provides a porous film getter structure and a preparation method thereof that can effectively increase the film deposition area and the adhesion between the film and the side wall. Not only can the amount of getter be greatly increased, but also the film can be effectively prevented from falling off and damaging the device, thereby achieving the advantages of improving the internal vacuum degree of the electronic device, extending the service life, and maintaining high stability.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A porous film getter structure comprises a wafer and a film getter, wherein the upper surface of the wafer has a groove structure, the inner wall of the groove structure is a porous structure, the porous structure is provided with a film getter, and the film getter covers the porous structure.
[0007] Preferably, the wafer is provided with more than two groove structures, and the wafer surface connecting adjacent groove structures is a porous structure, a thin film getter is provided on the porous structure, and the thin film getter covers the porous structure.
[0008] Preferably, gold particles are provided on the bottom surface of the pores of the porous structure, and the thin film getter covers the gold particles; the size of the gold particles is 20 nm to 5 μm.
[0009] Preferably, the cross section of the groove structure is a trapezoid, a V-shape or a " "shape.
[0010] Preferably, the pores are arranged at an angle to the inner wall of the groove structure; the angle is greater than 0 and less than 180°.
[0011] As a general inventive concept, the present invention also provides a method for preparing a porous thin film getter structure, comprising the following steps:
[0012] S1, forming a protective layer on the upper and lower surfaces of the wafer, and forming a patterned photoresist layer on the protective layer on the upper surface of the wafer, using the patterned photoresist layer as a mask to pattern the protective layer on the upper surface of the wafer to expose the wafer surface area that needs to be etched;
[0013] S2, using the patterned photoresist layer as a mask, dry-etching the wafer to form a groove structure, and then removing the patterned photoresist layer; or first removing the patterned photoresist layer, using the protective layer as a mask, and wet-etching the wafer to form a groove structure;
[0014] S3, forming a patterned photoresist layer in the groove structure area on the upper surface of the wafer, and forming a photoresist layer on the upper surface of the wafer outside the groove structure area, so as to form a patterned window on the inner wall of the groove in the groove structure area or on the inner wall of the groove and the wafer surface;
[0015] S4, forming a gold film on the patterned window surface in the groove structure area;
[0016] S5, annealing the gold-coated wafer at high temperature, so that the gold film is transformed into gold particles under the action of stress;
[0017] S6, using a corrosive liquid to wet-etch the wafer after high-temperature annealing, and corroding the groove structure area into a porous structure through the catalytic effect of gold;
[0018] S7. Depositing a thin film getter on the upper surface of the wafer by a photolithography stripping process.
[0019] Preferably, in step S2, the groove structure is one or more than two; when there is one groove structure, the groove structure constitutes a groove structure area, and when there are more than two groove structures, each groove structure and the area connecting adjacent groove structures constitute a groove structure area; when there are more than two groove structures, step S2 also includes removing the protective layer connecting adjacent groove structures by etching after forming the groove structure.
[0020] When there are more than two groove structures, in step S3, a patterned photoresist layer is formed in the groove structure area on the upper surface of the wafer, and a photoresist layer is formed on the upper surface of the wafer outside the groove structure area to form a patterned window on the inner wall of the groove in the groove structure area and the wafer surface.
[0021] Preferably, in step S2, the cross section is formed by dry etching. "-shaped groove, and the groove with a trapezoidal or V-shaped cross section is formed by wet etching.
[0022] Preferably, in step S5, the holding temperature of the high temperature annealing is 600-1000°C; the holding time of the high temperature annealing is 2-60 min; the heating rate of the high temperature annealing is 5-25°C / min; and the annealing rate of the high temperature annealing is 5-25°C / min.
[0023] Preferably, in step S1, the protective layer is one or more metal films selected from the group consisting of Ti, Pt, and Cr; and the protective layer is deposited by magnetron sputtering or evaporation.
[0024] Preferably, in step S6, the etching solution is a mixed etching solution of hydrofluoric acid and hydrogen peroxide; and the temperature of the wet etching is 25-60°C.
[0025] Preferably, in the mixed etching solution, the mass fraction of the hydrofluoric acid is 5-20%, and the mass fraction of the H2O2 is 5-30%.
[0026] Preferably, in step S4, the thickness of the gold film is 30-150 nm.
[0027] Step S4 specifically includes: forming a gold film on the upper surface of the wafer by evaporation, deposition or sputtering, then removing the patterned photoresist layer in the groove structure area and the photoresist layer on the upper surface of the wafer outside the groove structure area, forming a gold film on the patterned window in the groove structure area, and then cleaning the wafer.
[0028] Preferably, in step S1, the wafer is a double-polished silicon wafer, and before coating the protective layer, the silicon wafer is subjected to inorganic cleaning and organic cleaning.
[0029] Preferably, in step S2, the cross section of the groove structure is a trapezoid, a V-shape or a " "shape. <100> During wet etching, the silicon wafer will be corroded along the 110 crystal direction, with almost no corrosion on the 111 crystal surface. The corrosion structure presents a slope of 54.7°. The overall structure can form a V-shape or a trapezoidal shape according to the size and depth of the corrosion opening. Under dry etching conditions, a " "-shaped groove deep cavity structure.
[0030] Between step S6 and step S7 or after step S7, a step of removing the protective layer on the surface of the wafer is also included; the protective layer can be removed by etching.
[0031] In step S7, the thin film getter component is generally an alloy structure composed of several metals such as Zr, Co, Re, and Zn.
[0032] Compared with the prior art, the beneficial effects produced by the present invention are:
[0033] 1. The present invention adopts dry or wet etching combined with gold particles to assist in etching a three-dimensional thin film getter structure, and can prepare a porous structure on the prepared groove structure to increase the deposition area of the thin film getter and the volume of the deposited getter. The deposition area and the deposition amount are much larger than the existing three-dimensional concave-convex structure, thereby effectively increasing the getter performance and service life of the thin film getter; the gold film deposited by the evaporation-stripping process can form evenly distributed gold particles on the side wall and the base of the groove under the process conditions of high-temperature rapid annealing, and the annealed gold particles are used for the etching process to etch a uniformly distributed porous structure on the side wall, thereby avoiding the limitation of directly depositing gold particles for etching. The holes formed by etching, especially the holes on the side wall, can effectively increase the adhesion of the getter film and the side wall and bottom substrate after the getter is deposited, thereby avoiding the phenomenon of getter falling off and damaging the device.
[0034] 2. The gold particles on the inner wall of the groove and the surface of the wafer in the present invention cooperate with the etching liquid to etch holes with controllable diameters ranging from nanometers to several microns on the side walls and the surface of the wafer. The size parameters of the porous structure can be adjusted by setting the thickness of the gold plating film and the high-temperature annealing parameters. This is an effect that is difficult to obtain by dry etching and conventional wet processes. Therefore, it plays a great role in maintaining the internal vacuum of high-vacuum electronic devices and extending their service life. Moreover, the distribution spacing of the gold particles after high-temperature rapid annealing is relatively uniform, and an overly dense and messy structure will not be formed. Therefore, the porous structure formed has good structural stability and will not break or collapse due to being too dense. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic structural diagram of the porous film getter structure of Example 1.
[0036] Figure 2 This is a diagram of the preparation process of the porous thin film getter structure of Example 1.
[0037] Figure 3 This is a schematic structural diagram of the porous film getter structure of Example 2.
[0038] Figure 4 This is a diagram of the preparation process of the porous thin film getter structure of Example 2. DETAILED DESCRIPTION
[0039] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0040] In view of the current situation that the traditional two-dimensional planar structure thin film getter has a small deposition surface area, the side wall film of the three-dimensional structure has low adhesion, is easy to fall off and damage the device, and the size of the side wall opening is difficult to control, the present invention designs a porous thin film getter structure assisted by gold particles. The gold particle assisted etching is performed on the cavity structure after dry etching, which can effectively increase the deposition area of the thin film getter. On the other hand, the porous structure on the side wall of the cavity can effectively increase the film deposition area and the adhesion between the film and the side wall, and effectively avoid the phenomenon of film falling off and damage to the device. Thereby achieving the advantages of improving the internal vacuum degree of the electronic device, extending the service life, and maintaining high stability.
[0041] The present invention provides the following technical solutions:
[0042] Double-polished silicon wafers are used, and inorganic cleaning and organic cleaning are performed on the silicon wafers respectively. One or more metal films of Ti, Pt, and Cr are plated on the upper and lower surfaces of the double-polished silicon wafers by magnetron sputtering or evaporation as protective layers, and then the protective layer is patterned, that is, photoresist is coated on the surface of the wafer and patterned, and the surface protective layer is removed by etching.
[0043] The wafer surface is etched with regular and orderly vertical, trapezoidal or V-shaped grooves using dry etching or wet etching processes.
[0044] A layer of gold film is sputtered or evaporated on the concave or V-shaped cavity structure of the wafer using a lift-off process.
[0045] The wafer after gold film coating is subjected to high temperature rapid annealing process. The temperature can be rapidly increased first, with a heating rate of 5 to 25°C / min, and then the temperature is increased to 600 to 1000°C, and maintained for 2 to 60 minutes before the rapid annealing process is performed. The annealing rate (cooling rate) is between 5 and 25°C / min. The gold film will be converted into nano- or micron-sized gold particles under the action of stress, and evenly distributed on the side walls and base of the cavity structure. The melting points of the protective layers Ti and Pt are both above 1600°C and will not be affected by annealing;
[0046] A mixed etching solution of HF, H2O2 and H2O is prepared, and evenly distributed gold particles are used to perform wet etching on the side walls and base area of the cavity, thereby etching a porous structure on the side walls and bottom of the cavity.
[0047] The thin film getter is evaporated in the wafer area where coating is required.
[0048] Aiming at the current situation that the conventional two-dimensional planar structure thin film getter has a small deposition surface area, the side wall film of the three-dimensional structure has low adhesion, is easy to fall off and damage the device, and the size of the side wall opening is difficult to control, the present invention designs a gold film annealing process to prepare gold particles evenly distributed on the side wall and the substrate, and cooperates with HF and H2O2 solution to assist in etching the porous thin film getter structure. The gold particle-assisted etching on the cavity side wall and substrate structure after dry or wet etching has the following three advantages:
[0049] First: The combination of the two etching processes can effectively increase the deposition area of the thin film getter, and the deposition area is much larger than the original three-dimensional concave-convex structure.
[0050] Second: During the rapid annealing process of gold film annealing, due to the effect of stress, evenly distributed gold particles will be formed on the side wall after annealing is completed, and the evenly distributed porous structure can be etched on the side wall with the corrosive liquid, avoiding the limitation of directly depositing gold particles for etching. The porous structure on the side wall of the cavity can effectively increase the adhesion between the film and the side wall, effectively avoiding the phenomenon of film shedding and device damage.
[0051] Third: The diameter of the holes etched on the sidewalls and the substrate is controllable. The hole size can be designed and adjusted in the previous gold plating process stage. After high-temperature rapid annealing, the distribution spacing of the gold particles is relatively uniform, and will not form an overly dense and messy structure. Therefore, the formed porous structure will not break and collapse due to being too dense.
[0052] The present invention uses high-temperature rapid annealing of a gold film to form gold particles and a corrosive liquid to perform secondary processing on a three-dimensional groove or V-shaped cavity structure to form a porous structure of a thin film getter, which can achieve the advantages of improving the internal vacuum degree of electronic devices, extending service life, and maintaining high stability.
[0053] Example 1
[0054] A porous film getter structure, such as Figure 1 As shown, it includes a wafer and a thin film getter, the upper surface of the wafer has a plurality of groove structures, the inner walls of the groove structures are all porous structures, and the surface of the wafer connecting adjacent groove structures is also a porous structure, a thin film getter is arranged on the porous structure, and the thin film getter covers the porous structure.
[0055] The bottom surface of the pores of the porous structure is provided with gold particles, and the thin film getter covers the gold particles. The particle size of the gold particles is between tens of nanometers and several micrometers, and can be adjusted according to the required structural size of the thin film getter.
[0056] The cross section of the groove structure is " "shape.
[0057] The above-mentioned porous film getter structure, i.e., the production of the cap silicon wafer, the specific preparation process is shown in the figure Figure 2 As shown, the following steps are included:
[0058] S1. Use double-polished silicon wafers to perform inorganic cleaning and organic cleaning respectively. Plate protective layers of Ti (20-100nm) and Pt (200-500nm) on the front and back of the wafer, and form a patterned photoresist layer on the protective layer on the upper surface of the wafer. Use the patterned photoresist layer as a mask, and then etch to pattern the protective layer on the upper surface of the wafer to expose the wafer area that needs to be etched;
[0059] S2, using the patterned photoresist layer as a mask, dry-etching the wafer to form a plurality of regular and orderly groove structures, the cross-section of the groove structure is " " shape, remove the photoresist layer, and remove the protective layer on the wafer surface connecting adjacent grooves by etching;
[0060] S3, using a spraying and stripping process to expose the area where the thin film getter needs to be plated, that is, forming a patterned photoresist layer on the groove structure area on the upper surface of the wafer (that is, the inner wall of the groove structure and the wafer surface connecting adjacent groove structures), and forming a photoresist layer on the upper surface of the wafer outside the groove structure area to form a patterned window;
[0061] S4, forming a gold film on the upper surface of the wafer and the inner wall of the groove structure region by evaporation, then stripping and removing the patterned photoresist layer in the groove structure region and the photoresist layer on the upper surface of the wafer outside the groove structure region, forming a patterned gold film on the patterned windows in the groove structure region (the inner wall of the groove structure and the patterned windows of the connecting portion connecting adjacent groove structures), and then cleaning the wafer;
[0062] S5, annealing the gold-film-plated wafer at high temperature, so that the gold film is transformed into gold particles under the action of stress;
[0063] S6. Use a corrosive liquid to wet-etch the wafer after high-temperature annealing, and use the catalytic effect of gold to corrode the groove structure area into a porous structure. In this process, the thickness of the gold film evaporation determines the particle size after annealing, and the size of the gold particles determines the diameter of the porous structure. The thickness of the gold film coating can be changed according to the actual process requirements.
[0064] S7. Depositing a thin film getter on the upper surface of the wafer by a photolithography stripping process.
[0065] In step S2, the dry etching conditions are to use SF6 and C4F8 gases to perform deep silicon etching of the wafer cavity structure to etch out the groove structure. The specific etching parameters are: chamber pressure 40mTorr, source power 2500W, C4F8 gas volume flow rate 200cm 3 / min, SF6 gas volume flow rate 300cm 3 / min.
[0066] In step S5, the wafer after gold film coating is subjected to high temperature rapid annealing process, which can be first rapidly heated at a rate of 5 to 25°C / min, heated to 600 to 1000°C, and maintained for a period of 2 to 60 minutes, and then subjected to rapid annealing process at a rate of 5 to 25°C / min. The gold film will be converted into micron-sized gold particles under the action of stress, and evenly distributed on the sidewalls and base of the cavity structure. The melting points of the protective layers Ti and Pt are both above 1600°C and will not be affected by annealing.
[0067] In step S6, a mixed etching solution of hydrofluoric acid and hydrogen peroxide is prepared, and the prepared mixed etching solution is used to wet-etch the annealed wafer. The essence of the etching process is to use H2O2 / HF etching solution and gold particles to form an electrochemical etching system. The gold particles act as reaction catalysts to dig holes downward. The hole diameter and depth are jointly determined by the etching solution concentration, reaction temperature, and the diameter of the gold particles.
[0068] The etching liquid is a mixed etching liquid of hydrofluoric acid and hydrogen peroxide; in the mixed etching liquid, the mass fraction of hydrofluoric acid is 5-20%, and the mass fraction of H2O2 is 5-30%; the reaction temperature of the etching is 40°C.
[0069] In step S4, the thickness of the gold film is 3-150 nm.
[0070] In step S7, a thin film getter is deposited on the top of the wafer by using a photolithography stripping process, and the specific process is spraying, exposure, development, coating, and stripping. The thin film deposition process can be sputtering or evaporation, and the thin film getter component is generally an alloy structure composed of several metals such as Zr, Co, Re, and Zn.
[0071] Example 2
[0072] A porous film getter structure, such as Figure 3 As shown, it includes a wafer and a thin film getter, the upper surface of the wafer has a groove structure, the inner wall of the groove structure is a porous structure, the thin film getter is arranged on the porous structure, and the thin film getter covers the porous structure.
[0073] The bottom surface of the pores of the porous structure is provided with gold particles, and the thin film getter covers the gold particles. The particle size of the gold particles is from tens of nanometers to several micrometers; and the cross section of the groove structure is V-shaped.
[0074] The wafer is provided with more than two groove structures, and the wafer surface connecting adjacent groove structures is a porous structure, a thin film getter is provided on the porous structure, and the thin film getter covers the porous structure.
[0075] The above-mentioned porous film getter structure, i.e., the production of the cap silicon wafer, the specific preparation process is shown in the figure Figure 4 As shown, the following steps are included:
[0076] S1. Use double-polished silicon wafers to perform inorganic cleaning and organic cleaning respectively. Plate protective layers of Ti (20-100nm) and Pt (200-500nm) on the front and back of the wafer, and form a patterned photoresist layer on the protective layer on the upper surface of the wafer. Use the patterned photoresist layer as a mask to perform etching to pattern the protective layer on the upper surface of the wafer, exposing the wafer surface area that needs to be etched;
[0077] S2, removing the patterned photoresist layer, and then using the patterned protective layer as a mask, wet etching the wafer to form a plurality of regular and orderly groove structures, the cross-section of the groove structure is V-shaped, and removing the protective layer on the wafer surface connecting adjacent grooves by etching;
[0078] S3, using a spraying and stripping process to expose the area where the thin film getter needs to be plated, that is, forming a patterned photoresist layer on the groove structure area on the upper surface of the wafer (that is, the inner wall of the groove structure and the wafer surface connecting adjacent groove structures), and forming a photoresist layer on the upper surface of the wafer outside the groove structure area to form a patterned window;
[0079] S4, forming a gold film on the upper surface of the wafer by evaporation, then stripping and removing the patterned photoresist layer in the groove structure area and the photoresist layer on the upper surface of the wafer outside the groove structure area, forming a patterned gold film on the patterned window in the groove structure area, and then cleaning the wafer;
[0080] S5, annealing the gold-film-plated wafer at high temperature, so that the gold film is transformed into gold particles under the action of stress;
[0081] S6. Use a corrosive liquid to wet-etch the wafer after high-temperature annealing, and use the catalytic effect of gold to corrode the groove structure area into a porous structure. In this process, the thickness of the gold film evaporation determines the particle size after annealing, and the size of the gold particles determines the diameter of the porous structure. The thickness of the gold film coating can be changed according to the actual process requirements.
[0082] S7. Depositing a thin film getter on the upper surface of the wafer by a photolithography stripping process.
[0083] In step S2, the wet etching condition is to use TMAH (concentration 25%) or KOH solution (concentration 10-30%) at 25-80° C. The specific etching conditions can be changed according to actual process requirements.
[0084] In step S5, the wafer after gold film coating is subjected to high temperature rapid annealing process, which can be first rapidly heated at a rate of 5 to 25°C / min, heated to 600 to 1000°C, and maintained for a period of 2 to 60 minutes, and then subjected to rapid annealing process at a rate of 5 to 25°C / min. The gold film will be converted into micron-sized gold particles under the action of stress, and evenly distributed on the sidewalls and base of the cavity structure. The melting points of the protective layers Ti and Pt are both above 1600°C and will not be affected by annealing.
[0085] In step S6, a mixed etching solution of hydrofluoric acid and hydrogen peroxide is prepared to perform wet etching on the annealed wafer. The essence of the etching process is to use H2O2 / HF etching solution and gold particles to form an electrochemical etching system. The gold particles act as reaction catalysts to dig holes downward. The hole diameter and depth are jointly determined by the etching solution concentration, reaction temperature, and the diameter of the gold particles.
[0086] The etching liquid is a mixed etching liquid of hydrofluoric acid and hydrogen peroxide; in the mixed etching liquid, the mass fraction of hydrofluoric acid is 5-20%, and the mass fraction of H2O2 is 5-30%; the reaction temperature of the etching is 40°C.
[0087] In step S4, the thickness of the gold film is 30-150 nm.
[0088] In step S7, a thin film getter is deposited on the top of the wafer by using a photolithography stripping process, and the specific process is spraying, exposure, development, coating, and stripping. The thin film deposition process can be sputtering or evaporation, and the thin film getter component is generally an alloy structure composed of several metals such as Zr, Co, Re, and Zn.
[0089] The present invention adopts double-polished silicon wafers, and needs to first use dry or wet etching process to prepare a vertical or V-shaped groove substrate on the wafer surface, and plate a certain thickness of gold film. The thickness of the gold film directly affects the size of gold particles and the diameter of the sidewall and substrate etching holes. The uniform gold film adopts a rapid annealing process to prepare uniformly distributed gold particles, and uses HF and H2O2 mixed solution to etch the sidewall and bottom of the groove with gold particles to form a porous structure. The hole diameter size is controllable, and the hole size can be completely designed and regulated in the front gold film plating process stage. The size of the gold particles after annealing can be adjusted by adjusting the thickness of the gold film, so as to adjust the size of the porous structure to adapt to the structural size required for depositing the thin film getter. In addition, the porous structure not only effectively increases the deposition surface of the thin film getter, but also enhances the adhesion of the thin film getter to the sidewall, prolongs the service life of the MEMS chip under high vacuum, and prevents the getter from falling off during the use of the device, and the occurrence of device failure, damage to the device and other phenomena.
[0090] By using gold particles to assist in etching a three-dimensional thin film getter structure, a porous structure can be further prepared on the originally prepared groove or V-shaped cavity structure to increase the deposition area of the thin film getter, and the volume of the deposited getter can also be increased, thereby increasing the getter performance and service life of the thin film getter. Under the process conditions of high-temperature rapid annealing, the gold film can form evenly distributed gold particles on the side walls and base of the cavity. The gold particles on the side walls and base of the wall can be combined with the corrosive liquid to etch holes with controllable diameters ranging from nanometers to several microns on the side walls and base. The size parameters of the porous structure can be adjusted by setting the thickness of the gold-plated film and the high-temperature annealing parameters. This is an advantage that is difficult to achieve with dry etching and general wet processes. Therefore, it plays a great role in maintaining the internal vacuum of high-vacuum electronic devices and extending their service life.
[0091] Furthermore, the annealed gold particles are used for an etching process, and the holes formed by etching, especially the holes on the side walls, can effectively increase the adhesion between the getter film and the side walls and bottom substrate after the getter is deposited, thereby avoiding the getter falling off and damaging the device.
[0092] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for preparing a porous film getter structure, characterized in that: The steps include: S1, forming a protective layer on the upper and lower surfaces of the wafer, and forming a patterned photoresist layer on the protective layer on the upper surface of the wafer, and using the patterned photoresist layer as a mask to pattern the protective layer on the upper surface of the wafer to expose the wafer surface to be etched; S2, using the patterned photoresist layer as a mask, dry-etching the wafer to form a groove structure, and then removing the patterned photoresist layer; or first removing the patterned photoresist layer, using the protective layer as a mask, and wet-etching the wafer to form a groove structure; S3, forming a patterned photoresist layer in the groove structure area on the upper surface of the wafer, and forming a photoresist layer on the upper surface of the wafer outside the groove structure area to form a patterned window in the groove structure area; S4, forming a gold film on the patterned window; S5, annealing the gold-film-coated wafer at high temperature to convert the gold film into gold particles; S6, using a corrosive liquid to wet-etch the wafer after high-temperature annealing, and corroding the groove structure area into a porous structure through the catalytic effect of gold; S7. Depositing a thin film getter on the upper surface of the wafer by a photolithography stripping process.
2. The method for preparing a porous thin film getter structure according to claim 1, characterized in that: In step S2, the groove structure is one or more than two; when there is one groove structure, the groove structure constitutes a groove structure area, and when there are more than two groove structures, each groove structure and the area connecting adjacent groove structures constitute a groove structure area; when there are more than two groove structures, step S2 also includes removing the protective layer connecting adjacent groove structures after forming the groove structure.
3. The method for preparing a porous thin film getter structure according to claim 1 or 2, characterized in that: In step S5, the holding temperature of the high temperature annealing is 600-1000°C; the holding time of the high temperature annealing is 2-60min; the annealing rate of the high temperature annealing is 5-25°C / min; the heating rate of the high temperature annealing is 5-25°C / min; the size of the gold particles is 20nm-5μm.
4. The method for preparing a porous thin film getter structure according to claim 1 or 2, characterized in that: In step S1, the protective layer is one or more metal films selected from the group consisting of Ti, Pt, and Cr.
5. The method for preparing a porous thin film getter structure according to claim 1 or 2, characterized in that: In step S6, the etching solution is a mixed etching solution of hydrofluoric acid and hydrogen peroxide; the temperature of the wet etching is 25-60°C; Preferably, in the mixed etching solution, the mass fraction of the hydrofluoric acid is 5-20%, and the mass fraction of the H2O2 is 5-30%.
6. The method for preparing a porous thin film getter structure according to claim 1 or 2, characterized in that: In step S4, the thickness of the gold film is 30 to 150 nm; Step S4 specifically includes: forming a gold film on the upper surface of the wafer by evaporation, deposition or sputtering, and then removing the patterned photoresist layer in the groove structure area and the photoresist layer on the upper surface of the wafer outside the groove structure area to form a gold film on the patterned window in the groove structure area, and then cleaning the wafer.
7. A porous film getter structure, characterized in that: The method is used to prepare the wafer, comprising a wafer and a thin film getter, wherein the upper surface of the wafer has a groove structure, the inner wall of the groove structure is a porous structure, the thin film getter is arranged on the porous structure, and the thin film getter covers the porous structure.
8. The porous film getter structure according to claim 7, characterized in that: The wafer is provided with more than two groove structures, and the wafer surface connecting adjacent groove structures is a porous structure, a thin film getter is provided on the porous structure, and the thin film getter covers the porous structure.
9. The porous film getter structure according to claim 7 or 8, characterized in that: Gold particles are arranged on the bottom surface of the pores of the porous structure, and the thin film getter covers the gold particles; the size of the gold particles is 20nm to 5μm.
10. The porous film getter structure according to claim 7 or 8, characterized in that: The cross section of the groove structure is trapezoidal, V-shaped or "shape.